Crack repairing waterproof paint and preparation method thereof
By using components such as pure acrylic emulsion and styrene acrylic emulsion mixed base material and nylon fiber staple fiber in crack repair waterproof coatings, the problem of insufficient weather resistance of existing coatings is solved, and a high-strength and good weather resistance coating film is achieved. The service life of the concrete structure is extended and the restoration effect is maintained.
Patent Information
- Application Number
- CN202411272037.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Due to insufficient weather resistance, the existing crack repair waterproof coating cannot maintain the repair effect for a long time and cannot effectively extend the service life of the concrete structure.
Use pure acrylic emulsion and styrene acrylic emulsion to mix in a specific proportion as the base material, and use regulating the particle size and adding nylon fiber staple fibers, combining silicon sol and coupling agent to form a high-strength and good weather resistance coating film to realize the coating Excellent adhesion and filling effect.
It significantly improves the weather resistance and water resistance of the coating, extends the service life of the concrete structure, maintains the repair effect, and prevents the emergence of new cracks and further expansion of cracks.
Smart Images

Figure BDA0005038993160000081 
Figure BDA0005038993160000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of building materials, and more specifically, relates to a crack repair waterproof coating and a preparation method thereof. Background Art
[0002] Crack repair waterproof coating is a material specially designed to repair cracks in concrete structures and provide waterproofing. For concrete products, various cracks will inevitably appear in the later stage under the influence of various factors. Moreover, with the continuous accumulation of factors such as environmental degradation, the number of cracks will continue to increase, and the width and depth of a single crack will also increase. The existence and further expansion of cracks will have a serious impact on the service life of concrete products. This type of waterproof coating can inhibit the continued expansion of cracks to a certain extent, and plays a key role in the repair of concrete products, thereby extending the service life of the products.
[0003] However, the current mainstream waterproof coating products have a certain repair effect on various types of cracks in the early stages, but as time goes on, defects such as insufficient weather resistance begin to appear, resulting in the inability to maintain the repair effect for a long time. Summary of the invention
[0004] The technical problem to be solved by the present invention is that the mainstream crack repair waterproof coating has the defect that the repair effect cannot be effectively maintained due to insufficient weather resistance in the later period of use. A crack repair waterproof coating and a preparation method thereof are provided.
[0005] The purpose of the invention is to provide a crack repairing waterproof coating.
[0006] Another object of the present invention is to provide a method for preparing a crack repairing waterproof coating.
[0007] The above-mentioned purpose of the present invention is achieved through the following technical solutions:
[0008] A crack repair waterproof coating, comprising the following raw materials in parts by weight:
[0009] 100-110 parts base material, 55-65 parts filler, 2-6 parts additives;
[0010] Wherein, the base material is mixed with pure acrylic emulsion and styrene acrylic emulsion in a mass ratio of (5.2-5.8):1;
[0011] Furthermore, the solid content of the pure acrylic emulsion is 40-45%, and the solid content of the styrene acrylic emulsion is 45-50%;
[0012] The pure acrylic emulsion includes first emulsion particles, wherein the D50 of the first emulsion particles is 120-130 nm;
[0013] The styrene acrylic emulsion includes second emulsion particles, and the D50 of the second emulsion particles is 300-320nm.
