Organic waste liquid absorbing substance and preparation method thereof
A hypercrosslinked porous microsphere adsorbent material was prepared by secondary polymerization of monomer A, cycloalkane ester monomer B, and straight-chain alkane ester monomer C, and by free radical reaction controlled by 1,1-diphenylethylene. This method solved the adsorption problem of high-viscosity organic waste liquid and achieved safe and efficient treatment.
Patent Information
- Application Number
- CN202411036220.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing nuclear waste liquid absorbents are difficult to effectively adsorb high-viscosity liquid scintillation fluid and lubricating oil, resulting in high adsorption resistance and making it impossible to efficiently treat high-viscosity organic waste liquids.
A high-viscosity organic waste liquid adsorbent material with a hypercrosslinked porous microsphere structure was prepared by secondary polymerization of monomer A, cycloalkane ester monomer B, and straight-chain alkane ester monomer C, combined with the control agent 1,1-diphenylethylene to control the free radical reaction.
The prepared adsorbent material can efficiently adsorb high-viscosity organic waste liquid. After high-temperature pyrolysis, the material reduces its volume without producing harmful gases, thus achieving safe and efficient treatment of high-viscosity organic waste liquid.
Smart Images

Figure CN118930705A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nuclear waste treatment, in particular to an organic waste liquid absorbing material and a preparation method thereof. Background Art
[0002] Nuclear waste generally refers to the radioactive waste that is no longer needed after nuclear fuel production, processing and nuclear reactors. It also specifically refers to the spent fuel of nuclear reactors. After reprocessing to recover usable nuclear materials such as plutonium 239, the remaining uranium-238 and other radioactive waste that are no longer needed. The normal operation, maintenance and decommissioning of nuclear facilities produce a large amount of radioactive organic waste liquid, such as TBP / kerosene extractant, liquid scintillator, lubricating oil, etc. The radioactive organic waste liquid contains radioactive nuclides such as uranium, plutonium, cerium, strontium, cesium and cobalt, and has the characteristics of being flammable, explosive, volatile, easy to thermally decompose, easy to biodegrade and irradiate. Therefore, the safe and efficient treatment of radioactive organic waste liquid is an important guarantee for the decommissioning of nuclear facilities.
[0003] In order to avoid environmental pollution during the discharge of nuclear waste, organic waste liquid absorbents are used to effectively absorb and treat nuclear waste liquid. However, the existing nuclear waste liquid absorbents still have the following technical problems when used:
[0004] For low-viscosity organic waste liquid, the van der Waals force between the lipophilic group and the organic waste liquid is the main mass transfer force in the initial stage of adsorption, and then the stretching and swelling of the polymer chain segments complete the adsorption process. However, for high-viscosity liquid scintillator and lubricating oil, general adsorption materials cannot be used due to the large adsorption resistance.
[0005] Therefore, an organic waste liquid absorbing material and a preparation method are proposed to solve the above-mentioned problems. Summary of the invention
[0006] The object of the present invention is to provide an organic waste liquid absorbing material and a preparation method thereof to solve the problems raised in the above background technology.
[0007] To achieve the above-mentioned purpose, the present invention provides the following technical scheme: an organic waste liquid absorption material, the specific raw material components of the organic waste liquid absorption material include: 1-20 parts of monomer A, 1-50 parts of cycloalkane ester monomer B, 1-50 parts of linear alkane ester monomer C, 0.1-10 parts of initiator, 0.1-10 parts of control agent, 0.1-10 parts of polyvinyl alcohol aqueous solution and 10-50 parts of cross-linking agent.
[0008] Preferably, the concentration of the polyvinyl alcohol aqueous solution is 0.1-2%.
[0009] Preferably, the monomer A is a combination of one or more of 4-tert-butylstyrene, α-methylstyrene, β-methylstyrene and 4-methylstyrene.
[0010] Preferably, the cycloalkane ester monomer B is one or a combination of tetrahydrofuran acrylate and dicyclopentyl acrylate.
[0011] Preferably, the linear alkane ester monomer C is a combination of one or more of butyl acrylate, dodecyl acrylate and hexadecyl acrylate.
[0012] Preferably, the initiator is benzoyl peroxide; the crosslinking agent is divinylbenzene; and the control agent is 1,1-diphenylethylene.
