Preparation process of anti-aging injection molding corner window for new energy automobile

By using specific materials and additives in the injection molding angle window process to control injection molding and cooling parameters, the problems of injection molding angle window aging and yellowing are solved, and its anti-aging performance and service life are improved, ensuring the appearance and safety of the car.

CN118931144APending Publication Date: 2024-11-12JINHU LINENG VEHICLE IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411029544.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing injection molding angle window process has defects in material selection, injection molding and post-processing, which leads to injection molding angle windows being easily aged, yellowed and brittle during long-term use, affecting the appearance and service life of the car.

Method used

Use polycarbonate or polypropylene and add ultraviolet absorbers, antioxidants, light stabilizers, tougheners and lubricants to control injection molding parameters such as pressure, speed and cooling temperature, and perform post-treatment such as trimming and polishing. To improve the anti-aging performance of injection molded corner windows.

Benefits of technology

Effectively resist ultraviolet and oxygen erosion, improve the strength and toughness of injection molded corner windows, extend service life, reduce maintenance costs, and ensure safe and reliable vehicle performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931144A_ABST
    Figure CN118931144A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation process of an anti-aging injection molding corner window for a new energy automobile, and belongs to the technical field of new energy automobiles, and the preparation process comprises the following steps: step 1) selection of plastic raw materials: selecting the plastic raw materials suitable for injection molding of the corner window, generally adopting materials such as polycarbonate (PC) or polypropylene (PP) and the like, adding a proper amount of ultraviolet light absorber, antioxidant, light stabilizer, flexibilizer and lubricant; and (2) drying of the plastic raw materials, wherein the plastic raw materials are put into drying equipment to be subjected to drying treatment. According to the preparation process of the anti-aging injection-molded corner window for the new energy automobile, the injection-molded corner window is prevented from aging and yellowing, the antioxidant and the stabilizer are adopted, oxygen erosion is resisted, embrittlement is prevented, a chemical stable material is used, chemical substance erosion is resisted, and discoloration and deformation are avoided, so that the injection-molded corner window can resist erosion of external factors such as ultraviolet rays and oxygen, and the service life of the injection-molded corner window is prolonged. Strength and toughness are improved, pressure and vibration in the running process of a vehicle are borne, stable performance is kept, and fracture deformation is avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of new energy vehicles, and in particular to a preparation process of an anti-aging injection-molded corner window for new energy vehicles. Background Art

[0002] Injection molded corner windows are one of the indispensable and important parts in automobile manufacturing. They are usually used for side windows or rear windows of automobiles. The preparation process is a complex and delicate process that requires multiple steps to complete.

[0003] With the continuous development of the automobile industry, the quality and performance requirements for automobile parts are becoming higher and higher. As an important part of the appearance of the car, the injection molded corner window not only needs to have good transparency and glossiness, but also needs to have high strength and impact resistance to ensure that it can withstand various external forces and vibrations during driving.

[0004] The existing injection molding corner window process has some obvious defects when preparing the injection molding corner windows, which makes the injection molding corner windows prone to aging, yellowing, brittleness and other problems during long-term use, which seriously affects the appearance and service life of the car. First of all, the existing injection molding corner window process may have deficiencies in material selection. The plastic raw materials used may not have good anti-aging properties, or the anti-aging agents and other additives added to the raw materials are not effective enough to effectively resist the erosion of external factors such as ultraviolet rays and oxygen, which causes the injection molding corner windows to gradually age and turn yellow during use.

[0005] Secondly, the existing injection molding corner window process may have problems during the injection molding process. Improper settings of parameters such as temperature, pressure, and speed during the injection molding process may lead to problems such as stress concentration and uneven crystallization inside the injection molded corner window, thereby affecting the mechanical properties and anti-aging properties of the injection molded corner window.

[0006] In addition, the existing injection molding corner window process may not be perfect in post-processing. For example, during the cooling and solidification process of the injection molded corner window, the cooling speed is too fast or uneven, which may cause internal stress inside the injection molded corner window, thereby affecting its anti-aging performance. For example, during the surface treatment process of the injection molded corner window, improper treatment method or inappropriate selection of treatment agent may lead to a decrease in the anti-aging performance of the injection molded corner window surface.

