Low-odor food-grade polyethylene composition and preparation method thereof
Through the preparation of low-odor food-grade polyethylene compositions, the problems of large odor and poor processing fluidity of traditional polyethylene packaging materials are solved, the lubricity and aging resistance of the materials are improved, and the multiple performance needs of food-grade packaging are met.
Patent Information
- Application Number
- CN202411116467.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional polyethylene packaging materials have large odors, poor processing fluidity, and cannot meet food-grade requirements, and cannot meet the needs of hygiene, processing and mechanical properties at the same time.
Using low-odor food-grade polyethylene compositions, including linear high-density polyethylene powder, antioxidants, halogen absorbers and slippers, the high-speed stirring and twin-screw extrusion granulation process is used to prepare good processing performance. and food-grade polyethylene materials that are resistant to aging.
It improves the internal and external lubricity and aging resistance of the material, reduces the odor grade, and makes it suitable for food-grade packaging and meets the demand indicators of manufacturers.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyolefin materials, and specifically discloses a low-odor food-grade polyethylene composition and a preparation method thereof. Background Art
[0002] With the increasing improvement of people's living standards and quality of life and the accelerated pace of life, the consumption of instant foods such as pure water and milk has been rising year by year, driving the rapid growth of demand for food-grade polyethylene raw materials. At present, domestic polyethylene resins cannot meet the following three performance requirements at the same time: First, hygienic performance. This kind of food packaging needs to be in direct contact with milk, drinking water, etc. Due to the high attention paid by society and enterprises to food safety issues, the raw materials of this kind of packaging not only need to meet the requirements of the national "Sanitary Standards for Polyethylene Resins for Food Packaging", but also pass the manufacturer's strict test on the odor of polyethylene products; second, processing performance. Both bottle caps and bottles are produced by injection molding and pressing. This rapid processing technology requires this kind of raw materials to have good processing performance; third, mechanical properties. For cost control considerations, manufacturers are moving towards lightweight development and have put forward the demand for weight reduction for food packaging. Therefore, this kind of raw materials are also required to have excellent mechanical properties.
[0003] At present, traditional polyethylene packaging materials have shortcomings such as strong odor, failure to meet food grade requirements, and poor processing fluidity. Therefore, it is necessary to enhance the aging resistance and internal and external lubricity of the product, reduce the odor level of the product, so that the product can be used in the field of polyethylene food grade packaging and fully meet the demand indicators of downstream manufacturers. Summary of the invention
[0004] The technical solution adopted by the present invention is as follows:
[0005] In a first aspect, the present invention provides a low-odor food-grade polyethylene composition, specifically comprising the following components in parts by weight:
[0006] 100 parts of polyethylene powder;
[0007] Primary antioxidant 0.02-0.1 part;
[0008] Auxiliary antioxidant 0.02-0.3 parts;
[0009] Halogen absorber 0.1-0.4 parts;
[0010] Lubricant 0.1-0.2 parts;
[0011] The polyethylene powder has a melt mass flow rate of 2 to 5 g / 10 min (190° C., 2.16 kg) and a density of 0.943 to 0.963 kg / m 3 , linear high-density polyethylene with titanium element ≤10ppm;
[0012] The lubricant is one of erucamide and oleamide or a mixture of both.
[0013] Preferably, the main antioxidant is one of antioxidant 1010, antioxidant 1076, antioxidant 1098, or a mixture of more than one of them.
[0014] Preferably, the auxiliary antioxidant is one of antioxidant 168, antioxidant 626, antioxidant 3114, or a mixture of more than one of them.
[0015] Preferably, the halogen absorbent is one of zinc stearate, calcium stearate, synthetic hydrotalcite, or a mixture of more than one of them.
[0016] Preferably, the linear high-density polyethylene uses a Ziegler-Natta catalyst as an initiator, hexene and ethylene are dissolved in an isobutane solvent, and a polymerization reaction is carried out under the reaction conditions of a reaction temperature of 95-100° C. and a reaction pressure of 3.9-4.1 MPa.
[0017] In a second aspect, the present invention provides a method for preparing the low-odor food-grade polyethylene composition described in the first aspect, comprising the following steps: mixing polyethylene powder, a primary antioxidant, an auxiliary antioxidant, a halogen absorber, and a lubricant in a high-speed mixer for 2-3 minutes to obtain a mixture, and then extruding and granulating the mixture through a twin-screw extruder to obtain a low-odor food-grade polyethylene composition.
[0018] Preferably, the screw speed of the screw extruder is 180-240 rpm / min; and the extrusion temperature is 180°C-230°C.
[0019] Beneficial effects achieved by the present invention:
[0020] The present invention solves the shortcomings of traditional polyethylene packaging materials, such as strong odor, failure to meet food grade requirements, poor processing fluidity, etc., enhances the aging resistance and internal and external lubricity of the product, and reduces the odor level of the product. The product can be used in the field of polyethylene food grade packaging and fully meet the demand indicators of downstream manufacturers. DETAILED DESCRIPTION
[0021] In order to make the purpose, technical solution and advantages of the present invention more clear, the present invention is further described in detail in conjunction with the following examples. It should be noted that the present invention is not limited to the following examples.
