Thermal insulation coating with reflection, radiation and barrier functions and application thereof

By controlling the content of hollow glass microspheres and nano-sized silica aerogel, and modifying the acrylic emulsion, the problem of insufficient weather resistance of reflective heat insulation coatings was solved, achieving better heat insulation effect and stability.

CN118931307APending Publication Date: 2024-11-12HUZHOU GREEN BUILDING MATERIALS DEV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411325120.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing reflective heat insulation coatings have low weather resistance and are prone to aging and cracking in high-temperature environments, resulting in a decrease in reflective heat insulation performance.

Method used

By controlling the particle size range and content ratio of hollow glass microspheres, the content ratio of nano-sized silica aerogel and titanium dioxide, and by modifying the acrylic emulsion with polystyrene blocks, a better molding and stacking state is formed, thereby improving the weather resistance and hardness of the coating.

Benefits of technology

The coating's weather resistance and hardness have been improved, resulting in better thermal insulation and stability, and enabling it to maintain good thermal insulation performance in extreme environments.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of external wall heat insulation, and discloses a heat insulation coating with reflection, radiation and barrier functions and application thereof. In order to solve the problem that an existing reflective heat-insulating coating is low in weather resistance, the reflective heat-insulating coating can form a better forming and stacking state when a heat-insulating layer is formed by controlling the particle size range and the content ratio of hollow glass beads and the content ratio of nanoscale raw materials, namely silicon dioxide aerogel and titanium dioxide, so that the weather resistance of a heat-insulating layer is improved, and the weather resistance of the heat-insulating layer is improved. Furthermore, the acrylic emulsion is subjected to polystyrene block modification, so that the hardness of the thermal insulation layer is improved, functional molecular particles in the thermal insulation layer form a better forming state, and the formed thermal insulation layer is better in thermal insulation effect and better in stability of the thermal insulation effect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of exterior wall thermal insulation, and in particular to a thermal insulation coating with reflection, radiation and barrier functions and application thereof. Background Art

[0002] At present, in order to meet the requirements of thermal insulation, the external wall insulation is generally carried out by configuring an insulation layer. The commonly used insulation systems mainly include rock wool boards, expanded polystyrene boards, extruded polystyrene boards and building insulation mortars. The external wall insulation systems formed by these materials often have problems such as thick insulation layers, low insulation layer strength, and poor comprehensive performance such as crack resistance, which can easily cause the external wall insulation system to fall off, seep water, etc., resulting in the safety and service life of the external wall insulation system cannot be guaranteed.

[0003] Reflective thermal insulation coatings can be applied on the exterior walls of buildings to form reflective thermal insulation coatings, which can reduce internal and external heat transfer by reflecting sunlight, isolating external heat energy to maintain a lower temperature inside the building. Insulation through reflective thermal insulation coatings is not only simple in structure but also easy to construct, and is increasingly favored in the construction field. However, the current reflective thermal insulation coatings have low weather resistance. The coatings are prone to aging when exposed to high temperature environments for a long time, causing the coatings to crack, which in turn causes the reflectivity of the thermal insulation coatings to decrease, and the reflective thermal insulation effect to decrease.

[0004] For example, the patent application with the publication number CN101210146A discloses a composition of a thermal insulation coating with reflective, radiation and barrier functions, a double-layer thermal insulation coating and a method for making the same. The coating is simply made by mixing polymethyl methacrylate, propylene-styrene resin, propylene-butadiene-styrene resin and other resins with hollow ball fillers, reflective powder fillers and porous fillers. The coating thus formed is prone to cracking after long-term exposure, and the reflective thermal insulation effect is difficult to guarantee. Summary of the invention

[0005] The existing reflective heat-insulating coating has low weather resistance. In order to solve the above problems, the present invention provides a heat-insulating coating with reflective, radiative and barrier functions and its application. The present invention controls the particle size range and content ratio of hollow glass microspheres in the coating, and the content ratio of nano-scale raw materials silica aerogel and titanium dioxide, so that when forming the heat-insulating layer, a better molding state can be formed, and the weather resistance of the heat-insulating layer is increased. Furthermore, by modifying the acrylic emulsion with polystyrene blocks, the hardness of the heat-insulating layer is improved, and the functional molecular particles in the heat-insulating layer are formed in a better molding state, so that the heat-insulating layer formed has better heat-insulating and heat-insulating effects and better stability of the heat-insulating and heat-insulating effects.

