Antiskid rodlike rare earth modified polyurethane material and application thereof
By using rod-shaped rare earth oxide enhancer in polyurethane tires, the wear resistance and grip of the tire are improved, and the problem of insufficient grip caused by smooth surface of polyurethane tires is solved, achieving shorter brake distance and higher safety .
Patent Information
- Application Number
- CN202411219087.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The self-crusting effect of polyurethane solid tires leads to a smooth tire surface and insufficient grip, which especially affects the vehicle's handling performance and braking distance under slippery conditions.
Premixed materials are prepared from rod-shaped rare earth modified polyurethane materials, which are mixed with rod-shaped rare earth oxides, polyethylene glycol, glycerin, catalyst, water and color paste and isocyanate cured. The wear resistance of tires is improved by using the enhancement effect of rod-shaped rare earth oxides. and roughness, increasing friction performance with the ground.
It improves the grip of the tires, shortens the braking distance on various road surfaces, and enhances the wear resistance and safety of the tires.
Smart Images

Figure CN118930808A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of polyurethane foaming materials, and particularly relates to an anti-slip rod-shaped rare earth modified polyurethane material and application thereof. Background Art
[0002] The manufacturing process of the infused foamed polyurethane solid tire involves injecting the two-component solution of polyurethane - the polyether polyol component and the isocyanate component - into the tire mold. At a specific temperature, the mixture undergoes a chemical cross-linking reaction and finally solidifies to form a polyurethane elastic solid tire. This tire has many significant advantages: no need for inflation, insensitivity to punctures, high load-bearing capacity, low compression deformation, excellent shock absorption performance, long service life, and a wide range of adaptability. These characteristics minimize the inconvenience caused by tire punctures. In addition, the excellent stability and constant pressure effect of the tire further enhance its safety in hazardous environments.
[0003] However, despite the many advantages of foamed polyurethane tires, their self-skinning effect results in a relatively smooth tire surface, which is inferior to standard pneumatic tires in terms of ground grip, especially in slippery conditions, affecting the vehicle's handling performance and braking distance. Therefore, professionals and companies at home and abroad have been conducting continuous improvement research.
[0004] CN 108752910 A proposes a solution to improve the anti-skid and wear-resistant performance of polyurethane solid tires by adding aramid pulp and tetrafluoroethylene modified materials. This method not only ensures that no long marks will be left when braking, but also has strong environmental protection performance and simplicity of material preparation, while extending the service life. However, the patent has not yet published specific test data. In addition, CN 106832198 A discloses a method for preparing anti-skid polyurethane solid tires for cold storage environments. This method increases the content of soft segments in the polyurethane molecular chain by changing the structure of the reaction monomers, thereby improving the anti-skid effect of the tire at low temperatures. The above-mentioned prior art mainly enhances the anti-skid performance of polyurethane solid tires by adding or changing organic polymer compounds. Summary of the invention
[0005] The invention aims to provide a non-slip rod-shaped rare earth modified polyurethane material.
[0006] The technical solution of the present invention is as follows:
[0007] A non-slip rod-shaped rare earth modified polyurethane material is prepared by mixing and curing a premixed material and isocyanate, wherein the premixed material is prepared by mixing a rod-shaped rare earth oxide predispersion liquid, polyethylene glycol 600, glycerol, a catalyst, water and a color paste, and the rod-shaped rare earth oxide predispersion liquid is prepared by mixing polyethylene glycol 400, a dispersant, a defoaming agent and the rod-shaped rare earth oxide. The specific size specifications of the rod-shaped rare earth oxide are: length 100-200μm, width 2-15μm, thickness 500nm-5μm.
[0008] In a preferred embodiment of the present invention, the rod-shaped rare earth oxide is at least one of rod-shaped cerium oxide, rod-shaped lanthanum oxide, rod-shaped samarium oxide, rod-shaped neodymium oxide and rod-shaped yttrium oxide.
