Anti-crack self-repairing material and preparation method thereof

Through the crack-resistant self-repairing materials of A, B, and C, the three-dimensional network structure is formed using the exchange reaction of disulfide and thiol and catalysts, which solves the shortcomings of the existing self-repair coating in crack repair, and achieves the Effective repair of wall cracks and improved water resistance and corrosion resistance are suitable for high-demand buildings.

CN118931375APending Publication Date: 2024-11-12NIPPON PAINT CHINA
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411198201.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After being damaged by external forces or environmental damage, the existing self-repair coating is difficult to effectively repair, resulting in a reduced protective effect. The repair process is cumbersome and costly, and it cannot effectively solve the problem of wall cracks.

Method used

Using three components of A, B, and C, the three-dimensional network structure is formed through the exchange of disulfide and thiol, and the trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol and Nonionic hydroxy polyethylene oxide block copolymer realizes self-healing reaction under normal temperature conditions, converts the oily system into an aqueous system, and reduces the pungent odor of sulfur glue.

Benefits of technology

It realizes effective repair of wall cracks, extends the service life of the coating, reduces construction costs, has good water resistance, corrosion resistance and environmental friendliness, and is suitable for high-demand buildings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005017105520000091
    Figure BDA0005017105520000091
Patent Text Reader

Abstract

According to the anti-crack self-repairing material and the preparation method thereof, the anti-crack self-repairing material comprises a component A, a component B and a component C. The component A and the component B are oily systems, the component C is stirred at a high speed to obtain an aqueous compound, the component A and the component B are fully mixed during preparation, then the component C is added for high-speed stirring, and the anti-crack self-repairing material is prepared. Only the anti-cracking self-repairing material obtained according to the charging sequence can achieve an ideal self-repairing effect, otherwise, the self-repairing effect is difficult to achieve; in addition, a polysulfide mixture of the component A and the component B is emulsified through the component C, so that the oily sulfide is applied to a building coating water-based system, and the application range of the oily sulfide is expanded. Meanwhile, the emulsified polysulfide greatly reduces the pungent smell of the sulfur rubber, and the environment-friendly architectural concept is embodied.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of self-repairing coatings, and in particular relates to a crack-resistant self-repairing material and a preparation method thereof. Background Art

[0002] With the continuous development of my country's industrialization and urbanization, infrastructure construction will continue to maintain a large scale. At the same time, various new materials are also developing rapidly and emerging in an endless stream. Self-repairing coatings can recover by themselves or restore their original protective function under certain conditions after being damaged by external forces or environmental damage. It is an emerging intelligent protective material.

[0003] In recent years, the development of coating technology and materials science has been closely linked. Various functional coatings have emerged with the continuous progress of materials science. In this context, self-healing coatings have developed rapidly in both theoretical research and practical applications. Existing coatings often repair their protective capabilities in one of two ways: autonomous repair of embedded film-forming substances or corrosion inhibitors or non-autonomous repair with the help of external conditions. As a polymer-based composite material, self-healing coatings are widely used in many fields such as ocean, energy, construction, transportation, aerospace and military equipment. Organic coatings isolate the substrate from media such as moisture, carbon dioxide and ions through physical shielding, thereby inhibiting the speed of wall damage. However, the coating will inevitably be damaged by various external conditions, resulting in damage and cracking. If not repaired in a timely and effective manner, these defects will significantly reduce the protective effect of the coating on the substrate and the adhesion of the coating. At present, damaged coatings are mainly repaired or replaced manually, which is cumbersome and expensive.

[0004] The use of smart materials can make the coating have the ability to self-repair and repair damage by itself, which is beneficial to extending the service life of the coating. It has huge economic value and development space and is one of the most important research directions in the field of self-repairing materials at home and abroad in recent years. Summary of the invention

[0005] The purpose of the present invention is to solve the above-mentioned problems and provide a crack-resistant self-repairing material and a preparation method thereof. The crack-resistant self-repairing material prepared by the present invention can solve the cracks generated on the wall surface. At the same time, the self-repairing function of the crack-resistant self-repairing material can more effectively protect the wall body and achieve an aesthetic effect. It can also be widely used in various buildings with high requirements for wall surfaces, such as theme parks, museums, gymnasiums, government office buildings and other public buildings, and has broad market prospects.