[0006] The specific technical scheme of the present invention is: In a first aspect, the present invention provides a heat-insulating coating having reflective, radiative and barrier functions, comprising the following components in parts by weight: 100 parts of block modified acrylic emulsion, 5-10 parts of nanosilica aerogel, 10-20 parts of hollow glass microspheres, and 10-30 parts of nanotitanium dioxide; The hollow glass microspheres are composed of hollow glass microspheres with a particle size of 100-150 μm, hollow glass microspheres with a particle size of 50-80 μm, and hollow glass microspheres with a particle size of 1-20 μm, mixed in a mass ratio of 1:2-3:5-6; The block-modified acrylic emulsion is a polymethyl methacrylate emulsion modified by styrene blocks.

[0007] The present invention controls the particle size range and content ratio of hollow glass microspheres, and the content ratio of nano-scale raw materials silica aerogel and titanium dioxide, so that when forming a heat insulation layer, a better forming and stacking state can be formed, so that the weather resistance of the heat insulation layer is increased, and further, by modifying the acrylic emulsion with polystyrene blocks, the hardness of the heat insulation layer is improved, and the functional molecular particles in the heat insulation layer are formed into a better forming state, so that the formed heat insulation layer has a better heat preservation effect and a better stability of the heat preservation effect. Based on the above, the present invention provides a reflective heat insulation coating as described above.

[0008] In particular, the present invention uses hollow glass microspheres of various particle size ranges, grades the particle sizes, and forms a certain content ratio, so that a better forming and stacking state can be formed when forming a coating, and the weather resistance of the coating is increased, and the thermal insulation stability is increased. By controlling the particle size and its content ratio, a better forming and stacking state can be formed, and heat radiation can be scattered to a greater extent, thereby improving the thermal insulation effect.

[0009] In particular, the present invention performs polystyrene block modification on acrylic emulsion, thereby increasing the hardness of the heat insulation layer, increasing the weather resistance of the coating, increasing the thermal insulation stability, and improving the thermal insulation effect.

[0010] As a preferred component of the above-mentioned reflective heat-insulating coating, the sum of the masses of nano-silicon dioxide aerogel and nano-titanium dioxide is 1.5-3 times the mass of the hollow glass microspheres.

[0011] As a preferred component of the above-mentioned reflective heat-insulating coating, the particle size of the nanosilica aerogel is 100-800nm.

[0012] As a preferred component of the above-mentioned reflective heat-insulating coating, the particle size of nano-titanium dioxide is 20-50nm.

[0013] As a preferred component of the above-mentioned reflective heat-insulating coating, the block-modified acrylic emulsion is a triblock copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments, or a pentablock copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments.

[0014] Specifically, the preparation method of the triblock copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments comprises the following steps: (1) adding 10-20 parts by weight of styrene and 1-5 parts of an emulsifier to 100 parts of water, dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain an end-capped block polymer; (2) adding 30-40 parts of methyl methacrylate to the reaction system of step (1), dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain a polystyrene-polymethyl methacrylate polymer; (3) 10-20 parts of styrene are added to the reaction system of step (2), dispersed evenly, and 0.1-0.2 parts of potassium persulfate are added to react to obtain a block-modified acrylic emulsion, which is a triblock copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments.

[0015] Specifically, the preparation method of the five-block copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments comprises the following steps: (1) adding 10-20 parts by weight of styrene and 1-5 parts of an emulsifier to 100 parts of water, dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain an end-capped block polymer; (2) adding 30-40 parts of methyl methacrylate to the reaction system of step (1), dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain a polystyrene-polymethyl methacrylate polymer; (3) adding 10-20 parts of styrene to the reaction system of step (2), dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain a polystyrene-polymethyl methacrylate-polystyrene polymer; (4) adding 30-40 parts of methyl methacrylate to the reaction system of step (3), dispersing the mixture evenly, adding 0.1-0.2 parts of potassium persulfate, and reacting the mixture to obtain a polystyrene-polymethyl methacrylate-polystyrene-polymethyl methacrylate polymer; (5) 10-20 parts of styrene are added to the reaction system of step (3), dispersed evenly, and 0.1-0.2 parts of potassium persulfate are added to react to obtain a block-modified acrylic emulsion, which is a five-block copolymer emulsion formed by polystyrene segments and polymethyl methacrylate segments.