[0013] A method for preparing an organic waste liquid absorbing material as claimed in any one of claims 1 to 6, wherein the specific steps of the method for preparing an organic waste liquid absorbing material are as follows:
[0014] Step 1, pouring a polyvinyl alcohol aqueous solution into a container, and adding monomer A, an initiator, and a control agent into the polyvinyl alcohol aqueous solution, stirring it for 2-3 minutes using a stirring device, stirring and mixing it evenly, heating it by a heating device, raising the temperature of the mixed substance to 70-90 degrees Celsius, and starting to react when the temperature reaches the range, controlling the reaction time to 1-2 hours, and when the reaction is completely completed, starting to cool to room temperature to obtain a prepolymer containing a linear styrene hard segment;
[0015] Step 2, pouring the product obtained in step 1 into a container, and pouring the cycloalkane ester monomer B, the linear alkane ester monomer C, the initiator, and the crosslinking agent into the container, using a stirring device to continuously mix and stir for 1-2 minutes until the mixture is uniformly stirred, using a heating device to heat the mixture to raise the temperature of the mixed liquid to 70-90 degrees Celsius, and when the temperature rises to the range, starting the reaction, the reaction time is controlled to be 5-6 hours, until the reaction is completed, to obtain a hyper-crosslinked structure copolymer containing a hard segment and a soft segment;
[0016] Step three, cool the product obtained in step two to room temperature, filter it using a filtering device, and then wash it with deionized water. After washing, use a drying device to dry it, adjust the drying temperature to 40-80 degrees Celsius, and the drying time to 2-20 hours to obtain a high-viscosity organic waste liquid adsorption material with a super-cross-linked porous microsphere structure.
[0017] Compared with the prior art, the present invention has the following beneficial effects:
[0018] The present invention innovatively adopts the pre-reaction of monomer A with large steric hindrance to prepare long skeleton segments; adopts the secondary polymerization of monomers B and C to jointly adjust the microstructure of the adsorption material; adopts the control agent 1,1-diphenylethylene to control the secondary polymerization of free radical reaction; and innovatively proposes a method for adjusting the pore size through segment design to prepare a high-viscosity radioactive organic waste liquid adsorption material, and the material has a high volume reduction (weight) ratio after high-temperature pyrolysis and does not produce harmful gases. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 The surface morphology and internal pore size state diagram of the adsorption material prepared in Examples 1-4;
[0020] A: Example 1; B: Example 2; C: Example 3; D: Example 4.
[0021] Figure 2 Product photos of the adsorption materials prepared in Examples 1-4;
[0022] A: Example 1; B: Example 2; C: Example 3; D: Example 4. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] In the description of the present invention, it is necessary to understand that the terms "upper", "lower", "front", "back", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0025] See also Figure 1 , the present invention provides a technical solution:
[0026] An organic waste liquid absorbing material, the specific raw material components of the organic waste liquid absorbing material include: 1-20 parts of monomer A, 1-50 parts of cycloalkane ester monomer B, 1-50 parts of straight-chain alkane ester monomer C, 0.1-10 parts of initiator, 0.1-10 parts of control agent, 0.1-10 parts of polyvinyl alcohol aqueous solution and 10-50 parts of crosslinking agent.
[0027] The concentration of the polyvinyl alcohol aqueous solution is 0.1-2%.
[0028] The monomer A is a combination of one or more of 4-tert-butylstyrene, α-methylstyrene, β-methylstyrene and 4-methylstyrene.
[0029] The cycloalkane ester monomer B is one or a combination of tetrahydrofuran acrylate and dicyclopentyl acrylate.
[0030] The linear alkane ester monomer C is a combination of one or more of butyl acrylate, dodecyl acrylate and hexadecyl acrylate.
[0031] The initiator is benzoyl peroxide; the crosslinking agent is divinylbenzene; and the control agent is 1,1-diphenylethylene.