[0022] Example 1
[0023] 100 parts of polyethylene powder with the brand name of HD5502S, 0.03 parts of mixed antioxidants composed of antioxidants 1010 and 1076, 0.08 parts of mixed auxiliary antioxidants composed of antioxidants 168 and 626, 0.2 parts of mixed halogen absorbents composed of zinc stearate and calcium stearate, and 0.15 parts of erucic acid amide lubricant were weighed by mass and mixed in a high-speed mixer for 2-3 minutes to obtain a mixture, and then the mixture was extruded and granulated by a twin-screw extruder to obtain a low-odor food-grade polyethylene composition. The density of the polyethylene composition is 0.9532 kg / m 3, The melt mass flow rate is 3g / 10min, the tensile yield stress is 28MPa, the nominal strain at break is 720%, the flexural modulus is 907MPa, the environmental stress cracking time (F50) is 60h, and the odor level is 4.0;
[0024] The screw speed of the screw extruder is 200 rpm / min; the extrusion temperature is 225°C.
[0025] Example 2
[0026] 100 parts of polyethylene powder with the brand name of HD5502S, 0.05 parts of mixed antioxidants composed of antioxidants 1010 and 1076, 0.1 parts of mixed auxiliary antioxidants composed of antioxidants 168 and 626, 0.25 parts of mixed halogen absorbents composed of zinc stearate and calcium stearate, and 0.18 parts of erucic acid amide lubricant were weighed by mass and mixed in a high-speed mixer for 2-3 minutes to obtain a mixture, and then the mixture was extruded and granulated by a twin-screw extruder to obtain a low-odor food-grade polyethylene composition. The density of the polyethylene composition is 0.9532 kg / m 3, The melt mass flow rate is 3.3 g / 10 min, the tensile yield stress is 27 MPa, the nominal strain at break is 735%, the flexural modulus is 927 MPa, the environmental stress cracking time (F50) is 55 h, and the odor level is 4.3;
[0027] The screw speed of the screw extruder is 200 rpm / min; the extrusion temperature is 222°C.
[0028] Example 3
[0029] 100 parts of polyethylene powder with the brand name of HD5502S, 0.02 parts of a mixed antioxidant composed of antioxidant 1010 and antioxidant 1076, 0.06 parts of a mixed auxiliary antioxidant composed of antioxidant 168 and antioxidant 626, 0.18 parts of a mixed halogen absorber composed of zinc stearate and calcium stearate, and 0.1 parts of an erucic acid amide lubricant were weighed by mass and mixed in a high-speed mixer for 2-3 minutes to obtain a mixture, and then the mixture was extruded and granulated by a twin-screw extruder to obtain a low-odor food-grade polyethylene composition. The density of the polyethylene composition is 0.9535 kg / m 3, The melt mass flow rate is 2.4 g / 10 min, the tensile yield stress is 26 MPa, the nominal strain at break is 707%, the flexural modulus is 904 MPa, the environmental stress cracking time (F50) is 53 h, and the odor level is 3.2;
[0030] The screw speed of the screw extruder is 200 rpm / min; the extrusion temperature is 212°C.
Claims
1. A low-odor food-grade polyethylene composition, characterized in that Specifically include the following components by weight: 100 parts of polyethylene powder; Primary antioxidant 0.02-0.1 part; Auxiliary antioxidant 0.02-0.3 parts; Halogen absorber 0.1-0.4 parts; Lubricant 0.1-0.2 parts; The polyethylene powder has a melt mass flow rate of 2 to 5 g / 10 min (190° C., 2.16 kg) and a density of 0.943 to 0.963 kg / m 3 , linear high-density polyethylene with titanium element ≤10ppm; The lubricant is one of erucamide and oleamide or a mixture of both.
2. The low-odor food-grade polyethylene composition according to claim 1, characterized in that The main antioxidant is one of antioxidant 1010, antioxidant 1076, and antioxidant 1098, or a mixture of more than one of them.
3. The low-odor food-grade polyethylene composition according to claim 1, characterized in that The auxiliary antioxidant is one of antioxidant 168, antioxidant 626, and antioxidant 3114, or a mixture of more than one of them.
4. The low-odor food-grade polyethylene composition according to claim 1, characterized in that The halogen absorbent is one of zinc stearate, calcium stearate and synthetic hydrotalcite or a mixture of more than one of them.
5. The low-odor food-grade polyethylene composition according to claim 1, characterized in that The linear high-density polyethylene uses a Ziegler-Natta catalyst as an initiator, and hexene and ethylene are dissolved in an isobutane solvent to carry out polymerization under the reaction conditions of a reaction temperature of 95-100° C. and a reaction pressure of 3.9-4.1 MPa.
6. A method for preparing the low-odor food-grade polyethylene composition according to any one of claims 1 to 5, characterized in that: The method comprises the following steps: mixing the polyethylene powder, the main antioxidant, the auxiliary antioxidant, the halogen absorber and the lubricant in a high-speed mixer for 2-3 minutes to obtain a mixture, and then extruding and granulating the mixture through a twin-screw extruder to obtain a low-odor food-grade polyethylene composition.
7. The method for preparing the low-odor food-grade polyethylene composition according to claim 6, characterized in that: The screw speed of the screw extruder is 180-240 rpm / min; the extrusion temperature is 180° C.-230° C.