[0016] Preferably, the emulsifier is OP-10.

[0017] As a preferred embodiment of the above-mentioned reflective heat-insulating coating, the reflective heat-insulating coating further comprises the following components in parts by weight: 1-5 parts of film-forming aid, 0.1-3 parts of wetting agent, 0.8-2 parts of defoaming agent, and 0.5-2 parts of thickener.

[0018] In a second aspect, the present invention provides a method for preparing a thermal insulation coating having reflection, radiation and barrier functions, comprising the following steps: Step S1: adding block-modified acrylic emulsion, wetting agent and defoaming agent into water and mixing them evenly to obtain a premixed emulsion; Step S2: adding hollow glass microspheres and nano-silicon dioxide aerogel to the premixed milk while stirring, and mixing to obtain a premixed material; Step S3: adding nano-titanium dioxide to the premixed material while stirring, and mixing to obtain a mixed material; Step S4: adding a film-forming aid and a thickener to the mixture, and mixing them evenly to obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0019] With respect to the coating formula provided above, the present invention adaptively provides the optimal conditions for coating preparation, namely, controlling the stirring speed at a relatively low speed when mixing hollow glass microbeads of various particle sizes with nano-sized silica aerogel raw materials, and adjusting the stirring speed to a relatively high speed when subsequently mixing nano-titanium dioxide, so as to achieve the best mixing effect of the reflective thermal insulation coating and better thermal insulation effect of the thermal insulation layer formed by the prepared coating.

[0020] As a preferred embodiment of the above preparation method, in step S2, the stirring speed is 300-600 rpm.

[0021] As a preferred embodiment of the above preparation method, in step S2, the stirring speed is 1000-1500 rpm.

[0022] In a third aspect, the present invention provides a thermal insulation layer, which is prepared from the above-mentioned thermal insulation coating.

[0023] Compared with the prior art, the present invention has the following technical effects: (1) The present invention provides a reflective heat-insulating coating with good heat-insulating effect and heat-insulating stability. The present invention controls the particle size range and content ratio of hollow glass microspheres in the coating, and the content ratio of nano-scale raw materials silica aerogel and titanium dioxide, so that the coating is formed into a better molding and stacking state, and the weather resistance of the coating is increased. Furthermore, by modifying the acrylic emulsion with polystyrene blocks, the hardness of the coating is improved, and the functional molecular particles in the coating are formed into a better molding state, so that the formed coating has better heat-insulating effect and better stability of the heat-insulating effect.

[0024] (2) The thermal insulation coating of the present invention adds nano-scale raw material silica aerogel with a specific content and particle size, so that it cooperates with other raw materials to make the thermal insulation coating have multiple functions such as reflection, radiation and barrier functions. At the same time, the thermal insulation effect of the coating is good in weather resistance.

[0025] (3) The present invention provides a method for preparing a heat-insulating coating with reflective, radiative and barrier functions. With respect to the coating formula provided by the present invention, the optimal conditions for coating preparation are adaptively given, that is, when mixing hollow glass microspheres of various particle sizes with nano-sized silica aerogel raw materials, the stirring speed is controlled at a relatively low speed, and when subsequently mixing nano-titanium dioxide, the stirring speed needs to be adjusted to a relatively high speed, so that the mixing effect of the reflective heat-insulating coating is the best, and the heat-insulating layer formed by the prepared coating has a better heat-insulating and thermal-preserving effect. DETAILED DESCRIPTION

[0026] The present invention is further described below in conjunction with embodiments. A person skilled in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all of the embodiments. Therefore, based on the embodiments of the present invention, all other embodiments obtained by a person skilled in the art without making creative efforts, such as adding certain functional additives and fillers to the reflective thermal insulation coating provided by the present invention according to the experience and needs in the field, should all fall within the scope of protection of the present invention.

