Preparation and application of high vinyl functionalized polybutadiene liquid rubber

Through the anion polymerization method of new bicyclic amine compounds with alkyl lithium and functionalized monomers, the problem of 1,2-structure control in polybutadiene liquid rubber is solved, and the efficient preparation of ultra-high 1,2-structure content is achieved. Polybutadiene liquid rubber improves mechanical properties stability and molecular weight distribution uniformity, and is suitable for epoxy resins and high-frequency communication copper clad plate bonding and other fields.

CN118930734APending Publication Date: 2024-11-12HUNAN INSTITUTE OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411329003.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the 1,2-structure content in polybutadiene liquid rubber, resulting in aging of mechanical properties and uneven molecular weight distribution, and lack of research on ultra-high functionalized liquid rubber.

Method used

Using new bicyclic amine compounds as regulators, combining alkyl lithium and functionalized monomers, reacting under anhydrous and oxygen-free atmosphere through anionic polymerization method to prepare high vinyl functionalized polybutadiene liquid rubber to achieve ultra-high 1,2-Structural content and molecular weight are controllable.

Benefits of technology

The obtained polybutadiene liquid rubber has a 1,2-structure content of up to 90-100%, a narrow molecular weight distribution, controllable degree of functionalization, mild polymerization conditions, low cost, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The invention relates to preparation and application of high vinyl functionalized polybutadiene liquid rubber. According to the invention, through anionic polymerization reaction, butadiene polymerization is initiated by a novel bicyclic amine regulator / lithium alkylide in an inert organic solvent, and meanwhile, functionalized monomer in-situ copolymerization reaction is introduced, so that the high vinyl functionalized polybutadiene liquid rubber is obtained. The synthesized polybutadiene liquid rubber has the characteristics that the 1, 2-structure is adjustable in the range of 90%-100%, the functionalization degree is adjustable in the range of 0%-25%, the molecular weight is controllable, and the molecular weight distribution is narrow. The high vinyl functionalized liquid rubber can be applied to epoxy resin toughening processing or high-frequency communication copper-clad plate bonding resin. Compared with the prior art, the regulator designed by the invention has the characteristics of stronger structure regulation capability and temperature insensitivity, abundant types of functionalized monomers, mild reaction conditions and simplicity and convenience in operation.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of diene anionic polymerization, and in particular to a high-vinyl functionalized polybutadiene liquid rubber and a preparation method and application thereof. Background Art

[0002] Liquid rubber is in liquid form at room temperature. It can form a three-dimensional network structure through chemical or ionic cross-linking, and has mechanical properties similar to those of ordinary vulcanized rubber. Solid rubber must be formed through multiple processes such as mixing with various compounding agents, molding, and vulcanization, which is a very time-consuming process. However, liquid rubber can be made into products by simply mixing various compounding agents and undergoing high-temperature or light-curing cross-linking reactions. Liquid rubber has the following advantages: (1) Liquid rubber is a cast elastomer, and the processing technology is easy to achieve mechanization, continuity, and automation; (2) The investment in processing equipment and models is reduced; (3) Auxiliary costs are saved; (4) Processing in a liquid state is solvent-free and pollution-free; (5) With the help of main chain extension and cross-linking methods, the physical properties and vulcanization speed can be adjusted over a wide range. Therefore, the most widely used liquid rubber is liquid polybutadiene rubber, which is widely used in various fields such as high-frequency 6G communications / epoxy resin toughening / sealing devices.

