Water-based zinc ion battery coating, water-based zinc ion battery zinc negative electrode and application of water-based zinc ion battery zinc negative electrode
By coating the D-CeFe-PBA coating on the surface of the zinc negative electrode of the zinc ion battery, the dendrite growth and corrosion problems of the zinc negative electrode are solved, and more stable electrochemical performance and longer cycle life are achieved, which improves the battery Overall performance and security.
Patent Information
- Application Number
- CN202411141548.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-22
AI Technical Summary
Problems such as dendrites of zinc negative electrodes in aqueous zinc ion batteries affect the balun efficiency and cycle life of the battery, and the existing technology is difficult to effectively solve.
The surface of the zinc negative electrode was coated with D-CeFe-PBA, and the dodecahedral morphology with a three-dimensional open frame structure was formed by mixing the binder and D-CeFe-PBA and vacuum drying, preventing the direct effect of the zinc negative electrode and the electrolyte. Contact to inhibit the occurrence of side reactions.
It improves the reversibility and stability of the zinc negative electrode, extends the cycle life of the battery, and optimizes the electrochemical performance, which significantly improves the safety and performance of the battery.
Smart Images

Figure CN119009183A_ABST
Abstract
Description
Technical Field
[0002] The invention belongs to the technical field of zinc ion battery materials, and in particular relates to an aqueous zinc ion battery coating, a negative electrode and a battery. Background Art
[0004] Zinc-ion battery is a promising energy storage technology with advantages such as low cost, high safety, high energy density and low electrode potential. In recent years, zinc metal cathode materials such as manganese-based oxides, vanadium-based oxides, polyanion compounds, sustainable quinone compounds, Prussian blue compounds, etc. have become research hotspots, promoting significant progress in the research and development of ZIBs. In the research background of aqueous zinc-ion batteries, the key issues are mainly concentrated on the zinc negative electrode, including dendrite growth, corrosion and hydrogen evolution, which seriously affect the coulombic efficiency and cycle life of the battery.
[0005] To solve these problems, researchers have adopted a variety of strategies, one of which is to coat the surface of the zinc negative electrode with functional materials. These coatings can inhibit the growth of dendrites and reduce the occurrence of side reactions, while being simple to operate and easy to control. Through the application of interface modification strategies, it is expected to accelerate the practical application of zinc-ion batteries, achieve effective control and management of complex reactions inside the battery, and thus improve the performance and safety of the battery. With the continuous emergence of new materials and technologies, this field is expected to continue to develop rapidly, providing more possibilities for future energy storage solutions. Summary of the invention
[0007] The purpose of the present invention is to provide an aqueous zinc ion battery coating and its application in order to overcome the deficiencies and disadvantages of the prior art.
[0008] The binder was mixed with D-CeFe-PBA, and a proper amount of water and ethanol was added to prepare a uniform slurry, which was coated on the zinc negative electrode. After vacuum drying, a zinc negative electrode with a D-CeFe-PBA coating was obtained.
[0009] Preferably, in the above-mentioned method for preparing a metal zinc negative electrode having a D-CeFe-PBA coating, the mass ratio of the binder to D-CeFe-PBA is 1:50 to 1:5.
[0010] Preferably, in the above method for preparing a metal zinc negative electrode having a D-CeFe-PBA coating, the thickness of the zinc negative electrode is 10 to 50 μm.
[0011] Preferably, in the above-mentioned method for preparing a metal zinc negative electrode having a D-CeFe-PBA coating, the vacuum drying temperature is 60 to 90° C., and the vacuum drying time is 6 to 24 hours.
[0012] Preferably, in the above-mentioned method for preparing a metal zinc negative electrode having a D-CeFe-PBA coating, the zinc negative electrode comprises one or more of zinc element and zinc alloy.
[0013] Preferably, in the above-mentioned method for preparing a metal zinc negative electrode having a D-CeFe-PBA coating, the zinc negative electrode further includes a pretreatment process before use, specifically: The zinc negative electrode is cleaned and dried with water and anhydrous ethanol in turn, and then smashed.
[0014] The present invention also provides an application of a metal zinc negative electrode having a D-CeFe-PBA coating in assembling an aqueous zinc ion battery.
[0015] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects: (1) The present invention coats D-CeFe-PBA on the surface of metal zinc, and then vacuum dries to achieve the transformation from liquid phase to solid phase, thereby obtaining a metal zinc composite negative electrode with a D-CeFe-PBA coating. The main component of the coating, the D-CeFe-PBA molecule, has a three-dimensional open dodecahedral metal framework structure, and its wide channels make it possible for larger ions to be embedded / ejected.
