Sintering system and sintered article
Through the carrier mesh support and precisely controlled sintering process, the challenges of sintered products in consistency and deformation are solved, and high-quality production of long, thin and wide sintered products are achieved, ensuring the density of materials and dielectric properties.
Patent Information
- Application Number
- CN202411226844.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-09-11
- Filing Date
- 2017-12-19
- Publication Date
- 2024-11-12
AI Technical Summary
Existing sintering technologies are difficult to produce high-quality long, thin, and wide sintered products, especially in maintaining material consistency and avoiding deformation or cracking.
The carrier mesh is used to support the green strips and accurately control the separation of the carrier mesh from the green strips, combined with ultra-low tension floating rollers and independently controlled heating elements, to achieve precise control of sintered products, including in adhesives Control of air flow and heat distribution within the removal and sintering workstation.
Sintered products with high consistency, low deformation and low risk of fracture are produced, which can maintain long, thin and wide strip shapes in roll-roll processing and improve the density and dielectric properties of the sintered material.
Smart Images

Figure CN118931397A_ABST
Abstract
Description
[0001] This application is a divisional application of application number 202210369984.5, filed on December 19, 2017, entitled "Sintering System and Sintered Articles", which is a divisional application of application number 201780086844.4, filed on December 19, 2017, entitled "Sintering System and Sintered Articles".
[0002] priority
[0003] This application claims U.S. Application No. 62 / 437,157, filed December 21, 2016; U.S. Application No. 62 / 439,613, filed December 28, 2016; U.S. Application No. 62 / 470,550, filed March 13, 2017; U.S. Application No. 62 / 439,609, filed December 28, 2016; and U.S. Application No. 62 / 526,806, filed June 29, 2017. Priority claims to U.S. Application No. 62 / 439,598, filed December 28, 2016; U.S. Application No. 62 / 483,726, filed April 10, 2017; U.S. Application No. 62 / 484,106, filed April 11, 2017; and U.S. Application No. 62 / 556,712, filed September 11, 2017, on which this application is based and which are incorporated herein by reference in their entirety. Background Technology
[0004] This disclosure generally relates to processes for sintering, such as sintering green strips containing polycrystalline ceramic particles or other inorganic particles bonded in a binder, and continuous and discrete sintered articles manufactured by such processes, such as ceramic plates, strips, or sheets. This disclosure relates to articles, such as sheets, strips, tapes, or sheets of ceramic or other inorganic materials, with a wide range of potential uses, for example, as waveguides when the ceramic is transmissive to light, as substrates that can be coated or laminated, and integrated into batteries or other components, or used as substrates or bonded to substrates, for example, as dielectrics in electronic packaging (e.g., LED packaging), or other applications. Various material properties, particularly for ceramic materials, such as high resistivity, low reactivity, and low coefficient of thermal expansion, make such articles particularly suitable for a wide range of applications. Summary of the Invention
[0005] Some aspects of this disclosure relate to a strip separation system for sintering preparation. The strip separation system includes: a strip material source (which includes a green strip) and a carrier web supporting the green strip. The green strip includes particles of inorganic material in a binder. The strip separation system also includes a stripper and a vacuum drum, the stripper being used to guide the carrier web in a rewinding direction and the green strip in a downstream processing direction different from the rewinding direction, the vacuum drum being positioned and configured to receive strip material from the source and transfer the strip material to the stripper. The vacuum drum includes orifices for applying suction to the carrier web to promote tension of the carrier web, and the tension in the carrier web (in units of force per cross-sectional area) is greater than the tension in the green strip as the strip material is transported from the vacuum drum to the stripper, thereby mitigating deformation of the green strip during separation from the carrier web.
