Snowcrystal rock material with thin-layer material distribution and preparation method of snowcrystal rock material

By adjusting the composition and process of the tile materials, the problem of insufficient aesthetics of existing tile materials has been solved, and the three-dimensional texture, translucent feeling and hair color of Xuejingyan tiles have been improved. The side layers of the product are clear, and the surface is white and transparent, which is improved. Decorative effect and quality.

CN118930237APending Publication Date: 2024-11-12HUBEI ASA CERAMIC CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983469.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult for existing ceramic tile materials to achieve three-dimensional texture, good surface permeability and good color decorative effects, and the side bottom blank and white material on the product are not layered clearly, which lacks aesthetics.

Method used

Using thin-layer fabric snow crystal rock material, by adjusting the composition ratio and particle size of the base blank, white material, base glaze and glaze, combined with press mixing and kiln sintering technology, snow crystal with extreme flatness effect is prepared. Rock tiles.

Benefits of technology

The three-dimensional texture, good surface translucent and good color effect of Xuejing Rock tiles is achieved. The bottom blank on the side of the product and the white material are layered clearly, and the appearance is as white as snow and as bright as crystal, which improves the decorative effect and quality.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930237A_ABST
    Figure CN118930237A_ABST
Patent Text Reader

Abstract

The invention provides a snow crystal rock material for thin-layer material distribution, which comprises the following raw materials in parts by weight: 70-75 parts of a bottom blank, 12-15 parts of a white material, 1-5 parts of ground glaze and 1-5 parts of polishing glaze, when the snowcrystal rock material with the thin-layer cloth is used as a preparation material of a decorative ceramic tile, a prepared snowcrystal rock ceramic tile finished product has the characteristics of three-dimensional texture, good surface transparency, good color development, white appearance, clear layering of a bottom blank and a white material on the side surface of the product, three-dimensional white material on the side surface, pure white appearance like snow, transparency like crystal and the like; and the decorative visual effect is very attractive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic tile materials, and in particular to a thin layer of snow crystal rock material and a preparation method thereof. Background Art

[0002] With the development of society, people have a better yearning for life, customers have higher and higher aesthetic requirements for interior decoration, the market demand for ceramic tile taste is becoming more and more refined, and the surface technology of ceramic tiles is colorful and diverse. In order to improve the visual effect of ceramic tiles and meet market demand, it is necessary to develop new manufacturing processes to meet the demand.

[0003] In view of this, it is necessary to provide a new type of thin layer of snow crystal rock material and a preparation method thereof to overcome the above-mentioned defects. Summary of the invention

[0004] The purpose of the present invention is to provide a thin layer of snow crystal rock material as a preparation material for decorative tiles. The prepared snow crystal rock tile product has three-dimensional texture, good surface transparency, good color, white appearance, clear stratification between the bottom blank and the white material on the side of the product, three-dimensional white material on the side, and a snow-white appearance and a crystal-like translucent appearance, and the decorative visual effect is very beautiful.

[0005] In order to achieve the above object, the present invention provides a thin layer of snow crystal rock material, which comprises, by weight:

[0006] 70-75 pieces of base stock,

[0007] 12-15 portions of white material,

[0008] 1-5 parts of base glaze,

[0009] Apply glaze 1-5 times.

[0010] Preferably, the base blank contains 18-22 parts of kaolin.

[0011] Preferably, the base blank contains 2-4 parts of bentonite.

[0012] Preferably, the base blank contains 12-18 parts of potassium-sodium feldspar.

[0013] Preferably, the base blank contains 45-55 parts of potassium feldspar.

[0014] Preferably, the base blank contains 4-6 parts of talc.

[0015] Preferably, the base blank contains 5-10 parts of bauxite.

