High polymer humidity power generation system based on bio-based glass and preparation method of high polymer humidity power generation system

Through the combination of biomass glass polymer materials and conductive metals or graphite, the wet-electric effect is used to solve the problem of insufficient water resistance and mechanical properties of existing wet-energy power generation materials in high temperature and high humidity environments, and achieve efficient electrical energy output and System stability.

CN118930829AActive Publication Date: 2024-11-12CHUZHOU UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411060683.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-12
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

The existing wet energy power generation materials have poor water resistance and mechanical properties in high temperature and high humidity environments, and lack self-repair capabilities, resulting in loss of electrical performance and reduced life.

Method used

A polymer crosslinking network is prepared by using bio-based glass polymer materials, through the ester bond and ether bond crosslinking reaction of tartaric acid or malic acid with 1,4-butanediol diglycidyl ether, which combines conductive metals or Graphite material forms a positive and negative electrode structure and generates current by using the wet-electric effect.

Benefits of technology

In a high humidity environment, the material can spontaneously generate voltage and current, which improves the durability and practicality of the wet-energy power generation system and achieves efficient energy conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930829A_ABST
    Figure CN118930829A_ABST
Patent Text Reader

Abstract

The invention provides a bio-based glass polymer humidity power generation system and a preparation method thereof, belongs to the technical field of green energy power generation, and prepares a bio-based glass polymer material which can cooperate with an electrode to generate electric energy under the condition of humidity gradient. The bio-based glass macromolecules are solids formed by polymerization reaction of tartaric acid or malic acid or citric acid and 1, 4-butanediol diglycidyl ether. When the bio-based glass-like high polymer material is between the positive electrode material and the negative electrode material, high-efficiency output of current can be realized under the conditions of normal temperature and humidity gradient. The material has the advantages of being low in preparation cost, high in environment resistance, stable in energy output, capable of being repeatedly used and degradable and recycled, electric energy can be generated by absorbing water vapor in the natural environment, and the material can be applied to the field of green energy and has wide application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of green energy power generation, and in particular relates to a bio-based glass polymer humidity power generation system and a preparation method thereof. Background Art

[0002] Electricity has become an indispensable part of human life. In the face of energy shortage, the use of new energy is also being developed. In recent years, a series of materials have been used for wet power generation and hydropower generation, but their water resistance and mechanical properties are poor. The material structure is easily damaged and decomposed in high temperature and high humidity environments, and lacks self-repair ability. Accidental damage will cause loss of electrical performance, reducing its life and practicality.

[0003] Glass-like polymer materials are recyclable, weldable, reshapeable, easily chemically degradable, and biocompatible, and have shown good application prospects in many fields such as recyclable adhesives, self-healing coatings, and carbon fiber composites. Bio-based synthesis of glass-like polymers ensures a wide range of raw material sources.

[0004] The principle of the wet electric effect mainly involves the hygroscopic properties of biomass nanofiber materials. The surfaces of these materials are rich in hydrophilic groups, such as hydroxyl groups and carboxyl groups. When airflow with high humidity passes through these materials, the steam will be captured in the form of bound water and free water to form a double electric layer, thereby generating a flow potential. In addition, groups such as carboxyl groups and amino groups in biomass nanofibers can dissociate into freely moving ions to form ion transmission channels, further generating a potential difference and thus generating an electric current. According to the wet electric effect, in materials containing a large number of hydroxyl groups, moisture will react with hydroxyl groups, thereby causing hydroxyl groups to generate carriers. The gradient distribution of functional groups allows the carriers to diffuse from a high concentration section to a low concentration section, thereby forming voltage and current, and realizing the output of electrical energy. Since the movement of carriers is completely spontaneous, this energy conversion method has a high efficiency. Summary of the invention

[0005] The purpose of the present invention is to prepare a bio-based glass polymer wet gas power generation system, comprising a positive electrode material, a negative electrode material and a bio-based glass polymer material, wherein the bio-based glass polymer material is sandwiched between the positive electrode material and the negative electrode material; wherein the positive electrode material is a conductive metal or graphite, and at least one opening is provided on the positive electrode material, and the negative electrode material is a complete conductive metal or graphite sheet, and the bio-based glass polymer material is a solid obtained by polymerization reaction of tartaric acid or malic acid or citric acid and 1,4-butanediol diglycidyl ether; its general structural formula is shown in Figure 1 , Figure 2 and Figure 3 shown.