[0006] Other aspects of this disclosure relate to a strip processing system for sintering preparation. The system includes: a strip comprising a green portion of the strip having inorganic material particles in an organic binder; and a binder burn-off station comprising an active heater. The strip travels through the binder burn-off station, whereby the binder burn-off station receives the green portion of the strip, and when the green portion of the strip comes into contact with heat from the heater, the binder burn-off station causes the organic binder to char or burn, thereby forming a second portion of the strip prepared for sintering the inorganic material of the strip. In some embodiments, the strip simultaneously extends into, through, and out of the binder burn-off station in an instant, such that in an instant, the strip comprises a green portion continuously connected to the second portion, for example, wherein the binder burn-off station chars or burns at least a majority (by weight) of the organic binder from the green portion of the strip without causing significant sintering of the inorganic material particles. In some embodiments, the strip processing system for sintering preparation further includes ultra-low tension floating rollers, which include lightweight, low-inertia rollers that change the direction of the strip without applying significant tension, such that the tension in the second portion of the strip is less than 500 g force per mm. 2 The cross-section reduces the likelihood of breakage in the second portion of the strip and facilitates sintering of the long, continuous length of the strip. In some embodiments, as the strip travels through the binder burn-off station, the strip processing system for sintering preparation blows and / or draws gas onto the strip, and the binder burn-off station heats the strip to a temperature higher than the temperature at which the organic binder would ignite without gas blowing and / or drawing gas onto the strip, thus causing the organic binder to char or burn but the strip not to ignite.
[0007] Additional aspects of this disclosure relate to a production line comprising the aforementioned system for processing strips, wherein the binder burn-off station is a first station, and the production line further comprises a second station spaced apart from the first station. The second station at least partially sintersulates the inorganic material of the second portion of the strip to form a third portion of the strip, wherein, instantaneously, the strip comprises a green portion continuously connected to the third portion in a manner consistent with the second portion. For example, in some such embodiments, the third portion of the strip is significantly more flexible than the second portion, such that its minimum bending radius without breakage is less than half the minimum bending radius of the second portion, and the green portion is significantly more flexible than the second portion, such that its minimum bending radius without breakage is less than half the minimum bending radius of the second portion. The production line also includes the strip separation system described above.
[0008] Some aspects of this disclosure relate to a sintering system comprising a strip material containing inorganic material particles and a sintering workstation. The sintering workstation includes an inlet, an outlet, and a channel extending between the inlet and the outlet. In an instant, the strip material extends into the inlet of the sintering workstation, extends through the channel, and extends out of the outlet. Heat within the channel sintersulates the inorganic material, resulting in the inorganic material having a first porosity at the inlet and a second porosity less than the first porosity at the outlet. Furthermore, the strip material is positively taut as it passes through the channel of the sintering workstation, thereby mitigating warping. In some embodiments, the strip material moves through the sintering workstation at a speed of at least 1 inch per minute. In some embodiments, the channel of the sintering workstation is heated by at least two independently controlled heating elements, wherein the heating elements create a temperature distribution, wherein the temperature of the channel increases along the length of the channel in a direction from the inlet to the outlet of the sintering workstation, and wherein the sintering temperature in the channel exceeds 800°C. In some embodiments, the sintering system further includes a curved surface located along a channel of the sintering workstation, wherein the strip material bends about the curved surface relative to the width axis of the strip material as it moves through the sintering workstation, thereby affecting the shape of the strip material. In some embodiments, the outlet and inlet of the sintering workstation are located in a substantially horizontal plane such that the angle defined between the outlet and inlet of the sintering workstation and the horizontal plane is less than 10 degrees, thereby at least partially controlling the flow of gas relative to the channel; for example, in some such embodiments, the sintering workstation also includes an upward-facing channel surface (which defines the lower surface of the channel) and a downward-facing channel surface (which defines the upper surface of the channel), wherein the downward-facing channel surface is located close to the upper surface of the strip material such that the gap between the upper surface of the strip material and the downward-facing channel surface is less than 0.5 inches, thereby at least partially controlling the gas flow in the channel. The strip material can be particularly wide, long, and thin, with a width greater than 5 mm, a length greater than 30 cm, and a thickness of 3 micrometers to 1 mm, and the inorganic material of the strip can be at least one of polycrystalline ceramic materials and synthetic minerals.
