Toughened heat-resistant physical-aging-resistant modified polylactic acid sheet as well as preparation and application thereof
By adding modified tackifying resin and polybutylene succinate to the polylactic acid sheet and using a specific process to form a viscoelastic three-dimensional network structure, the polylactic acid sheet is insufficient toughness and poor heat resistance and The problem of poor physical aging resistance has achieved comprehensive performance of high toughness, high heat resistance and physical aging resistance, and is suitable for food packaging and other fields.
Patent Information
- Application Number
- CN202310516164.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
The existing polylactic acid sheets are inadequate toughness, poor heat resistance and poor physical aging resistance, especially in the warehousing and logistics stage, which is prone to physical aging and becoming brittle, which cannot meet the comprehensive performance requirements in the fields of food packaging and other fields.
A melt blend of 65-99 parts of polylactic acid, 1-35 parts of modified tackifying resin, 1-20 parts of polybutylene succinate was used, and the modified mixture was formed by a specific transesterification catalyst and process. Polylactic acid sheets, including graft modification and esterification reaction, prepare modified tackifying resins, form viscoelastic three-dimensional network structure, and improve toughness and heat resistance.
It significantly improves the physical aging resistance of modified polylactic acid sheets, maintains the toughness unchanged, improves tensile strength, elongation at break and impact strength, avoids the transformation of toughness to brittleness, and meets the application needs in food packaging and other fields.
Smart Images

Figure BDA0004219214470000121 
Figure BDA0004219214470000131 
Figure HDA0004219214480000011
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of extruded sheets, and in particular relates to a toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet and a preparation method and application thereof. Background Art
[0002] With the rapid expansion of the takeout market, the demand for packaging materials such as take-out boxes and disposable plates has increased dramatically. However, the raw materials of current packaging materials basically come from petrochemical resources, such as polyolefins, polystyrene, polyethylene terephthalate, etc. However, petrochemical-based resins themselves and related additives in take-out boxes have certain food safety issues. In addition, the non-degradability of petrochemical-based resins can easily cause environmental pollution, which affects the application of sheets made of petrochemical-based resins in the packaging field. Therefore, it is particularly important to develop biodegradable polyester sheets that can be used in the field of food packaging.
[0003] The most representative biodegradable plastic is polylactic acid (PLA). PLA has good biocompatibility and degradability. During the composting process, it is decomposed by microorganisms to form lactic acid, which can eventually decompose into carbon dioxide and water. It is one of the earliest biodegradable plastics certified by the US Food and Drug Administration (FDA). With the maturity of PLA large-scale production technology and the gradual reduction of its production cost, PLA has attracted widespread attention in the fields of biomedicine, textiles, packaging, etc. in recent years. However, many literatures (Macromolecules 2007, 40, 9664-9671; Macromolecules 2019, 52, 8878-8894; Polymer 2020, 186, 122014; Macromolecules 2019, 52, 5429-5441) report that PLA is a semi-crystalline polymer, and the amorphous phase is very prone to physical aging below the glass transition temperature, making the material rapidly brittle. In particular, physical aging is very likely to occur below the glass transition temperature, causing the toughened and modified polylactic acid to still become brittle (European Polymer Journal 2015, 66, 533-542).
[0004] There are many public reports on the preparation of PLA extruded sheets, which mainly focus on improving the toughness and heat resistance of the sheets. CN102206406A discloses a method for preparing a transparent heat-resistant polylactic acid modified material, which uses a nucleating agent to change the crystal state of polylactic acid, a chain extender to cross-link and change the molecular structure of polylactic acid, and a high glass transition temperature (T g) The three methods of polymer material blending synergistically improve the heat resistance of polylactic acid. CN103540111A discloses a high-strength, high-temperature resistant fully degradable polylactic acid sheet and its manufacturing method, which uses polylactic acid as the matrix resin material, biodegradable plastic with good flexibility as the toughening component, inorganic fillers as reinforcing agents, coupling agents, antioxidants, lubricants and other additives to achieve heat resistance and toughening modification of polylactic acid materials. CN114702799A discloses a biodegradable polylactic acid blister sheet. The weight proportions of each component are: 50-95 parts of PLA, 3-35 parts of PBAT, 3-10 parts of compatibilizer, 2-20 parts of nucleating agent, 0.01-5 parts of dispersant, 0.01-5 parts of plasticizer, 0.01-5 parts of coupling agent, 0.01-5 parts of chain extender and 1-95 parts of filler. By strictly controlling the content of each component, a polylactic acid sheet with significantly improved toughness and heat resistance is obtained. In addition, CN112521732A discloses a biaxially stretched polylactic acid film material resistant to physical aging, a preparation method and application thereof, which achieves the effect of physical aging resistance by rapidly quenching the polylactic acid melt after stretching and orienting it, maintaining the oriented structure, and inhibiting the relaxation of the molecular chain.