[0027] Example 1 Provide a variety of block modified acrylic emulsion raw materials, the specific operation steps are as follows: 1. Provide block modified acrylic emulsion A (1) 12 parts by weight of styrene and 3 parts of OP-10 emulsifier were added to 100 parts of water, dispersed evenly, 0.1 parts of potassium persulfate were added, and the temperature was raised to 60° C. and reacted for 20 minutes to obtain an end-capped block polymer; (2) adding 30 parts of methyl methacrylate to the reaction system of step (1), dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate polymer; (3) 12 parts of styrene were added to the reaction system of step (2), dispersed evenly, 0.1 parts of potassium persulfate were added, and the mixture was reacted at 60° C. for 30 min to obtain a triblock copolymer emulsion composed of polystyrene segments and polymethyl methacrylate segments, i.e., block-modified acrylic emulsion A.

[0028] 2. Provide block modified acrylic emulsion B (1) 12 parts by weight of styrene and 3 parts of OP-10 emulsifier were added to 100 parts of water, dispersed evenly, 0.1 parts of potassium persulfate were added, and the temperature was raised to 60° C. and reacted for 20 minutes to obtain an end-capped block polymer; (2) adding 30 parts of methyl methacrylate to the reaction system of step (1), dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate polymer; (3) adding 12 parts of styrene to the reaction system of step (2), dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate-polystyrene polymer; (4) adding 30 parts of methyl methacrylate to the reaction system of step (3), dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate-polystyrene-polymethyl methacrylate polymer; (5) 12 parts of styrene were added to the reaction system of step (3), dispersed evenly, 0.1 parts of potassium persulfate were added, and the mixture was reacted at 60° C. for 30 min to obtain a five-block copolymer emulsion composed of polystyrene segments and polymethyl methacrylate segments, i.e., block-modified acrylic emulsion B.

[0029] 3. Provide block modified acrylic emulsion C (1) 12 parts by weight of styrene and 3 parts of OP-10 emulsifier were added to 100 parts of water, dispersed evenly, 0.1 parts of potassium persulfate were added, and the temperature was raised to 60° C. and reacted for 20 minutes to obtain an end-capped block polymer; (2) adding 30 parts of methyl methacrylate to the reaction system in the previous step, dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate polymer; (3) adding 12 parts of styrene to the reaction system in the previous step, dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate-polystyrene polymer; (4) Repeat steps (2) to (3) twice to obtain a seven-block copolymer emulsion composed of polystyrene segments and polymethyl methacrylate segments, namely, block-modified acrylic emulsion C.

[0030] 4. Provide block modified acrylic emulsion D Compared with the block-modified acrylic emulsion A, the main difference of emulsion D is that the polystyrene segment is the middle block.

[0031] (1) 30 parts by weight of methyl methacrylate and 3 parts of OP-10 emulsifier were added to 100 parts of water, dispersed evenly, 0.1 parts of potassium persulfate were added, and the temperature was raised to 60° C. and reacted for 20 minutes to obtain an end-capped block polymer; (2) adding 12 parts of styrene to the reaction system of step (1), dispersing evenly, adding 0.1 parts of potassium persulfate, and reacting at 60° C. for 30 minutes to obtain a polystyrene-polymethyl methacrylate polymer; (3) 30 parts of methyl methacrylate were added to the reaction system of step (2) and dispersed evenly. 0.1 parts of potassium persulfate were added and reacted at 60° C. for 30 min to obtain a triblock copolymer emulsion formed by polymethyl methacrylate segments and polystyrene segments, i.e., block-modified acrylic emulsion D.

[0032] 5. Provide acrylic emulsion E Compared with the block-modified acrylic emulsion A, the main difference of emulsion E is that no polystyrene chain segments are inserted.

[0033] By weight, 90 parts of methyl methacrylate and 3 parts of OP-10 emulsifier were added to 100 parts of water and dispersed evenly. 0.2 parts of potassium persulfate were added and the temperature was raised to 60° C. for reaction for 2 hours to obtain acrylic emulsion E.

[0034] Example 2 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion A, 2 parts of wetting agent sodium hexametaphosphate, 1 part of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0035] Step S2: under slow stirring at 500 rpm, 15 parts of hollow glass microspheres and 8 parts of nano-silica aerogel are added to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6; the average particle size of the nano-silica aerogel is 300 nm.

[0036] Step S3: Increase the stirring speed to 1200 rpm, add 22 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide be twice the mass of the hollow glass microspheres, in the range of 1.5-3 times, and mix well to obtain a mixture. The average particle size of the nano-titanium dioxide is 40 nm.