[0009] Other aspects of this disclosure relate to a process for manufacturing ceramic strips, comprising the steps of sintering a strip containing polycrystalline ceramic to a porosity of less than 20% by volume by exposing polycrystalline ceramic particles to a heat source to induce sintering between the particles. The strip is particularly thin, such that its thickness is less than 500 μm, thereby facilitating rapid sintering via thermal infiltration. Furthermore, the strip is at least 5 mm wide and at least 300 cm long. In some embodiments, the process further includes a step of tensioning the strip in the forward length direction during sintering. In some such embodiments, the process further includes a step of moving the strip toward and then away from the heat source during sintering. In some embodiments, the sintering time is particularly short, totaling less than 2 hours, thereby helping to maintain small particle sizes in the ceramic strip; for example, in some such embodiments, the total sintering time is less than 1 hour, and after sintering, the polycrystalline ceramic has a density greater than 95% by volume, is dense, and / or the strip includes closed pores after sintering. In some embodiments, the strip includes a volatile component that evaporates during sintering, wherein the volatile component is inorganic, and wherein the strip contains at least 1 volume more volatile component before sintering than after sintering.
[0010] Other aspects of this disclosure relate to strips comprising a body comprising particles of inorganic material sintered together. The body extends between first and second main surfaces, wherein the body has a thickness defined as the distance between the first and second main surfaces, a width defined as a first dimension of the first main surface perpendicular to the thickness, and a length defined as a second dimension of the first main surface perpendicular to both the thickness and the width. The strip is long, having a length of about 300 cm or greater. The strip is thin, having a thickness of about 3 μm to about 1 mm. The strip is particularly wide, having a width of about 5 mm or greater. According to an exemplary embodiment, the geometric consistency of the strip is such that when measured at positions spaced 1 m apart in a length direction, the width difference of the strip is less than 100 μm; and when measured along the center of the width direction of the strip at positions spaced 1 m apart in a length direction, the thickness difference of the strip is less than 10 μm. In some embodiments, the strip is flat or planarizable such that a 10 cm long strip pressed between parallel flat surfaces is planarized to within 0.05 mm of contact with the parallel flat surfaces without cracking; for example, in some such embodiments, when planarized to within 0.05 mm of contact with the parallel flat surfaces, the maximum in-plane stress exhibited by the strip does not exceed 1% of its Young's modulus. In some embodiments, the first and second main surfaces of the strip have a granular profile, wherein the particles are ceramic, and wherein at least some individual particles of the adjacent ceramic have little to no intervening amorphous material, such that the thickness of the amorphous material between two adjacent particles is less than 5 nm. In some embodiments, the body has a porosity of less than 10% by volume, and / or the body has closed pores. In some embodiments, the particles include lithium, and the ionic conductivity of the body is greater than 5 x 10⁻⁶. -5 S / cm. In some embodiments, the body has a particularly fine particle size, which is 5 μm or less. In some embodiments, the strip also includes a conductive metal attached to a first main surface of the body, wherein, in some such embodiments, the body includes a repeating pattern of holes, and the conductive metal is arranged in a repeating pattern. In some embodiments, the first and second main surfaces have a granular profile, and the strip also includes a coating covering the granular profile of the first main surface, wherein the outer-facing surface of the coating is not as rough as the granular profile of the first surface, wherein the conductive metal is attached to the first main surface by bonding to the outer-facing surface of the coating. In some embodiments, the viscosity of the inorganic material at temperatures greater than 900°C is 12.5 poise.
[0011] Additional aspects of this disclosure relate to a strip roller of any of the embodiments described above, wherein the strip is wound and overlapped around itself, bent to a radius of less than 30 cm.
[0012] Other aspects of this disclosure relate to multiple plates cut from strips of any of the embodiments described above.
[0013] Some aspects of this disclosure relate to strips comprising a body containing mutually sintered ceramic particles, the body extending between first and second main surfaces, wherein the body has a thickness defined as the distance between the first and second main surfaces, a width defined as a first dimension of the first main surface perpendicular to the thickness, and a length defined as a second dimension of the first main surface perpendicular to both the thickness and the width; wherein the strip is thin, having a thickness of about 3 μm to about 1 mm; and wherein the first and second main surfaces of the strip have a granular profile, and at least some individual particles of the adjacent ceramics have little to no intercalary amorphous material, such that the thickness of the amorphous material between two adjacent particles is less than 5 nm.