[0005] Although the above known technologies can prepare toughened, heat-resistant modified or toughened and heat-resistant synergistically modified polylactic acid sheets, there are still the following limitations: (1) Under current technical conditions, polylactic acid sheets and blister products still have problems such as weak impact resistance; (2) The polylactic acid sheets undergo preheating treatment before blistering, and the resulting blister products are prone to physical aging during the storage and logistics stage, causing them to become brittle rapidly; (3) The heat-set polylactic acid sheets and their blister products are prone to physical aging during the storage and logistics stage, causing them to become brittle rapidly. Therefore, it is necessary to develop new heat-resistant, toughened and physically aging-resistant polylactic acid sheets and their preparation methods to meet the high requirements for comprehensive performance of various applications. Summary of the invention
[0006] The first purpose of the present invention is to overcome the problems of the prior art such as insufficient toughness, poor heat resistance and poor physical aging resistance of polylactic acid sheets, and to provide a toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet, the physical aging resistance of which is significantly improved.
[0007] A toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet is a melt blend comprising the following raw material components in parts by weight: 65-99 parts of polylactic acid (PLA), 1-35 parts of modified tackifying resin, and 1-20 parts of polybutylene succinate (PBS);
[0008] Preferably, the content of polylactic acid is 75-95 parts by weight, and the content of modified tackifying resin is 5-25 parts by weight; more preferably, the content of polylactic acid is 82-90 parts by weight, and the content of modified tackifying resin is 10-18 parts by weight.
[0009] Preferably, the content of polybutylene succinate is 5-15 parts by weight; more preferably, the content of polybutylene succinate is 7-13 parts by weight.
[0010] Preferably, the weight average molecular weight of the polylactic acid is 80,000-500,000, and the molar content of the L optical isomer in the polylactic acid is 85-99%; more preferably, the weight average molecular weight of the polylactic acid is 150,000-350,000, and the molar content of the L optical isomer in the polylactic acid is 92-98%.
[0011] Preferably, the weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%; more preferably, the weight average molecular weight of the modified tackifying resin is 800-3000, and the molar grafting ratio is 30-55%.
[0012] The modified tackifying resin is prepared by the following method:
[0013] 80-98 parts by weight of tackifying resin and 2-20 parts by weight of maleic anhydride are mixed for graft modification to obtain maleic anhydride grafted tackifying resin; 35-65 parts by weight of maleic anhydride grafted tackifying resin and 35-65 parts by weight of lactic acid oligomer are subjected to esterification reaction to obtain modified tackifying resin.
[0014] Specifically, the method comprises the following steps:
[0015] Step (1), melt blending 80-98 parts by weight of a tackifying resin (Cx), 2-20 parts by weight of maleic anhydride (MAH), and 0.1-1.2 parts by weight of dicumyl peroxide to form a maleic anhydride grafted tackifying resin (Cx-g-MAH), the reaction temperature being 100-150° C., and the reaction time being 4-12 minutes;
[0016] Step (2), mixing 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol and 0.1-1.2 parts by weight of stannous chloride for esterification reaction to form lactic acid oligomers, the reaction temperature is 110-155° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 4-12 hours;
[0017] Step (3), further mixing 35-65 parts by weight of the maleic anhydride grafted tackifying resin (Cx-g-MAH) obtained in step (1) with 35-65 parts by weight of the lactic acid oligomer obtained in step (2) and 0.1-1.2 parts by weight of stannous octoate to carry out an esterification reaction to obtain the modified tackifying resin, the reaction temperature is 155-195° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 1-4 hours.