[0003] The glass transition temperature of polybutadiene liquid rubber products generally increases with the increase of molecular weight. When the glass transition temperature is higher than room temperature, it will present the appearance of solid rubber. Therefore, its molecular weight is generally low, between 1000-20000. At present, the methods for synthesizing liquid rubber mainly include anionic polymerization, free radical polymerization and coordination polymerization. There are many varieties of liquid polybutadiene and a wide range of uses. Those without functional groups are mainly used as additive modifiers for coatings, thermosetting resins, and other rubbers and resins. Random carboxyl liquid polybutadiene can be cross-linked and cured with epoxy resins, acid anhydrides, and zinc and magnesium oxides, and is used as an adhesive for rocket solid propellants. Carboxyl-terminated polybutadiene is mainly used as sealing materials, coatings and adhesives, and has good cold resistance, dielectric properties and water resistance. Halogen-terminated polybutadiene can mainly produce adhesives, sealing materials and waterproof materials with excellent bonding properties to wood, metal, concrete and glass. Hydroxyl-terminated polybutadiene is widely used. In addition to being used as adhesives, rubber and plastic modifiers, it can also be made into special coatings that are resistant to low temperatures, corrosion, electrical insulation and water-soluble; it can be used as a sealing material for encapsulating electrical and electronic components, and it can be moisture-proof and shock-proof; it can also be cast into rubber products, used as insulating sleeves, belts, shockproof materials and special-shaped products with complex shapes, etc. Therefore, compared with non-modified products, functionalized products have higher added value.

[0004] Structurally, the microstructure of polybutadiene includes linear 1,4-structure and side group 1,2-structure. Compared with free radical polymerization and coordination polymerization, anionic polymerization has greater advantages in regulating the microstructure, molecular weight and distribution of polybutadiene. Since 1,4-polybutadiene contains a large number of double bonds in the main chain, it is easy to age after cross-linking, and its mechanical properties are greatly affected by the breakage of double bonds. On the contrary, the side chain double bonds of 1,2-polybutadiene are not only conducive to cross-linking, but also have little loss of mechanical properties before and after aging. Therefore, the control of the 1,2-structure of polybutadiene is of great significance. Traditional Lewis base substances, such as ethers and amines, can increase the 1,2-structure content in polybutadiene to a certain extent, but it is difficult to stabilize it above 90%. As a special bicyclic amine substance, dipiperidine ethane has a special chelating effect with butyl lithium, which makes the 1,2-structure content in polybutadiene higher than 90% under low temperature conditions (room temperature). However, its regulation ability is extremely dependent on the polymerization temperature and the amount of regulator. Theoretically, the introduction of electron-donating groups and the enhancement of steric hindrance effects on cyclic amines can further enhance the coordination between cyclic amines and alkyl lithiums, thereby enhancing their temperature-insensitive properties and their ability to regulate 1,2-structures. In addition, there is a lack of research on functionalized liquid rubbers with ultra-high 1,2-structure content. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a preparation and application of a high vinyl functionalized polybutadiene liquid rubber. The preparation method provided by the present invention uses a new type of bicyclic amine compound as a key regulator and a functionalized monomer as a comonomer to provide a method for preparing a high vinyl functionalized polybutadiene liquid rubber by anionic polymerization. To achieve the above-mentioned invention purpose, the present invention provides the following technical solutions:

[0006] The present invention provides a method for preparing a high vinyl functionalized polybutadiene liquid rubber, comprising the following steps:

[0007] In an anhydrous and oxygen-free inert gas atmosphere, an organic solvent, a novel bicyclic amine structure regulator, an alkyl lithium initiator, butadiene and a functionalized monomer are mixed for anionic polymerization to obtain a functionalized polybutadiene liquid rubber with an ultra-high 1,2-structure. Preferably, the novel bicyclic amine regulator is one or more of the structural compounds shown in NN-1 to 12, more preferably NN4-NN-12.

[0008] Preferably, the molar ratio of the novel bicyclic amine regulator to the alkyl lithium is (0.1-10): 1, more preferably (0.25-5): 1. Preferably, the functionalized monomer described is one or more of the structural compounds shown in VB-1~11.

[0009] Preferably, the functionalized monomer accounts for 0-25% of the monomer mass fraction. Preferably, the polymerization reaction temperature is 0-50 ° C, and the time is 0.25-12 h.