[0007] In summary, the existing injection molding corner window process has some problems in material selection, injection molding and post-processing. These problems together lead to the injection molding corner window being prone to aging, yellowing, brittleness and other problems during long-term use, thus affecting the appearance and service life of the car. Summary of the invention

[0008] 1. Technical issues to be resolved

[0009] In view of the shortcomings of the prior art, the present invention provides a process for preparing anti-aging injection-molded corner windows for new energy vehicles, which has the advantages of being able to effectively resist erosion by external factors such as ultraviolet rays and oxygen, and improving the strength and toughness of the injection-molded corner windows. It solves the problem that the existing injection-molded corner window process is prone to aging, yellowing, brittleness, cracking, deformation, etc. during long-term use, which affects the appearance and service life of the vehicle.

[0010] (II) Technical solution

[0011] In order to achieve the above-mentioned purpose of effectively resisting erosion by external factors such as ultraviolet rays and oxygen and improving the strength and toughness of the injection-molded corner window, the present invention provides the following technical solution: a preparation process for an anti-aging injection-molded corner window for new energy vehicles, comprising the following steps:

[0012] Step 1) Selection of plastic raw materials: Select plastic raw materials suitable for injection molding corner windows, usually polycarbonate (PC) or polypropylene (PP) and other materials, and add appropriate amounts of ultraviolet absorbers, antioxidants, light stabilizers, toughening agents and lubricants;

[0013] Step 2) Drying of plastic raw materials: Place the plastic raw materials in a drying device for drying to remove moisture from the raw materials and avoid problems such as bubbles or hydrolysis during the injection molding process;

[0014] Step 3) Debugging of injection molding machine: According to the shape and size of the injection molding corner window, debug the parameters of the injection molding machine, such as injection pressure, injection speed, injection time, etc., to ensure the stability and consistency of the injection molding process;

[0015] Step 4) Mold installation: Install the injection mold on the injection molding machine, and debug and preheat it to ensure that the temperature and pressure of the mold are evenly distributed;

[0016] Step 5) Injection molding: Add the dried plastic raw material into the barrel of the injection molding machine, heat and melt the plastic raw material through the screw of the injection molding machine, and inject it into the mold. During the injection molding process, it is necessary to control parameters such as injection pressure, injection speed and injection time to ensure the quality and performance of the injection-molded corner window;

[0017] Step 6) Cooling and curing: After the injection molding is completed, the injection-molded corner window is taken out of the mold and placed in a cooling device for cooling and curing. During the cooling process, the cooling temperature and cooling time need to be controlled to avoid deformation or cracking of the injection-molded corner window;

[0018] Step 7) Post-processing: The injection-molded corner window after cooling and solidification needs to be post-processed, such as trimming, grinding, polishing, etc., to remove burrs and defects on the surface of the injection-molded corner window and improve its surface quality and glossiness;

[0019] Step 8) Inspection and packaging: Inspect the injection molded corner windows to ensure that their quality and performance meet the requirements. After passing the inspection, the injection molded corner windows are packaged for transportation and storage.

[0020] Preferably, the selection of the plastic raw material in step 1) further includes selecting a blend of polycarbonate (PC) and polypropylene (PP) as the plastic raw material, with the amount of polycarbonate (PC) being 40%-45% and the amount of polypropylene (PP) being 40%-45%.

[0021] Preferably, in step 2), the plastic raw material is dried at a temperature of 80° C. to 90° C. for 3 to 4 hours.

[0022] Preferably, in step 3) and step 5), the injection pressure is 100 MPa to 120 MPa, the injection speed is 50 mm / s to 60 mm / s, and the injection time is 0.8 s to 10 s.

[0023] Preferably, in step 4), the mold temperature is 80°C to 90°C.

[0024] Preferably, in step 6), the cooling temperature is 20° C. to 25° C., and the cooling and curing time is 20 minutes to 30 minutes.

[0025] Preferably, the plastic raw material is polycarbonate (PC) and the usage amount is 80% to 95%.

[0026] Preferably, the plastic raw material is polypropylene (PP) and the amount used is 80% to 95%.