[0006] To solve the above problems, the present invention is implemented through the following technical solutions:

[0007] The first object of the present invention is:

[0008] Provided is a method for preparing a crack-resistant self-repairing material, which comprises three components A, B and C, wherein the mass ratio of component A: component B: component C is 100:9-60:15-70;

[0009] The A component includes the following components in weight percentage:

[0010] Liquid polysulfide 10-50%, bentonite 1-20%, heavy calcium carbonate 20-60%, additives 1-10%, the sum of all components is 100%;

[0011] The liquid polysulfide is an epoxy-terminated liquid polysulfide;

[0012] The B component includes the following components in weight percentage:

[0013] Sulfur rubber 80-98%, catalyst 2%-20%, the sum of all components is 100%;

[0014] The catalyst is a trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol;

[0015] The sulfur rubber is a sulfur rubber with mercaptan as the terminal group;

[0016] The C component includes the following components in weight percentage:

[0017] Water 55-95%, emulsifier 5-45%, the sum of all components is 100%;

[0018] The emulsifier is a nonionic hydroxy polyethylene oxide block copolymer;

[0019] It comprises the following preparation steps:

[0020] Preparation of component A:

[0021] A1. Weigh liquid polysulfide according to the formula ratio and place it in a container;

[0022] A2. Start stirring and dispersing at a speed of 600 r / min, add additives, and mix and stir for 5 minutes;

[0023] A3. Add heavy calcium carbonate and stir for 10 minutes, then add bentonite. After adding, mix and stir for 10 minutes;

[0024] A4. Adjust the speed to 900r / min, disperse and stir for 15 minutes, then turn off the power and stop stirring to obtain component A;

[0025] Preparation of component B:

[0026] B1. Weigh the sulfur rubber according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min;

[0027] B2. Then add the catalyst, mix and stir for 10 minutes and then stop stirring to obtain component B;

[0028] Preparation of component C:

[0029] C1. Weigh water according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min;

[0030] C2. Then add the emulsifier, mix and stir for 5 minutes and then stop stirring to obtain component C;

[0031] Preparation of crack-resistant self-repairing materials:

[0032] After component A, component B and component C are prepared, component A and component B are first stirred and mixed in proportion for 1 to 10 minutes, and then component C is added and stirred at a high speed of 1500 r / min for 15 minutes to obtain the crack-resistant self-repairing material.

[0033] The preparation of the anti-crack self-repairing material of the present invention is further optimized as follows:

[0034] The bentonite in the A component is organic bentonite.

[0035] The preparation of the anti-crack self-repairing material of the present invention is further optimized as follows:

[0036] The heavy calcium carbonate in the A component is one or a combination of 200-1000 meshes.

[0037] The preparation of the anti-crack self-repairing material of the present invention is further optimized as follows:

[0038] The additive in the component A is one or a combination of a defoamer, a bactericide and a neutralizer.

[0039] The second object of the present invention is:

[0040] Provided is a crack-resistant self-repairing material, which is prepared according to the above-mentioned method for preparing the crack-resistant self-repairing material.

[0041] The anti-crack self-repairing material prepared by the present invention is coated by a conventional method.