[0018] Preferably, the lactic acid oligomer is a hydroxy-terminated lactic acid oligomer; the molecular weight of the lactic acid oligomer is 72-720.
[0019] Preferably, the tackifying resin includes one or more combinations of C5 tackifying resin, C5 hydrogenated tackifying resin, C9 hydrogenated tackifying resin, C9 cold-polymerized tackifying resin, C9 hot-polymerized tackifying resin, C5 / C9 copolymerized tackifying resin, terpene resin, and rosin ester, but is not limited thereto.
[0020] Preferably, the weight average molecular weight of the polybutylene succinate is 80,000-300,000, and more preferably, the weight average molecular weight of the PBS is 120,000-250,000.
[0021] The toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet provided by the present invention has a tensile strength of 43-62 MPa, an elongation at break of 74%-186%, and a notched impact strength of 10.4-25.2 KJ / m 2 , heat deformation temperature is 76-102℃. g After sufficient storage time (shelf life), the change rate of tensile strength before and after storage is generally less than 15%; the change rate of impact strength before and after storage is also less than 15%; the change rate of elongation at break is generally less than 35%, and there is no transition from toughness to brittleness; the storage time is greater than or equal to 5 hours.
[0022] The second object of the present invention is to provide a method for preparing the above-mentioned toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet, the method comprising:
[0023] (1) reacting polylactic acid, modified tackifying resin and polybutylene succinate by melt blending under the catalysis of an ester exchange catalyst to obtain a blend;
[0024] (2) The blend is subjected to melt extrusion, cast film, and uniaxial stretching to obtain a modified polylactic acid sheet.
[0025] Preferably, the transesterification catalyst is one of zinc acetate, sodium octoate, and stannous octoate; the weight portion of the transesterification catalyst is 0.01-1.2 parts; more preferably, the content of the transesterification catalyst is 0.05-0.8 parts by weight; most preferably, the content of the transesterification catalyst is 0.1-0.6 parts by weight.
[0026] Preferably, the extrusion temperature of the melt extrusion is 160-220°C, and the casting roll temperature of the cast sheet is 20-50°C; more preferably, the extrusion temperature is 180-210°C, and the casting roll temperature is 20-40°C.
[0027] Preferably, the stretching temperature of the uniaxial stretching is 75-145° C., and the stretching ratio is 2-8 times; more preferably, the stretching temperature is 90-130° C., and the stretching ratio is 3-7 times.
[0028] Preferably, the composition further comprises drying before melt extrusion.
[0029] Preferably, the drying temperature is 90-98° C. and the drying time is 5-10 h.
[0030] The third object of the present invention is to provide the use of the above-mentioned toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet as a food packaging material.
[0031] Compared with the prior art, the beneficial effects of the present invention are at least:
[0032] (1) The present invention selects polylactic acid, modified tackifying resin and polybutylene succinate with specific component contents, and cooperates with an ester exchange agent with specific component contents, so that the prepared modified polylactic acid sheet has physical aging resistance;
[0033] (2) The modified polylactic acid sheet obtained by the present invention using conventional cast sheet extrusion equipment still has physical aging resistance and does not require special preparation processes (such as high-multiple drafting, quenching treatment, and preventing molecular chain relaxation);
[0034] (3) The modified polylactic acid sheet prepared by the present invention is further heat-treated and the obtained blister products also have the property of physical aging resistance, thus solving the technical problem that the polylactic acid sheet resistant to physical aging cannot be heat-treated;
[0035] (4) The present invention uses a relatively high molecular weight polylactic acid to improve the melt strength of the blending system and improve the mechanical properties of the polylactic acid sheet; the polylactic acid selected has a relatively high molar content of the L optical isomer, which can improve the crystallization ability of the blending system, thereby improving the mechanical properties of the modified polylactic acid sheet; the modified tackifying resin with a medium weight average molecular weight and molar grafting ratio is selected to significantly improve the compatibility of the tackifying resin with polylactic acid, thereby improving the melt strength of the blending system and the toughness of the modified polylactic acid sheet, while giving the modified polylactic acid sheet resistance to physical aging; the polybutylene succinate with a medium molecular weight is selected to make its crystals become nucleation sites of the blending system, thereby improving the crystallization ability of the blending system, and at the same time, its relatively low melting temperature (<120°C) enables it to melt and deform to absorb energy when the blending system encounters an impact, thereby improving the impact performance of the blending system, thereby improving the heat resistance of the modified polylactic acid sheet;
[0036] Among them, the modified tackifying resin forms a viscoelastic three-dimensional network structure in the polylactic acid matrix, which reduces the yield stress during tensile deformation, so that the modified polylactic acid sheet maintains tough fracture and there is no transition from toughness to brittleness. As a result, the prepared modified polylactic acid sheet has the characteristics of physical aging resistance, breaking through the performance bottlenecks of conventional polylactic acid sheets, such as poor toughness and heat resistance, and especially prone to physical aging leading to brittleness, thereby fully meeting the use requirements and greatly expanding its application areas. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 1 is the stress-strain curve of the modified polylactic acid sheet prepared in Example 1 before and after physical aging. DETAILED DESCRIPTION
[0038] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0039] In the present invention, unless otherwise specified, "PLA" refers to polylactic acid; and "PBS" refers to polybutylene succinate.