[0016] The present invention also provides a method for preparing a thin layer of snow crystal rock material, comprising the following steps:

[0017] A. Preparation of base blank:

[0018] A1. Mix the raw materials according to the formula to obtain a mixture;

[0019] A2, dividing the mixed material obtained in step A1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling by adding water to obtain at least 2 portions of ball milled materials having different average particle sizes;

[0020] B. White material preparation:

[0021] B1. Mix the raw materials according to the formula to obtain a mixture;

[0022] B2, dividing the mixed material obtained in step B1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water to obtain at least 2 portions of ball milled materials with different average particle sizes;

[0023] C. Base glaze preparation:

[0024] C1. Mix the raw materials according to the formula to obtain a mixed material;

[0025] C2, dividing the mixture obtained in step C1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water;

[0026] D. Glaze preparation:

[0027] D1. Mix the raw materials according to the formula to obtain a mixture;

[0028] D2, dividing the mixture obtained in step D1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water;

[0029] E. Send the prepared base powder to press hopper 1, and send the white powder to press hopper 2;

[0030] F. The press machine first spreads the base material, then spreads the white material on the base material surface, and presses it into shape;

[0031] G. After drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and the semi-finished product is then applied and polished;

[0032] H. The semi-finished product is sintered in a kiln at high temperature, and then polished, edged and packaged to obtain the finished snow crystal rock material.

[0033] Preferably, the average particle size of the mixture in steps A and B is 60-180 μm; the average particle size of the mixture in steps C and D is 20-50 μm; the thickness of the white material in step E is 1.2-2 mm; the total thickness of the base and white material in step F is 10.8-11.6 mm.

[0034] Preferably, the specific sintering process described in step H is:

[0035] (i) heating the temperature to 400-500°C at a heating rate of 8-10°C / min and keeping the temperature for 5-10 min;

[0036] (ii) heating the temperature to 800-900°C at a heating rate of 6-8°C / min and keeping the temperature for 15-25 min;

[0037] (iii) heating the temperature to 1150-1250°C at a heating rate of 4-6°C / min and keeping the temperature for 10-20 min;

[0038] (iv) Rapid cooling to room temperature to complete sintering.

[0039] Compared with the prior art, the beneficial effect lies in that the purpose of the present invention is to provide a thin layer of snow crystal rock material as a preparation material for decorative tiles. The prepared snow crystal rock tile product has three-dimensional texture, good surface transparency, good color, white appearance, clear stratification between the bottom blank and the white material on the side of the product, the three-dimensional white material on the side, the appearance is as white as snow, and the appearance is as translucent as crystal, and the decorative effect is very beautiful.

[0040] Other features and advantages of the present invention will be set forth in the following description, and part will be apparent from the description, or can be understood by implementation of the present invention. Features and advantages of the present invention can be realized and obtained by the elements and combinations specifically pointed out in the appended application scope. These and other features of the present invention will become more clearly understood according to the following description and the appended claims, or can be understood by the implementation of the embodiments described in the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The present invention provides a flow chart of a method for preparing a thin layer of snow crystal rock material. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and beneficial technical effect of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and specific implementation methods. It should be understood that the specific implementation methods described in this specification are only for explaining the present invention, not for limiting the present invention.

[0043] The present invention provides a thin layer of snow crystal rock material, which comprises, by weight:

[0044] 70-75 parts of base stock: (including 18-22 parts of kaolin, 2-4 parts of bentonite, 12-18 parts of potassium-sodium feldspar, 45-55 parts of potassium feldspar, 4-6 parts of talc, 5-10 parts of bauxite),

[0045] 12-15 parts of white material: (including 20-30 parts of potassium-sodium feldspar, 38-48 parts of potassium feldspar, 26-32 parts of kaolin, 3-5 parts of talc, and 2-3 parts of wollastonite),

[0046] Base glaze 1-5 parts: (including 33-40 parts of albite, 4-8 parts of nepheline syenite, 14-18 parts of aluminum nepheline, 15-20 parts of quartz powder, 13-16 parts of high white alumina, 1-3 parts of dolomite powder, 7-10 parts of kaolin, 1-6 parts of calcined talc powder, 6-9 parts of zirconium silicate powder),

[0047] Glaze 1-5 parts: (including 35-42 parts of albite, 6-8 parts of potassium feldspar, 4-6 parts of active zinc oxide, 1-3 parts of quartz powder, 8-12 parts of dolomite powder, 6-8 parts of kaolin, 6-10 parts of calcined talc, 4-7 parts of calcite powder, 2-4 parts of strontium carbonate, 1-3 parts of composite strontium, 2-4 parts of calcined clay powder, 5-7 parts of 5211 frit powder).

[0048] The present invention utilizes four layers of raw materials with different expansion coefficients, namely base blank, white material, base glaze and polishing glaze, and fully analyzes and adjusts them to achieve an extremely smooth effect of the thin layer of snow crystal rock material.