[0027] Preferably, in step 8), the tensile strength of the injection-molded corner window is 55 to 60 MPa, the bending strength is 80 to 90 MPa, and the impact strength is 10 to 15 kJ / m 2 , transparency is 90 to 95%, gloss is 90 to 95%, and yellowing index is 0.5 to 1.0.

[0028] Preferably, in step 1), the ultraviolet absorber is 0.5% to 1%; the antioxidant is 0.5% to 1%; the light stabilizer is 0.5% to 1%; the toughening agent is 5% to 10%; the lubricant is 0.5% to 1%, the ultraviolet absorber is benzotriazole, the antioxidant is phosphite, the light stabilizer is hindered amine, the toughening agent is thermoplastic elastomer, and the lubricant is fatty acid ester.

[0029] (III) Beneficial effects

[0030] Compared with the prior art, the present invention provides a process for preparing an anti-aging injection-molded corner window for new energy vehicles, which has the following beneficial effects:

[0031] 1. The preparation process of anti-aging injection-molded corner windows for new energy vehicles uses special UV absorbers and stabilizers, which can effectively absorb and block UV radiation, thereby avoiding aging, yellowing and other problems of the injection-molded corner windows when exposed to sunlight for a long time. Secondly, the process uses special antioxidants and stabilizers, which can effectively resist oxygen erosion, thereby avoiding problems such as brittleness of the injection-molded corner windows during long-term use. In addition, the process also uses special chemically stable materials that can effectively resist erosion by various chemical substances, thereby avoiding problems such as discoloration and deformation of the injection-molded corner windows during long-term use, and can enable the injection-molded corner windows to effectively resist erosion by external factors such as UV rays and oxygen.

[0032] 2. The anti-aging injection-molded corner window preparation process for new energy vehicles uses special reinforcing materials, which can effectively improve the strength and toughness of the injection-molded corner windows, and improve the ability to withstand various pressures and vibrations during vehicle driving, ensuring that the injection-molded corner windows can maintain stable performance, thereby avoiding problems such as cracking and deformation of the injection-molded corner windows during long-term use. This not only greatly extends the service life of the injection-molded corner windows and reduces maintenance costs, but also provides safer and more reliable protection for drivers and passengers. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 This is a schematic diagram of the performance test results of the anti-aging injection-molded corner window of the present invention;

[0034] Figure 2 for Figure 1 Schematic diagram of performance test results of medium tensile strength;

[0035] Figure 3 for Figure 1 Schematic diagram of performance test results of medium bending strength;

[0036] Figure 4 for Figure 1 Schematic diagram of performance test results of medium impact strength;

[0037] Figure 5 for Figure 1 Schematic diagram of performance test results of medium transparency;

[0038] Figure 6 for Figure 1 Schematic diagram of performance test results for medium gloss;

[0039] Figure 7 for Figure 1 Schematic diagram of the performance test results of the medium yellowing index. DETAILED DESCRIPTION

[0040] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0041] See also Figures 1 to 7 The present invention provides a technical solution: a process for preparing an anti-aging injection-molded corner window for new energy vehicles, comprising the following steps:

[0042] In the first embodiment, polycarbonate (PC) is selected as the plastic raw material.

[0043] Step 1) Selection of plastic raw materials: Polycarbonate (PC) is selected as the plastic raw material, and its usage is 80%. In addition, 0.5% of ultraviolet absorber, 0.5% of antioxidant, 0.5% of light stabilizer, 5% of toughening agent and 0.5% of lubricant are added;

[0044] The ultraviolet absorber is a benzotriazole, such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole (UV-326), etc., the antioxidant is a phosphite, such as tris(2,4-di-tert-butylphenyl)phosphite (Antioxidant 168), etc., the light stabilizer is a hindered amine, such as N,N'-bis(2,2,6 ,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (light stabilizer 944), N-(2,2,6,6-tetramethyl-4-piperidinyl)-n-butylamine (light stabilizer 770), etc. The toughening agent is a thermoplastic elastomer: such as styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), etc. The lubricant is a fatty acid ester: such as butyl stearate, calcium stearate, etc.;

[0045] Polycarbonate has good transparency, strength and heat resistance, and is suitable for injection molding corner windows. UV absorbers, antioxidants and light stabilizers help improve the anti-aging performance of corner windows and extend their service life. Tougheners can increase the toughness of the material and improve the impact resistance of corner windows, while lubricants help improve fluidity during the injection molding process.

