Thermoplastic polyolefin waterproof roll as well as preparation method and application thereof

By using a composite system of modified magnesium hydroxide and phosphorus-nitrogen flame retardants in thermoplastic polyolefin waterproof coils, the influence of traditional TPO waterproof coils on color and performance is solved, and a white appearance and low water absorption are achieved. and high aging resistance.

CN118931002APending Publication Date: 2024-11-12KESHUN WATERPROOF TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410991125.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After adding flame retardant, traditional thermoplastic polyolefin (TPO) waterproof coils are easily affected by their color and waterproof performance, and have poor aging resistance.

Method used

Compound flame retardants, including modified magnesium hydroxide and phosphorus-nitrogen flame retardants, are prepared with excellent flame retardant, low water absorption and high through specific mass ratios and modification treatments, combined with multivariate hindered phenol antioxidants. TPO waterproof coil material with aging resistance.

Benefits of technology

It realizes the white appearance of TPO waterproof coil, maintains excellent flame retardant performance, reduces water absorption, improves aging resistance, and meets environmental protection and economic benefits requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004958904760000101
    Figure BDA0004958904760000101
  • Figure BDA0004958904760000111
    Figure BDA0004958904760000111
  • Figure BDA0004958904760000121
    Figure BDA0004958904760000121
Patent Text Reader

Abstract

The invention discloses a thermoplastic polyolefin waterproof coiled material and a preparation method and application thereof, the thermoplastic polyolefin waterproof coiled material comprises 70-78% of thermoplastic polyolefin resin, 19-27% of a composite flame retardant, 0.9-3% of an antioxidant and 0.9-3% of a color master batch based on the weight of the waterproof coiled material; wherein the composite flame retardant comprises modified magnesium hydroxide and a phosphorus-nitrogen flame retardant. The waterproof coiled material has excellent flame retardance, low water absorption and excellent aging resistance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of building waterproofing, and in particular to a thermoplastic polyolefin waterproofing coiled material and a preparation method and application thereof. Background Art

[0002] In traditional technology, flame retardants are usually added to thermoplastic polyolefin (TPO) waterproof membranes to provide flame retardant effects of thermoplastic polyolefin waterproof membranes. Considering factors such as environmental protection and economic benefits, the flame retardants used in flame retardant thermoplastic polyolefin waterproof membranes are usually inorganic flame retardants or phosphorus-nitrogen flame retardants.

[0003] These commonly used flame retardants usually have some adverse effects on the performance of TPO waterproof membranes, especially on the color or waterproof performance of the waterproof membranes. Therefore, it is necessary to further improve the performance of TPO waterproof membranes, for example, while ensuring its flame retardancy, taking into account water absorption and aging resistance. Summary of the invention

[0004] In view of this, the present invention provides a thermoplastic polyolefin waterproof roll material and a preparation method and use thereof. The waterproof roll material has excellent flame retardancy, low water absorption and excellent aging resistance.

[0005] The present invention provides the following technical solutions:

[0006] A thermoplastic polyolefin waterproofing coiled material comprises 70-78% of thermoplastic polyolefin resin, 19-27% of composite flame retardant, 0.9-3% of antioxidant, and 0.9-3% of masterbatch, based on the weight of the waterproofing coiled material; wherein the composite flame retardant comprises modified magnesium hydroxide and phosphorus nitrogen flame retardant.

[0007] The present invention provides the following non-conventional alternatives:

[0008] The mass ratio of the modified magnesium hydroxide to the phosphorus-nitrogen flame retardant is (1-3):1.

[0009] The phosphorus-nitrogen flame retardant is a polyolefin flame retardant masterbatch containing phosphorus and nitrogen or melamine phosphate.

[0010] The phosphorus-nitrogen flame retardant is a polyolefin flame retardant masterbatch containing phosphorus and nitrogen, wherein the polyolefin is a carrier.

[0011] The modified magnesium hydroxide is magnesium hydroxide modified by a modifier, wherein the modifier comprises silane or C16-20 alkyl carboxylic acid.

[0012] The C16-20 alkyl carboxylic acid is stearic acid.

[0013] In the modified magnesium hydroxide, the content of magnesium oxide is 60% to 69% or the content of magnesium hydroxide is 80% to 95%, based on the weight of the modified magnesium hydroxide.