[0037] Step S4: Add 3 parts of film-forming aid dipropylene glycol methyl and 1.2 parts of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0038] Example 3 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion A, 2 parts of wetting agent sodium hexametaphosphate, 1 part of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0039] Step S2: under slow stirring at 500 rpm, 15 parts of hollow glass microspheres and 8 parts of nano-silica aerogel are added to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6; the average particle size of the nano-silica aerogel is 300 nm.

[0040] Step S3: Increase the stirring speed to 1200 rpm, add 14.5 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide 1.5 times the mass of hollow glass microspheres, within the range of 1.5-3 times, and mix to obtain a mixture. The average particle size of the nano-titanium dioxide is 40 nm.

[0041] Step S4: Add 3 parts of film-forming aid dipropylene glycol methyl and 1.2 parts of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0042] Example 4 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion A, 2 parts of wetting agent sodium hexametaphosphate, 1 part of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0043] Step S2: Under slow stirring at 500 rpm, add 10 parts of hollow glass microspheres and 10 parts of nano-silica aerogel to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6; the average particle size of the nano-silica aerogel is 300 nm.

[0044] Step S3: Increase the stirring speed to 1200 rpm, add 30 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide be 3 times the mass of the hollow glass microspheres, within the range of 1.5-3 times, and mix to obtain a mixture. The average particle size of the nano-titanium dioxide is 40 nm.

[0045] Step S4: Add 3 parts of film-forming aid dipropylene glycol methyl and 1.2 parts of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0046] Example 5 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion A, 0.5 parts of wetting agent sodium hexametaphosphate, 0.8 parts of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0047] Step S2: under slow stirring at 300 rpm, 15 parts of hollow glass microspheres and 5 parts of nano-silica aerogel are added to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 100 μm, hollow glass microspheres with an average particle size of 50 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6; the average particle size of the nano-silica aerogel is 300 nm.

[0048] Step S3: Increase the stirring speed to 1000 rpm, add 30 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide 2.3 times the mass of hollow glass microspheres, within the range of 1.5-3 times, and mix well to obtain a mixture. The average particle size of the nano-titanium dioxide is 25 nm.

[0049] Step S4: Add 5 parts of film-forming aid dipropylene glycol methyl and 2 parts of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0050] Example 6 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion A, 3 parts of wetting agent sodium hexametaphosphate, 2 parts of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0051] Step S2: Under slow stirring at 600 rpm, add 20 parts of hollow glass microspheres and 10 parts of nano-silica aerogel to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 150 μm, hollow glass microspheres with an average particle size of 80 μm, and hollow glass microspheres with an average particle size of 20 μm, which are mixed in a mass ratio of 1:3:6; and the average particle size of the nano-silica aerogel is 300 nm.

[0052] Step S3: Increase the stirring speed to 1500 rpm, add 22 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide 1.6 times the mass of hollow glass microspheres, within the range of 1.5-3 times, and mix well to obtain a mixture. The average particle size of the nano-titanium dioxide is 50 nm.

[0053] Step S4: Add 1 part of film-forming aid dipropylene glycol methyl and 0.5 part of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0054] Example 7 Provided is a heat-insulating coating with reflection, radiation and barrier functions, which is prepared according to the following steps: Step S1: by weight, 100 parts of block-modified acrylic emulsion B, 2 parts of wetting agent sodium hexametaphosphate, 1 part of defoaming agent polysiloxane are added into a dispersion tank, and 20 parts of water are added, stirring is started, and mixing is performed uniformly to obtain a premixed emulsion.

[0055] Step S2: under slow stirring at 500 rpm, 15 parts of hollow glass microspheres and 8 parts of nano-silica aerogel are added to the premixed milk while stirring to obtain a premixed material. The hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6; the average particle size of the nano-silica aerogel is 300 nm.

[0056] Step S3: Increase the stirring speed to 1200 rpm, add 22 parts of nano-titanium dioxide to the premix while stirring, and make the sum of the mass of nano-silica aerogel and nano-titanium dioxide be twice the mass of the hollow glass microspheres, in the range of 1.5-3 times, and mix well to obtain a mixture. The average particle size of the nano-titanium dioxide is 40 nm.

[0057] Step S4: Add 3 parts of film-forming aid dipropylene glycol methyl and 1.2 parts of thickener methyl cellulose to the mixture, mix well, and obtain a heat-insulating coating with reflection, radiation and barrier functions.