[0049] The present invention utilizes the mutual cooperation of the components in the process, so that the thin layer of snow crystal rock material can improve the product quality and appearance when used in production. Moreover, the various layers of the present invention cooperate with each other, so that the blank and glaze can be combined more smoothly during the firing process, the glaze surface has better color and transparency, and the layer has a stronger three-dimensional effect.

[0050] The key technology of the process of the present invention is the control of the expansion coefficient of the base blank and the white material, and the research and development of the base glaze and polishing glaze formula is innovative and groundbreaking, and the research and development is very challenging; for different combinations of multiple layers, it is very difficult to control the brick shape with extreme flatness; at the same time, in terms of molding, it is very difficult to control the thickness uniformity of the two layers of blanks; during the molding process, it is very difficult to control the mixing of the press.

[0051] In the snow crystal rock material of the thin layer cloth provided by the present invention, the base blank is 70-75 parts, for example, it can be 70 parts, 71 parts, 72 parts, 73 parts, 74 parts or 75 parts, but is not limited to the listed values. Other values ​​not listed in the numerical range are also applicable, preferably 72-75 parts.

[0052] In the base blank provided by the present invention, kaolin: 18-22 parts, for example, it can be 18 parts, 19 parts, 20 parts, 21 parts or 22 parts, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 18-20 parts.

[0053] In the base blank provided by the present invention, bentonite: 2-4 parts, for example, it can be 2 parts, 2.5 parts, 3 parts, 3.5 parts or 4 parts, but it is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 2-3 parts.

[0054] In the base blank provided by the present invention, potassium-sodium feldspar: 12-18 parts, for example, it can be 12 parts, 13 parts, 14 parts, 15 parts, 16 parts, 17 parts or 18 parts, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 14-17 parts.

[0055] In the base blank provided by the present invention, potassium feldspar: 45-55 parts, for example, it can be 45 parts, 46 parts, 47 parts, 48 ​​parts, 49 parts, 50 parts or 51 parts, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 46-50 parts.

[0056] In the base blank provided by the present invention, talc is 4-6 parts, for example, it can be 4 parts, 4.5 parts, 5 parts, 5.5 parts or 6 parts, but it is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 4-5 parts.

[0057] In the base blank provided by the present invention, bauxite: 5-10 parts, for example, it can be 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 9.5 parts or 10 parts, but is not limited to the listed values. Other unlisted values ​​within the numerical range are also applicable, preferably 8-10 parts.

[0058] In the snow crystal rock material of the thin layer cloth provided by the present invention, the white material: 12-15 parts, for example, it can be 12 parts, 13 parts, 14 parts or 15 parts, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 12-14 parts. The white material formula components are calculated by weight, and the proportion components are the same as the base blank, and are not listed here one by one.

[0059] In the snow crystal rock material of the thin layer of cloth provided by the present invention, the base glaze: 1-5 parts, for example, it can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 4 parts or 5 parts, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 1-4 parts. The base glaze formula components are calculated by weight, and the proportion components are the same as the base blank, and are not listed here one by one.

[0060] In the snow crystal rock material of the thin layer cloth provided by the present invention, the glaze is 1-5 parts, for example, it can be 1 part, 1.5 parts, 2 parts, 2.5 parts, 3 parts, 4 parts or 5 parts, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable, preferably 1-4 parts. The glaze formula components are calculated by weight, and the proportion components are the same as the base blank, and are not listed here one by one.

[0061] Please refer to the figure, the present invention also provides a method for preparing a thin layer of snow crystal rock material, the preparation method comprising the following steps:

[0062] A. Preparation of base blank:

[0063] (1) mixing raw materials according to formula amounts to obtain a mixed material;

[0064] (2) dividing the mixed material obtained in step (1) into at least two powders, and respectively subjecting the at least two powders to ball milling with water to obtain at least two ball milled materials with different average particle sizes;

[0065] (3) The slurry obtained in step (2) is sprayed and granulated to obtain desired powders of different particle sizes, which are stored for later use.

[0066] B. White material preparation:

[0067] (1) mixing raw materials according to formula amounts to obtain a mixed material;

[0068] (2) dividing the mixed material obtained in step (1) into at least two powders, and respectively subjecting the at least two powders to ball milling with water to obtain at least two ball milled materials with different average particle sizes;

[0069] (3) The slurry obtained in step (2) is sprayed and granulated to obtain desired powders of different particle sizes, which are stored for later use.