[0010] The functionalized polybutadiene liquid rubber obtained by the preparation method provided by the present invention has a 1,2-structure content of 90-100%. Preferably, the functionalized polybutadiene liquid rubber has a number average molecular weight of 1000-50000 g / mol. Preferably, the functionalized polybutadiene liquid rubber has a molecular weight distribution of 1.03-1.30.

[0011] The high-vinyl functionalized polybutadiene liquid rubber prepared by anionic polymerization uses a novel bicyclic amine compound as a key regulator and a functionalized monomer as a comonomer. The obtained polybutadiene liquid rubber has an ultra-high 1,2-structure, a controllable molecular weight, a very narrow molecular weight distribution, a controllable degree of functionalization, and a wide range of functionalized group selection. The preparation method provided by the invention has mild polymerization conditions, low cost, and is suitable for industrialization. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is the H-NMR spectrum of 98% polybutadiene liquid rubber.

[0013] Figure 2 This is the H-NMR spectrum of polybutadiene liquid rubber with 95% 1,2-structure and 5% tertiary amine functionalization.

[0014] Figure 3 This is the GPC spectrum of polybutadiene liquid rubber with 1,2-structure of 95% containing 0-15% tertiary amine functional monomer. DETAILED DESCRIPTION

[0015] The present invention provides a method for preparing a high vinyl functionalized polybutadiene liquid rubber, comprising the following steps:

[0016] In an anhydrous and oxygen-free inert gas atmosphere, an organic solvent, a novel bicyclic amine structure regulator, an alkyl lithium initiator, butadiene and a functionalized monomer are mixed for anionic polymerization to obtain a functionalized polybutadiene liquid rubber with an ultra-high 1,2-structure.

[0017] In the present invention, the organic solvent preferably includes one or more of cyclohexane, cyclopentane, toluene, hexane, ether, cyclopentyl methyl ether, and tetrahydrofuran. The present invention has no particular limitation on the amount of the organic solvent, and any amount that can evenly mix the raw materials will meet the requirements.

[0018] In the present invention, the novel bicyclic amine regulator described is one or more of the compounds with structures shown in NN-1~12.

[0019] In the present invention, the mechanism of action of the novel bicyclic amine regulator is shown in the figure:

[0020] In the present invention, the novel bicyclic amine regulator can be prepared by an organic synthesis method well known to those skilled in the art.

[0021] In the present invention, the molar ratio of the novel bicyclic amine regulator to the alkyl lithium is preferably (0.1-10): 1, and the preferred ratio is 0.25-5.0.

[0022] In the present invention, the functionalized monomer is one or more of the compounds with structures shown in VB-1 to 11.

[0023] In the present invention, the functionalized monomer accounts for 0-25% of the monomer mass fraction.

[0024] In the present invention, the order of adding the organic solvent, the novel bicyclic amine regulator, the alkyl lithium initiator, the butadiene monomer and the functionalized monomer is preferably: adding the organic solvent, the novel bicyclic amine regulator and the alkyl lithium initiator to the reaction kettle, and then continuously adding the butadiene and functionalized monomer mixed monomers; or adding the organic solvent, the novel bicyclic amine regulator, the butadiene and functionalized monomer mixed monomers to the reaction kettle, and then adding the alkyl lithium initiator.

[0025] In the present invention, the polymerization reaction temperature is preferably room temperature, no additional heat source or cooling source is required, and the reaction time is 0.1-12 h.

[0026] In the present invention, all raw materials need to be treated in anhydrous and oxygen-free conditions, and the polymerization reaction is carried out in an inert gas atmosphere.

[0027] In the present invention, after the polymerization reaction, preferably, a terminator and an antioxidant are added, and alcohol substances are precipitated or high-temperature steam is used to wash the rubber to obtain the above-mentioned polybutadiene liquid rubber.