[0058] Comparative Example 1 Compared with Example 2, the main difference of this comparative example is that the proportion of nano-titanium dioxide is 25 parts, so that the sum of the mass of nano-silica aerogel and nano-titanium dioxide is 3.5 times the mass of hollow glass microspheres, and the proportion of hollow glass microspheres is adaptively adjusted to 10 parts and the proportion of nano-silica aerogel is 10 parts. The rest is the same as Example 2.

[0059] Comparative Example 2 The main difference between this comparative example and Example 2 is that the proportion of nano-titanium dioxide is 44.5 parts, so that the sum of the mass of nano-silica aerogel and nano-titanium dioxide is 3.5 times the mass of hollow glass microspheres. The rest is the same as Example 2.

[0060] Comparative Example 3 Compared with Example 2, the main difference between this comparative example and Example 2 is that the number of nano-titanium dioxide is 10 parts, so that the sum of the mass of nano-silica aerogel and nano-titanium dioxide is 1.2 times the mass of hollow glass microspheres. Others are the same as Example 2.

[0061] Comparative Example 4 Compared with Example 2, the main difference between this comparative example and Example 2 is that the number of nano-titanium dioxide is 8 parts, so that the sum of the mass of nano-silica aerogel and nano-titanium dioxide is 1.2 times the mass of hollow glass microspheres, and the number of nano-silica aerogel is adaptively adjusted to 10 parts. Other parts are the same as Example 2.

[0062] Comparative Example 5 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:1:1. The rest is the same as Example 2.

[0063] Comparative Example 6 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 6:3:1. The rest is the same as Example 2.

[0064] Comparative Example 7 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 180 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0065] Comparative Example 8 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 70 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0066] Comparative Example 9 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 100 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0067] Comparative Example 10 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 30 μm, and hollow glass microspheres with an average particle size of 10 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0068] Comparative Example 11 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 40 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0069] Comparative Example 12 Compared with Example 2, the main difference of this comparative example is that the hollow glass microspheres are composed of hollow glass microspheres with an average particle size of 120 μm, hollow glass microspheres with an average particle size of 60 μm, and hollow glass microspheres with an average particle size of 0.5 μm, which are mixed in a mass ratio of 1:3:6. The rest is the same as Example 2.

[0070] Comparative Example 13 The main difference between this comparative example and Example 2 is that the block-modified acrylic emulsion A is replaced by the block-modified acrylic emulsion C. The other parts are the same as those in Example 2.

[0071] Comparative Example 14 The main difference between this comparative example and Example 2 is that the block-modified acrylic emulsion A is replaced by the block-modified acrylic emulsion D. The other parts are the same as those in Example 2.

[0072] Comparative Example 15 The main difference between this comparative example and Example 2 is that the block-modified acrylic emulsion A is replaced by acrylic emulsion E. The other parts are the same as Example 2.

[0073] Comparative Example 16 The main difference between this comparative example and Example 2 is that the stirring speed in step S2 is 1000 rpm. The other parts are the same as Example 2.

[0074] Comparative Example 17 The main difference between this comparative example and Example 2 is that the stirring speed in step S3 is 500 rpm. The other parts are the same as Example 2.

[0075] Comparative Example 18 The main difference between this comparative example and Example 2 is that the stirring speed in step S3 is 2000 rpm. The other parts are the same as Example 2.

[0076] Performance Testing The coatings prepared in Examples 2-7 and Comparative Examples 1-18 were tested for thermal insulation performance. The results are shown in Table 1. The temperature of the first test is not much different from the temperature of the second test, indicating that the thermal insulation performance of the coating is relatively stable. The test method is as follows: the coatings prepared in Examples 2-7 and Comparative Examples 1-18 are uniformly coated on a test steel plate (the size of the steel plate is 200mm×200mm×2.5mm), and dried at 30°C to form a thermal insulation coating. The thickness of the thermal insulation coating is 1mm. An infrared lamp (250W) is used to simulate a sunlight source for irradiation. The distance between the steel plate and the lamp source is 3cm, so that the surface of the thermal insulation coating is directly irradiated by the light source. After irradiation for 30 minutes, a contact infrared thermometer is used to measure the temperature of the center of the back of the steel plate, which is the temperature of the first test; then the above-mentioned test steel plate coated with the thermal insulation coating is placed in a 100°C oven for 180 days, taken out, and placed in a ventilated place to room temperature. Then an infrared lamp (250W) is used to simulate a sunlight source for irradiation. The distance between the steel plate and the lamp source is 3cm, so that the surface of the thermal insulation coating is directly irradiated by the light source. After irradiation for 30 minutes, a contact infrared thermometer is used to measure the temperature of the center of the back of the steel plate, which is the temperature of the second test. The simulated sunlight source irradiation and temperature measurement operations are carried out in a closed state.