[0042] The main purpose of the anti-crack self-repairing material of the present invention is to provide a new type of anti-crack self-repairing material for modern civil buildings to solve the wall cracks caused by wall cracking. The design concept of the anti-crack self-repairing material is:

[0043] The mutual exchange of disulfide (S=S) and thiol (SH) is used to form a three-dimensional network structure to achieve the repair effect. First, the disulfide bond is an important dynamic reversible chemical bond with low bond energy. It can undergo exchange reactions under a variety of external stimuli, and the conditions of the exchange reaction are mild and easy to regulate. Furthermore, in the thiol (SH) bond, the electronegativity of the sulfur atom is high, which can attract the electrons of the hydrogen atom to form a stronger SH bond. When the thiol contacts a compound containing a disulfide bond, the sulfur-hydrogen bond and the disulfide bond react competitively. The sulfur-hydrogen bond in the thiol breaks, and the sulfur atom contributes a pair of electrons to form a new sulfur-sulfur bond with the two sulfur atoms in the disulfide bond. When attacking the disulfide (S=S) bond, a new molecular chain can be formed. In addition, there are hydrogen bonds between thiols (SH), and the hydrogen bonds can be connected to each other through van der Waals forces. Through the combination of bonds, a three-dimensional network structure system is finally formed.

[0044] The anti-cracking self-repairing material of the present invention comprises three components, A, B and C, wherein the components A and B are oily systems, and the aqueous compound is obtained by the component C under high-speed stirring conditions. During preparation, the components A and B are first fully mixed, and then the component C is added for high-speed stirring. Only the anti-cracking self-repairing material obtained in this order of addition can achieve the ideal self-repairing effect, otherwise it is difficult to achieve. The present invention emulsifies the polysulfide mixture of the components A and B through the component C, thereby realizing the application of oily sulfides to the aqueous system of architectural coatings and expanding its application range. At the same time, the emulsified polysulfide greatly reduces the pungent smell of the sulfur glue itself, reflecting the environmentally friendly architectural concept.

[0045] An innovative point of the present invention is that the trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol is used to react and solidify the epoxy-terminated liquid polysulfide and the thiol-terminated sulfur gel to form a film at room temperature, which is not easy to react. The possibility of using the polysulfide at room temperature is realized. The action mechanism of the trimerization catalyst is to reduce the activation energy required for the reaction. At room temperature, the sulfur-sulfur bond breaks and opens to form free radicals, and then the free radicals are exchanged to form new bonds.

[0046] Another innovation of the present invention is the addition of nonionic hydroxy polyethylene oxide block copolymer, which not only realizes the conversion of pungent oily system into environmentally friendly water-based system, but also the nonionic hydroxy polyethylene oxide block copolymer is involved in the three-dimensional network system constructed by epoxy-terminated liquid polysulfide and sulfur glue with thiol as end group. The epoxy groups in the nonionic hydroxy polyethylene oxide block copolymer molecules can react with thiol to form a more stable three-dimensional network structure. Secondly, the addition of trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol enables the system to be realized under normal temperature conditions and has an unexpected self-healing effect.

[0047] The crack-resistant self-repairing material prepared according to the aforementioned composition and preparation method has the following characteristics:

[0048] The anti-crack self-repairing material of the present invention is an organic elastomer material, and compared with inorganic non-elastic materials, it has a better anti-cracking effect on the appearance of the wall;

[0049] The anti-crack self-repairing material of the present invention has outstanding water resistance and corrosion resistance, can withstand the long-term test of harsh environments, and has good practicality;

[0050] The anti-crack self-repairing material of the present invention can complete self-repair at room temperature, which can reduce the influence of environmental factors;

[0051] The anti-crack self-repairing material of the present invention can not only repair fine cracks on the base surface and beautify the wall surface, but also can repair relatively wide cracks due to its excellent elasticity retention rate, thus extending its service life, saving costs, and having broad application prospects;

[0052] The anti-cracking self-repairing material of the present invention belongs to a water-based architectural coating, and compared with oily materials, has low odor, is easy to construct, and is more environmentally friendly. DETAILED DESCRIPTION

[0053] In order to make the purpose, technical solutions and advantages of the present invention clearer, the present invention is described in detail below in conjunction with specific embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not limited to the present invention. All simple improvements to the preparation method of the present invention under the premise of the present invention's conception belong to the protection scope of the present invention.