[0016] (2) The D-CeFe-PBA coating provided by the present invention can physically prevent the direct contact between the zinc negative electrode and the electrolyte, so that the metal zinc negative electrode is protected from corrosion by water molecules in the electrolyte, and the deprotonation of water molecules in the solvent sheath is inhibited, thereby improving the reversibility and stability of the zinc negative electrode.
[0017] (3) The D-CeFe-PBA coating provided by the present invention has a uniform dodecahedral morphology. Compared with the D-CeFe-PBA coating that does not have the special dodecahedral morphology, the coating with a uniform dodecahedral morphology structure exhibits more stable and longer-lasting electrochemical performance when applied to the zinc negative electrode. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings: In order to more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art description. Figure 1 It is a test diagram of the cycle life of zinc symmetric batteries of comparative examples and experimental examples; Figure 2It is the contact angle measurement diagram of comparative example and experimental example; Figure 3 It is a full-battery electrochemical performance test diagram of the comparative example and the experimental example. DETAILED DESCRIPTION
[0021] The present invention provides a zinc negative electrode with a D-CeFe-PBA coating and application thereof, comprising the following steps: Step 1, dissolving a cerium salt in water to prepare a cerium salt solution; Step 2, under stirring, add acetylacetone and then add ammonia water to form a yellow flocculent precipitate; Step 3: adding potassium ferrocyanide solution to the yellow flocculent precipitate prepared in step 2, and then placing it in air for aging; the precipitate is centrifuged, washed three times with deionized water, washed three times with anhydrous ethanol, and dried to obtain a light yellow product; Step 4: Mix the binder with the light yellow product, add an appropriate amount of water and ethanol to prepare a uniform slurry, coat it on the zinc negative electrode, and obtain a zinc negative electrode with a D-CeFe-PBA coating after vacuum drying.
[0022] In the present invention, the zinc negative electrode comprises one or more of zinc element and zinc alloy, and is more preferably zinc element. In the present invention, the zinc negative electrode also includes a pretreatment process before use, specifically: The zinc negative electrode is cleaned and dried with water and anhydrous ethanol in turn, and then smashed.
[0023] In the present invention: 1. A MOF-based phase interface with D-CeFe-PBA as raw material was constructed. The special crystal faces exposed by the special dodecahedral morphology structure enable it to achieve perfect lattice matching with the zinc negative electrode, guiding the uniform deposition of zinc ions. The interfacial shielding effect of the uniform and even seamless MOF phase interface can not only protect the zinc negative electrode from corrosion, but also inhibit a series of side reactions such as hydrogen evolution.
[0024] 2. The 3D open framework structure of D-CeFe-PBA uniformly grown on the surface of the zinc negative electrode effectively optimizes the inhomogeneous electric field at the electrode / electrolyte interface, homogenizes the zinc ion flux, forms a fast and stable zinc electroplating kinetics, and avoids the inhomogeneous zinc nucleation growth caused by the tip effect.
[0025] 3. D-CeFe-PBA has a special open ion channel and can be used as a highly zinc-affinity mediator and ion sieve, effectively avoiding the strong Coulomb interaction between zinc ions and the surrounding water sheath layer and the small local pH increase at the Helmholtz layer, which greatly reduces the original high desolvation energy barrier and inhibits the occurrence of hydrogen evolution reaction and the formation of by-product hydroxyzinc sulfate hexahydrate.
