Environment-friendly recycled asphalt modifier and preparation method thereof

The old asphalt performance is solved by using a combination modifier of base oil, phase change reaction materials, interface agents and thermoplastic rubber in regenerated asphalt technology to activate the performance of old asphalt and improve the water stability and low temperature performance of the regenerated asphalt mixture. The problem of insufficient improvement of the performance of matrix asphalt has achieved more efficient utilization and cost reduction of recycled asphalt.

CN118931208APending Publication Date: 2024-11-12CCCC SHEC DONGMENG ENG CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411099332.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing regenerated asphalt technology, the performance of old asphalt is not fully activated, resulting in poor water stability and low-temperature performance of regenerated asphalt mixture, and insufficient performance improvement of matrix asphalt paving after the traffic load increases.

Method used

The environmentally friendly regenerated asphalt modifier consisting of base oil, phase change reaction materials, interface agents and thermoplastic rubber is used to connect the molecular bonds of the phase change reaction materials to the thermoplastic rubber, combine the interface agent to reduce the interfacial tension, activate the performance of old asphalt, and Improve low-temperature crack resistance by thermoplastic rubber.

Benefits of technology

It significantly improves the water stability and low-temperature performance of recycled asphalt mixture, reduces the mixing temperature, increases the proportion of old materials, and achieves the purpose of energy saving, emission reduction and cost reduction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses an environment-friendly recycled asphalt modifier which is prepared from the following components in parts by weight: 75-95 parts of base oil, 2-5 parts of a phase change reaction material, 5-10 parts of an interface material and 3-6 parts of thermoplastic rubber. According to the environment-friendly recycled asphalt modifier, the phase-change reaction material is adopted to modify the base oil, meanwhile, the interface active agent is added, the interface energy of a regenerant is reduced, the performance of old asphalt is better activated and recovered, and the performance of a waste asphalt mixture is further improved through the thermoplastic latex; the water stability and the low-temperature crack resistance of the recycled asphalt mixture are improved; in addition, the invention also discloses a preparation method of the environment-friendly recycled asphalt modifier.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of road asphalt, and in particular to an environmentally friendly recycled asphalt modifier and a preparation method thereof. Background Art

[0003] Statistics released by the Ministry of Transport show that currently in my country, the amount of waste asphalt pavement materials generated each year in major and medium-sized maintenance projects of trunk roads alone is as high as 160 million tons. If they are utilized, the material costs can be saved by about 30 billion yuan each year, and a large amount of land occupied by waste mixtures can also be reduced.

[0004] Asphalt is one of the main components of asphalt pavement and is derived from petroleum. Petroleum resources are not renewable, and excessive exploitation will lead to resource depletion. In 2012, my country's apparent asphalt consumption exceeded 21 million tons, most of which was road asphalt. About 350 to 400 tons of asphalt per kilometer of expressway (4 lanes) are consumed. Recycling these asphalt mixtures will produce great economic and social benefits.

[0005] Asphalt pavement regeneration technology is a process in which the old asphalt pavement is pre-treated by milling, recycling, and screening, and then remixed with new asphalt pavement materials in a certain proportion using corresponding regeneration technology to form an asphalt mixture that can meet certain road performance requirements and is then used to resurface the road. Traditional asphalt pavement regeneration technology is mainly hot-regeneration asphalt mixture technology, which is to add asphalt regeneration agent to the old asphalt mixture and heat it to a high temperature of 150°C-180°C to mix it with new asphalt and mineral materials for regeneration.