[0077] Table 1 Temperature of the first test (℃) Temperature of the second test (℃) Example 2 122 123 Example 3 123 123 Example 4 125 127 Example 5 126 128 Example 6 125 130 Example 7 120 119 Comparative Example 1 154 173 Comparative Example 2 167 191 Comparative Example 3 152 174 Comparative Example 4 160 191 Comparative Example 5 155 199 Comparative Example 6 163 200 Comparative Example 7 155 192 Comparative Example 8 149 168 Comparative Example 9 152 171 Comparative Example 10 159 188 Comparative Example 11 157 189 Comparative Example 12 161 190 Comparative Example 13 152 181 Comparative Example 14 168 227 Comparative Example 15 170 234 Comparative Example 16 150 164 Comparative Example 17 151 167 Comparative Example 18 149 164 Data Analysis: (1) The present invention controls the particle size range and content ratio of hollow glass microspheres in the coating, and the content ratio of nano-scale raw material silica aerogel and titanium dioxide, so that the coating forms a better formed stacking state when forming the coating, so that the weather resistance of the coating is increased, and further, by modifying the acrylic emulsion with polystyrene blocks, the hardness of the coating is improved, and the functional molecular particles in the coating form a better formed state, thereby making the formed coating have better thermal insulation effect and better stability of the thermal insulation effect. It can be seen from the characterization data of Examples 2-7 that the coating formed by the coating provided by the present invention has a good thermal insulation effect, can isolate external heat energy, so as to maintain a lower temperature inside the target object, and the temperature of the first test is compared with the temperature of the second test after being placed in an extreme environment for 180 days. The coating formed by the coating provided by the present invention has a good stability of thermal insulation effect, and after being placed in an extreme environment, the thermal insulation effect of the formed coating is still good.

[0078] (2) By comparing Comparative Examples 1-2 with Example 2, it can be seen that the content of nano-scale raw materials silica aerogel and titanium dioxide in Comparative Example 1 is 3.5 times the content of hollow glass microspheres, and the proportion is too high. The thermal insulation effect of the coating formed thereby becomes worse, and the stability of the thermal insulation effect is poor. The content of nano-scale raw materials silica aerogel and titanium dioxide in Comparative Example 1 is 3.5 times the content of hollow glass microspheres, and the proportion of nano-titanium dioxide is too high. The thermal insulation effect of the coating formed thereby is worse, and the stability of the thermal insulation effect is worse.

[0079] By comparing Comparative Examples 3-4 with Example 2, it can be seen that the content of nano-scale raw materials silica aerogel and titanium dioxide in Comparative Example 3 is 1.2 times the content of hollow glass microspheres, and the proportion is too low. The thermal insulation effect of the coating formed thereby becomes worse, and the stability of the thermal insulation effect is poor. In Comparative Example 4, the content of nano-scale raw materials silica aerogel and titanium dioxide is 1.2 times the content of hollow glass microspheres, and the proportion of nano-titanium dioxide is too low. The thermal insulation effect of the coating formed thereby is even worse, and the stability of the thermal insulation effect is even worse.

[0080] In summary, the coating provided by the present invention needs to control the mass ratio of the content of the nano-scale raw materials silicon dioxide aerogel and titanium dioxide to the content of the hollow glass microspheres within a certain range.

[0081] (3) Comparative Examples 5-12 study the effect of hollow glass microsphere raw materials on coating performance. Comparison of Comparative Examples 5-12 with Example 2 shows that by using hollow glass microspheres of various particle size ranges, grading the particle size, and forming a certain content ratio, a better forming and stacking state can be formed when forming a coating, and the weather resistance and thermal insulation stability of the coating can be increased. By controlling the particle size and its content ratio, a better forming and stacking state can be formed, and thermal radiation can be scattered to a greater extent, thereby improving the thermal insulation effect.