[0028] The functionalized polybutadiene liquid rubber obtained by the preparation method provided by the present invention has a 1,2-structure content in the range of 90-100%, preferably greater than 95%.

[0029] In the present invention, the number average molecular weight of the functionalized polybutadiene liquid rubber is 1000-50000 g / mol, preferably 2000-20000 g / mol.

[0030] In the present invention, the molecular weight distribution of the functionalized polybutadiene liquid rubber is 1.02-1.30, preferably 1.03-1.15.

[0031] The present invention also provides the functionalized polybutadiene liquid rubber described in the above scheme, which can be applied to epoxy resin toughening or high-frequency communication copper-clad laminate bonding resin.

[0032] To further illustrate the present invention, the functionalized polybutadiene liquid rubber provided by the present invention and its preparation method and application are described in detail below in conjunction with examples, but they should not be construed as limiting the scope of protection of the present invention.

[0033] Embodiment 1:

[0034] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-2 regulator, and 100 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 500 g of butadiene was slowly added dropwise. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The polybutadiene liquid rubber solution was poured into 2 L ethanol containing 40 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. It was then repeatedly washed with acidic deionized water and ethanol. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 89%, a molecular weight of 2200 g / mol, and a molecular weight distribution of 1.06.

[0035] Embodiment 2:

[0036] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-2 regulator and 100 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-1 ether functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The ether-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 90%, VB-1 ether functional monomer accounted for 10.3%, molecular weight of 2500 g / mol, and molecular weight distribution of 1.07.

[0037] Embodiment 3:

[0038] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-6 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 475 g of butadiene and 25 g of VB-2 amine functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 1 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The amine-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 95%, VB-2 amine functional monomer accounted for 5.1%, molecular weight of 5400 g / mol, and molecular weight distribution of 1.05.

[0039] Embodiment 4:

[0040] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-7 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-4 amine functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The amine-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 98%, VB-4 amine functional monomer accounted for 9.7%, molecular weight of 5200 g / mol, and molecular weight distribution of 1.04.

[0041] Embodiment 5:

[0042] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-9 regulator and 100 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-5 thioether functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The thioether-functionalized polybutadiene liquid rubber solution was poured into 2 L ethanol containing 40 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 94%, VB-5 thioether functional monomer accounted for 9.5%, molecular weight of 2400 g / mol, and molecular weight distribution of 1.09.

[0043] Embodiment 6:

[0044] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 25 mL of 0.5 M NN-10 regulator and 25 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-6 silicon-functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The silicon-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 93%, VB-6 silicon-functional monomer accounted for 9.8%, molecular weight of 11500 g / mol, and molecular weight distribution of 1.12.

[0045] Embodiment 7:

[0046] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 50 mL of 0.5 M NN-11 regulator and 25 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-2 amine functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The amine-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 98%, VB-5 amine functional monomer accounted for 9.9%, molecular weight of 10600 g / mol, and molecular weight distribution of 1.10.

[0047] Embodiment 8:

[0048] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 100 mL of 0.5 M NN-12 regulator, and 25 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-7 phosphine-containing functional monomer were slowly added. The polymerization reaction was carried out at 0 °C for 4 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The phosphine-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 99.8%, VB-7 phosphine-containing functional monomer accounted for 9.5%, molecular weight was 10100 g / mol, and molecular weight distribution was 1.11.

[0049] Embodiment 9:

[0050] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 200 mL of 0.5 M NN-12 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-8 germanium-containing functional monomer were slowly added. The polymerization reaction was carried out at 10 °C for 1 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The germanium-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer had a 1,2-structure of 97%, VB-8 germanium-containing functional monomer accounted for 9.9%, molecular weight was 11200 g / mol, and molecular weight distribution was 1.25.

[0051] Embodiment 10:

[0052] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 200 mL of 0.5 M NN-9 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-9 ether functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 1 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The ether-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer 1,2-structure was 97%, VB-9 contained ether functional monomers accounted for 10.5%, 3,4-structure content was 69%, molecular weight was 12300 g / mol, and molecular weight distribution was 1.22.