[0070] C. Base glaze preparation:

[0071] (1) mixing raw materials according to formula amounts to obtain a mixed material;

[0072] (2) Dividing the mixed material obtained in step (1) into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water to obtain at least 2 portions of ball milled materials with different average particle sizes, which are stored for later use.

[0073] D. Glaze preparation:

[0074] (1) mixing raw materials according to formula amounts to obtain a mixed material;

[0075] (2) Dividing the mixed material obtained in step (1) into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water to obtain at least 2 portions of ball milled materials with different average particle sizes, which are stored for later use.

[0076] E. Send the prepared base powder to press hopper 1, and send the white powder to press hopper 2;

[0077] F. The press machine first spreads the base material, then spreads the white material on the base material surface, and presses it into shape;

[0078] G. After drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and the semi-finished product is then applied and polished;

[0079] H. The semi-finished product is sintered in a kiln at high temperature, and then polished, edged and packaged to obtain the finished snow crystal rock material.

[0080] The finished snow crystal rock tile prepared in the embodiment of the present invention has the characteristics of three-dimensional texture, good surface transparency, good color, white appearance, clear stratification between the bottom blank and the white material on the side of the product, three-dimensional white material on the side, snow-white appearance, and crystal-like translucent appearance.

[0081] Preferably, the average particle size of the mixture in steps A and B is 60-180 μm.

[0082] Preferably, the average particle size of the mixture in steps C and D is 20-50 μm.

[0083] Preferably, the thickness of the white material in step E is 1.2-2 mm, and the total thickness of the base blank and the white material in step F is 10.8-11.6 mm.

[0084] The specific process of sintering described in step H is:

[0085] (i) heating the temperature to 400-500°C at a heating rate of 8-10°C / min and keeping the temperature for 5-10 min;

[0086] (ii) heating the temperature to 800-900°C at a heating rate of 6-8°C / min and keeping the temperature for 15-25 min;

[0087] (iii) heating the temperature to 1150-1250°C at a heating rate of 4-6°C / min and keeping the temperature for 10-20 min;

[0088] (iv) Rapid cooling to room temperature to complete sintering.

[0089] During the sintering process, the holding time of step (ii) is 5-10 min, for example, it can be 5 min, 6 min, 7 min, 8 min, 9 min or 10 min, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable. During the sintering process, the heating rate of step (iii) is 4-6°C / min, for example, it can be 4°C / min, 4.5°C / min, 5°C / min, 5.5°C / min or 6°C / min, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0090] During the sintering process, the heating temperature of step (iii) is 1150-1250°C, for example, 1150°C,

[0091] 1160°C, 1170°C, 1180°C, 1190°C, 1200°C, 1210°C, 1220°C, 1230°C, 1240°C or 1250°C, but not limited to the listed values, other unlisted values ​​within the numerical range are also applicable.

[0092] During the sintering process, the holding time of step (iii) is 20-60 min, for example, 20 min, 30 min, 40 min, 45 min, 500 min, 55 min or 60 min, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0093] Example 1

[0094] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 18 parts of kaolin, 2 parts of bentonite, 12 parts of potassium feldspar, 45 parts of potassium feldspar, 4 parts of talc, and 5 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0095] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 20 parts of potassium feldspar, 38 parts of potassium feldspar, 26 parts of kaolin, 3 parts of talc, and 2 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0096] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 33 parts of albite, 4 parts of nepheline syenite, 14 parts of aluminum nepheline, 15 parts of quartz powder, 13 parts of high white alumina, 1 part of dolomite powder, 7 parts of kaolin, 1 part of calcined talc powder, and 6 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0097] Preparation of polishing glaze: Mix raw materials according to the formula amount of 5 parts (including 35 parts of albite, 6 parts of potassium feldspar, 4 parts of active zinc oxide, 1 part of quartz powder, 8 parts of dolomite powder, 6 parts of kaolin, 6 parts of calcined talc powder, 4 parts of calcite powder, 2 parts of strontium carbonate, 1 part of composite strontium, 2 parts of calcined clay powder, and 5 parts of 5211 frit powder) to obtain a mixture;

[0098] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain at least two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0099] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0100] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0101] The finished product of the snow crystal rock material prepared in Example 1 has three-dimensional texture, good surface transparency, good color, and white appearance. The bottom blank and the white material on the side of the product are clearly layered, the white material is three-dimensional on the side, the appearance is as white as snow, and the appearance is as transparent as crystal.