[0046] Step 2) Drying of the plastic raw material: placing the polycarbonate raw material in a drying device and drying it at 80° C. for 3 hours to remove moisture;

[0047] Drying treatment can prevent the moisture in the raw materials from generating bubbles or hydrolysis during the injection molding process, which will affect the quality of the corner window.

[0048] Step 3) Debugging of injection molding machine: According to the shape and size of the injection molding corner window, debug the parameters of the injection molding machine. The injection molding pressure is set to 100MPa, the injection molding speed is 50mm / s, and the injection molding time is 8s;

[0049] Reasonable injection molding parameters can ensure the stability and consistency of the injection molding process and guarantee the quality and performance of the corner windows.

[0050] Step 4) Mold installation: Install the injection mold on the injection molding machine, and debug and preheat it.

[0051] The mold temperature was set to 80°C;

[0052] Correct installation and preheating of the mold help ensure a smooth injection molding process, as well as the dimensional accuracy and surface quality of the corner window.

[0053] Step 5) Injection molding: Add the dried polycarbonate raw material into the barrel of an injection molding machine, heat and melt the raw material through the screw of the injection molding machine, and inject it into the mold;

[0054] Injection molding is a key step in transforming plastic raw materials into corner window products.

[0055] Step 6) Cooling and curing: After the injection molding is completed, the injection-molded corner window is taken out of the mold, placed in a cooling device, and cooled and cured at a temperature of 20° C. for 20 minutes;

[0056] Cooling and solidification stabilize the shape and size of the corner window to avoid deformation or cracking.

[0057] Step 7) Post-processing: trimming, grinding and polishing the injection-molded corner window after cooling and solidification to remove burrs and flaws on the surface and improve surface quality and glossiness;

[0058] Post-processing can make the corner window surface smoother and improve the appearance quality.

[0059] Step 8) Inspection and packaging: Inspect the injection-molded corner windows to ensure that their quality and performance meet the requirements. After passing the inspection, package them for transportation and storage;

[0060] Inspection and packaging are important links to ensure product quality and delivery. After passing the inspection, the injection molded corner windows will be packaged for transportation and storage.

[0061] The data of the injection-molded corner window after actual testing: tensile strength is 55MPa, bending strength is 80MPa, and impact strength is 10kJ / m 2 , transparency is 90%, glossiness is 90%, and yellowing index is 0.5.

[0062] In the second embodiment, polypropylene (PP) is selected as the plastic raw material. The polypropylene (PP) material has low cost and good chemical resistance, and is suitable for some applications with high cost requirements. In addition, the polypropylene (PP) material has good processing performance and is easy to be injection molded.

[0063] Step 1) Selection of plastic raw materials: Polycarbonate (PC) is selected as the plastic raw material, and its usage is 90%. In addition, 0.7% of ultraviolet absorber, 0.7% of antioxidant, 0.7% of light stabilizer, 7% of toughening agent and 0.7% of lubricant are added;

[0064] The ultraviolet absorber is a benzotriazole, such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole (UV-326), etc., the antioxidant is a phosphite, such as tris(2,4-di-tert-butylphenyl)phosphite (Antioxidant 168), etc., the light stabilizer is a hindered amine, such as N,N'-bis(2,2,6 ,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (light stabilizer 944), N-(2,2,6,6-tetramethyl-4-piperidinyl)-n-butylamine (light stabilizer 770), etc. The toughening agent is a thermoplastic elastomer: such as styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), etc. The lubricant is a fatty acid ester: such as butyl stearate, calcium stearate, etc.;

[0065] Polycarbonate has good transparency, strength and heat resistance, and is suitable for injection molding corner windows. UV absorbers, antioxidants and light stabilizers help improve the anti-aging performance of corner windows and extend their service life. Tougheners can increase the toughness of the material and improve the impact resistance of corner windows, while lubricants help improve fluidity during the injection molding process.