[0014] Some aspects of this disclosure relate to strips comprising a body containing mutually sintered ceramic particles, the body extending between first and second main surfaces, wherein the body has a thickness defined as the distance between the first and second main surfaces, a width defined as a first dimension of the first main surface perpendicular to the thickness, and a length defined as a second dimension of the first main surface perpendicular to both the thickness and the width; wherein the strip is thin, having a thickness of about 3 μm to about 1 mm; wherein the first and second main surfaces of the strip have a granular profile; and wherein the particles contain lithium, and the body has a thickness greater than 5 x 10⁻⁶. - 5 Ionic conductivity in S / cm.
[0015] Other features and advantages are set forth in the following detailed description, some of which will be readily understood by those skilled in the art, or will be recognized by practicing the embodiments described in the text description and its claims and drawings.
[0016] It should be understood that the general description above and the detailed description below are merely exemplary, intended to provide an overall assessment or framework for understanding the nature and characteristics of the claims.
[0017] The accompanying drawings provide a further understanding and are incorporated in and form a part of this specification. The drawings illustrate one or more embodiments and, together with the specification, serve to explain the principles and operation of various embodiments. Attached Figure Description
[0018] Figure 1 Examples of deformed sintered ceramic strip materials formed without the techniques disclosed herein (e.g., controlled green strip tensioning and other techniques discussed herein).
[0019] Figure 2 This shows an example of a sintered ceramic strip material produced using a temperature distribution and strip speed that result in non-uniform sintering.
[0020] Figure 3 This is a roller-roll system for producing sintered products, according to an exemplary embodiment.
[0021] Figure 4 According to an exemplary implementation, Figure 3 An enlarged view of an embodiment of the separation system shown.
[0022] Figure 5 This is a side view of a continuous strip material according to an exemplary embodiment.
[0023] Figure 6 This is a perspective view of a vacuum drum according to an exemplary embodiment.
[0024] Figure 7 According to an exemplary implementation Figure 6 An enlarged view of the vacuum drum shown.
[0025] Figure 8 According to an exemplary implementation Figure 4 An enlarged view of the peeler shown.
[0026] Figure 9 This is a conceptual side view of a workstation in a production line that prepares green strips for sintering, according to an exemplary embodiment.
[0027] Figure 10 According to an exemplary implementation Figure 9 Front perspective view of the workstation.
[0028] Figure 11 The block diagram is based on an exemplary embodiment of a method for processing green strips, at least partially preparing green strips for sintering.
[0029] Figure 12 According to an exemplary implementation, Figure 3 Detailed diagrams of the adhesive removal workstation and sintering workstation of the system.
[0030] Figure 13 According to an exemplary implementation, Figure 12 Detailed image of the strip material inside the passageway of the sintering furnace.
[0031] Figure 14 The image shows sintered strip material leaving the sintering furnace, according to an exemplary embodiment.
[0032] Figure 15 According to an exemplary implementation Figure 12A view of the sintering workstation, showing the heating system.
[0033] Figure 16 According to an exemplary implementation, for different strip transport speeds, the heat distribution is predicted and the relationship between sintering shrinkage and distance is modeled.
[0034] Figure 17 The image shows a predicted sintering temperature distribution projected along the channels of a sintering furnace, according to an exemplary embodiment.
[0035] Figure 18 This illustrates an online multi-furnace sintering workstation according to an exemplary embodiment.
[0036] Figure 19 The illustration is based on an exemplary implementation. Figure 18 The predicted temperature distribution of the two sintering furnaces.
[0037] Figure 20 This illustrates a sintering system having two parallel production systems, according to an exemplary embodiment.
[0038] Figure 21 This is a sintering shrinkage graph of zirconium oxide at various temperatures and temperatures and times, including data fitting curves for each temperature.
[0039] Figure 22 It is a curve fitting graph of the mathematical function of the sintering shrinkage of zirconia strips at various temperatures and at various temperatures and times.