[0102] Example 2

[0103] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 20 parts of kaolin, 2.5 parts of bentonite, 13 parts of potassium feldspar, 46 parts of potassium feldspar, 4.5 parts of talc, and 6 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0104] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 21 parts of potassium-sodium feldspar, 39 parts of potassium feldspar, 27 parts of kaolin, 3.5 parts of talc, and 2.2 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0105] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 34 parts of albite, 4.5 parts of nepheline syenite, 15 parts of aluminum nepheline, 16 parts of quartz powder, 14 parts of high white alumina, 1.5 parts of dolomite powder, 7 parts of kaolin, 2 parts of calcined talc, and 7 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0106] Preparation of polishing glaze: Mix raw materials according to 5 parts of formula (including 36 parts of albite, 6.5 parts of potassium feldspar, 4.5 parts of active zinc oxide, 1.5 parts of quartz powder, 9 parts of dolomite powder, 6.5 parts of kaolin, 7 parts of calcined talc powder, 5 parts of calcite powder, 2.5 parts of strontium carbonate, 1.5 parts of composite strontium, 2.5 parts of calcined clay powder, and 5.5 parts of 5211 frit powder) to obtain a mixture;

[0107] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain at least two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0108] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0109] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0110] Example 3

[0111] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 20.5 parts of kaolin, 3 parts of bentonite, 14 parts of potassium feldspar, 47 parts of potassium feldspar, 5 parts of talc, and 7 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0112] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 22 parts of potassium feldspar, 40 parts of potassium feldspar, 28 parts of kaolin, 4 parts of talc, and 2.5 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0113] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 35 parts of albite, 5 parts of nepheline syenite, 16 parts of chalcanthite, 17 parts of quartz powder, 14.5 parts of high white alumina, 1.8 parts of dolomite powder, 7.5 parts of kaolin, 3 parts of calcined talc, and 7.5 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0114] Preparation of polishing glaze: Mix raw materials according to 5 parts of formula (including 36 parts of albite, 6.5 parts of potassium feldspar, 4.5 parts of active zinc oxide, 1.5 parts of quartz powder, 9 parts of dolomite powder, 6.5 parts of kaolin, 7 parts of calcined talc powder, 5 parts of calcite powder, 2.5 parts of strontium carbonate, 1.5 parts of composite strontium, 2.5 parts of calcined clay powder, and 5.5 parts of 5211 frit powder) to obtain a mixture;

[0115] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0116] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0117] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0118] Example 4

[0119] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 21 parts of kaolin, 3.5 parts of bentonite, 15 parts of potassium feldspar, 49 parts of potassium feldspar, 5.5 parts of talc, and 8 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0120] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 23 parts of potassium-sodium feldspar, 41 parts of potassium feldspar, 29 parts of kaolin, 4.5 parts of talc, and 2.5 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0121] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 36 parts of albite, 6 parts of nepheline syenite, 17 parts of chalcanthite, 18 parts of quartz powder, 15 parts of high white alumina, 2 parts of dolomite powder, 8 parts of kaolin, 4 parts of calcined talc, and 8 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0122] Preparation of polishing glaze: Mix raw materials according to 5 parts of the formula (including 37 parts of albite, 7 parts of potassium feldspar, 5 parts of active zinc oxide, 2 parts of quartz powder, 10 parts of dolomite powder, 7 parts of kaolin, 8 parts of calcined talc powder, 6 parts of calcite powder, 3 parts of strontium carbonate, 2 parts of composite strontium, 3 parts of calcined clay powder, and 6 parts of 5211 frit powder) to obtain a mixture;

[0123] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0124] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0125] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0126] Example 5