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example 1 Dissolve cerium salt in deionized water to obtain a 1 mol / L cerium salt solution. Under stirring conditions at a speed of 200 r / min and a temperature of 25°C, add 10 mL of water, 0.1 ml of acetylacetone and 0.2 mL of ammonia water in sequence. After the appearance of yellow flocs, add 6 mL of 0.5 mol / L potassium ferrocyanide solution. Potassium ferrocyanide needs to be added after ammonia water and acetylacetone; the precipitate is centrifuged, washed three times with deionized water, washed three times with anhydrous ethanol, and dried to obtain light yellow D-CeFe-PBA. Grind the binder and D-CeFe-PBA in a mortar at a mass ratio of 1:50, add appropriate amount of water and ethanol and grind into a uniform slurry. Coat the uniform slurry on metal zinc, and then place it in a vacuum drying oven at 80°C for 12 hours to obtain a metal zinc negative electrode with a D-CeFe-PBA coating. Figure 1 As shown, the obtained metal zinc negative electrode with D-CeFe-PBA coating was applied to an aqueous zinc ion battery, and the charge and discharge cycles of the comparative example and the experimental example were carried out at the same time. The battery cycle life of the comparative example was less than 400 hours, while the experimental example had an ultra-long cycle life of nearly 4300 hours. As shown in Figure 2, the contact angle of the zinc negative electrode of the experimental example was 122.2°, compared with 99.6° of the comparative example. The D-CeFe-PBA coating greatly improved the contact between the electrode and the electrolyte, making it easier for zinc ions in the electrolyte to reach the negative electrode side, ensuring sufficient zinc ion supply during the cycle. Figure 3 As shown, since the D-CeFe-PBA coating plays an important role in suppressing the generation of dendrites and by-products, the D-CeFe-PBA@Zn-based full battery achieves long-term cycle stability. After 1000 cycles, the D-CeFe-PBA@Zn-based full battery has a retention rate of 57.33% compared with 47.58% of the Zn-based full battery.
[0027] Example 2 The binder and D-CeFe-PBA were ground evenly in a mortar at a mass ratio of 1:20, and then ground into a uniform slurry by adding an appropriate amount of water and ethanol. The uniform slurry was coated on the metal zinc, and then placed in a vacuum drying oven at 80 ° C for 12 h to obtain a metal zinc negative electrode with a D-CeFe-PBA coating.
[0028] Example 3 The binder and D-CeFe-PBA were ground evenly in a mortar at a mass ratio of 1:5, and then ground into a uniform slurry by adding an appropriate amount of water and ethanol. The uniform slurry was coated on the metal zinc, and then placed in a vacuum drying oven at 80 ° C for 12 h to obtain a metal zinc negative electrode with a D-CeFe-PBA coating.
[0029] For example, certain words are used in the specification and claims to refer to specific components or methods. Those skilled in the art should understand that different regions may use different nouns to refer to the same component. This specification and claims do not use differences in names as a way to distinguish components. For example, "including" mentioned throughout the specification and claims is an open term, so it should be interpreted as "including but not limited to". "Approximately" means that within an acceptable error range, those skilled in the art can solve the technical problem within a certain error range and basically achieve the technical effect. The subsequent description of the specification is a preferred embodiment of the present application, but the description is for the purpose of illustrating the general principles of the present application, and is not used to limit the scope of the present application. The scope of protection of the present application shall be determined by the attached claims.
[0030] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such a product or system. In the absence of more restrictions, the elements defined by the sentence "comprises a ..." do not exclude the existence of other identical elements in the product or system including the elements.
[0031] The above description shows and describes several preferred embodiments of the invention, but as mentioned above, it should be understood that the invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. Changes and modifications made by those skilled in the art should be within the scope of protection of the claims attached to the invention without departing from the spirit and scope of the invention.
Claims
1. An aqueous zinc ion battery coating, characterized in that: The invention comprises a binder and polyhedral cerium-ferro-Prussian blue (D-CeFe-PBA).
2. The aqueous zinc ion battery coating according to claim 1, characterized in that: The mass ratio of the binder to D-CeFe-PBA is 1:50-1:
5.
3. The aqueous zinc ion battery coating according to claim 1, characterized in that: The morphology structure of the polyhedral ferrocerium Prussian blue (D-CeFe-PBA) is a dodecahedron.
4. The aqueous zinc ion battery coating according to claim 1, characterized in that: The binder is one or a mixture of PTFE, PVDF, CMC, SBR, PAA and PVA.
5. A zinc negative electrode for an aqueous zinc ion battery, characterized in that: The invention comprises a zinc base layer and an aqueous zinc ion battery coating as claimed in any one of claims 1 to 4 attached to the zinc base layer.
6. An aqueous zinc ion battery coating, characterized in that: The coating method is one or more of drip coating, scraper coating and spin coating.
7. Use of the aqueous zinc ion battery coating according to claims 1-6 in an aqueous zinc ion battery or a zinc ion electrochemical energy storage device.
Citation Information
Cited By
Aqueous zinc ion battery and preparation and application of modified zinc negative electrode of aqueous zinc ion battery
CN119833526A
Preparation and application of aqueous zinc-ion battery and modified zinc anode thereof
CN119833526B