[0014] Since both pure acrylic emulsion and styrene acrylic emulsion have excellent weather resistance, when they are used as the base material of waterproof coating for crack repair, the product can obtain relatively excellent weather resistance, thereby extending the service life of the product and maintaining the repair effect; however, the inventors found that styrene acrylic emulsion has higher cohesion, while pure acrylic emulsion can show more excellent water resistance, but if only styrene acrylic emulsion is used, since cracks often present irregular shapes, the stress distribution in the plane direction and depth direction of the cracks is often very uneven. Therefore, although the higher cohesion of the coating during the curing process can make the coating adhere better, it is also easy to generate greater stress, thereby causing new cracks to appear during use. If there is water in the external environment, it is easy to further cause the repair of the cracks to fail; in addition, if only pure acrylic emulsion is used, although it has certain weather resistance and water resistance, its own cohesion is relatively weak, and the strength of the coating film after curing is also relatively small. Therefore, it is difficult to form an effective support for the cracks, so when the cracks expand, repair failure is likely to occur;
[0015] If styrene acrylic emulsion and pure acrylic emulsion are mixed, it is expected that the advantages of both will be combined, but simple mixing is not easy to achieve. However, the inventors have found that this can be achieved by regulating the particle sizes of the two and the corresponding addition ratio. This is mainly because the styrene acrylic emulsion with larger particles can clamp the small particles of pure acrylic emulsion with excellent elasticity in it during the curing film-forming process, thereby achieving the filling of the gaps between the styrene acrylic emulsion particles by the pure acrylic emulsion particles, thereby utilizing the styrene acrylic emulsion particles as a skeleton and the pure acrylic emulsion particles as fillers. The relative size of the skeleton is limited by the size of the styrene acrylic emulsion particles, and the amount of the skeleton is limited by the addition ratio of the two. Therefore, reasonable matching of the particle size and the amount of addition can achieve the regulation of the size and amount of the skeleton after the coating is cured, and regulate the amount of internal fillers, ultimately achieving the organic coordination and unity of the performance of the two.
[0016] Furthermore, the filler is a mixture of rutile titanium dioxide and silica sol in a mass ratio of (1-1.2):2;
[0017] Wherein, the solid content of the silica sol is 40-45%.
[0018] Silica sol can serve as a supplementary cross-linking point to assist in the formation of a three-dimensional network skeleton during the curing process of polymer coatings.
[0019] Furthermore, the silica sol further comprises a coupling agent in an amount of 10-12% by mass of the silica sol;
[0020] The coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
[0021] Furthermore, the auxiliary agent includes the following raw materials in parts by weight:
[0022] 10-15 parts of dispersant, 10-15 parts of wetting agent, 8-10 parts of plasticizer, 3-5 parts of preservative, 2-4 parts of defoamer;
[0023] Wherein, the dispersant is selected from any one of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate;
[0024] The wetting agent is selected from any one of nonylphenol polyethylene oxide ether, polyoxyethylene alkylphenyl ether, and polyoxyethylene fatty acid ester;
[0025] The plasticizer is selected from any one of dibutyl phthalate and dioctyl phthalate;
[0026] The preservative is selected from any one of phenoxyethanol and parabens;
[0027] The defoamer is selected from any one of an organosilicon defoamer and a mineral oil defoamer.
[0028] Furthermore, the crack repair waterproof coating further comprises nylon fiber staple fibers accounting for 8-10% of the filler mass;
[0029] The average aspect ratio of the nylon staple fibers is (8-10):1; and the average length of the nylon staple fibers is 10-12 mm.
[0030] By adding nylon fibers, they can be used as "reinforcement ribs" after the coating is cured, thereby achieving a good reinforcement effect. The inventors further discovered that if short fibers are used, more fiber segments can be obtained with the same mass of added fibers. In particular, due to the overall irregular structure of the cracks, longer fibers are easy to diffuse in wider cracks, but when encountering narrow cracks, they are easily trapped, thereby hindering the coating's own repair effect on the cracks. The use of short fibers can allow them to diffuse well, and even in narrow cracks, excellent reinforcement effects can be achieved.
[0031] Furthermore, a coupling agent is adsorbed on the surface of the nylon staple fiber;
[0032] The coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
[0033] A method for preparing a crack repair waterproof coating, the specific preparation steps comprising:
[0034] Weigh each component according to the raw material composition;
[0035] First disperse and dissolve the additives in the base material;
[0036] Then add filler, mix and disperse evenly to obtain crack repairing waterproof coating.
[0037] Furthermore, the specific preparation steps also include:
[0038] After the fillers are mixed and dispersed evenly, nylon staple fibers are added, and after they are mixed and dispersed evenly, a crack repairing waterproof coating is obtained. DETAILED DESCRIPTION
[0039] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0040] Unless otherwise specified, the reagents and materials used in the following examples are commercially available.