[0053] Embodiment 11:

[0054] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 200 mL of 0.5 M NN-8 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 450 g of butadiene and 50 g of VB-10 amine functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 1 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The amine-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer 1,2-structure was 98%, VB-9 contained amine functional monomers accounting for 10.1%, 3,4-structure content was 65%, molecular weight was 10500 g / mol, and molecular weight distribution was 1.19.

[0055] Embodiment 12:

[0056] A 5 L reactor was filled with high-purity nitrogen, and 2500 mL of cyclohexane, 200 mL of 0.5 M NN-5 regulator and 50 mL of 2.5 M n-butyl lithium initiator were added in sequence. The mixed solution was stirred at room temperature for 5 min, and then 475 g of butadiene and 25 g of VB-11 silicon-functional monomer were slowly added. The polymerization reaction was carried out at room temperature for 2 h, and 1 M hydrochloric acid methanol solution was added to terminate the reaction. The silicon-functionalized polybutadiene liquid rubber solution was poured into 2.5 L ethanol containing 50 mL of antioxidant (ethanol solution of 2,6-di-tert-butyl-4-methylphenol), and the polymer was precipitated. Then, it was washed with acidic deionized water and ethanol in turn. The obtained polymer was dried in a vacuum drying oven to obtain a polymer with a yield of 100%. The polymer 1,2-structure was 96%, VB-9 silicon-functional monomer accounted for 4.5%, 3,4-structure content was 65%, molecular weight was 98900 g / mol, and molecular weight distribution was 1.09.

[0057] Finally, it should be noted that the above embodiments are only used to illustrate the implementation process and features of the present invention, rather than to limit the technical methods of the present invention. Although the present invention has been described in detail with reference to the above embodiments, ordinary technicians in this field should understand that the present invention can still be modified or replaced by equivalents, and any modification or partial replacement that does not depart from the spirit and scope of the present invention should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a high vinyl functionalized polybutadiene liquid rubber, characterized in that: The following steps are involved: In an anhydrous and oxygen-free inert gas atmosphere, an organic solvent, a novel bicyclic amine regulator, an alkyl lithium initiator, butadiene and a functionalized monomer are mixed, and anionic polymerization is carried out at a polymerization temperature to obtain a functionalized polybutadiene liquid rubber with an ultra-high 1,2-structure.

2. The preparation method according to claim 1, characterized in that: The described novel bicyclic amine modulator is any one of the compounds of structures shown in NN-1 to 12:

3. According to the preparation method described in claim 1, the molar ratio of the novel bicyclic amine regulator to the alkyl lithium is (0.1-10):

1.

4. The preparation method according to claim 1, characterized in that: The functionalized monomer described is any one of the structural compounds shown in VB-1~11:

5. The preparation method according to claim 1, characterized in that: The functionalized monomers described account for 0-25% of the monomer mass fraction.

6. The preparation method according to claim 1, characterized in that: The polymerization reaction temperature described is 0-50°C and the time is 0.25-12 h.

7. The functionalized polybutadiene liquid rubber obtained according to the preparation method described in claims 1-6, wherein the 1,2-structure content is 80-100%.

8. The functionalized polybutadiene liquid rubber according to claim 7, characterized in that: The functionalized polybutadiene liquid rubber has a number average molecular weight of 1000-50000 g / mol.

9. The functionalized polybutadiene liquid rubber according to claim 7, characterized in that: The molecular weight distribution of the functionalized polybutadiene liquid rubber is 1.02-1.

30.

10. The functionalized liquid rubber according to any one of claims 7 to 9 can be used in epoxy resin toughening processing or in high-frequency communication copper-clad laminate bonding resin.

Citation Information

Cited By

  • Preparation method of dimorpholine ethane crystal

    CN122464840A