[0014] The antioxidant is a mixture of a polyhydric hindered phenol antioxidant and a phosphite antioxidant, wherein the weight ratio of the polyhydric hindered phenol antioxidant to the phosphite antioxidant is 1:2-2:1.

[0015] The present invention also provides a method for preparing the thermoplastic polyolefin waterproof roll material as described above, which comprises: providing a composite flame retardant comprising modified magnesium hydroxide and a phosphorus nitrogen flame retardant; mixing a thermoplastic polyolefin resin, the composite flame retardant, an antioxidant, and a masterbatch, melt-extruding, shaping, and cooling, thereby obtaining the thermoplastic polyolefin waterproof roll material.

[0016] The present invention also provides use of the thermoplastic polyolefin waterproof membrane as described above for waterproofing the surface of a building.

[0017] According to the technical solution of the present invention, the thermoplastic polyolefin waterproofing membrane contains a specific amount of composite flame retardant, and the composite flame retardant includes modified magnesium hydroxide and phosphorus nitrogen flame retardant. The composite flame retardant itself is white and does not affect the original appearance of the thermoplastic polyolefin waterproofing membrane; at the same time, the modified magnesium hydroxide, due to its low polarity, not only improves its dispersion effect in non-polar polyolefin materials, but also can effectively reduce the water absorption rate of the waterproofing membrane; and the phosphorus nitrogen flame retardant can effectively reduce the amount of modified magnesium hydroxide used, further reducing the impact of the addition of conventional inorganic flame retardants on the aging resistance and other properties of the waterproofing membrane. Therefore, the thermoplastic polyolefin waterproofing membrane has a white appearance, excellent flame retardancy, low water absorption and excellent aging resistance. DETAILED DESCRIPTION

[0018] For ease of understanding of the present invention, the present invention will be described more fully below with reference to examples. Preferred embodiments of the present invention are provided in the examples. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0019] In traditional technology, in order to improve the flame retardancy of TPO waterproofing membranes, phosphorus-nitrogen flame retardants and carbon black are usually added as flame retardants in some TPO waterproofing membranes, but this will make the appearance of the waterproofing membrane black, resulting in increased absorption of solar heat by the waterproofing membrane, thereby reducing the aging resistance of the waterproofing membrane. Some TPO waterproofing membranes add inorganic flame retardants, such as aluminum hydroxide, magnesium hydroxide, zinc borate, etc., and the amount added can usually reach up to 50% of the weight of the TPO waterproofing membrane. These inorganic flame retardants are polar materials, while the main component of TPO waterproofing membranes, thermoplastic polyolefin resin, is a non-polar material. Therefore, when the amount of inorganic flame retardant added is too much, it is easy to cause the inorganic flame retardant to be unevenly dispersed in the thermoplastic polyolefin resin, which causes the physical and mechanical properties of the prepared TPO waterproofing membrane to be adversely affected, and causes the water absorption rate of the waterproofing membrane to increase, thereby reducing the anti-penetration ability of the waterproofing membrane. The thermoplastic polyolefin waterproofing membrane of this embodiment contains a specific amount of composite flame retardant, and the composite flame retardant includes modified magnesium hydroxide and phosphorus nitrogen flame retardant. Therefore, the thermoplastic polyolefin waterproofing membrane has a white appearance, and has low water absorption (i.e., high waterproof performance) and excellent aging resistance while having excellent flame retardancy.

[0020] The thermoplastic polyolefin waterproof roll material of this embodiment includes 70-78% of thermoplastic polyolefin resin, 19-27% of composite flame retardant, 0.9-3% of antioxidant, and 0.9-3% of masterbatch, based on the weight of the waterproof roll material; the sum of the weight percentages of the components in the thermoplastic polyolefin waterproof roll material is 100%, based on the weight of the waterproof roll material; wherein the composite flame retardant includes modified magnesium hydroxide and phosphorus nitrogen flame retardant.

[0021] Thermoplastic polyolefin resin TPO is usually in granular form with a density of 0.800-0.980g / cm 3 , measured at 23°C according to ISO1183; the melt index is 0.60-14g / 10min, such as 0.6-1.5g / 10min, 0.8-1.2g / 10min, measured at 230°C under a load of 2.16kg according to ISO1133. The melt index is an important parameter of thermoplastic polyolefin resin TPO used for waterproofing membranes in the form of a single substance or a mixture, which is used to measure the relative molecular mass of the product. The higher the melt flow rate, the lower the relative molecular mass. TPO may include one or more of the following: CA10A, CA60A purchased from LyondellBasell Industries of the Netherlands; NS06 purchased from Sinopec; 3020, 6102, 3000 purchased from ExxonMobil. TPO may be a mixture of two or more TPO resins, and the melt index of the mixture meets the above requirements.