[0041] Example 1
[0042] Pretreatment of nylon staple fibers:
[0043] Add nylon staple fibers into water at a mass ratio of 1:8, and ultrasonically disperse them for 50 minutes at an ultrasonic frequency of 80 kHz, then add a coupling agent of 15% of the mass of the nylon staple fibers, and then stir and react at a constant temperature of 75°C and a stirring speed of 500 r / min for 3 hours, filter, wash the filter cake with water, and dry to obtain pretreated nylon staple fibers;
[0044] The average aspect ratio of the nylon staple fibers is 8:1; and the average length of the nylon staple fibers is 10 mm;
[0045] The coupling agent is selected from silane coupling agent KH-550;
[0046] Preparation of filling:
[0047] A coupling agent of 10% of the mass of the silica sol is added to the silica sol, and the mixture is first dispersed by ultrasound at an ultrasonic frequency of 100 kHz for 30 minutes, and then subjected to constant temperature ultrasonic reaction at a temperature of 75°C and an ultrasonic frequency of 60 kHz for 3 hours, and then naturally cooled to room temperature to obtain a pretreated silica sol;
[0048] The solid content of the silica sol is 40%;
[0049] The coupling agent is selected from silane coupling agent KH-550;
[0050] The rutile titanium dioxide and the pretreated silica sol are mixed in a mass ratio of 1:2, and the mixture is continuously stirred and mixed for 45 minutes at a rotation speed of 400 r / min, thereby completing the preparation of the filler;
[0051] Preparation of waterproof coating:
[0052] Take 100 parts of base material, 55 parts of filler, 2 parts of auxiliary agent, and 8% of the mass of the filler pretreated nylon staple fiber in sequence by weight;
[0053] First, pour the additive into the base material, stir and mix with a stirrer at a speed of 800r / min for 30min, then add the filler, continue to stir and disperse at a speed of 400r / min for 80min, then add the pretreated nylon fiber staple, continue to stir and disperse at a speed of 300r / min for 60min, and discharge the material to obtain the crack repair waterproof coating;
[0054] Wherein, the base material is a mixture of pure acrylic emulsion and styrene acrylic emulsion in a mass ratio of 5.2:1;
[0055] Furthermore, the solid content of the pure acrylic emulsion is 40%, and the solid content of the styrene acrylic emulsion is 45%;
[0056] The pure acrylic emulsion includes first emulsion particles, and the D50 of the first emulsion particles is 120 nm;
[0057] The styrene-acrylic emulsion includes second emulsion particles, and the D50 of the second emulsion particles is 300 nm;
[0058] The auxiliary agent includes the following raw materials in parts by weight:
[0059] 10 parts dispersant, 10 parts wetting agent, 8 parts plasticizer, 3 parts preservative, 2 parts defoamer;
[0060] Wherein, the dispersant is selected from sodium dodecylbenzene sulfonate;
[0061] The wetting agent is selected from nonylphenol polyethylene oxide ether;
[0062] The plasticizer is selected from dibutyl phthalate;
[0063] The preservative is selected from phenoxyethanol;
[0064] The defoamer is selected from silicone defoamers.