[0066] Step 2) Drying of the plastic raw material: placing the polycarbonate raw material in a drying device and drying it at 88° C. for 4 hours to remove moisture;

[0067] Drying treatment can prevent the moisture in the raw materials from generating bubbles or hydrolysis during the injection molding process, which will affect the quality of the corner window.

[0068] Step 3) Debugging of injection molding machine: According to the shape and size of the injection molding corner window, debug the parameters of the injection molding machine. The injection molding pressure is set to 110MPa, the injection molding speed is 55mm / s, and the injection molding time is 9s;

[0069] Reasonable injection molding parameters can ensure the stability and consistency of the injection molding process and guarantee the quality and performance of the corner windows.

[0070] Step 4) Mold installation: Install the injection mold on the injection molding machine, and debug and preheat it.

[0071] The mold temperature was set to 85°C;

[0072] Correct installation and preheating of the mold help ensure a smooth injection molding process, as well as the dimensional accuracy and surface quality of the corner window.

[0073] Step 5) Injection molding: Add the dried polycarbonate raw material into the barrel of an injection molding machine, heat and melt the raw material through the screw of the injection molding machine, and inject it into the mold;

[0074] Injection molding is a key step in transforming plastic raw materials into corner window products.

[0075] Step 6) Cooling and curing: After the injection molding is completed, the injection-molded corner window is taken out of the mold, placed in a cooling device, and cooled and cured at a temperature of 23° C. for 25 minutes;

[0076] Cooling and solidification stabilize the shape and size of the corner window to avoid deformation or cracking.

[0077] Step 7) Post-processing: trimming, grinding and polishing the injection-molded corner window after cooling and solidification to remove burrs and flaws on the surface and improve surface quality and glossiness;

[0078] Post-processing can make the corner window surface smoother and improve the appearance quality.

[0079] Step 8) Inspection and packaging: Inspect the injection-molded corner windows to ensure that their quality and performance meet the requirements. After passing the inspection, package them for transportation and storage;

[0080] Inspection and packaging are important links to ensure product quality and delivery. After passing the inspection, the injection molded corner windows will be packaged for transportation and storage.

[0081] The data of the injection-molded corner window after actual testing: tensile strength is 57MPa, bending strength is 86MPa, and impact strength is 13kJ / m 2 , transparency is 93%, glossiness is 92%, and yellowing index is 0.8.

[0082] In the third embodiment, a blend of polycarbonate (PC) and polypropylene (PP) is selected as the plastic raw material, with the amount of polycarbonate (PC) being 40% and the amount of polypropylene (PP) being 40%. This blend can combine the advantages of polycarbonate (PC) and polypropylene (PP) to improve the comprehensive performance of the injection-molded corner window.

[0083] Blends of polycarbonate (PC) and polypropylene (PP) offer high strength, toughness and heat resistance at a relatively low cost. Such blends can also improve the chemical resistance and processing properties of injection-molded corner windows.

[0084] Step 1) Selection of plastic raw materials: A blend of polycarbonate (PC) and polypropylene (PP) is used as the plastic raw material, with the amount of polycarbonate (PC) being 40% and the amount of polypropylene (PP) being 40%. In addition, 1% of ultraviolet absorber, 1% of antioxidant, 1% of light stabilizer, 10% of toughening agent and 1% of lubricant are added;

[0085] The ultraviolet absorber is a benzotriazole, such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (UV-P), 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole (UV-326), etc., the antioxidant is a phosphite, such as tris(2,4-di-tert-butylphenyl)phosphite (Antioxidant 168), etc., the light stabilizer is a hindered amine, such as N,N'-bis(2,2,6 ,6-tetramethyl-4-piperidinyl)-1,6-hexanediamine (light stabilizer 944), N-(2,2,6,6-tetramethyl-4-piperidinyl)-n-butylamine (light stabilizer 770), etc. The toughening agent is a thermoplastic elastomer: such as styrene-butadiene-styrene block copolymer (SBS), styrene-isoprene-styrene block copolymer (SIS), etc. The lubricant is a fatty acid ester: such as butyl stearate, calcium stearate, etc.;

[0086] Polycarbonate has good transparency, strength and heat resistance, and is suitable for injection molding corner windows. UV absorbers, antioxidants and light stabilizers help improve the anti-aging performance of corner windows and extend their service life. Tougheners can increase the toughness of the material and improve the impact resistance of corner windows, while lubricants help improve fluidity during the injection molding process.