[0009] In a preferred embodiment of the present invention, in the rod-shaped rare earth oxide pre-dispersion liquid, the mass ratio of polyethylene glycol 400, dispersant, defoamer and rod-shaped rare earth oxide is 350-450:1-2:2.5-5:22-32.
[0010] Further preferably, in the premixed material, the mass ratio of the rod-shaped rare earth oxide pre-dispersion liquid, polyethylene glycol 600, glycerol, catalyst, water and color paste is 384-486.5:467-538:30.5-60:1.5-3:2-4:11-15.
[0011] More preferably, the mass ratio of the premix to the isocyanate is 5-6:4-5.
[0012] In a preferred embodiment of the present invention, the catalyst is an organotin catalyst T-12.
[0013] In a preferred embodiment of the present invention, the dispersant is Euka U680, and the defoamer is BYK-093.
[0014] The method for preparing the above-mentioned anti-slip rod-shaped rare earth modified polyurethane material comprises the following steps:
[0015] (1) polyethylene glycol 400, a dispersant and a defoamer are mixed uniformly, and then rod-shaped rare earth oxide is added and dispersed until the temperature reaches 50-60° C., stirring is continued for 8-12 minutes, and then stirring is stopped. After cooling, a rod-shaped rare earth oxide pre-dispersion liquid is obtained;
[0016] (2) polyethylene glycol 600, glycerol, catalyst, water and color paste are stirred and mixed uniformly, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) is added, and stirring is continued for 10-15 minutes to obtain a premixed material;
[0017] (3) After the premixed material obtained in step (2) is evenly mixed with isocyanate, the mixture is poured into a mold, and the mold is heated to a temperature of 70-80° C. within 2 minutes. The heating is immediately stopped, and the mold is opened after 2-4 minutes.
[0018] The use of the anti-skid rod-shaped rare earth modified polyurethane material in the preparation of anti-skid tires.
[0019] An anti-skid tire is made of the anti-skid rod-shaped rare earth modified polyurethane material.
[0020] The beneficial effects of the present invention are as follows: the present invention utilizes the reinforcing effect of the rod-shaped rare earth oxide to improve the wear resistance and roughness of the tire. Specifically, the needle-shaped effect of the rod-shaped rare earth oxide distributed on the surface is utilized to improve the surface roughness of the foamed tire, and the ground-penetrating effect of the rod-shaped end is utilized to increase the friction performance with the ground, especially the wet and slippery ground, thereby improving the grip. In addition, the local rapid foaming effect of the rod-shaped rare earth oxide is utilized to control the hardness of the tire, increase the wear resistance of the tire, and increase the contact area between the tire and the ground under a constant load, thereby further improving the friction coefficient, and ultimately achieving excellent grip of the tire and shortening the braking distance on various road surfaces. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 SEM photograph of the rod-shaped lanthanum oxide in Example 2 of the present invention.
[0022] Figure 2 This is a surface photograph of the finished tire prepared in Comparative Example 2 of the present invention.
[0023] Figure 3 This is a surface photograph of the finished tire prepared in Example 2 of the present invention.
[0024] Figure 4 This is a photo of the braking distance of the finished tire prepared in Comparative Example 2 of the present invention.
[0025] Figure 5 This is a photo of the braking distance of the finished tire made in Example 2 of the present invention. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.
[0027] Example 1
[0028] (1) Add 409.0 g of PEG400 (purity above 95%), 1.5 g of dispersant U680 and 2.5 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 22.0 g of rod-shaped cerium oxide (purity above 95%, with specific dimensions: average length 100 μm, average width 8 μm, average thickness 2 μm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800 r / min, and when the temperature of the material reaches 50°C, continue to stir for 10 min, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0029] (2) 500.0 g PEG600 (purity above 95%), 45.0 g glycerol, 3.0 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 2.0 g grade 3 deionized water and 15.0 g black color paste (purchased from Guangzhou Panyu Kedi Color Co., Ltd., concentration of 10±0.5%) were added to the dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0030] (3) 600.0 g of the premixed material obtained in step (2) and 400.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) are added to a pull cylinder and mixed quickly and evenly, then poured into a tire mold coated with a release agent, and the tire mold is heated to a temperature of 80° C. within 2 min. The heating is immediately stopped, and the tire mold is opened after 3 min to take out the foamed tire.