[0065] Example 2
[0066] Pretreatment of nylon staple fibers:
[0067] Add nylon staple fibers into water at a mass ratio of 1:8, and ultrasonically disperse them for 50 minutes at an ultrasonic frequency of 80 kHz, then add a coupling agent of 15% of the mass of the nylon staple fibers, and then stir and react at a constant temperature of 75°C and a stirring speed of 500 r / min for 3 hours, filter, wash the filter cake with water, and dry to obtain pretreated nylon staple fibers;
[0068] The average aspect ratio of the nylon staple fibers is 9:1; and the average length of the nylon staple fibers is 11 mm;
[0069] The coupling agent is selected from silane coupling agent KH-560;
[0070] Preparation of filling:
[0071] A coupling agent of 11% by mass of the silica sol was added to the silica sol, and the mixture was first dispersed by ultrasound at an ultrasonic frequency of 100 kHz for 30 minutes, and then subjected to constant temperature ultrasonic reaction at a temperature of 75°C and an ultrasonic frequency of 60 kHz for 3 hours, and then naturally cooled to room temperature to obtain a pretreated silica sol;
[0072] The solid content of the silica sol is 42%;
[0073] The coupling agent is selected from silane coupling agent KH-560;
[0074] The rutile titanium dioxide and the pretreated silica sol are mixed in a mass ratio of 1.1:2, and the mixture is continuously stirred and mixed for 45 minutes at a rotation speed of 400 r / min, thereby completing the preparation of the filler;
[0075] Preparation of waterproof coating:
[0076] Take, in parts by weight, 105 parts of base material, 60 parts of filler, 4 parts of auxiliary agent, and 9% of the mass of the filler pretreated nylon staple fiber;
[0077] First, pour the additive into the base material, stir and mix with a stirrer at a speed of 800r / min for 30min, then add the filler, continue to stir and disperse at a speed of 400r / min for 80min, then add the pretreated nylon fiber staple, continue to stir and disperse at a speed of 300r / min for 60min, and discharge the material to obtain the crack repair waterproof coating;
[0078] Wherein, the base material is a mixture of pure acrylic emulsion and styrene acrylic emulsion in a mass ratio of 5.5:1;
[0079] Furthermore, the solid content of the pure acrylic emulsion is 42%, and the solid content of the styrene acrylic emulsion is 48%;
[0080] The pure acrylic emulsion includes first emulsion particles, and the D50 of the first emulsion particles is 125nm;
[0081] The styrene-acrylic emulsion includes second emulsion particles, and the D50 of the second emulsion particles is 310 nm;
[0082] The auxiliary agent includes the following raw materials in parts by weight:
[0083] 12 parts dispersant, 13 parts wetting agent, 9 parts plasticizer, 4 parts preservative, 3 parts defoamer;
[0084] Wherein, the dispersant is selected from sodium dodecyl sulfate;
[0085] The wetting agent is selected from polyoxyethylene alkyl phenyl ether;
[0086] The plasticizer is selected from dioctyl phthalate;
[0087] The preservative is selected from parabens;
[0088] The defoamer is selected from mineral oil defoamers.
[0089] Example 3
[0090] Pretreatment of nylon staple fibers:
[0091] Add nylon staple fibers into water at a mass ratio of 1:8, and ultrasonically disperse them for 50 minutes at an ultrasonic frequency of 80 kHz, then add a coupling agent of 15% of the mass of the nylon staple fibers, and then stir and react at a constant temperature of 75°C and a stirring speed of 500 r / min for 3 hours, filter, wash the filter cake with water, and dry to obtain pretreated nylon staple fibers;
[0092] The average aspect ratio of the nylon staple fibers is 10:1; and the average length of the nylon staple fibers is 12 mm;
[0093] The coupling agent is selected from silane coupling agent KH-570;
[0094] Preparation of filling:
[0095] A coupling agent of 12% by mass of the silica sol was added to the silica sol, and the mixture was first dispersed by ultrasound at an ultrasonic frequency of 100 kHz for 30 minutes, and then subjected to constant temperature ultrasonic reaction at a temperature of 75°C and an ultrasonic frequency of 60 kHz for 3 hours, and then naturally cooled to room temperature to obtain a pretreated silica sol;
[0096] The solid content of the silica sol is 45%;