[0040] Figure 23 This is a modeling diagram showing the functional relationship between the peak stress at the centerline of the zirconia strip and the number of heated zones, the number of passes, the strip transport speed, and the strip width during the sintering process.
[0041] Figure 24 The graphs show the functional relationships between the peak stress at the edge of the zirconia strip and the number of heated zones, the number of passes, the strip transport speed, and the strip width during the sintering process.
[0042] Figure 25 This is a shrinkage modeling diagram of zirconia strips during the sintering process of passing through a single hot zone furnace twice, for two different strip transport speeds.
[0043] Figure 26 This is a stress modeling diagram of zirconia strips during the sintering process of passing through a single hot zone furnace twice, for two different strip transport speeds.
[0044] Figure 27 This is a shrinkage modeling diagram of zirconia strips during the sintering process of passing through 10 hot zone furnaces twice, for two different strip transport speeds.
[0045] Figure 28 This is a stress (in MPa) modeling diagram of zirconia strips during sintering processes involving two strip transport speeds and various strip widths, using two passes through 10 hot zone furnaces.
[0046] Figure 29 This is a schematic perspective view of a portion of a sintered article according to an exemplary embodiment.
[0047] Figure 30A It is a digital image of the unpolished surface of a sintered product.
[0048] Figure 30B yes Figure 30A The conceptual side profile of the sintered product.
[0049] Figure 31A It is a digital image of the polished surface of the sintered product.
[0050] Figure 31B yes Figure 31A The conceptual side profile of the sintered product.
[0051] Figure 32 It is a side view along the width of the sintered article according to one or more embodiments.
[0052] Figure 33 The attached diagram shows the thin bending balance.
[0053] Figure 34A This is a perspective side view of a roll-sintered article according to an exemplary embodiment.
[0054] Figure 34B According to an exemplary implementation, Figure 34A A cross-sectional view of the roller-sintered product.
[0055] Figure 35 This is the height profile of the sintered product of Example 5 before planarization, showing that the measured height is higher than the planarization plane.
[0056] Figure 36 This is the height profile of the sintered product of Example 6 before planarization, showing that the measured height is higher than the planarization plane.
[0057] Figure 37 The height profile of the sintered product of Comparative Example 7 before planarization shows that the measured height is higher than the planarized plane.
[0058] Figure 38 The height profile of the sintered product of Comparative Example 8 before planarization shows that the measured height is higher than the planarized plane.
[0059] Figure 39It is the maximum height above the planarization plane of each of the sintered products of Examples 5-6 and Comparative Examples 7-8.
[0060] Figure 40 This is a diagram showing the forces required to planarize each of the sintered products of Examples 5-6 and Comparative Examples 7-8.
[0061] Figure 41 This is a graph showing the pressure required to planarize the sintered products of Examples 5-6 and Comparative Examples 7-8.
[0062] Figure 42 These are the maximum in-plane stress diagrams of the sintered products of Examples 5-6 and Comparative Examples 7-8 after planarization.
[0063] Figure 43A The deformation diagram shows the stress measured on the bottom surface of the sintered product of Example 5 after planarization.
[0064] Figure 43B The deformation diagram shows the stress measured on the top surface of the sintered product of Example 5 after planarization.
[0065] Figure 44A The deformation diagram shows the stress measured on the bottom surface of the sintered product of Example 6 after planarization.
[0066] Figure 44B The deformation diagram shows the stress measured on the top surface of the sintered product of Example 6 after planarization.
[0067] Figure 45A The deformation diagram shows the stress measured on the bottom surface of the sintered product of Comparative Example 7 after planarization.
[0068] Figure 45B The deformation diagram shows the stress measured on the top surface of the sintered product of Comparative Example 7 after planarization.
[0069] Figure 46A The deformation diagram shows the stress measured on the bottom surface of the sintered product of Comparative Example 8 after planarization.
[0070] Figure 46B The deformation diagram shows the stress measured on the top surface of the sintered product of Comparative Example 8 after planarization.
[0071] Figure 47 This is a cross-sectional view of a package containing a sintered article according to an exemplary embodiment.
[0072] Figure 48 It is a cross-sectional view along the length of a package containing a sintered article according to an exemplary embodiment.