[0040] The first aspect of the present invention provides a toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet, which comprises polylactic acid, a modified tackifying resin, and polybutylene succinate, wherein the content of the polybutylene succinate is 1-20 parts by weight, compared to 100 parts by weight of the polylactic acid and the modified tackifying resin (65-99 parts by weight of polylactic acid, 1-35 parts by weight of the modified tackifying resin).
[0041] The weight average molecular weight of the PLA is 80,000-500,000, and the molar content of the L optical isomer in the PLA is 85-99%.
[0042] The lactic acid oligomer is prepared by the following method:
[0043] 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol, and 0.1-1.2 parts by weight of stannous chloride are subjected to esterification reaction to form lactic acid oligomers.
[0044] The modified tackifying resin is a product obtained by mixing a tackifying resin with maleic anhydride for graft modification and then subjecting the mixture to an esterification reaction with a lactic acid oligomer. The weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%. The molecular weight of the lactic acid oligomer is 72-720. Specifically, the modified tackifying resin is prepared by the following method:
[0045] Step (1), melt blending 80-98 parts by weight of tackifying resin Cx, 2-20 parts by weight of maleic anhydride MAH, and 0.1-1.2 parts by weight of dicumyl peroxide to form a maleic anhydride grafted tackifying resin Cx-g-MAH, the reaction temperature is 100-150° C., and the reaction time is 4-12 minutes;
[0046] Step (2), mixing 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol and 0.1-1.2 parts by weight of stannous chloride to carry out esterification reaction to form terminal hydroxyl lactic acid oligomers, the reaction temperature is 110-155° C., the reaction pressure is 0.5-101 kPa, and the reaction time is 4-12 hours;
[0047] Step (3), further mixing 35-65 parts by weight of the maleic anhydride grafted tackifying resin Cx-g-MAH obtained in step (1) with 35-65 parts by weight of the terminal hydroxyl lactic acid oligomer obtained in step (2) and 0.1-1.2 parts by weight of stannous octoate to carry out esterification reaction to obtain the modified tackifying resin, the reaction temperature is 155-195°C, the reaction pressure is 0.5-101 kPa, and the reaction time is 1-4 hours.
[0048] The weight average molecular weight of the PBS is 80,000-300,000.
[0049] The second aspect of the present invention provides a method for preparing a toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet, the method comprising:
[0050] (1) reacting and melt-blending the polylactic acid, modified tackifying resin and polybutylene succinate as described above under the catalysis of an ester exchange agent to obtain a blend;
[0051] (2) The blend is dried at 90-98° C. for 5-10 h, and then melt-extruded and cast at an extrusion temperature of 160-220° C. and a casting roll temperature of 20-50° C., and then uniaxially stretched by 2-8 times at 75-145° C., cooled and rolled to obtain a modified polylactic acid sheet.
[0052] The transesterification catalyst is one of zinc acetate, sodium octoate and stannous octoate; the content of the transesterification catalyst is 0.01-1.2 parts by weight.
[0053] The third aspect of the present invention provides the use of the toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet as a food packaging material.