[0006] A preparation method of a bio-based glass polymer humidity power generation system, the preparation method of the bio-based glass polymer material comprising the following steps: dissolving tartaric acid in water, preheating 1,4-butanediol diglycidyl ether at 90±5°C, mixing the tartaric acid aqueous solution with 1,4-butanediol diglycidyl ether, stirring at 120-130°C to obtain a light yellow homogeneous solution; preheating the light yellow homogeneous solution on a flat plate vulcanizer at 150-170°C to obtain a viscous liquid, and pressurizing and heat-insulating at 150-170°C after exhaust treatment to obtain the bio-based glass polymer material.

[0007] At least two holes are made on the positive electrode material, the bio-based glass polymer material is cut into blocks, and placed between the positive electrode material and the negative electrode material to ensure that the bio-based glass polymer material touches and conducts electricity with the positive electrode material and the negative electrode material, and the blocks are aligned and fixed to ensure that moisture can enter the bio-based glass polymer material, thereby obtaining a bio-based glass polymer wet gas power generation system.

[0008] Wherein, the tartaric acid is either malic acid or citric acid.

[0009] Wherein, the molar ratio of the tartaric acid or malic acid or citric acid to 1,4-butanediol diglycidyl ether is 0.8-1.2.

[0010] Wherein, the stirring treatment time is 6.5-7.5h, and the stirring speed is 200-250r / min.

[0011] Wherein, the preheating time is 40 to 80 minutes.

[0012] Among them, the exhaust treatment is to pressurize to 20-25Mpa, release the pressure after reaching the pressure requirement, and perform exhaust operations at least twice in succession.

[0013] The pressurized heat preservation treatment time is 4 to 6 hours, and the pressure is 8 to 12 MPa.

[0014] Beneficial Effects

[0015] The present invention prepares a polymer cross-linked network connected by ester bonds and ether bonds by performing addition polymerization of L-(+)-tartaric acid and 1,4-butanediol diglycidyl ether. Under the condition of humidity gradient, voltage can be generated inside the material, so that current can be output externally.

[0016] The power generation principle of the wet gas power generation system prepared by the present invention is as follows: (1) The general room temperature is higher than the glass transition temperature of the material of the power generation system, that is, the polymer chain segments of the material are movable in a general environment. (2) Since the chain segments contain a large number of carboxyl groups and hydroxyl groups, the carboxyl groups and hydroxyl groups react with water molecules to release protons. After a large number of protons are accumulated, an ion concentration gradient is formed inside the material to promote the directional movement of protons, thereby forming an electric current. When the internal balance is reached, the water molecules are desorbed again, promoting the protons to move in the original direction, forming a secondary current. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 : A simplified structural diagram of the bio-based glass polymer prepared in Example 1 of the present invention.

[0018] Figure 2 : A simplified structural diagram of the bio-based glass polymer prepared in Example 4 of the present invention.

[0019] Figure 3 : A simplified structural diagram of the bio-based glass polymer prepared in Example 5 of the present invention.

[0020] Figure 4 : Schematic diagram of power generation principle of the present invention.

[0021] Figure 5 : Physical diagram of the matrix material structure of the present invention.

[0022] Figure 6 : Schematic diagram of the power generation state of the matrix material of the present invention. DETAILED DESCRIPTION

[0023] In the embodiment, the L-(+)-tartaric acid, D-(+)-tartaric acid, DL-(+)-tartaric acid, malic acid, citric acid, and 1,4-butanediol diglycidyl ether are all purchased from Anaiji Chemical, the wires, copper sheets, and aluminum sheets are all purchased from Taobao, and the multimeter is OWON B41T.