[0127] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 21.5 parts of kaolin, 3.5 parts of bentonite, 16 parts of potassium feldspar, 50 parts of potassium feldspar, 5.5 parts of talc, and 9 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0128] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 24 parts of potassium feldspar, 42 parts of potassium feldspar, 30 parts of kaolin, 4.5 parts of talc, and 2.5 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0129] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 38 parts of albite, 7 parts of nepheline syenite, 17.5 parts of chalcanalite, 19 parts of quartz powder, 15.5 parts of high white alumina, 2.5 parts of dolomite powder, 9 parts of kaolin, 5 parts of calcined talc, and 8.5 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0130] Preparation of polishing glaze: Mix raw materials according to 5 parts of the formula (including 38 parts of albite, 7.5 parts of potassium feldspar, 5.5 parts of active zinc oxide, 2.5 parts of quartz powder, 11 parts of dolomite powder, 7.5 parts of kaolin, 9 parts of calcined talc powder, 6.5 parts of calcite powder, 3.5 parts of strontium carbonate, 2.5 parts of composite strontium, 3.5 parts of calcined clay powder, and 6.5 parts of 5211 frit powder) to obtain a mixture;

[0131] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0132] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0133] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0134] Example 6

[0135] Preparation of base blank: Mix raw materials according to the formula amount of 75 parts (including 22 parts of kaolin, 4 parts of bentonite, 18 parts of potassium feldspar, 55 parts of potassium feldspar, 6 parts of talc, and 10 parts of bauxite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0136] Preparation of white material: Mix raw materials according to the formula amount of 15 parts (including 30 parts of potassium feldspar, 48 parts of potassium feldspar, 32 parts of kaolin, 5 parts of talc, and 3 parts of wollastonite) to obtain a mixture; divide the obtained mixture into 2 parts of powder, and ball-mill the 2 parts of powder respectively by adding water to obtain 2 parts of ball-milled materials with different average particle sizes.

[0137] Preparation of base glaze: Mix raw materials according to the formula amount of 5 parts (including 40 parts of albite, 8 parts of nepheline syenite, 18 parts of chalcanthite, 20 parts of quartz powder, 16 parts of high white alumina, 3 parts of dolomite powder, 10 parts of kaolin, 6 parts of calcined talc, and 9 parts of zirconium silicate powder) to obtain a mixture; divide the obtained mixed raw materials into 2 parts of powder, and ball-mill the 2 parts of powder separately by adding water to obtain 2 parts of ball-milled materials with different average particle sizes, and store them for later use.

[0138] Preparation of polishing glaze: Mix raw materials according to 5 parts of the formula (including 42 parts of albite, 8 parts of potassium feldspar, 6 parts of active zinc oxide, 3 parts of quartz powder, 12 parts of dolomite powder, 8 parts of kaolin, 10 parts of calcined talc powder, 7 parts of calcite powder, 4 parts of strontium carbonate, 3 parts of composite strontium, 4 parts of calcined clay powder, and 7 parts of 5211 frit powder) to obtain a mixture;

[0139] The obtained mixture is divided into two portions of powders, and the two portions of powders are respectively ball-milled with water to obtain two portions of ball-milled materials with different average particle sizes, which are stored for later use.

[0140] The prepared base powder is sent to the first hopper of the press, and the white powder is sent to the second hopper of the same press. The press first spreads the base, and then spreads the white powder on the surface of the base, and presses it into shape; after drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and then the semi-finished product is glazed and polished to obtain the semi-finished product;

[0141] The semi-finished products are fired in a kiln at high temperature, and then polished, edged, graded and packaged to obtain the finished snow crystal rock material.

[0142] When the snow crystal rock material prepared in Examples 1-6 is used as the material of the decorative tiles, the flatness, light transmittance and wear resistance of the decorative tiles of the comparative example are tested, wherein the flatness is tested using a gloss meter and the light transmittance is tested using a light transmittance meter; the measurement method of the national 3C standard is carried out in accordance with the method specified in GB,

[0143] The test results are shown in Table 1:

[0144]

[0145] It can be seen from Table 1 that when the snow crystal rock prepared in Examples 1-6 of the present invention is used as a material for decorative tiles, the warping of the decorative tiles made therefrom is significantly smaller than that of traditional decorative tiles (the smaller the warping, the higher the flatness), the light transmittance of the decorative tiles made therefrom is lower than that of traditional decorative tiles, the wear amount of the decorative tiles made therefrom is significantly smaller than that of traditional decorative tiles, and the strength of the decorative tiles made therefrom is slightly higher than that of traditional decorative tiles, indicating that the comprehensive performance of the snow crystal rock prepared in Examples 1-6 of the present invention as a material for decorative tiles is better than that of traditional decorative tiles.