[0073] Figure 49This is another cross-sectional view of a segment of a package containing a sintered article according to an exemplary embodiment.
[0074] Figure 50 This is an exemplary method for manufacturing a package containing a sintered article, according to an exemplary embodiment.
[0075] Figure 51 This is another exemplary method for manufacturing a package containing a sintered article, according to an exemplary embodiment.
[0076] Figure 52 This is an exemplary cross-sectional view of a package comprising a sintered article and a "flip-chip" structure according to an exemplary embodiment.
[0077] Figure 53 This is another exemplary cross-sectional view of a segment of a package comprising a sintered article and a "flip-chip" construction according to an exemplary embodiment.
[0078] Figure 54 This is another exemplary cross-sectional view of a segment of a package comprising a sintered article and a "flip-chip" construction according to an exemplary embodiment.
[0079] Figure 55 This is another cross-sectional view of a segment of a package containing a sintered article according to an exemplary embodiment.
[0080] Figure 56 This illustrates, according to an exemplary embodiment, a roll-to-roll system and related processes for producing sintered articles comprising a length of threaded material.
[0081] Figure 57 Detailed diagrams are shown according to an exemplary embodiment. Figure 56 The bonding between a section of threaded material and strip material in the system.
[0082] Figure 58 This illustrates a roll-to-roll system according to an exemplary embodiment, which includes a sintering workstation configured to form a bend in the longitudinal direction along a continuous length of strip material.
[0083] Figure 59 The detailed drawing is of a sintering workstation according to an exemplary embodiment, which includes an insert with a curved lower surface defining a sintering channel.
[0084] Figure 60 This is a side view of the passage of a sintering workstation according to an exemplary embodiment, having opposing curved upper and lower surfaces that define the sintering passage.
[0085] Figure 61This is a side view of a sintering workstation according to an exemplary embodiment, whose radius of curvature varies along the sintering channel.
[0086] Figure 62 This illustrates a gas bearing according to an exemplary embodiment, which has a curved upper surface that defines a curved surface for sintering channels.
[0087] Figure 63 This illustrates a roller arrangement according to an exemplary embodiment, used to form longitudinal bends along a continuous length of the strip during the sintering process.
[0088] Figure 64 The illustration shows an arrangement of multiple rollers according to an exemplary embodiment, which is used to form multiple longitudinal bends along a continuous length of the strip during the sintering process.
[0089] Figure 65 This illustrates a free loop arrangement according to an exemplary embodiment, which is used to form longitudinal bends along the continuous length of the strip during the sintering process.
[0090] Figure 66 The images are digital images of the sintered strips, confirming the flattening that occurs when the strips are bent during the sintering process.
[0091] Figure 67A and 67B This is a digital image of a sintered ceramic strip roll according to an exemplary embodiment.
[0092] Figure 68 This is a digital image of a sintered ceramic strip roll according to another embodiment.
[0093] Figure 69 This is a digital image of a sintered ceramic strip roll according to another embodiment.
[0094] Figure 70 The diagram, based on an exemplary embodiment, shows the sintering time diagram of conventional batch firing versus the sintering time diagram of the technique disclosed herein.
[0095] Figure 71A and 71B This is a top view of the surface of a sintered article according to an exemplary embodiment.
[0096] Figure 72A and 72B This is a side perspective view of the surface of a sintered article according to an exemplary embodiment.
[0097] Figure 73A , 73B 73C are micrographs of the particle boundaries of sintered articles according to exemplary embodiments.
[0098] Figure 74 and75 This is a micrograph of the particle boundaries of a sintered article according to other exemplary embodiments.
[0099] Figure 76 and 77 This is a top view of the surface of a sintered article according to an exemplary embodiment.
[0100] Figure 78 It is a digital image of a strip of a sintered article according to an exemplary embodiment.
[0101] Figure 79A and 79B This is a side view of a sintered article according to an exemplary embodiment.
[0102] Figure 80 This is a side view of a sintered article according to an exemplary embodiment.
[0103] Figure 81 This is a side view of a sintered article according to another exemplary embodiment, wherein the sintered material appears to be amorphous.