[0032] A method for preparing an organic waste liquid absorbing material as claimed in any one of claims 1 to 6, wherein the specific steps of the method for preparing an organic waste liquid absorbing material are as follows:
[0033] Step 1, pouring a polyvinyl alcohol aqueous solution into a container, and adding monomer A, an initiator, and a control agent into the polyvinyl alcohol aqueous solution, stirring it for 2-3 minutes using a stirring device, stirring and mixing it evenly, heating it by a heating device, raising the temperature of the mixed substance to 70-90 degrees Celsius, and starting to react when the temperature reaches the range, controlling the reaction time to 1-2 hours, and when the reaction is completely completed, starting to cool to room temperature to obtain a prepolymer containing a linear styrene hard segment;
[0034] Step 2, pouring the product obtained in step 1 into a container, and pouring the cycloalkane ester monomer B, the linear alkane ester monomer C, the initiator, and the crosslinking agent into the container, using a stirring device to continuously mix and stir for 1-2 minutes until the mixture is uniformly stirred, using a heating device to heat the mixture to raise the temperature of the mixed liquid to 70-90 degrees Celsius, and when the temperature rises to the range, starting the reaction, the reaction time is controlled to be 5-6 hours, until the reaction is completed, to obtain a hyper-crosslinked structure copolymer containing a hard segment and a soft segment;
[0035] Step three, cool the product obtained in step two to room temperature, filter it using a filtering device, and then wash it with deionized water. After washing, use a drying device to dry it, adjust the drying temperature to 40-80 degrees Celsius, and the drying time to 2-20 hours to obtain a high-viscosity organic waste liquid adsorption material with a super-cross-linked porous microsphere structure.
[0036] Embodiment 1:
[0037] 5 g of monomer α-methylstyrene, 5 g of monomer butyl acrylate, 5 g of monomer tetrahydrofuran acrylate, 0.5 g of crosslinking agent divinylbenzene, and 0.1 g of initiator benzoyl peroxide were added to 100 g of 1% polyvinyl alcohol aqueous solution, and the mixture was heated to 85° C. at a speed of 280 r / min for 6 h; then the mixture was cooled to room temperature with stirring, filtered, washed and dried to obtain a spherical adsorption material with a smooth surface ( Figure 1 A).
[0038] 10 g of the adsorbent material was placed in a sample bottle, and machine oil (Calvo L-HM46, kinematic viscosity: 48.71 mm2 / s, viscosity index: 97) was added in a mass ratio of 1:1. It was observed that the machine oil liquid could not be completely adsorbed;
[0039] Embodiment 2:
[0040] The reaction of Example 1 was carried out in two steps: first, 5 g of the monomer α-methylstyrene, 0.1 g of the initiator, and 0.01 g of the control agent were added to 100 g of a 1% aqueous solution of polyvinyl alcohol, and the mixture was stirred at a speed of 280 r / min and heated to 85°C for reaction for 0.5 h; then stirred and cooled to room temperature. Then, 5 g of the monomer butyl acrylate, 5 g of the monomer tetrahydrofuran acrylate, and 0.5 g of the crosslinking agent divinyl were added to the mixture, and the mixture was heated to 85°C and reacted for 6 h. After filtering and drying, a super-crosslinked spherical adsorption material with a microporous structure ( Figure 1 B).
[0041] Take 10g of the adsorbent material and place it in a sample bottle. Add machine oil (Calvo L-HM46, kinematic viscosity: 48.71mm2 / s, viscosity index: 97) at a ratio of 1:1. Leave it to stand and observe that the machine oil is completely adsorbed in about 23 minutes. Take out some of the material and place it on filter paper to press. No exudate is observed on the filter paper surface.
[0042] Embodiment 3:
[0043] The monomers in Example 2 were changed: 2.5 g of α-methylstyrene, 2.5 g of 4-tert-butylstyrene, 0.1 g of initiator, and 0.01 g of control agent were added to 100 g of 1% polyvinyl alcohol aqueous solution, stirred at a speed of 280 r / min, heated to 85°C for reaction for 0.5 h; then stirred and cooled to room temperature. Then, 5 g of dicyclopentyl acrylate, 5 g of tetradecyl acrylate, and 0.5 g of divinyl crosslinker were added to the mixture, heated to 85°C for reaction for 6 h, filtered and dried to obtain a super-crosslinked spherical adsorption material with a microporous structure ( Figure 1 C).
[0044] Take 10g of the adsorbent material and place it in a sample bottle. Add machine oil (Calvo L-HM46, kinematic viscosity: 48.71mm2 / s, viscosity index: 97) in a ratio of 1:1. Leave it to stand and observe that the machine oil is completely adsorbed in about 19 minutes. Take out some of the material and place it on filter paper to press. No exudate is observed on the surface of the filter paper.