[0087] Step 2) Drying of the plastic raw material: placing the polycarbonate raw material in a drying device and drying it at 95° C. for 4 hours to remove moisture;

[0088] Drying treatment can prevent the moisture in the raw materials from generating bubbles or hydrolysis during the injection molding process, which will affect the quality of the corner window.

[0089] Step 3) Debugging of injection molding machine: According to the shape and size of the injection molding corner window, debug the parameters of the injection molding machine. The injection molding pressure is set to 115MPa, the injection molding speed is 60mm / s, and the injection molding time is 10s;

[0090] Reasonable injection molding parameters can ensure the stability and consistency of the injection molding process and guarantee the quality and performance of the corner windows.

[0091] Step 4) Mold installation: Install the injection mold on the injection molding machine, and debug and preheat it.

[0092] The mold temperature was set to 90°C;

[0093] Correct installation and preheating of the mold help ensure a smooth injection molding process, as well as the dimensional accuracy and surface quality of the corner window.

[0094] Step 5) Injection molding: Add the dried polycarbonate raw material into the barrel of an injection molding machine, heat and melt the raw material through the screw of the injection molding machine, and inject it into the mold;

[0095] Injection molding is a key step in transforming plastic raw materials into corner window products.

[0096] Step 6) Cooling and curing: After the injection molding is completed, the injection-molded corner window is taken out of the mold, placed in a cooling device, and cooled and cured at a temperature of 25° C. for 30 minutes;

[0097] Cooling and solidification stabilize the shape and size of the corner window to avoid deformation or cracking.

[0098] Step 7) Post-processing: trimming, grinding and polishing the injection-molded corner window after cooling and solidification to remove burrs and flaws on the surface and improve surface quality and glossiness;

[0099] Post-processing can make the corner window surface smoother and improve the appearance quality.

[0100] Step 8) Inspection and packaging: Inspect the injection-molded corner windows to ensure that their quality and performance meet the requirements. After passing the inspection, package them for transportation and storage;

[0101] Inspection and packaging are important links to ensure product quality and delivery. After passing the inspection, the injection molded corner windows will be packaged for transportation and storage.

[0102] The data of the injection-molded corner window after actual testing: tensile strength is 60MPa, bending strength is 90MPa, and impact strength is 15kJ / m 2 , transparency is 94%, glossiness is 95%, and yellowing index is 0.9.

[0103] Compared with other embodiments, embodiment three has good comprehensive performance, combining the advantages of PC and PP, and has higher strength, toughness and heat resistance. Secondly, the cost is lower. By using a blend, the cost can be reduced to a certain extent. Finally, its chemical resistance is effectively improved, and the chemical resistance of the blend is better than that of a single polycarbonate (PC) or polypropylene (PP) material.

[0104] Compared with the existing technology: the preparation process of the anti-aging injection-molded corner window for new energy vehicles adopts special ultraviolet absorbers and stabilizers, which can effectively absorb and block ultraviolet radiation, thereby avoiding the aging and yellowing of the injection-molded corner window when exposed to sunlight for a long time. Secondly, the process adopts special antioxidants and stabilizers, which can effectively resist the erosion of oxygen, thereby avoiding the brittleness of the injection-molded corner window during long-term use. In addition, the process also adopts special chemically stable materials, which can effectively resist the erosion of various chemical substances, thereby avoiding the discoloration and deformation of the injection-molded corner window during long-term use. The corner windows can effectively resist the erosion of external factors such as ultraviolet rays and oxygen. The special reinforcing materials used can effectively improve the strength and toughness of the injection-molded corner windows, and improve the ability to withstand various pressures and vibrations during vehicle driving, ensuring that the injection-molded corner windows can maintain stable performance, thereby avoiding the injection-molded corner windows from cracking, deformation and other problems during long-term use. It not only greatly extends the service life of the injection-molded corner windows and reduces maintenance costs, but also provides drivers and passengers with safer and more reliable protection, and solves the problem that the existing injection-molded corner window process is prone to aging, yellowing, brittleness, cracking, deformation and other problems during long-term use, affecting the appearance and service life of the car.