[0022] In the composite flame retardant, the mass ratio of modified magnesium hydroxide to phosphorus nitrogen flame retardant is (1-3): 1, for example, 3: 1. In the TPO waterproofing membrane, the weight ratio of the composite flame retardant to TPO is (0.25-0.4): 1, for example, 0.25:1.

[0023] Phosphorus-nitrogen flame retardants are polyolefin flame retardant masterbatches or melamine phosphates containing phosphorus and nitrogen, such as polyolefin flame retardant masterbatches containing phosphorus and nitrogen. Melamine phosphates can be obtained by reacting phosphates with melamine and its derivatives; they usually include one or more of the following: melamine orthophosphate, melamine pyrophosphate, dimelamine pyrophosphate, and melamine polyphosphate. The phosphorus content of melamine phosphate is >14%, the nitrogen content is >42%, and the density is 1.72-1.75g / cm 3 The polyolefin flame retardant masterbatch containing phosphorus and nitrogen uses polyolefin, such as thermoplastic polyolefin TPO, as a carrier to load the flame retardant material containing phosphorus and nitrogen. The thermoplastic polyolefin carrier can be the same as or different from the above TPO, for example, the same. The polyolefin flame retardant masterbatch is usually white particles, does not contain halogen elements and heavy metal elements, and has a density of 1.5g / cm 3 The phosphorus content is at least 19%, and the nitrogen content is at least 18%, based on the weight of the flame retardant masterbatch. For example, the polyolefin flame retardant masterbatch containing phosphorus and nitrogen can be 5250M purchased from Guangdong Shunde Tongcheng New Material Technology Co., Ltd.

[0024] Modified magnesium hydroxide is magnesium hydroxide modified by a modifier, wherein the modifier includes silane or C16-20 alkyl carboxylic acid. Modified magnesium hydroxide can be a commercially available product commonly used in the art or prepared by a method commonly used by those skilled in the art, such as modifying magnesium hydroxide by a modifier, specifically, dispersing magnesium hydroxide in water to form a magnesium hydroxide suspension; dissolving the modifier in a solvent such as ethanol to form a modified solution; heating the magnesium hydroxide suspension to 40-80°C, dripping the modified solution dropwise into the magnesium hydroxide suspension, stirring the reaction for 1-2h, and maintaining the speed within the range of 400-600r / min. After the reaction is completed, washing with distilled water and drying can obtain modified magnesium hydroxide. The content of magnesium oxide in the silane-modified magnesium hydroxide is 60% to 69%, such as 61%, 64%, 66%, 67.8%, 68% or 68.9%, etc., based on the weight of the modified magnesium hydroxide. The silane may be a silane or a silane coupling agent known to those skilled in the art, for example, it may include one or more of the following: monosilane, disilane, n-octyl triethoxysilane, vinyl triethoxysilane, vinyl-tri(2-methoxyethoxy)silane, γ-aminopropyl triethoxysilane, γ-(2,3-epoxypropoxy)propyl trimethoxysilane, γ-methacryloxypropyl trimethoxysilane, N-(β-aminoethyl)-γ-aminopropyl trimethoxy (or ethyl) silane. The content of magnesium hydroxide in the C16-20 alkyl carboxylic acid modified magnesium hydroxide is 80-95%, for example, 88-92%, for example, 89%, 90% or 90.8%. The C16-20 alkyl carboxylic acid may include stearic acid, hexadecanoic acid or eicosanoic acid, for example, the chemical formula of stearic acid (octadecanoic acid) is C 18 H 36 O2, molecular weight is 284.48. For example, the modified magnesium hydroxide can be silane-modified magnesium hydroxide ZH-E6-1 and stearic acid-modified magnesium hydroxide ZH-E6-Y purchased from Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.