[0031] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire.
[0032] Example 2
[0033] (1) Add 450.0 g of PEG400 (purity above 95%), 1.0 g of dispersant Euka U680 and 3.5 g of defoamer BYK-093 to a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 32.0 g of rod-shaped lanthanum oxide (such as Figure 1 As shown, the purity is more than 95%, and its specific size specifications are: average length 160μm, average width 15μm, average thickness 1μm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800r / min, when the temperature of the material reaches 60°C, continue stirring for 10min, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0034] (2) 467.0 g PEG600 (purity above 95%), 30.5 g glycerol, 2.0 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 3.0 g grade 3 deionized water and 11.0 g black color paste (purchased from Guangzhou Panyu Cody Color Co., Ltd., concentration of 10±0.5%) were added to a dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0035] (3) Add 550.0 g of the premixed material obtained in step (2) and 450.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) into a pull cylinder and mix them quickly and evenly, then pour them into a tire mold coated with a release agent, heat the tire mold so that its temperature rises to 80° C. within 2 minutes, stop heating immediately, open the tire mold after 3 minutes, and take out the foamed tire.
[0036] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire (surface Figure 3 As shown in Table 1 and Figure 5 shown).
[0037] Example 3
[0038] (1) Add 350.0 g of PEG400 (purity above 95%), 2.0 g of dispersant Uka U680 and 5.0 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 27.0 g of rod-shaped samarium oxide (purity above 95%, with specific dimensions: average length 200 μm, average width 2 μm, average thickness 500 nm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800 r / min, and continue to stir for 10 min when the temperature of the material reaches 60°C, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0039] (2) 538.0 g PEG600 (purity above 95%), 60.0 g glycerol, 1.5 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 4.0 g grade 3 deionized water and 12.5 g black color paste (purchased from Guangzhou Panyu Kedi Color Co., Ltd., concentration of 10±0.5%) were added to a dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0040] (3) 500.0 g of the premixed material obtained in step (2) and 500.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) are added into a pull cylinder and mixed quickly and evenly, then poured into a tire mold coated with a release agent, and the tire mold is heated to a temperature of 70° C. within 2 min. The heating is immediately stopped, and the tire mold is opened after 3 min to take out the foamed tire.
[0041] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire.
[0042] Comparative Example 1
[0043] (1) Add 450.0 g of PEG400 (purity above 95%), 1.0 g of dispersant U680 and 3.5 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 0 g of rod-shaped lanthanum oxide, continue to disperse at a stirring rate of 800 r / min, and when the temperature of the material reaches 60°C, continue to stir for 10 min, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0044] (2) 499.0 g PEG600 (purity above 95%), 30.5 g glycerol, 2.0 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 3.0 g grade 3 deionized water and 11.0 g black color paste (purchased from Guangzhou Panyu Cody Color Co., Ltd., concentration of 10±0.5%) were added to a dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0045] (3) Add 550.0 g of the premixed material obtained in step (2) and 450.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) into a pull cylinder and mix them quickly and evenly, then pour them into a tire mold coated with a release agent, heat the tire mold so that its temperature rises to 80° C. within 2 minutes, stop heating immediately, open the tire mold after 3 minutes, and take out the foamed tire.
[0046] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire.