[0054] Example 1

[0055] A method for preparing a crack-resistant self-repairing material, comprising three components A, B, and C, wherein the mass ratio of component A: component B: component C is 100:9-60:15-70;

[0056] The A component includes the following components in weight percentage:

[0057] Liquid polysulfide 10-50%, bentonite 1-20%, heavy calcium carbonate 20-60%, additives 1-10%, the sum of all components is 100%;

[0058] The liquid polysulfide is an epoxy-terminated liquid polysulfide;

[0059] The B component includes the following components in weight percentage:

[0060] Sulfur rubber 80-98%, catalyst 2%-20%, the sum of all components is 100%;

[0061] The catalyst is a trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol;

[0062] The sulfur rubber is a sulfur rubber with mercaptan as the terminal group;

[0063] The C component includes the following components in weight percentage:

[0064] Water 55-95%, emulsifier 5-45%, the sum of all components is 100%;

[0065] The emulsifier is a nonionic hydroxy polyethylene oxide block copolymer;

[0066] It comprises the following preparation steps:

[0067] Preparation of component A:

[0068] A1. Weigh liquid polysulfide according to the formula ratio and place it in a container;

[0069] A2. Start stirring and dispersing at a speed of 600 r / min, add additives, and mix and stir for 5 minutes;

[0070] A3. Add heavy calcium carbonate and stir for 10 minutes, then add bentonite. After adding, mix and stir for 10 minutes;

[0071] A4. Adjust the speed to 900r / min, disperse and stir for 15 minutes, then turn off the power and stop stirring to obtain component A;

[0072] Preparation of component B:

[0073] B1. Weigh the sulfur rubber according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min;

[0074] B2. Then add the catalyst, mix and stir for 10 minutes and then stop stirring to obtain component B;

[0075] Preparation of component C:

[0076] C1. Weigh water according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min;

[0077] C2. Then add the emulsifier, mix and stir for 5 minutes and then stop stirring to obtain component C;

[0078] Preparation of crack-resistant self-repairing materials:

[0079] After component A, component B and component C are prepared, component A and component B are first stirred and mixed in proportion (mixing time 5 minutes) until they are evenly mixed, and then component C is added and stirred at a high speed of 1500r / min for 15 minutes to obtain the crack-resistant self-healing material.

[0080] The specific raw material composition of Example 1 is shown in Table 1.

[0081] The preparation method of Example 2 is the same as that of Example 1, except that the amounts of some raw materials used are different;

[0082] The preparation method of Comparative Example 1 is the same as that of Example 1, except that: in Comparative Example 1, instead of adding 2,4,6-tris(dimethylaminomethyl)phenol, sodium tripolyphosphate is added;

[0083] The preparation method of Comparative Example 2 is the same as that of Example 1, except that: Comparative Example 2 does not add 2,4,6-tris(dimethylaminomethyl)phenol;

[0084] The difference between Comparative Example 3 and Example 2 is that the order of adding materials in Example 2 is to mix components A and B first, and then add component C; the order of adding materials in Comparative Example 3 is to stir and mix components A, B, and C at the same time.

[0085] Table 1 Specific raw material composition of the embodiments and comparative examples (parts by weight)

[0086]

[0087]

[0088] It has been determined that:

[0089] In Example 1: after the crack-resistant self-repairing material is broken, the self-healing rate is 73% under normal temperature conditions;

[0090] In Example 2: after the crack-resistant self-repairing material is broken, the self-healing rate is 75% under normal temperature conditions;

[0091] In comparative example 1: after the crack-resistant self-repairing material is broken, the self-healing rate is 0% under normal temperature conditions;

[0092] In comparative example 2: after the crack-resistant self-repairing material is broken, the self-healing rate is 0% under normal temperature conditions;

[0093] In Comparative Example 3: after the anti-crack self-repairing material is broken, the self-healing rate is 0% under normal temperature conditions.

[0094] By comparison, the self-healing rate of the crack-resistant self-repairing material obtained without adding a trimerization catalyst or adding other catalysts under normal temperature conditions is 0%; when the order of adding materials is changed (Comparative Example 3), the self-healing rate is also 0%; only when liquid polysulfide, sulfur rubber, and trimerization catalyst are added at the same time without changing the order of adding materials, the self-healing rate of the prepared crack-resistant self-repairing material reaches more than 70%.