[0054] The present invention will be described in detail below by way of examples. In the following examples and comparative examples:
[0055] (1) Glass transition temperature was measured by differential scanning calorimetry (DSC);
[0056] (2) Mechanical properties (including tensile strength and elongation at break) were measured using a universal tensile testing machine (referring to the national standard GB / T14344);
[0057] (3) Impact properties (such as notched impact strength) are measured by an Izod impact tester (refer to national standard GB / T1843-2008);
[0058] (5) Heat resistance (such as heat deformation temperature) is measured by heat deformation temperature test device (refer to national standard GB / T1634);
[0059] (4) Polylactic acid, polybutylene succinate, tackifying resin, lactic acid, maleic anhydride and catalyst were all purchased from commercial sources.
[0060] The preparation method of the modified tackifying resin used in the following examples includes:
[0061] (1) 85 parts by weight of a tackifier resin (one of a C5 tackifier resin, a terpene resin, and a rosin ester) are melt-blended with 15 parts by weight of maleic anhydride (MAH) and 0.6 parts by weight of dicumyl peroxide to form a tackifier resin having a carboxylic acid group by grafting, the reaction temperature being 120° C. and the reaction time being 10 min;
[0062] (2) 50 parts by weight of L-lactic acid, 50 parts by weight of 1,4-butanediol and 0.8 parts by weight of stannous chloride were mixed for esterification reaction to form terminal hydroxyl lactic acid oligomers, the reaction temperature was 130° C., the reaction pressure was 2 kPa, and the reaction time was 6 h;
[0063] (3) 58 parts by weight of the maleic anhydride grafted tackifier resin was further mixed with 42 parts by weight of terminal hydroxyl lactic acid oligomer and 0.4 parts by weight of stannous octoate for esterification reaction to form a lactic acid oligomer modified tackifier resin. The reaction temperature was 160° C., the reaction pressure was 10 kPa, and the reaction time was 2 h to obtain a modified tackifier resin.
[0064] Example 1
[0065] (1) Take 90 parts by weight of polylactic acid with a weight average molecular weight of 200,000, wherein the molar content of the L optical isomer is 98%; take 10 parts by weight of a modified tackifying resin with a weight average molecular weight of 1200, wherein the molar grafting ratio is 42%; take 8 parts by weight of PBS with a weight average molecular weight of 140,000;
[0066] (2) selecting zinc acetate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.2 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 95±2° C. for 8 hours, with a water content of 42 ppm;
[0067] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 185°C, and the casting roller temperature was 35°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 95°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1. The stress-strain curves before and after physical aging are shown in Table 1. Figure 1 shown.
[0068] Example 2
[0069] (1) Take 82 parts by weight of polylactic acid with a weight average molecular weight of 250,000, wherein the molar content of the L optical isomer is 97%; take 18 parts by weight of a modified tackifying resin with a weight average molecular weight of 2000, wherein the molar grafting ratio is 48%; take 10 parts by weight of PBS with a weight average molecular weight of 180,000;
[0070] (2) selecting zinc acetate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.4 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 94±2° C. for 7 hours, with a water content of 48 ppm;
[0071] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 200°C, and the casting roll temperature was 25°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 115°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0072] Example 3
[0073] (1) Take 86 parts by weight of polylactic acid with a weight average molecular weight of 230,000, wherein the molar content of the L optical isomer is 98%; take 14 parts by weight of a modified tackifying resin with a weight average molecular weight of 1700, wherein the molar grafting ratio is 45%; take 9 parts by weight of PBS with a weight average molecular weight of 160,000;
[0074] (2) selecting zinc acetate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.3 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 97±2° C. for 8 hours, with a water content of 46 ppm;
[0075] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 192°C, and the casting roll temperature was 28°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 102°C, and the stretching ratio was 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0076] Example 4
[0077] (1) Take 65 parts by weight of polylactic acid with a weight average molecular weight of 250,000, wherein the molar content of the L optical isomer is 99%; take 35 parts by weight of a modified tackifying resin with a weight average molecular weight of 300, wherein the molar grafting ratio is 15%; take 20 parts by weight of PBS with a weight average molecular weight of 80,000;