[0006] The aging of asphalt is mainly caused by the reduction of aromatic components in asphalt. Conventional regeneration agents on the market can restore the performance of old asphalt by supplementing aromatic components and blending asphalt components. However, there is a problem of fusion with old asphalt during the addition of existing regeneration agents. It is only added from the component level, without truly activating the old asphalt from the interface, which makes the asphalt performance in the old material unable to be fully exerted, resulting in poor water stability and low temperature performance of the regenerated asphalt mixture; in addition, many early asphalt pavements were paved with base asphalt. With the increase of traffic load, it is also a problem to be solved to significantly improve the performance of the road surface after regeneration. Summary of the invention

[0007] The main technical problem solved by the present invention is to overcome the above-mentioned existing problems and provide an environmentally friendly recycled asphalt modifier, which can not only fully integrate the regeneration agent with the old asphalt from the interface, activate the asphalt performance, and significantly improve the water stability and low-temperature performance of the asphalt mixture, but also further modify the old material through the regeneration agent to improve the pavement performance of the recycled asphalt mixture.

[0008] In order to solve the above technical problems, a technical solution adopted by the present invention is: an environmentally friendly recycled asphalt modifier, which is made of the following components: Base oil 75~95 parts; 2~5 parts of phase change reaction material; 5~10 parts of interface agent; Thermoplastic rubber 3~6 parts; The above parts are all by weight.

[0009] Preferably, the base oil is lubricating oil base oil, furfural extracted oil, C6~C 10 Alkane solvent, C8~C 10 One or more of aromatic base oil, catalytic cracking slurry, cracking tar, vacuum residue, atmospheric residue, cycloalkyl atmospheric or vacuum residue.

[0010] Preferably, the phase change reaction material is trans-polyoctene rubber.

[0011] Preferably, the interfacial agent is a cationic surfactant.

[0012] Preferably, the cationic surfactant is C 12 ~C 18 Quaternary amine, lignin amine, C 12 ~C 18 Alkyl ether polyamine, C 12 ~C 18 Alkyl ether amines, tannin amine derivatives, phenolic resin amine derivatives, amine-modified polyacrylates; C 12 ~C 18 Fatty amide amine and C 12 ~C 18 Fatty acids and their derivatives, saturated C 12 ~C 18 Alkyl monoamines, unsaturated C 12 ~C 18 Alkyl monoamines, saturated C 12 ~C 18 Alkyl polypropylene polyamine, unsaturated C 12 ~C 18 Alkyl polypropylene polyamine, saturated C containing polyoxyethylene groups 12 ~C 18 Alkyl monoamines, unsaturated C 12 ~C 18 Alkyl monoamines, saturated C 12 ~C 18 Alkyl polypropylene polyamine, unsaturated C 12 ~C 18 Alkyl polypropylene polyamine, saturated C 12 ~C 18 Alkyl aryl monoamines, unsaturated C12 ~C18 alkyl aromatic monoamines, saturated C 12 ~C 18 Alkyl aromatic polypropylene polyamine and unsaturated C 12 ~C 18 One or more of alkylaryl polypropylene polyamines.

[0013] Preferably, the thermoplastic rubber is a styrene-butadiene block copolymer.

[0014] The present invention also provides a method for preparing the above-mentioned environmentally friendly regenerated asphalt modifier, comprising the following steps: (1) Weigh 75-95 parts of base oil by weight and heat to 160-170°C; (2) Add 3 to 6 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 20 to 30 minutes; (3) Control the temperature to 130-140°C, turn off the vacuum device, add 2-5 parts of phase change reaction material to the above mixture, stir for 10-15 minutes, cool to 60-70°C, add 5-10 parts of interface agent, stir for 5-10 minutes to obtain environmentally friendly recycled asphalt modifier.

[0015] Preferably, in the above step (2), the vacuum degree of the vacuum device is controlled at 10-30 Pa.