[0024] Example 1

[0025] This embodiment provides a method for preparing a bio-based glass polymer wet gas power generation system, wherein the bio-based glass polymer wet gas power generation system comprises a bio-based glass polymer material, a positive electrode material and a negative electrode material. The specific preparation method is as follows:

[0026] (1) Preparation method of bio-based glass polymer.

[0027] Weigh 24.25g of L-(+)-tartaric acid and dissolve it in 30mL of water. Weigh 38.88g of 1,4-butanediol diglycidyl ether (the molar ratio of tartaric acid to epoxy resin is 0.8) and preheat it in a 90℃ oil bath. Add L-(+)-tartaric acid aqueous solution dropwise to 1,4-butanediol diglycidyl ether and stir with a stirrer at a speed of 250r / min. Adjust the temperature of the oil bath to 120℃, heat and stir for 7.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 160℃ flat plate vulcanizer for 40min. After preheating, quickly pressurize the mold to 20Mpa for exhaust operation for 5 consecutive times. Finally, the material is cured at 160℃ for 5h. A light yellow transparent solid is obtained, which is a L-TA / BDE bio-based material. The structural formula of the light yellow transparent solid is shown in Figure 1 shown.

[0028] (2) Preparation methods of positive and negative electrode materials.

[0029] In this embodiment, a 3.5cm×1.8cm×0.1cm copper sheet is used as the positive electrode, and four small holes with a diameter of 2mm are made on the top of the copper electrode. A seamless 3.5cm×1.8cm×0.1cm copper sheet is used as the negative electrode.

[0030] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0031] The L-TA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm×1.8 cm×0.1 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the L-TA / BDE bio-based material touches and conducts electricity with the positive electrode material and the negative electrode material, and is aligned and fixed. The fixing method is to tighten the material with a clip, and ensure that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0032] (4) Measurement of output voltage of wet gas power generation system.

[0033] Connect the assembled wet gas power generation system with a multimeter, adjust the multimeter to V, and measure the output voltage. The data is shown in the following table.

[0034] Example 1 Output voltage of wet gas power generation system under copper electrode

[0035]

[0036]

[0037] Example 2

[0038] This embodiment provides a method for preparing a bio-based glass polymer wet gas power generation system, wherein the bio-based glass polymer wet gas power generation system comprises a bio-based glass polymer material, a positive electrode material and a negative electrode material. The specific preparation method is as follows:

[0039] (1) Preparation method of bio-based glass polymer.

[0040] Weigh 24.25g D-(+)-tartaric acid and dissolve it in 30mL water, weigh 32.68g 1,4-butanediol diglycidyl ether (the molar ratio of tartaric acid to epoxy resin is 1) and preheat it in an 85℃ oil bath. Add 1,4-butanediol diglycidyl ether to the D-(+)-tartaric acid aqueous solution and stir with a stirrer at a speed of 200r / min. Adjust the temperature of the oil bath to 125℃, heat and stir for 6.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 170℃ flat vulcanizer for 40min. After preheating, quickly pressurize the mold to 25Mpa for exhaust operation, twice in a row. Finally, the material is cured, and the curing process is 170℃ for 4h. A light yellow transparent solid is obtained, which is a D-TA / BDE bio-based material.

[0041] (2) Preparation methods of positive and negative electrode materials.

[0042] In this embodiment, a 3.5cm×1.8cm×0.1cm copper sheet is used as the positive electrode, and two small holes with a diameter of 2mm are made on the top of the copper electrode. A seamless 3.5cm×1.8cm×0.1cm aluminum sheet is used as the negative electrode.

[0043] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0044] The D-TA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm × 1.8 cm × 0.1 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the D-TA / BDE bio-based material touches and conducts electricity with the positive electrode material and the negative electrode material, and is aligned and fixed. The fixing method is to tighten the material with a clip, and ensure that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0045] (4) Measurement of output voltage of wet gas power generation system

[0046] Connect the assembled wet gas power generation system with a multimeter, adjust the multimeter to V, and measure the output voltage. The data is shown in the following table.