[0025] The antioxidant may be a commonly used antioxidant known to those skilled in the art, for example, a mixture of a polyhedral hindered phenol antioxidant and a phosphite antioxidant, wherein the weight ratio of the polyhedral hindered phenol antioxidant to the phosphite antioxidant is 1:2-2:1. The polyhedral hindered phenol antioxidant may include one or more of tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate]pentaerythritol ester and 1,3,5-tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanuric acid, for example, antioxidant 1010 or 3114 purchased from BASF, Germany; the phosphite antioxidant may include one or more of tris[2,4-di-tert-butylphenyl]phosphite and bis(2,4-di-tert-butylphenol)pentaerythritol diphosphite, for example, antioxidant 168 or 626 purchased from BASF, Germany. The antioxidant may be a combination of antioxidant 1010 or 3114 and antioxidant 168 or 626.

[0026] The masterbatch can be any color masterbatch particles commonly used in the art except black, such as white pigments, blue pigments, etc. The white pigments are usually a mixture of titanium dioxide and a thermoplastic polyolefin resin carrier, which contains more than 80% of titanium dioxide, based on the weight of the masterbatch. The tinting strength of the white pigment (also called white masterbatch) is 95%-105%, and the density is 1.70g / cm 3 -2.00g / cm 3 The thermoplastic polyolefin resin carrier may be the same as or different from the above TPO, for example, the same as the above TPO. The blue pigment filler may be selected from one or more of ultramarine, iron blue, or cobalt blue.

[0027] Those skilled in the art can arrange reinforcing materials or backing materials, such as polyester mesh cloth or non-woven fabric, inside or on the surface of the TPO waterproof membrane as required.

[0028] In this embodiment, the method for preparing the thermoplastic polyolefin waterproof membrane as described above includes: providing a composite flame retardant including modified magnesium hydroxide and a phosphorus nitrogen flame retardant; uniformly mixing the thermoplastic polyolefin resin, the composite flame retardant, the antioxidant, and the masterbatch, melt-extruding, shaping, and cooling, thereby obtaining the thermoplastic polyolefin waterproof membrane.

[0029] The mixture is usually conveyed to a single-screw or twin-screw extruder for melt extrusion at a temperature of 180-220° C., such as 190-210° C., and is shaped, cooled, trimmed, and rolled up by three rollers to obtain a TPO waterproof membrane.

[0030] TPO waterproofing membrane is used for waterproofing of building surfaces. For example, TPO waterproofing membrane can be used as the waterproofing layer of exposed or non-exposed roofs and underground waterproofing of buildings; it can also be used in waterproofing and moisture-proofing projects such as drinking water reservoirs, toilets, basements, tunnels, grain depots, subways, reservoirs, etc.

[0031] The present invention is described below by specific examples. The examples described below are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this area or the product instructions are used. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be obtained commercially.

[0032] raw material

[0033] TPO:

[0034] CA10A: Density 0.880g / cm 3 ; Melt index is 0.6g / 10min, purchased from Anderbasel Industries, The Netherlands

[0035] CA60A: Density 0.880g / cm 3 ; Melt index is 14g / 10min, purchased from Anderbasel Industries, Netherlands

[0036] NS06: Density 0.880g / cm 3 ; Melt index is less than 1g / 10min, purchased from China Petrochemical Corporation

[0037] Modified magnesium hydroxide:

[0038] Silane-modified magnesium hydroxide ZH-E6-1, 61% MgO, purchased from Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.;

[0039] Stearic acid modified magnesium hydroxide ZH-E6-Y, with a magnesium hydroxide content of 90%, was purchased from Jiangsu Zehui Magnesium-based New Material Technology Co., Ltd.;

[0040] Phosphorus and nitrogen flame retardants:

[0041] 5250M, TPO as carrier, purchased from Guangdong Shunde Tongcheng New Materials Technology Co., Ltd.;

[0042] Melamine phosphate: 7564, phosphorus content>14%, nitrogen content>42%, density 1.73g / cm 3 , purchased from Shanghai Xiangu Chemical Co., Ltd.;

[0043] Color masterbatch:

[0044] White masterbatch: Model HT84997, tinting strength 100%, density 1.90g / cm 3 , purchased from Heshan Hancai Masterbatch Co., Ltd.

[0045] Example 1

[0046] 1) Provide composite flame retardant

[0047] 750 g of ZH-E6-1 modified magnesium hydroxide and 250 g of 5250M were fully mixed to obtain a composite flame retardant.