[0078] (2) Sodium octanoate is selected as an ester exchange catalyst, and the content of the ester exchange catalyst is 1.2 parts by weight; the raw materials in step (1) are mixed, and melt blended under the action of the ester exchange catalyst to obtain a blend, and the blend is hot-air dried at a drying temperature of 98±2° C. for 10 hours, and the water content is 38 ppm;
[0079] (3) The dried blend was melt-extruded and cast into sheets through conventional sheet extrusion equipment, with the melt extrusion temperature being 160°C and the casting roll temperature being 50°C; subsequently, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, with the stretching temperature being 75°C and the stretching ratio being 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0080] Example 5
[0081] (1) Take 80 parts by weight of polylactic acid with a weight average molecular weight of 250,000, wherein the molar content of the L optical isomer is 95%; take 20 parts by weight of a modified tackifying resin with a weight average molecular weight of 8,000, wherein the molar grafting ratio is 80%; take 13 parts by weight of PBS with a weight average molecular weight of 300,000;
[0082] (2) Sodium octanoate is selected as an ester exchange catalyst, and the content of the ester exchange catalyst is 0.6 parts by weight; the raw materials in step (1) are mixed, and melt blended under the action of the ester exchange catalyst to obtain a blend, and the blend is hot-air dried at a drying temperature of 96±2° C. for 8 hours, and the water content is 52 ppm;
[0083] (3) The dried blend was melt-extruded and cast into sheets through conventional sheet extrusion equipment, with the melt extrusion temperature being 182°C and the casting roll temperature being 40°C; subsequently, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, with the stretching temperature being 95°C and the stretching ratio being 8 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0084] Example 6
[0085] (1) Take 95 parts by weight of polylactic acid with a weight average molecular weight of 80,000, wherein the molar content of the L optical isomer is 99%; take 5 parts by weight of a modified tackifying resin with a weight average molecular weight of 800, wherein the molar grafting ratio is 35%; take 5 parts by weight of PBS with a weight average molecular weight of 120,000;
[0086] (2) Sodium octanoate is selected as an ester exchange catalyst; the content of the ester exchange catalyst is 0.05 parts by weight; the raw materials in step (1) are mixed, reacted and melt-blended under the action of the ester exchange catalyst to obtain a blend, and the blend is hot-air dried at a drying temperature of 94±2° C. for 6 hours, and the water content is 54 ppm;
[0087] (3) The dried blend was melt-extruded and cast into sheets through conventional sheet extrusion equipment, with the melt extrusion temperature being 202°C and the casting roll temperature being 35°C; subsequently, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, with the stretching temperature being 120°C and the stretching ratio being 3 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0088] Example 7
[0089] (1) Take 99 parts by weight of polylactic acid with a weight average molecular weight of 80,000, wherein the molar content of the L optical isomer is 99%; take 1 part by weight of a modified tackifying resin with a weight average molecular weight of 3,000, wherein the molar grafting ratio is 65%; take 1 part by weight of PBS with a weight average molecular weight of 250,000;
[0090] (2) selecting stannous octoate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.01 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 98±2° C. for 5 hours, with a water content of 47 ppm;
[0091] (3) The dried blend was melt-extruded and cast into sheets through conventional sheet extrusion equipment, with the melt extrusion temperature being 205°C and the casting roll temperature being 32°C; subsequently, the modified polylactic acid sheet was obtained by uniaxial stretching and cooling and winding, with the stretching temperature being 130°C and the stretching ratio being 2. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0092] Example 8
[0093] (1) Take 96 parts by weight of polylactic acid with a weight average molecular weight of 500,000, wherein the molar content of the L optical isomer is 85%; take 4 parts by weight of a modified tackifying resin with a weight average molecular weight of 2000, wherein the molar grafting ratio is 40%; take 4 parts by weight of PBS with a weight average molecular weight of 220,000;
[0094] (2) selecting stannous octoate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.03 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 90±2° C. for 7 hours, with a water content of 64 ppm;
[0095] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 220°C, and the casting roll temperature was 20°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 145°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0096] Example 9
[0097] (1) Take 80 parts by weight of polylactic acid with a weight average molecular weight of 500,000, wherein the molar content of the L optical isomer is 90%; take 20 parts by weight of a modified tackifying resin with a weight average molecular weight of 5000, wherein the molar grafting ratio is 65%; take 17 parts by weight of PBS with a weight average molecular weight of 260,000;