[0047] Example 2 Output voltage of wet gas power generation system under aluminum electrode

[0048]

[0049]

[0050] Example 3

[0051] This embodiment provides a method for preparing a bio-based glass polymer wet gas power generation system, wherein the bio-based glass polymer wet gas power generation system comprises a bio-based glass polymer material, a positive electrode material and a negative electrode material. The specific preparation method is as follows:

[0052] (1) Preparation method of bio-based glass polymer.

[0053] Weigh 24.71g DL-(+)-tartaric acid and dissolve it in 30mL hot water. Weigh 27.65g 1,4-butanediol diglycidyl ether (the molar ratio of tartaric acid to epoxy resin is 1.2) and preheat it in a 95℃ oil bath. Add 1,4-butanediol diglycidyl ether to the DL-(+)-tartaric acid aqueous solution and stir with a stirrer at a speed of 250r / min. Adjust the temperature of the oil bath to 120℃, heat and stir for 7.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 150℃ flat vulcanizer for 80min. After preheating, quickly pressurize the mold to 25Mpa for exhaust operation for 5 consecutive times. Finally, the material is cured at 150℃ for 6h. A light yellow transparent solid is obtained, which is a DL-TA / BDE bio-based material.

[0054] (2) Preparation methods of positive and negative electrode materials.

[0055] In this embodiment, a 3.5cm×1.8cm×0.1cm graphite sheet is used as the positive electrode, and 8 small holes with a diameter of 1.5mm are made on the top of the graphite electrode. A seamless 3.5cm×1.8cm×0.1cm aluminum sheet is used as the negative electrode.

[0056] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0057] The DL-TA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm×1.8 cm×0.1 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the DL-TA / BDE bio-based material touches and conducts electricity with the positive electrode material and the negative electrode material, and is aligned and fixed. The fixing method is to tighten the material with a clip, and ensure that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0058] (4) Measurement of output voltage of wet gas power generation system

[0059] Connect the assembled wet gas power generation system with a multimeter, adjust the multimeter to V, and measure the output voltage. The data is shown in the following table.

[0060] Example 3 Output voltage of wet gas power generation system under graphite aluminum electrode

[0061]

[0062]

[0063] Example 4

[0064] This embodiment provides a method for preparing a bio-based glass polymer wet gas power generation system, wherein the bio-based glass polymer wet gas power generation system comprises a bio-based glass polymer material, a positive electrode material and a negative electrode material. The specific preparation method is as follows:

[0065] (1) Preparation method of bio-based glass polymer.

[0066] Weigh 24.25g of hydrated citric acid and dissolve it in 30mL of hot water to obtain a citric acid solution. Weigh 21.41g of 1,4-butanediol diglycidyl ether (the molar ratio of hydrated citric acid to epoxy resin is 1) and preheat it in a 90°C oil bath. Add citric acid aqueous solution dropwise to 1,4-butanediol diglycidyl ether and stir with a stirrer at a speed of 250r / min. Adjust the temperature of the oil bath to 120°C, heat and stir for 7.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 160°C flat plate vulcanizer for 40min. After preheating, quickly pressurize the mold to 20Mpa for exhaust operation for 5 consecutive times. Finally, the material is cured at 160°C for 5h. A light yellow transparent solid is obtained, which is a CA / BDE bio-based material. The structural formula of the light yellow transparent solid is shown in Figure 2 shown.

[0067] (2) Preparation methods of positive and negative electrode materials.

[0068] In this embodiment, the positive electrode is a 3.5cm×1.8cm×0.1cm aluminum sheet, and four small holes with a diameter of 2mm are made on the top of the copper electrode. The negative electrode is a seamless 3.5cm×1.8cm×0.1cm copper sheet.

[0069] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0070] The CA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm×1.8 cm×0.1 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the CA / BDE bio-based material touches and is conductive to the positive electrode and the negative electrode, and aligned and fixed. Tape is selected as the fixing method, and it is ensured that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0071] (4) Measurement of output voltage of wet gas power generation system

[0072] Connect the assembled wet gas power generation system with a multimeter, adjust the multimeter to V, and measure the output voltage. The data is shown in the following table.