[0016] The beneficial effects of the present invention are as follows: different from the prior art, the environmentally friendly recycled asphalt modifier uses phase change reaction materials to modify the base oil, and adds a surfactant at the same time to reduce the interfacial energy of the regeneration agent, better activate and restore the performance of the old asphalt, and further improve the performance of the waste asphalt mixture through thermoplastic rubber, improve the water stability and low-temperature crack resistance of the recycled asphalt mixture; in addition, the environmentally friendly recycled asphalt modifier of the present invention can also reduce the mixing temperature of the recycled asphalt mixture due to the interfacial effect, avoid secondary aging of the old asphalt, further increase the addition ratio of RAP, and achieve the purpose of energy saving, emission reduction and cost reduction. DETAILED DESCRIPTION

[0017] The present invention provides an environmentally friendly recycled asphalt modifier, which is prepared from the following components: 75-95 parts of base oil, 2-5 parts of phase change reaction material, 5-10 parts of interface agent, and 3-6 parts of thermoplastic rubber; the above parts are all measured by weight.

[0018] The mechanism of action of the environmentally friendly recycled asphalt modifier of the present invention is as follows: the thermoplastic rubber is wrapped by the phase change material, a molecular bond is formed between the base oil and the thermoplastic rubber, and at the same time, the interfacial tension of the regeneration agent is reduced by the interfacial agent, so as to achieve better fusion and modification with the asphalt in the old material, fully activate the performance of the old asphalt, enhance the adhesion between the asphalt and the aggregate, prevent water from entering between the asphalt and the aggregate, and reduce the risk of water damage; in addition, through the modification effect of the thermoplastic rubber, the temperature sensitivity of the asphalt is reduced, and the low-temperature crack resistance of the recycled asphalt mixture is improved.

[0019] In addition, the present invention also provides a method for preparing the above-mentioned environmentally friendly regenerated asphalt modifier, comprising the following steps: (1) Weigh 75-95 parts of base oil by weight and heat to 160-170°C; (2) Add 3 to 6 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 20 to 30 minutes; (3) Control the temperature to 130-140°C, turn off the vacuum device, add 2-5 parts of phase change reaction material to the above mixture, stir for 10-15 minutes, cool to 60-70°C, add 5-10 parts of interface agent, stir for 5-10 minutes to obtain environmentally friendly recycled asphalt modifier.

[0020] Add 5% to 10% of the asphalt weight of environmentally friendly recycled asphalt modifier to the molten base asphalt, heat to 140℃~170℃ and stir for 20 minutes, then spray it into the mixing tank as recycled modified asphalt to mix with old and new materials to produce recycled asphalt mixture.

[0021] The following specific examples and comparative examples of the present invention will further clarify the present invention, but they are not intended to limit the present invention. In the examples and comparative examples of the present invention, the base asphalt used is petroleum asphalt. In a broad sense, asphalt is a material containing natural asphalt as a main component or a material obtained as a residue through an oil refining process. In a narrow sense, asphalt is a black high-viscosity liquid or semi-solid component present in crude oil; it also includes corresponding polymer-modified asphalt, but the present invention is not limited to this. The asphalt quality requirements meet the technical requirements for road asphalt in the Technical Specifications for Highway Asphalt Pavement Construction promulgated by the Ministry of Transport.

[0022] In addition, in the embodiments of the present invention, the softening point test, ductility test and penetration test of asphalt, the mixing and molding process test of asphalt mixture, the void ratio test, the Marshall residual stability test, the freeze-thaw cracking strength ratio test, the rutting dynamic stability test and the low-temperature beam bending test and other test methods all adopt the test methods specified in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011).

[0023] The same batch of recycled asphalt pavement (RAP) was used in the embodiment and the comparative example. The asphalt content in the RAP was 3.1% after testing; the amount of RAP added in the recycled asphalt mixture was 35%.

[0024] The commercially available regeneration agent in the comparative example was purchased from Hubei Fengteng Petroleum Products Co., Ltd. RA25 asphalt regeneration agent.

[0025] Embodiment 1: (1) Weigh 75 parts of furfural extracted oil by weight and heat to 160°C; (2) Add 3 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 20 minutes; (3) Control the temperature to 130°C, turn off the vacuum device, add 2.5 parts of trans-polyoctene rubber to the above mixture, stir for 15 minutes, cool to 60°C, add 5 parts of C 18 Alkyl ether polyamine, stir for 5 minutes to obtain the environmentally friendly recycled asphalt modifier.