[0095] To sum up, the above are only preferred embodiments of the present invention and are not intended to limit the present invention in any form. Any equivalent changes, modifications and evolutions made by technicians familiar with the profession without departing from the scope of the technical solution of the present invention using the disclosed technical content are regarded as equivalent embodiments of the present invention. At the same time, any equivalent changes, modifications and evolutions made to the above embodiments based on the essential technology of the present invention are still within the protection scope of the technical solution of the present invention.

[0096] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0097] The experimental methods without specific conditions in the present invention are usually carried out according to conventional conditions or conditions recommended by the manufacturer.

[0098] Unless otherwise stated, the various optimization technical solutions in the present invention can be combined with each other.

[0099] Unless otherwise indicated, percentages and parts are by weight.

[0100] Experimental methods without specific conditions specified in the instructions and examples are usually carried out under conventional conditions or conditions recommended by the manufacturers.

[0101] Unless otherwise specified, various raw materials, reagents and components used in the present invention are corresponding raw materials commonly used in the art.

[0102] Unless otherwise defined, all professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention.

Claims

1. A method for preparing a crack-resistant self-repairing material, characterized in that: It includes three components A, B and C, and the mass ratio of component A: component B: component C is 100:9-60:15-70; The A component includes the following components in weight percentage: Liquid polysulfide 10-50%, bentonite 1-20%, heavy calcium carbonate 20-60%, additives 1-10%, the sum of all components is 100%; The liquid polysulfide is an epoxy-terminated liquid polysulfide; The B component includes the following components in weight percentage: Sulfur rubber 80-98%, catalyst 2%-20%, the sum of all components is 100%; The catalyst is a trimerization catalyst 2,4,6-tris(dimethylaminomethyl)phenol; The sulfur rubber is a sulfur rubber with mercaptan as the terminal group; The C component includes the following components in weight percentage: Water 55-95%, emulsifier 5-45%, the sum of all components is 100%; The emulsifier is a nonionic hydroxy polyethylene oxide block copolymer; It comprises the following preparation steps: Preparation of component A: A1. Weigh liquid polysulfide according to the formula ratio and place it in a container; A2. Start stirring and dispersing at a speed of 600 r / min, add additives, and mix and stir for 5 minutes; A3. Add heavy calcium carbonate and stir for 10 minutes, then add bentonite. After adding, mix and stir for 10 minutes; A4. Adjust the speed to 900r / min, disperse and stir for 15 minutes, then turn off the power and stop stirring to obtain component A; Preparation of component B: B1. Weigh the sulfur rubber according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min; B2. Then add the catalyst, mix and stir for 10 minutes and then stop stirring to obtain component B; Preparation of component C: C1. Weigh water according to the formula ratio, place it in a stirring container, turn on the stirring switch, and adjust the speed to 500r / min; C2. Then add the emulsifier, mix and stir for 5 minutes and then stop stirring to obtain component C; Preparation of crack-resistant self-repairing materials: After component A, component B and component C are prepared, component A and component B are first stirred and mixed in proportion for 1 to 10 minutes, and then component C is added and stirred at a high speed of 1500 r / min for 15 minutes to obtain the crack-resistant self-repairing material.

2. The method for preparing the crack-resistant self-repairing material according to claim 1, characterized in that: The bentonite in the A component is organic bentonite.

3. The method for preparing the crack-resistant self-repairing material according to claim 1, characterized in that: The heavy calcium carbonate in the A component is one or a combination of 200-1000 meshes.

4. The method for preparing the crack-resistant self-repairing material according to claim 1, characterized in that: The additive in the component A is one or a combination of a defoamer, a bactericide and a neutralizer.

5. A crack-resistant self-repairing material, characterized in that: The material is prepared according to the method for preparing the crack-resistant self-repairing material according to any one of claims 1 to 4.