[0073] Example 4 Output voltage of wet gas power generation system under copper-aluminum electrodes

[0074]

[0075]

[0076] Example 5

[0077] This embodiment provides a method for preparing a bio-based glass polymer wet gas power generation system, wherein the bio-based glass polymer wet gas power generation system comprises a bio-based glass polymer material, a positive electrode material and a negative electrode material. The specific preparation method is as follows:

[0078] (1) Preparation method of bio-based glass polymer.

[0079] Weigh 24.25g of malic acid and dissolve it in 30mL of water to obtain a malic acid aqueous solution. Weigh 33.56g of 1,4-butanediol diglycidyl ether (the molar ratio of malic acid to epoxy resin is 1.1) and preheat it in a 90°C oil bath. Add the malic acid aqueous solution dropwise to 1,4-butanediol diglycidyl ether and stir with a stirrer at a speed of 250r / min. Adjust the temperature of the oil bath to 120°C, heat and stir for 7.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 160°C flat plate vulcanizer for 40min. After preheating, quickly pressurize the mold to 20Mpa for exhaust operation for 5 consecutive times. Finally, the material is cured at 160°C for 5h. A light yellow transparent solid is obtained, which is a MA / BDE bio-based material. The structural formula of the light yellow transparent solid is shown in Figure 3 shown.

[0080] (2) Preparation methods of positive and negative electrode materials.

[0081] In this embodiment, a 3.5cm×1.8cm×0.1cm copper sheet is used as the positive electrode, and four small holes with a diameter of 2mm are made on the top of the copper electrode. A seamless 3.5cm×1.8cm×0.1cm copper sheet is used as the negative electrode.

[0082] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0083] The MA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm × 1.8 cm × 0.1 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the MA / BDE bio-based material touches the positive electrode material and the negative electrode material and is conductive, and aligned and fixed by tying with a rubber band, and ensuring that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0084] (4) Measurement of output voltage of wet gas power generation system

[0085] Connect the assembled wet gas power generation system with a multimeter, adjust the multimeter to V, and measure the output voltage. The data is shown in the following table.

[0086] Example 1 Output voltage of wet gas power generation system under copper electrode

[0087]

[0088]

[0089] Example 6

[0090] (1) Preparation method of bio-based glass polymer.

[0091] Weigh 24.25g L-(+)-tartaric acid and dissolve it in 30mL hot water, weigh 38.88g 1,4-butanediol diglycidyl ether and preheat it in a 90℃ oil bath (the molar ratio of tartaric acid to epoxy resin is 0.8). Add 1,4-butanediol diglycidyl ether to the L-(+)-tartaric acid aqueous solution and stir with a stirrer at a speed of 250r / min. Adjust the temperature of the oil bath to 120℃, heat and stir for 7.5h to obtain a light yellow homogeneous solution. Pour the light yellow homogeneous solution into a mold with release paper and preheat it on a 160℃ flat vulcanizer for 40min. After preheating, quickly pressurize the mold to 20Mpa for exhaust operation for 5 consecutive times. Finally, the material is cured at 160℃ for 5h. A light yellow transparent solid is obtained.

[0092] (2) Preparation methods of positive and negative electrode materials.

[0093] In this embodiment, the positive electrode is a 3.5cm×1.8cm×0.1cm iron sheet, and four small holes with a diameter of 2mm are made on the top of the iron electrode. The negative electrode is a seamless 3.5cm×1.8cm×0.1cm iron sheet.

[0094] (3) Assembly of bio-based glass polymer wet gas power generation system.

[0095] The MA / BDE bio-based material prepared in step (1) is cut into blocks of 3.5 cm × 1.8 cm × 0.2 cm, and placed between the positive electrode and the negative electrode prepared in step (2), ensuring that the TA / BDE bio-based material touches the positive electrode material and the negative electrode material and is conductive, aligned and fixed, and fixed by rubber bands, and ensuring that moisture can effectively enter the material to obtain a bio-based glass polymer wet gas power generation system.