[0048] 2) Preparation of waterproof membrane

[0049] i) Mixing: by weight, 70 parts of thermoplastic polyolefin resin CA10A, 10 parts of CA60A, 20 parts of the composite flame retardant prepared above, 2 parts of antioxidant (antioxidant 1010:168 weight ratio is 1:1) and 2 parts of white masterbatch are added into a blender and mixed evenly to obtain a mixture.

[0050] ii) Extrusion: The mixture is conveyed to a single screw extruder for melt extrusion at a temperature of 200° C., shaped by three rollers, cooled to room temperature, trimmed, and rolled to obtain a TPO waterproof membrane.

[0051] The types and contents of each component are summarized in Tables 1 and 2 below.

[0052] Example 2

[0053] The operating steps of Example 1 were repeated, except that the silane-modified magnesium hydroxide in the composite flame retardant was stearic acid-modified magnesium hydroxide ZH-E6-Y.

[0054] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0055] Example 3

[0056] The operation steps of Example 1 were repeated, except that 1) a composite flame retardant was provided: 500 g of ZH-E6-1 modified magnesium hydroxide and 500 g of 5250M were fully mixed to obtain a composite flame retardant. The composition and content of the relevant components are summarized in Tables 1 and 2.

[0057] Example 4

[0058] The operating steps of Example 2 were repeated, except that in the mixing step of 2) preparing the waterproof membrane, the antioxidant 168 was replaced by the antioxidant 626.

[0059] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0060] Example 5

[0061] The operating steps of Example 1 were repeated, except that in the step 2) of preparing the waterproof membrane, the weight ratio of the two antioxidants was 2:1.

[0062] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0063] Example 6

[0064] The operating steps of Example 1 were repeated, except that the type and content of the thermoplastic polyolefin resin were changed in the step 2) of preparing the waterproof membrane.

[0065] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0066] Example 7

[0067] The operating steps of Example 1 were repeated, except that the 5050M flame retardant was replaced by the 7564 flame retardant in 1) providing the composite flame retardant.

[0068] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0069] Examples 8-10

[0070] The operating steps of Example 1 were repeated, except that the amounts of the composite flame retardant, antioxidant and masterbatch were changed in the step 2) of preparing the waterproof membrane.

[0071] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0072] Embodiment 11

[0073] The operating steps of Example 1 were repeated, except that in the step of 2) preparing the waterproof membrane, the weight ratio of the two antioxidants in the antioxidant was changed to 1:2.

[0074] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0075] Example 12

[0076] The steps of Example 1 were repeated, except that in the step of 2) preparing the waterproof membrane, the mass ratio of antioxidant 1010:168 was 1:3.

[0077] Example 13

[0078] The steps of Example 12 were repeated, except that in the step of 2) preparing the waterproof membrane, the antioxidant 168 was replaced by the antioxidant 626.

[0079] Comparative Example 1

[0080] The steps of Example 1 were repeated, except that in the step of 1) providing a composite flame retardant, only the phosphorus-nitrogen flame retardant 5250M was used.

[0081] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0082] Comparative Example 2

[0083] The steps of Comparative Example 1 were repeated, except that the phosphorus-nitrogen flame retardant 5250M was replaced by magnesium hydroxide. The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0084] Comparative Example 3

[0085] The steps of Example 1 were repeated, except that in the step of 1) providing a composite flame retardant, the modified magnesium hydroxide in the composite flame retardant was replaced with magnesium hydroxide.

[0086] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0087] Comparative Example 4

[0088] The steps of Example 13 were repeated, except that in the step 2) of preparing the waterproof membrane, the amount of the antioxidant used was 40 parts by weight. The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0089] Comparative Example 5

[0090] The steps of Example 1 were repeated, except that in the step of 1) providing a composite flame retardant, only ZH-E6-1 modified magnesium hydroxide was used.

[0091] The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0092] Comparative Example 6

[0093] The steps of Example 1 were repeated, except that in the step 2) of preparing the waterproof coiled material, the amount of the antioxidant used was 0.5 parts by weight. The compositions and contents of the relevant components are summarized in Tables 1 and 2.

[0094] Table 1 Composition of flame retardants and antioxidants in waterproof membranes of various embodiments and comparative examples

[0095]

[0096] 1) The flame retardant refers to a composite flame retardant in the examples and refers to various components added as flame retardants in the comparative examples.

[0097] Table 2 Composition of the waterproof membrane of each embodiment and comparative example

[0098]

[0099] 1) The flame retardant refers to a composite flame retardant in the examples and refers to various components added as flame retardants in the comparative examples.