[0047] Comparative Example 2
[0048] (1) Add 450.0 g of PEG400 (purity above 95%), 1.0 g of dispersant Uka U680 and 3.5 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 32.0 g of rod-shaped lanthanum oxide (purity above 95%, with specific dimensions: average length 200 μm, average width 2 μm, average thickness 500 nm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800 r / min, and when the temperature of the material reaches 50°C, continue to stir for 10 min, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0049] (2) 467.0 g PEG600 (purity above 95%), 30.5 g glycerol, 2.0 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 3.0 g grade 3 deionized water and 11.0 g black color paste (purchased from Guangzhou Panyu Cody Color Co., Ltd., concentration of 10±0.5%) were added to a dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0050] (3) Add 550.0 g of the premixed material obtained in step (2) and 450.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) into a pull cylinder and mix them quickly and evenly, then pour them into a tire mold coated with a release agent, heat the tire mold so that its temperature rises to 90° C. within 2 minutes, stop heating immediately, open the tire mold after 3 minutes, and take out the foamed tire.
[0051] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire (surface Figure 2 As shown in Table 1 and Figure 4 shown).
[0052] Comparative Example 3
[0053] (1) Add 917.0 g of PEG400 (purity above 95%), 1.0 g of dispersant Uka U680 and 3.5 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 32.0 g of rod-shaped lanthanum oxide (purity above 95%, with specific dimensions: average length 200 μm, average width 2 μm, average thickness 500 nm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800 r / min, and continue to stir for 10 min when the temperature of the material reaches 60°C, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0054] (2) 0g PEG600 (purity above 95%), 30.5g glycerol, 2.0g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 3.0g grade 3 deionized water and 11.0g black color paste (purchased from Guangzhou Panyu Kedi Color Co., Ltd., concentration of 10±0.5%) were added to the dispersion tank in sequence, stirred at a stirring rate of 500r / min for 10min, and then, the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800r / min for 15min to obtain a premixed material.
[0055] (3) Add 550.0 g of the premixed material obtained in step (2) and 450.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) into a pull cylinder and mix them quickly and evenly, then pour them into a tire mold coated with a release agent, heat the tire mold so that its temperature rises to 80° C. within 2 minutes, stop heating immediately, open the tire mold after 3 minutes, and take out the foamed tire.
[0056] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire.
[0057] Comparative Example 4
[0058] (1) Add 450.0 g of PEG400 (purity above 95%), 1.0 g of dispersant Euka U680 and 3.5 g of defoamer BYK-093 into a pull cylinder, stir at a stirring rate of 500 r / min for 15 min, then add 32.0 g of lanthanum oxide (non-rod-shaped, purity above 95%, and its specific size specifications are: spherical powder with an average diameter of 2 μm, purchased from Xiamen Rare Earth Materials Research Center, Haixi Institute, Chinese Academy of Sciences), continue to disperse at a stirring speed of 800 r / min, and when the temperature of the material reaches 60°C, continue to stir for 10 min, then stop stirring, and obtain a rod-shaped rare earth oxide pre-dispersion liquid after cooling.
[0059] (2) 467.0 g PEG600 (purity above 95%), 30.5 g glycerol, 2.0 g organotin catalyst T-12 (purchased from American Gas, solid content of 18±0.5%), 3.0 g grade 3 deionized water and 11.0 g black color paste (purchased from Guangzhou Panyu Cody Color Co., Ltd., concentration of 10±0.5%) were added to a dispersion tank in sequence, stirred at a stirring rate of 500 r / min for 10 min, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) was added, and the mixture was dispersed at a stirring rate of 800 r / min for 15 min to obtain a premixed material.
[0060] (3) Add 550.0 g of the premixed material obtained in step (2) and 450.0 g of N3390 isocyanate curing agent (Bayer or Desmodur) into a pull cylinder and mix them quickly and evenly, then pour them into a tire mold coated with a release agent, heat the tire mold so that its temperature rises to 80° C. within 2 minutes, stop heating immediately, open the tire mold after 3 minutes, and take out the foamed tire.
[0061] (4) trimming the foamed tire obtained in step (3) to obtain a finished tire.