[0096] (3) Use a bio-based glass polymer moisture power generation system to light up a small light bulb.

[0097] Connect the positive and negative electrodes of the assembled moisture power generation system to the positive and negative electrodes of the small light bulb respectively. When moisture is present, the light bulb will light up.

[0098] Obviously, the present invention proposes a bio-based glass polymer wet gas power generation system, the size of its positive and negative electrode materials and bio-based glass polymer materials will not affect the operation of its power generation system. The larger the material, the greater the power generation.

Claims

1. A bio-based glass polymer humidity power generation system, characterized by: The bio-based glass polymer humidity power generation system comprises a positive electrode material, a negative electrode material and a bio-based glass polymer material, wherein the bio-based glass polymer material is sandwiched between the positive electrode material and the negative electrode material; wherein the positive electrode material is a conductive metal or graphite, and at least one opening is provided on the positive electrode material, and the negative electrode material is a complete conductive metal or graphite sheet, and the bio-based glass polymer material is a solid obtained by polymerization reaction of tartaric acid or malic acid or citric acid and 1,4-butanediol diglycidyl ether; and its general structural formula is as follows:

2. A method for preparing the bio-based glass polymer humidity power generation system according to claim 1, characterized in that: The preparation method of the bio-based glass polymer material comprises the following steps: dissolving tartaric acid in water, preheating 1,4-butanediol diglycidyl ether at 90±5° C., mixing the aqueous solution of tartaric acid and 1,4-butanediol diglycidyl ether, and stirring at 120-130° C. to obtain a light yellow homogeneous solution; preheating the light yellow homogeneous solution on a flat plate vulcanizer at 150-170° C. to obtain a viscous liquid, and pressurizing and heat-insulating at 150-170° C. after exhaust treatment to obtain the bio-based glass polymer material; At least two holes are made on the positive electrode material, the bio-based glass polymer material is cut into blocks, and placed between the positive electrode material and the negative electrode material to ensure that the bio-based glass polymer material touches and conducts electricity with the positive electrode material and the negative electrode material, and the blocks are aligned and fixed to ensure that moisture can enter the bio-based glass polymer material, thereby obtaining a bio-based glass polymer wet gas power generation system.

3. The method for preparing the bio-based glass polymer humidity power generation system according to claim 2, characterized in that: The tartaric acid is either malic acid or citric acid.

4. The bio-based glass polymer humidity power generation system and preparation method thereof according to claim 3, characterized in that: The molar ratio of the tartaric acid or malic acid or citric acid to 1,4-butanediol diglycidyl ether is 0.8-1.

2.

5. The bio-based glass polymer humidity power generation system and preparation method thereof according to claim 3, characterized in that: The stirring treatment time is 6.5-7.5h, and the stirring speed is 200-250r / min.

6. The bio-based glass polymer humidity power generation system and preparation method thereof according to claim 3, characterized in that: The preheating time is 40 to 80 minutes.

7. The bio-based glass polymer humidity power generation system and preparation method thereof according to claim 3, characterized in that: The exhaust treatment is to pressurize to 20-25Mpa, release the pressure after reaching the pressure requirement, and perform exhaust operation at least twice in succession.

8. The bio-based glass polymer humidity power generation system and preparation method thereof according to claim 3, characterized in that: The pressurized heat preservation treatment time is 4 to 6 hours, and the pressure is 8 to 12 MPa.

Citation Information

Patent Citations

  • Composition containing hydroxylated condensation resin for forming film under resist

    CN101473270A

  • Cathode active material for secondary battery, and secondary battery comprising same

    CN107408678A

  • Polyurethane waterproof coating and preparation method thereof

    CN113072869A

  • Polymer moisture generator based on porous support, preparation method and application thereof

    CN116247969A

  • Glass body having high proton conductivity and method for producing the same, water electrolysis apparatus, gas generating apparatus, fuel cell and hydrogen sensor

    JP2003192380A