[0045] Embodiment 4:
[0046] The first step reaction time of Example 3 was extended: 2.5 g of monomer α-methylstyrene, 2.5 g of 4-tert-butylstyrene, 0.1 g of initiator, and 0.01 g of control agent were added to 100 g of 1% polyvinyl alcohol aqueous solution, stirred at a speed of 280 r / min and heated to 85°C for 1 hour; then stirred and cooled to room temperature. Then, 5 g of monomer dicyclopentyl acrylate, 5 g of monomer tetradecyl acrylate, and 0.5 g of crosslinking agent divinyl were added to the mixed solution, and the temperature was raised to 85°C for 6 hours. After filtering and drying, a super-crosslinked spherical adsorption material with a microporous structure ( Figure 1 D).
[0047] Take 10g of the adsorbent material and put it in a sample bottle, add lubricating oil in a ratio of 1:1, and leave it to stand for about 15 minutes until the machine oil is completely adsorbed. Take out some of the material and put it on filter paper to press it, and no seepage is observed on the filter paper surface.
[0048] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. For those skilled in the art, it is obvious that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention; therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is limited by the attached claims rather than the above description. Therefore, it is intended to include all changes within the meaning and scope of the equivalent elements of the claims in the present invention, and any figure marks in the claims should not be regarded as limiting the claims involved.
[0049] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An organic waste liquid absorbing material, It is characterized in that The specific raw material components of the organic waste liquid absorption material include: 1-20 parts of monomer A, 1-50 parts of cycloalkane ester monomer B, 1-50 parts of linear alkane ester monomer C, 0.1-10 parts of initiator, 0.1-10 parts of control agent, 0.1-10 parts of polyvinyl alcohol aqueous solution and 10-50 parts of crosslinking agent.
2. The organic waste liquid absorbing material according to claim 1, Features: The concentration of the polyvinyl alcohol aqueous solution is 0.1-2%.
3. The organic waste liquid absorbing material according to claim 1, Features: The monomer A is a combination of one or more of 4-tert-butylstyrene, α-methylstyrene, β-methylstyrene and 4-methylstyrene.
4. The organic waste liquid absorbing material according to claim 1, Features: The cycloalkane ester monomer B is one or a combination of tetrahydrofuran acrylate and dicyclopentyl acrylate.
5. The organic waste liquid absorbing material according to claim 1, Features: The linear alkane ester monomer C is a combination of one or more of butyl acrylate, dodecyl acrylate and hexadecyl acrylate.
6. The organic waste liquid absorbing material according to claim 1, Features: The initiator is benzoyl peroxide; the crosslinking agent is divinylbenzene; and the control agent is 1,1-diphenylethylene.
7. A method for preparing an organic waste liquid absorbing material as claimed in any one of claims 1 to 6, Features: The specific steps of the preparation method of the organic waste liquid absorption material are as follows: Step 1, pouring a polyvinyl alcohol aqueous solution into a container, and adding monomer A, an initiator, and a control agent into the polyvinyl alcohol aqueous solution, stirring it for 2-3 minutes using a stirring device, stirring and mixing it evenly, heating it by a heating device, raising the temperature of the mixed substance to 70-90 degrees Celsius, and starting to react when the temperature reaches the range, controlling the reaction time to 1-2 hours, and when the reaction is completely completed, starting to cool to room temperature to obtain a prepolymer containing a linear styrene hard segment; Step 2, pouring the product obtained in step 1 into a container, and pouring the cycloalkane ester monomer B, the linear alkane ester monomer C, the initiator, and the crosslinking agent into the container, using a stirring device to continuously mix and stir for 1-2 minutes until the mixture is uniformly stirred, using a heating device to heat the mixture to raise the temperature of the mixed liquid to 70-90 degrees Celsius, and when the temperature rises to the range, starting the reaction, the reaction time is controlled to be 5-6 hours, until the reaction is completed, to obtain a hyper-crosslinked structure copolymer containing a hard segment and a soft segment; Step three, cool the product obtained in step two to room temperature, filter it using a filtering device, and then wash it with deionized water. After washing, use a drying device to dry it, adjust the drying temperature to 40-80 degrees Celsius, and the drying time to 2-20 hours to obtain a high-viscosity organic waste liquid adsorption material with a super-cross-linked porous microsphere structure.
Citation Information
Patent Citations
BE719105A
Hydrophobic high-micropore polymeric adsorbent, preparation and uses thereof
CN101314124A
High-viscosity organic waste liquid adsorption material and preparation method thereof
CN118930704A
Organic fine particle and method for producing the same
JP2019073582A
Liquid Composition Containing Hollow Particle, Process For Producing The Same, And Optical Article
US20080227893A1