[0146] In summary, the snow crystal rock material made of thin layer cloth in Examples 1-6 of the present invention, when used for porcelain glazed tiles, has porcelain glazed tiles that meet the national 3C performance, and has high transparency and high temperature resistance and wear resistance. The snow crystal rock material made of thin layer cloth described in the present invention is widely used and can be widely used in various specifications, such as: 900*1800, 750*1500, 600*1200, 800*800, 800*1300, etc.; at the same time, it can be widely used in various fields, such as: floor tiles, wall tiles, background walls, outdoor tiles, etc.; and the prepared porcelain glazed tiles have three-dimensional texture, good surface transparency, good color, white appearance, the bottom blank and white material on the side of the product are clearly layered, the side shows three-dimensional white material, the appearance is white as snow, and it is known for its translucent appearance like crystal.

[0147] The present invention is not limited to what is described in the specification and implementation modes, and therefore additional advantages and modifications can be easily realized by those skilled in the art. Therefore, without departing from the spirit and scope of the general concept defined by the claims and their equivalents, the present invention is not limited to the specific details, representative devices, and illustrative examples shown and described herein.

Claims

1. A thin layer of snow crystal rock material, measured by weight, characterized in that: The constituent raw materials include: 70-75 pieces of base stock, 12-15 portions of white material, 1-5 parts of base glaze, Apply glaze 1-5 times.

2. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The base blank contains 18-22 parts of kaolin.

3. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The bottom blank contains 2-4 parts of bentonite.

4. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The base blank contains 12-18 parts of potassium-sodium feldspar.

5. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The base blank contains 45-55 parts of potassium feldspar.

6. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The base blank contains 4-6 parts of talc.

7. The snow crystal rock material of the thin layer of cloth as claimed in claim 1, characterized in that: The bottom blank contains 5-10 parts of bauxite.

8. A method for preparing the snow crystal rock material for the thin layer cloth as claimed in any one of claims 1 to 7, characterized in that: The steps include: A. Preparation of base blank: A1. Mix the raw materials according to the formula to obtain a mixture; A2, dividing the mixed material obtained in step A1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling by adding water to obtain at least 2 portions of ball milled materials having different average particle sizes; B. White material preparation: B1. Mix the raw materials according to the formula to obtain a mixture; B2, dividing the mixed material obtained in step B1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water to obtain at least 2 portions of ball milled materials with different average particle sizes; C. Base glaze preparation: C1. Mix the raw materials according to the formula to obtain a mixed material; C2, dividing the mixture obtained in step C1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water; D. Glaze preparation: D1. Mix the raw materials according to the formula to obtain a mixture; D2, dividing the mixture obtained in step D1 into at least 2 portions of powder, and respectively subjecting the at least 2 portions of powder to ball milling with water; E. Send the prepared base powder to press hopper 1, and send the white powder to press hopper 2; F. The press machine first spreads the base material, then spreads the white material on the base material surface, and presses it into shape; G. After drying and forming the double-layer body to a moisture content of less than 0.5%, the base glaze is applied, the pattern is printed by an inkjet printer, and the semi-finished product is then applied and polished; H. The semi-finished product is sintered in a kiln at high temperature, and then polished, edged and packaged to obtain the finished snow crystal rock material.

9. The method for preparing the snow crystal rock material for the thin layer of cloth according to claim 8, characterized in that: The average particle size of the mixture in steps A and B is 60-180 μm; the average particle size of the mixture in steps C and D is 20-50 μm; the thickness of the white material in step E is 1.2-2 mm; the total thickness of the base and white material in step F is 10.8-11.6 mm.

10. The method for preparing the snow crystal rock material for the thin layer of cloth according to claim 8, characterized in that: The specific process of sintering described in step H is: (i) heating the temperature to 400-500°C at a heating rate of 8-10°C / min and keeping the temperature for 5-10 min; (ii) heating to 800-900°C at a heating rate of 6-8°C / min and keeping at that temperature for 15-25 min; (iii) heating the temperature to 1150-1250°C at a rate of 4-6°C / min and maintaining the temperature for 10-20 min; (iv) Rapid cooling to room temperature to complete sintering.