[0097] The coupling agent is selected from silane coupling agent KH-570;
[0098] The rutile titanium dioxide and the pretreated silica sol are mixed in a mass ratio of 1.2:2, and the mixture is continuously stirred and mixed for 45 minutes at a rotation speed of 400 r / min, thereby completing the preparation of the filler;
[0099] Preparation of waterproof coating:
[0100] Take, in parts by weight, 110 parts of base material, 65 parts of filler, 6 parts of auxiliary agent, and 10% of the mass of the filler pretreated nylon staple fiber;
[0101] First, pour the additive into the base material, stir and mix with a stirrer at a speed of 800r / min for 30min, then add the filler, continue to stir and disperse at a speed of 400r / min for 80min, then add the pretreated nylon fiber staple, continue to stir and disperse at a speed of 300r / min for 60min, and discharge the material to obtain the crack repair waterproof coating;
[0102] Wherein, the base material is a mixture of pure acrylic emulsion and styrene acrylic emulsion in a mass ratio of 5.8:1;
[0103] Furthermore, the solid content of the pure acrylic emulsion is 45%, and the solid content of the styrene acrylic emulsion is 50%;
[0104] The pure acrylic emulsion includes first emulsion particles, and the D50 of the first emulsion particles is 130 nm;
[0105] The styrene-acrylic emulsion includes second emulsion particles, and the D50 of the second emulsion particles is 320 nm;
[0106] The auxiliary agent includes the following raw materials in parts by weight:
[0107] 15 parts dispersant, 15 parts wetting agent, 10 parts plasticizer, 5 parts preservative, 4 parts defoamer;
[0108] Wherein, the dispersant is selected from sodium dodecylbenzene sulfonate;
[0109] The wetting agent is selected from polyoxyethylene fatty acid esters;
[0110] The plasticizer is selected from dibutyl phthalate;
[0111] The preservative is selected from phenoxyethanol;
[0112] The defoamer is selected from silicone defoamers.
[0113] Example 4
[0114] The present embodiment differs from the embodiment 1 in that no nylon staple fibers are added, and the other conditions remain unchanged.
[0115] Example 5
[0116] The present embodiment is different from the embodiment 1 in that the average aspect ratio of the nylon staple fibers is 6:1; and the average length of the nylon staple fibers is 10 mm; and the other conditions remain unchanged.
[0117] Example 6
[0118] The present embodiment is different from the embodiment 1 in that the average aspect ratio of the nylon staple fibers is 12:1, and the average length of the nylon staple fibers is 10 mm, and the other conditions remain unchanged.
[0119] Example 7
[0120] The difference between this embodiment and embodiment 1 is that no silica sol is added, and other conditions remain unchanged.
[0121] Example 8
[0122] The present embodiment differs from the embodiment 1 in that no rutile titanium dioxide is added, and the other conditions remain unchanged.
[0123] Comparative Example 1
[0124] The difference between this comparative example and Example 1 is that no styrene acrylic emulsion is added, and the other conditions remain unchanged.
[0125] Comparative Example 2
[0126] The difference between this comparative example and Example 1 is that pure acrylic emulsion is not added, and other conditions remain unchanged.
[0127] Comparative Example 3
[0128] The difference between this comparative example and Example 1 is that the D50 of the styrene acrylic emulsion is 120 nm, and the other conditions remain unchanged.
[0129] The performance tests of the products obtained in the above embodiments or comparative examples are carried out, and the specific test methods and test results are as follows:
[0130] The raw materials for making the benchmark test blocks are as follows: cement is ordinary Portland cement PO42.5; sand is medium sand in zone II with a fineness modulus of 2.6; the crushed stone particle size is 5-30mm, with continuous grading; water is municipal tap water, which complies with JGJ 63-2006 "Standard for Water Use in Concrete";
[0131] The reference test block was immersed in water for 1 hour, then frozen at -18°C for 8 hours, and then allowed to stand at 35°C for 12 hours. The immersion, freezing and standing cycles were repeated 150 times to obtain the accelerated aging cracking reference test block.