[0062] The following are the test data of the finished tires obtained in Examples 1 to 3 and Comparative Examples 1 to 4, wherein the tire braking distance test uses a 250W rear axle motor, vehicle speed: 6.5KM, voltage: 24.5V, test load: 73KG, slope: 9°. Hardness (Shore A) indicates the hardness of the tire, which is generally used to measure the comfort and wear resistance of the tire during driving. Too hard comfort deteriorates, and too soft wear resistance decreases. Roughness indicates the friction with the ground. Under constant load, the increase in roughness will increase the friction with the ground, thereby shortening the braking distance on various ground surfaces. The shorter the braking distance, the better the tire grip and the higher the safety factor.
[0063] Table 1 Performance results of examples and comparative examples
[0064]
[0065] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.
Claims
1. A non-slip rod-shaped rare earth modified polyurethane material, Features: It is prepared by mixing and curing a premixed material and isocyanate, wherein the premixed material is prepared by mixing a rod-shaped rare earth oxide predispersion liquid, polyethylene glycol 600, glycerol, a catalyst, water and a color paste, and the rod-shaped rare earth oxide predispersion liquid is prepared by mixing polyethylene glycol 400, a dispersant, a defoaming agent and a rod-shaped rare earth oxide. The specific size specifications of the rod-shaped rare earth oxide are: length 100-200μm, width 2-15μm, thickness 500nm-5μm.
2. The anti-slip rod-shaped rare earth modified polyurethane material according to claim 1, Features: The rod-shaped rare earth oxide is at least one of rod-shaped cerium oxide, rod-shaped lanthanum oxide, rod-shaped samarium oxide, rod-shaped neodymium oxide and rod-shaped yttrium oxide.
3. The anti-slip rod-shaped rare earth modified polyurethane material according to claim 1 or 2, Features: In the rod-shaped rare earth oxide pre-dispersion liquid, the mass ratio of polyethylene glycol 400, dispersant, defoamer and rod-shaped rare earth oxide is 350-450:1-2:2.5-5:22-32.
4. The anti-slip rod-shaped rare earth modified polyurethane material according to claim 3, Features: In the premixed material, the mass ratio of the rod-shaped rare earth oxide pre-dispersion liquid, polyethylene glycol 600, glycerol, catalyst, water and color paste is 384-486.5:467-538:30.5-60:1.5-3:2-4:11-15.
5. The anti-slip rod-shaped rare earth modified polyurethane material according to claim 4, Features: The mass ratio of the premixed material to the isocyanate is 5-6:4-5.
6. The anti-slip rod-shaped rare earth modified polyurethane material according to any one of claims 1 to 5, Features: The catalyst is an organotin catalyst T-12.
7. The anti-slip rod-shaped rare earth modified polyurethane material according to any one of claims 1 to 5, Features: The dispersant is Euka U680, and the defoamer is BYK-093.
8. A method for preparing a non-slip rod-shaped rare earth modified polyurethane material according to any one of claims 1 to 7, Features: The steps include: (1) polyethylene glycol 400, a dispersant and a defoamer are mixed uniformly, and then rod-shaped rare earth oxide is added and dispersed until the temperature reaches 50-60° C., stirring is continued for 8-12 minutes, and then stirring is stopped. After cooling, a rod-shaped rare earth oxide pre-dispersion liquid is obtained; (2) polyethylene glycol 600, glycerol, catalyst, water and color paste are stirred and mixed uniformly, and then the rod-shaped rare earth oxide pre-dispersion liquid obtained in step (1) is added, and stirring is continued for 10-15 minutes to obtain a premixed material; (3) After the premixed material obtained in step (2) is evenly mixed with isocyanate, the mixture is poured into a mold, and the mold is heated to a temperature of 70-80° C. within 2 minutes. The heating is immediately stopped, and the mold is opened after 2-4 minutes.
9. Use of the anti-skid rod-shaped rare earth modified polyurethane material according to any one of claims 1 to 7 in the preparation of anti-skid tires. 10.An anti-skid tire, Features: It is made of the anti-slip rod-shaped rare earth modified polyurethane material described in any one of claims 1 to 7.