[0100] Performance Testing

[0101] Combustion performance (Limiting oxygen index)

[0102] The combustion performance test was carried out according to GB / T10707-2008.

[0103] Water absorption performance (water absorption rate)

[0104] Water absorption test is carried out according to GB 27789-2011. The lower the water absorption of the waterproof membrane, the stronger its anti-penetration ability and the better its waterproof performance.

[0105] UV resistance test

[0106] First, a tensile test was performed according to GB / T328.9-2007, with a tensile speed of 250 mm / min and a test gauge length of 25 mm; the tensile strength and elongation at break of the sample were recorded. Then the sample was placed in a UV irradiation test box, using a 500W UV high-pressure mercury lamp, a light temperature of 45°C, and a UV irradiation time of 30 days. After that, a tensile test was performed according to GB / T328.9-2007, with a tensile speed of 250 mm / min and a test gauge length of 25 mm; the tensile strength and elongation at break of the sample were recorded. The tensile strength retention rate and elongation at break retention rate of the sample were calculated.

[0107] Table 3 Performance test of waterproof membranes of various embodiments and comparative examples

[0108]

[0109]

[0110] It can be seen from the above examples that the TPO waterproofing membrane of this embodiment not only has a high limiting oxygen index, which is basically above 25, but also has a low water absorption rate, which is basically maintained below 3%, which is far lower than the national standard requirement (≤4.0%); at the same time, it has good aging resistance, and the tensile strength retention rate after 30 days of ultraviolet light irradiation is above 90%, and its appearance is white, which further improves its aging resistance. Moreover, it can be concluded from the above examples that the modified magnesium hydroxide and phosphorus nitrogen flame retardant in the composite flame retardant of this embodiment play a synergistic role in improving the performance of the TPO waterproofing membrane, such as flame retardancy and waterproof performance.

[0111] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions may occur depending on design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A thermoplastic polyolefin waterproofing membrane, characterized in that: The invention comprises 70-78% of thermoplastic polyolefin resin, 19-27% of composite flame retardant, 0.9-3% of antioxidant, and 0.9-3% of masterbatch, based on the weight of the waterproof roll; wherein The composite flame retardant comprises modified magnesium hydroxide and phosphorus-nitrogen flame retardant.

2. The waterproof coiled material according to claim 1, characterized in that: The mass ratio of the modified magnesium hydroxide to the phosphorus-nitrogen flame retardant is (1-3):

1.

3. The waterproof coiled material according to claim 1 or 2, characterized in that: The phosphorus-nitrogen flame retardant is a polyolefin flame retardant masterbatch containing phosphorus and nitrogen or melamine phosphate.

4. The waterproof coiled material according to claim 3, characterized in that: The phosphorus-nitrogen flame retardant is a polyolefin flame retardant masterbatch containing phosphorus and nitrogen, wherein the polyolefin is a carrier.

5. The waterproof coiled material according to claim 1 or 2, characterized in that: The modified magnesium hydroxide is magnesium hydroxide modified by a modifier, wherein the modifier comprises silane or C16-20 alkyl carboxylic acid.

6. The waterproof coiled material according to claim 5, characterized in that: The C16-20 alkyl carboxylic acid is stearic acid.

7. The waterproof coiled material according to claim 1 or 2, characterized in that: In the modified magnesium hydroxide, the content of magnesium oxide is 60% to 69% or the content of magnesium hydroxide is 80% to 95%, based on the weight of the modified magnesium hydroxide.

8. The waterproof coiled material according to claim 1 or 2, characterized in that: The antioxidant is a mixture of a polyhydric hindered phenol antioxidant and a phosphite antioxidant, wherein the weight ratio of the polyhydric hindered phenol antioxidant to the phosphite antioxidant is 1:2-2:

1.

9. A method for preparing the thermoplastic polyolefin waterproofing membrane according to any one of claims 1 to 8, characterized in that: include: Providing a composite flame retardant comprising modified magnesium hydroxide and a phosphorus-nitrogen flame retardant; Thermoplastic polyolefin resin, composite flame retardant, antioxidant and masterbatch are mixed, melt-extruded, shaped and cooled to obtain the thermoplastic polyolefin waterproof coiled material.

10. Use of the thermoplastic polyolefin waterproof membrane according to any one of claims 1 to 8 for waterproofing the surface of a building.