[0132] The above-mentioned products of each embodiment or comparative example are applied to the surface of the cracking reference test block of accelerated aging by brushing. After the first coating is dry, the second coating is applied. The interval between the two coatings should be 6-12 hours. The coating should be applied evenly without local precipitation and bubbles. The amount of coating is controlled to be 2.4kg / m 2 ; After the coating is completely cured, a test block with a coating is obtained;
[0133] The coated test blocks were then aged for 35 days at a temperature of 65°C and a relative humidity of 75%, then taken out and left to stand at room temperature for 24 hours to dry naturally. Whether new cracks appeared on the surface of each test block was observed. The naturally dried test blocks were placed in water for 2 hours and then taken out to test the mass change rate before and after immersion as the water absorption rate. The higher the water absorption rate, the more relative number of microscopic and macroscopic new cracks appeared. The detailed test results are shown in Table 1:
[0134] Table 1: Product performance test results
[0135]
[0136]
[0137] Among them, the blank case is the cracking benchmark test block with accelerated aging, which is not coated with paint;
[0138] It can be seen from the test results in Table 1 that the product obtained by the present invention can effectively repair the cracks of the test block, and can still show good water resistance after accelerated aging for 35 days.
[0139] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A crack repair waterproof coating, characterized in that: The invention comprises the following raw materials in parts by weight: 100-110 parts base material, 55-65 parts filler, 2-6 parts additives; Wherein, the base material is mixed with pure acrylic emulsion and styrene acrylic emulsion in a mass ratio of (5.2-5.8):1; Furthermore, the solid content of the pure acrylic emulsion is 40-45%, and the solid content of the styrene acrylic emulsion is 45-50%; The pure acrylic emulsion includes first emulsion particles, wherein the D50 of the first emulsion particles is 120-130 nm; The styrene acrylic emulsion includes second emulsion particles, and the D50 of the second emulsion particles is 300-320nm.
2. A crack repair waterproof coating according to claim 1, characterized in that: The filler is prepared by mixing rutile titanium dioxide and silica sol in a mass ratio of (1-1.2):2; Wherein, the solid content of the silica sol is 40-45%.
3. A crack repair waterproof coating according to claim 2, characterized in that: The silica sol also includes a coupling agent in an amount of 10-12% by mass of the silica sol; The coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
4. The crack repair waterproof coating according to claim 1, characterized in that: The auxiliary agent includes the following raw materials in parts by weight: 10-15 parts of dispersant, 10-15 parts of wetting agent, 8-10 parts of plasticizer, 3-5 parts of preservative, 2-4 parts of defoamer; Wherein, the dispersant is selected from any one of sodium dodecylbenzene sulfonate and sodium dodecyl sulfate; The wetting agent is selected from any one of nonylphenol polyethylene oxide ether, polyoxyethylene alkylphenyl ether, and polyoxyethylene fatty acid ester; The plasticizer is selected from any one of dibutyl phthalate and dioctyl phthalate; The preservative is selected from any one of phenoxyethanol and parabens; The defoamer is selected from any one of an organosilicon defoamer and a mineral oil defoamer.
5. The crack repair waterproof coating according to claim 1, characterized in that: The crack repair waterproof coating also includes nylon fiber staple fibers accounting for 8-10% of the filler mass; The average aspect ratio of the nylon staple fibers is (8-10):1; and the average length of the nylon staple fibers is 10-12 mm.
6. A crack repair waterproof coating according to claim 5, characterized in that: A coupling agent is adsorbed on the surface of the nylon staple fiber; The coupling agent is selected from any one of silane coupling agent KH-550, silane coupling agent KH-560 and silane coupling agent KH-570.
7. A method for preparing the crack repair waterproof coating according to any one of claims 1 to 6, characterized in that: The specific preparation steps include: Weigh each component according to the raw material composition; First disperse and dissolve the additives in the base material; Then add filler, mix and disperse evenly to obtain crack repairing waterproof coating.
8. The method for preparing a crack repair waterproof coating according to claim 7, characterized in that: The specific preparation steps also include: After the fillers are mixed and dispersed evenly, nylon staple fibers are added, and after they are mixed and dispersed evenly, a crack repairing waterproof coating is obtained.
Citation Information
Cited By
Skin-touch art coating and preparation process thereof
CN120399552A
Skin-feeling artistic paint and preparation process thereof
CN120399552B