[0098] (2) selecting stannous octoate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.9 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 92±2° C. for 10 hours, with a water content of 58 ppm;
[0099] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 200°C, and the casting roll temperature was 30°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 120°C, and the stretching ratio was 4 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0100] Example 10
[0101] (1) Take 85 parts by weight of polylactic acid with a weight average molecular weight of 80,000, wherein the molar content of the L optical isomer is 95%; take 15 parts by weight of a modified tackifying resin with a weight average molecular weight of 300, wherein the molar grafting ratio is 28%; take 10 parts by weight of PBS with a weight average molecular weight of 80,000;
[0102] (2) selecting zinc acetate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.4 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 97±2° C. for 8 hours, with a water content of 41 ppm;
[0103] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 170°C, and the casting roll temperature was 45°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 90°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0104] Embodiment 11
[0105] (1) Take 82 parts by weight of polylactic acid with a weight average molecular weight of 500,000, wherein the molar content of the L optical isomer is 94%; take 18 parts by weight of a modified tackifying resin with a weight average molecular weight of 8,000, wherein the molar grafting ratio is 75%; take 16 parts by weight of PBS with a weight average molecular weight of 300,000;
[0106] (2) Sodium octanoate is selected as an ester exchange catalyst, and the content of the ester exchange catalyst is 0.9 parts by weight; the raw materials in step (1) are mixed, and reacted and melt-blended under the action of the ester exchange catalyst to obtain a blend, and the blend is hot-air dried at a drying temperature of 93±2° C. for 10 hours, and the water content is 39 ppm;
[0107] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 210°C, and the casting roll temperature was 25°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 125°C, and the stretching ratio was 5 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0108] Example 12
[0109] (1) Take 92 parts by weight of polylactic acid with a weight average molecular weight of 80,000, wherein the molar content of the L optical isomer is 98%; take 8 parts by weight of a modified tackifying resin with a weight average molecular weight of 8,000, wherein the molar grafting ratio is 75%; take 7 parts by weight of PBS with a weight average molecular weight of 300,000;
[0110] (2) selecting stannous octoate as an ester exchange catalyst, the content of the ester exchange catalyst being 0.1 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 97±2° C. for 9 hours, with a water content of 39 ppm;
[0111] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 180°C, and the casting roll temperature was 35°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 95°C, and the stretching ratio was 6 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0112] Example 13
[0113] (1) Take 70 parts by weight of polylactic acid with a weight average molecular weight of 500,000, wherein the molar content of the L optical isomer is 88%; take 30 parts by weight of a modified tackifying resin with a weight average molecular weight of 300, wherein the molar grafting ratio is 32%; take 18 parts by weight of PBS with a weight average molecular weight of 80,000;
[0114] (2) selecting stannous octoate as an ester exchange catalyst, the content of the ester exchange catalyst being 1.0 parts by weight; mixing the raw materials in step (1), reacting and melt blending under the action of the ester exchange catalyst to obtain a blend, and hot-air drying the blend at a drying temperature of 93±2° C. for 6 hours, with a water content of 45 ppm;
[0115] (3) The dried blend was melt-extruded and cast through a conventional sheet extrusion device, the melt extrusion temperature was 190°C, and the casting roll temperature was 30°C; then, the modified polylactic acid sheet was obtained by uniaxial stretching, cooling and winding, the stretching temperature was 115°C, and the stretching ratio was 7 times. The properties of the modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0116] Comparative Example 1
[0117] The modified polylactic acid sheet was prepared according to the method of Example 2, except that "18 parts of modified tackifying resin" was replaced by "50 parts". The properties of the prepared modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0118] Comparative Example 2
[0119] The modified polylactic acid sheet was prepared according to the method of Example 2, except that the modified tackifying resin was not added. The properties of the prepared modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0120] Comparative Example 3
[0121] The modified polylactic acid sheet was prepared according to the method of Example 7, except that the modified tackifying resin was not added. The properties of the prepared modified polylactic acid sheet were tested, and the test results are shown in Table 1.