[0105] It should be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or device including the element.

[0106] While the embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that many changes, modifications, substitutions and variations can be made to the embodiments without departing from the principles and spirit of the invention.

Claims

1. A process for preparing anti-aging injection-molded corner windows for new energy vehicles. It is characterized in that The following steps are involved: Step 1) Selection of plastic raw materials: Select plastic raw materials suitable for injection molding corner windows, usually polycarbonate (PC) or polypropylene (PP) and other materials, and add appropriate amounts of ultraviolet absorbers, antioxidants, light stabilizers, toughening agents and lubricants; Step 2) Drying of plastic raw materials: Place the plastic raw materials in a drying device for drying to remove moisture from the raw materials and avoid problems such as bubbles or hydrolysis during the injection molding process; Step 3) Debugging of injection molding machine: According to the shape and size of the injection molding corner window, debug the parameters of the injection molding machine, such as injection pressure, injection speed, injection time, etc., to ensure the stability and consistency of the injection molding process; Step 4) Mold installation: Install the injection mold on the injection molding machine, and debug and preheat it to ensure that the temperature and pressure of the mold are evenly distributed; Step 5) Injection molding: Add the dried plastic raw material into the barrel of the injection molding machine, heat and melt the plastic raw material through the screw of the injection molding machine, and inject it into the mold. During the injection molding process, it is necessary to control parameters such as injection pressure, injection speed and injection time to ensure the quality and performance of the injection-molded corner window; Step 6) Cooling and curing: After the injection molding is completed, the injection-molded corner window is taken out of the mold and placed in a cooling device for cooling and curing. During the cooling process, the cooling temperature and cooling time need to be controlled to avoid deformation or cracking of the injection-molded corner window; Step 7) Post-processing: The injection-molded corner window after cooling and solidification needs to be post-processed, such as trimming, grinding, polishing, etc., to remove burrs and defects on the surface of the injection-molded corner window and improve its surface quality and glossiness; Step 8) Inspection and packaging: Inspect the injection molded corner windows to ensure that their quality and performance meet the requirements. After passing the inspection, the injection molded corner windows are packaged for transportation and storage.

2. According to claim 1, a process for preparing an anti-aging injection-molded corner window for new energy vehicles, Features: The selection of plastic raw materials in step 1) also includes selecting a blend of polycarbonate (PC) and polypropylene (PP) as the plastic raw material, with the amount of polycarbonate (PC) being 40%-45% and the amount of polypropylene (PP) being 40%-45%.

3. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In the step 2), the plastic raw material is dried at a temperature of 80° C. to 90° C. for 3 to 4 hours.

4. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In step 3) and step 5), the injection pressure is 100 MPa to 120 MPa, the injection speed is 50 mm / s to 60 mm / s, and the injection time is 8 s to 10 s.

5. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In the step 4), the mold temperature is 80°C to 90°C.

6. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In step 6), the cooling temperature is 20° C. to 25° C., and the cooling and curing time is 20 minutes to 30 minutes.

7. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: The plastic raw material is polycarbonate (PC) and the usage amount is 80% to 95%.

8. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: The plastic raw material is polypropylene (PP) and the usage is 80% to 95%.

9. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In step 8), the injection-molded corner window has a tensile strength of 55 to 60 MPa, a flexural strength of 80 to 90 MPa, and an impact strength of 10 to 15 kJ / m 2 , transparency is 90 to 95%, gloss is 90 to 95%, and yellowing index is 0.5 to 1.

0.

10. The process for preparing an anti-aging injection-molded corner window for new energy vehicles according to claim 1, Features: In the step 1), the ultraviolet absorber is 0.5% to 1%; the antioxidant is 0.5% to 1%; the light stabilizer is 0.5% to 1%; the toughening agent is 5% to 10%; the lubricant is 0.5% to 1%, the ultraviolet absorber is benzotriazole, the antioxidant is phosphite, the light stabilizer is hindered amine, the toughening agent is thermoplastic elastomer, and the lubricant is fatty acid ester.