[0026] 10% of the asphalt weight of environmentally friendly recycled asphalt modifier is added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as recycled modified asphalt to mix with RAP and new aggregate to produce recycled asphalt mixture.

[0027] The specific technical indicators of the obtained recycled modified asphalt and recycled asphalt mixture are shown in Table 1.

[0028] Embodiment 2: (1) Weigh 95 parts of aromatic oil by weight and heat to 160°C; (2) Add 6 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 30 minutes; (3) Control the temperature to 140°C, turn off the vacuum device, add 5 parts of trans-polyoctene rubber to the above mixture, stir for 20 minutes, cool to 65°C, add 10 parts of lignin amine, and stir for 10 minutes to obtain an environmentally friendly recycled asphalt modifier.

[0029] 5% of the asphalt weight of environmentally friendly recycled asphalt modifier is added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as recycled modified asphalt to mix with RAP and new aggregate to produce recycled asphalt mixture.

[0030] The specific technical indicators of the obtained recycled modified asphalt and recycled asphalt mixture are shown in Table 1.

[0031] Embodiment 3: (1) Weigh 45 parts of aromatic oil and 45 parts of furfural extracted oil by weight and heat to 155°C; (2) Add 4.5 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 30 minutes; (3) Control the temperature to 135°C, turn off the vacuum device, add 4.5 parts of trans-polyoctene rubber to the above mixture, stir for 20 minutes, cool to 60°C, add 5 parts of alkyl ether amine and 3 parts of amine-modified polyacrylate, stir for 15 minutes, and obtain an environmentally friendly recycled asphalt modifier.

[0032] 6% of the asphalt weight of environmentally friendly recycled asphalt modifier is added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as recycled modified asphalt to mix with RAP and new aggregate to produce recycled asphalt mixture.

[0033] The specific technical indicators of the obtained recycled modified asphalt and recycled asphalt mixture are shown in Table 1.

[0034] Embodiment 4: (1) Weigh 35 parts of aromatic oil and 45 parts of vacuum residue oil by weight and heat them to 160°C; (2) Add 4 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 30 minutes; (3) Control the temperature to 130°C, turn off the vacuum device, add 3 parts of trans-polyoctene rubber to the above mixture, stir for 20 minutes, cool to 60°C, add 6 parts of alkyl ether amine, and stir for 15 minutes to obtain an environmentally friendly recycled asphalt modifier.

[0035] 7% of the asphalt weight of environmentally friendly recycled asphalt modifier is added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as recycled modified asphalt to mix with RAP and new aggregate to produce recycled asphalt mixture.

[0036] The specific technical indicators of the obtained recycled modified asphalt and recycled asphalt mixture are shown in Table 1.

[0037] Comparative Example 1: In this comparative example, RA25 asphalt regeneration agent with a weight of 10% of asphalt was added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as regenerated modified asphalt to mix with RAP and new aggregate to produce regenerated asphalt mixture. The specific technical indicators of the obtained regenerated modified asphalt and regenerated asphalt mixture are shown in Table 1.

[0038] Comparative Example 2: In this comparative example, RA25 asphalt regeneration agent with a weight of 5% of asphalt was added to the molten base asphalt, heated to 145°C and stirred for 20 minutes, and then sprayed into the mixing tank as a regenerated modified asphalt to mix with RAP and new aggregate to produce a regenerated asphalt mixture. The specific technical indicators of the regenerated asphalt mixture are shown in Table 1. The results of the Marshall residual stability test, freeze-thaw splitting strength ratio, dynamic stability and low-temperature bending test of the asphalt mixture are shown in Table 1: Table 1 It can be seen from Table 1 that compared with Comparative Examples 1 and 2, the water stability and high-temperature rutting resistance of the asphalt mixtures of Examples 1 to 4 are significantly improved, and the low-temperature crack resistance is also greatly improved.