[0122] Table 1 Performance test results of modified polylactic acid sheets obtained in Examples 1-13 and Comparative Examples 1-3
[0123]
[0124]
[0125] As can be seen from Table 1, the modified polylactic acid sheet of the present invention has good comprehensive performance, breaking through the performance bottleneck of conventional polylactic acid sheets that are prone to physical aging and become brittle, thereby fully meeting the use requirements and being applicable to the fields of food packaging materials.
[0126] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet, which is a melt blend, characterized in that: The invention comprises the following raw material components: 65-99 parts by weight of polylactic acid, 1-35 parts by weight of modified tackifying resin, and 1-20 parts by weight of polybutylene succinate; The modified tackifying resin is prepared by the following method: 80-98 parts by weight of tackifying resin and 2-20 parts by weight of maleic anhydride are mixed for grafting modification to obtain maleic anhydride grafted tackifying resin; 35-65 parts by weight of maleic anhydride grafted tackifying resin and 35-65 parts by weight of lactic acid oligomer are esterified to obtain modified tackifying resin.
2. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to claim 1, characterized in that: The lactic acid oligomer is a hydroxyl-terminated lactic acid oligomer.
3. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to claim 2, characterized in that: The lactic acid oligomer is prepared by the following method: 40-60 parts by weight of L-lactic acid, 40-60 parts by weight of 1,4-butanediol, and 0.1-1.2 parts by weight of stannous chloride are subjected to esterification reaction to form lactic acid oligomers.
4. The modified polylactic acid sheet according to claim 1, characterized in that: The tackifying resin Cx includes one or more of C5 tackifying resin, C5 hydrogenated tackifying resin, C9 hydrogenated tackifying resin, C9 cold-polymerized tackifying resin, C9 hot-polymerized tackifying resin, C5 / C9 copolymerized tackifying resin, terpene resin, and rosin ester.
5. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to any one of claims 1 to 4, characterized in that: The preparation method of the modified tackifying resin specifically comprises the following steps: Step (1), melt-blending the tackifying resin Cx, maleic anhydride MAH and dicumyl peroxide at 100-150° C. for 4-12 minutes to graft to form a maleic anhydride grafted tackifying resin Cx-g-MAH; Step (2), mixing L-lactic acid with 1,4-butanediol and stannous chloride, and subjecting the mixture to an esterification reaction at 110-155° C. and 0.5-101 kPa for 4-12 hours to form lactic acid oligomers; Step (3), mixing the maleic anhydride grafted tackifying resin Cx-g-MAH obtained in step (1) with the lactic acid oligomer and stannous octoate obtained in step (2), and subjecting the mixture to an esterification reaction at 155-195° C. and 0.5-101 kPa for 1-4 hours to obtain the modified tackifying resin.
6. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to claim 1, characterized in that: The weight average molecular weight of the polylactic acid is 80,000-500,000, and the molar content of the L optical isomer in the polylactic acid is 85-99%.
7. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to claim 1 or 6, characterized in that: The weight average molecular weight of the modified tackifying resin is 300-8000, and the molar grafting ratio is 15-80%.
8. The toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet according to claim 1 or 6, characterized in that: The weight average molecular weight of the polybutylene succinate is 80,000-300,000.
9. A method for preparing a toughened, heat-resistant, and physically aging-resistant modified polylactic acid sheet as claimed in any one of claims 1 to 8, characterized in that: The method comprises the following steps: (1) reacting polylactic acid, modified tackifying resin and polybutylene succinate under the catalysis of an ester exchange catalyst to melt blend to obtain a blend; the ester exchange catalyst is one of zinc acetate, sodium octoate and stannous octoate; (2) After drying the blended material, the blended material is melt-extruded, cast into sheets, and uniaxially stretched to obtain a modified polylactic acid sheet.
10. Use of the toughened, heat-resistant and physically aging-resistant modified polylactic acid sheet according to any one of claims 1 to 7 as a food packaging material.
Citation Information
Patent Citations
Method for preparing transparent heat-resistance polylactic acid modification material
CN102206406A
Fully degradable polylactic acid sheet material with high strength and high-temperature resistance, and preparation method thereof
CN103540111A
Physical-aging-resistant biaxially-oriented polylactic acid membrane material, and preparation method and application thereof
CN112521732A
Biodegradable polylactic acid plastic uptake sheet
CN114702799A