[0082] (4) Comparative Examples 13-15 study the effect of acrylic emulsion raw materials on coating performance. Comparison of Comparative Examples 13-15 with Example 2 shows that the present invention modifies the acrylic emulsion with polystyrene blocks, thereby increasing the hardness of the thermal insulation layer, the weather resistance of the coating, the thermal insulation stability, and the thermal insulation effect.

[0083] (5) Comparative Examples 16-18 are used to study the coating preparation process. Comparison of Comparative Examples 16-18 with Example 2 shows that, for the coating formulation provided by the present invention, when mixing hollow glass microspheres of various particle sizes with nano-sized silica aerogel raw materials, the stirring speed needs to be controlled at a relatively low speed, and when subsequently mixing nano-titanium dioxide, the stirring speed needs to be adjusted to a relatively high speed, so that the mixing effect of the reflective heat-insulating coating is the best, and the heat-insulating layer formed by the prepared coating has a better heat-insulating effect.

[0084] The nano-titanium dioxide raw material used in the embodiment of the present invention is rutile titanium dioxide with a particle size of 20-50 nm.

[0085] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.

[0086] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A thermal insulation coating with reflection, radiation and barrier functions, characterized in that: The composition comprises the following components in parts by weight: 100 parts of block modified acrylic emulsion, 5-10 parts of nanosilica aerogel, 10-20 parts of hollow glass microspheres, and 10-30 parts of nanotitanium dioxide; The hollow glass microspheres are composed of hollow glass microspheres with a particle size of 100-150 μm, hollow glass microspheres with a particle size of 50-80 μm, and hollow glass microspheres with a particle size of 1-20 μm, mixed in a mass ratio of 1:2-3:5-6; The block-modified acrylic emulsion is a polymethyl methacrylate emulsion modified by styrene blocks.

2. The heat-insulating coating with reflection, radiation and barrier functions as claimed in claim 1, characterized in that: The sum of the mass of nano-silica aerogel and nano-titania is 1.5-3 times the mass of hollow glass microspheres.

3. The heat-insulating coating with reflection, radiation and barrier functions as claimed in claim 1, characterized in that: The particle size of nanosilica aerogel is 100-800nm.

4. The heat-insulating coating with reflection, radiation and barrier functions as claimed in claim 1, characterized in that: The particle size of nano-titanium dioxide is 20-50nm.

5. The heat-insulating coating with reflection, radiation and barrier functions as claimed in claim 1, characterized in that: The block-modified acrylic emulsion is a triblock copolymer emulsion formed by a polystyrene segment and a polymethyl methacrylate segment, or a pentablock copolymer emulsion formed by a polystyrene segment and a polymethyl methacrylate segment.

6. The heat-insulating coating with reflection, radiation and barrier functions as claimed in claim 1, characterized in that: The invention also comprises the following components in parts by weight: 1-5 parts of a film-forming aid, 0.1-3 parts of a wetting agent, 0.8-2 parts of a defoaming agent, and 0.5-2 parts of a thickener.

7. A method for preparing a heat-insulating coating having reflection, radiation and barrier functions according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step S1: adding block-modified acrylic emulsion, wetting agent and defoaming agent into water and mixing them evenly to obtain a premixed emulsion; Step S2: adding hollow glass microspheres and nanosilica aerogel to the premixed milk while stirring, and mixing to obtain a premixed material; Step S3: adding nano-titanium dioxide to the premix while stirring, and mixing to obtain a mixture; Step S4: adding a film-forming aid and a thickener to the mixture, and mixing them evenly to obtain a heat-insulating coating with reflection, radiation and barrier functions.

8. The preparation method according to claim 7, characterized in that: In step S2, the stirring speed is 300-600 rpm.

9. The preparation method according to claim 7, characterized in that: In step S2, the stirring speed is 1000-1500 rpm.

10. A heat insulation layer, characterized in that: The thermal insulation coating is prepared from the thermal insulation coating as described in any one of claims 1 to 6.

Citation Information

Cited By

  • Preparation method of heat insulation coating for air fryer

    CN119490788A

  • Thermally insulating coating compositions

    GB2703701A

  • Thermally insulating coating compositions

    WO2026131185A1