[0039] The beneficial effects of the present invention are as follows: different from the prior art, the environmentally friendly recycled asphalt modifier uses phase change reaction materials to modify the base oil, and adds a surfactant at the same time to reduce the interfacial energy of the regeneration agent, better activate and restore the performance of the old asphalt, and further improve the performance of the waste asphalt mixture through thermoplastic rubber, improve the water stability and low-temperature crack resistance of the recycled asphalt mixture; in addition, the environmentally friendly recycled asphalt modifier of the present invention can also reduce the mixing temperature of the recycled asphalt mixture due to the interfacial effect, avoid secondary aging of the old asphalt, further increase the addition ratio of RAP, and achieve the purpose of energy saving, emission reduction and cost reduction.

[0040] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the specification of the present invention, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. An environmentally friendly recycled asphalt modifier, characterized in that: Made from the following components: Base oil 75~95 parts; 2~5 parts of phase change reaction material; 5~10 parts of interface agent; Thermoplastic rubber 3~6 parts; The above parts are all by weight.

2. The environmentally friendly regenerated asphalt modifier according to claim 1, characterized in that: The base oil is lubricating oil base oil, furfural extracted oil, C6~C 10 Alkane solvent, C8~C 10 One or more of aromatic oil, catalytic cracking slurry, cracking tar, vacuum residue, atmospheric residue, cycloalkyl atmospheric or vacuum residue.

3. The environmentally friendly regenerated asphalt modifier according to claim 1, characterized in that: The phase change reaction material is trans-polyoctene rubber.

4. The environmentally friendly regenerated asphalt modifier according to claim 1, characterized in that: The interfacial agent is a cationic surfactant.

5. The environmentally friendly regenerated asphalt modifier according to claim 4, characterized in that: The cationic surfactant is C 12 ~C 18 Quaternary amine, lignin amine, C 12 ~C 18 Alkyl ether polyamine, C 12 ~C 18 Alkyl ether amines, tannin amine derivatives, phenolic resin amine derivatives, amine-modified polyacrylates; C 12 ~C 18 Fatty amide amine and C 12 ~C 18 Fatty acids and their derivatives, saturated C 12 ~C 18 Alkyl monoamines, unsaturated C 12 ~C 18 Alkyl monoamines, saturated C 12 ~C 18 Alkyl polypropylene polyamine, unsaturated C 12 ~C 18 Alkyl polypropylene polyamine, saturated C containing polyoxyethylene groups 12 ~C 18 Alkyl monoamines, unsaturated C 12 ~C 18 Alkyl monoamines, saturated C 12 ~C 18 Alkyl polypropylene polyamine, unsaturated C 12 ~C 18 Alkyl polypropylene polyamine, saturated C 12 ~C 18 Alkyl aryl monoamines, unsaturated C 12 ~C18 alkyl aromatic monoamines, saturated C 12 ~C 18 Alkyl aromatic polypropylene polyamine and unsaturated C 12 ~C 18 One or more of alkylaryl polypropylene polyamines.

6. The environmentally friendly regenerated asphalt modifier according to claim 1, characterized in that: The thermoplastic rubber is a styrene-butadiene block copolymer.

7. A method for preparing the environmentally friendly regenerated asphalt modifier according to any one of claims 1 to 6, characterized in that: The steps include: (1) Weigh 75-95 parts of base oil by weight and heat to 160-170°C; (2) Add 3 to 6 parts of thermoplastic rubber to the above base oil, start the vacuum device and perform mechanical stirring for 20 to 30 minutes; (3) Control the temperature to 130-140°C, turn off the vacuum device, add 2-5 parts of phase change reaction material to the above mixture, stir for 10-15 minutes, cool to 60-70°C, add 5-10 parts of interface agent, stir for 5-10 minutes to obtain environmentally friendly recycled asphalt modifier.

8. The method for preparing the environmentally friendly regenerated asphalt modifier according to claim 7, characterized in that: In the above step (2), the vacuum degree of the vacuum device is controlled at 10~30Pa.