[0104] Figure 82 It is a representative diagram.
[0105] Figure 83 and 84 This is a side perspective view of the surface of a sintered article according to an exemplary embodiment.
[0106] Figure 85A and 85B This is a side perspective view of the surface of an unsintered green material according to an exemplary embodiment.
[0107] Figure 86A and 86B This is a side perspective view of the surface of a sintered material according to an exemplary embodiment.
[0108] Figure 87 The diagram illustrates the relationship between viscosity and temperature for various materials.
[0109] Figure 88A The illustration represents the temperature distribution through the sintering furnace according to an exemplary embodiment.
[0110] Figure 88B yes Figure 88A A schematic diagram of the sintering furnace.
[0111] Figure 89 This is a schematic diagram of a sintering furnace according to another exemplary embodiment.
[0112] Figure 90A The illustration represents the temperature distribution through a sintering furnace according to another exemplary embodiment.
[0113] Figure 90B yes Figure 90A A schematic diagram of the sintering furnace.
[0114] Figure 91A and 91B This is a side perspective view of the surface of a sintered material according to an exemplary embodiment.
[0115] Figure 92 This is a side view of a sintered material according to an exemplary embodiment.
[0116] Figure 93 This is a schematic diagram of an electronic device in the form of a battery according to an exemplary embodiment.
[0117] Figure 94 and 95 The illustrations represent sintering schemes according to exemplary embodiments.
[0118] Figure 96 The illustration represents the relationship between sintering temperature and ionic conductivity of a sintered article according to an exemplary embodiment.
[0119] Figure 97 The illustration represents the relationship between the sintering temperature and the percentage of cubic garnet in a sintered article according to an exemplary embodiment.
[0120] Figure 98 and 99 This is a side perspective view of the surface of a sintered material according to an exemplary embodiment.
[0121] Figure 100A and 100B This is a top view of one side surface of the sintered material according to an exemplary embodiment, and Figure 101A and 101B This is a top view of the surface on the other side of the sintered material.
[0122] Figure 102 This is a side view of a sintered material according to an exemplary embodiment.
[0123] Figure 103 It is a digital image of a sintered material according to an exemplary embodiment, which has a layer that provides a smooth surface.
[0124] Figure 104 This is a schematic diagram of an electronic component in the form of a stack of sintered articles according to an exemplary embodiment. Detailed Implementation
[0125] Referring generally to the accompanying drawings, systems and processes for manufacturing long, thin, and / or wide sintered articles are shown and described. For the term sintering, the applicant refers to the process of agglomerating (e.g., directly bonding together) particles or (e.g., powdered or granular materials) into a solid or porous body by heating the particles without completely dissolving them, thereby preserving the crystalline structure of the particles or granules within the aggregate. However, aspects of the present invention can also be used to manufacture amorphous materials, such as those that a person skilled in the art of inorganic materials processing might directly consider difficult or impossible to process using conventional manufacturing techniques. Furthermore, the applicant has found that, using the systems / processes discussed herein, new sintered articles with various properties previously unattainable using existing techniques can be formed. Specifically, the applicant has developed material handling systems and processes that achieve a very precise level of control over the various conditions / forces experienced by the material during the formation of sintered articles, and this precise control / material handling enables the production of long, thin, and / or wide sintered strip materials that are believed to be unattainable using existing technology systems. Furthermore, articles manufactured using the techniques disclosed herein may possess other unique qualities, such as: strength, which may be due to a low number of defects; purity, which may be due to controlled airflow and sintering duration, and properties related to purity, such as dielectric constant and impermeability; consistency, such as along the length and / or width direction, such as flatness, thickness, roughness, grain size, etc.; and other unique properties.
[0126] In general, the system described herein employs an input roller supporting a green strip with a web wound on a spool or reel. As explained in more detail below, the web-supported green strip comprises green strip material including particles of inorganic material (e.g., particles of ceramic material, particles of polycrystalline ceramic material, metal particles or particles of synthetic material) bonded to an organic binder, and the green strip material is supported on a carrier web (e.g., a polymer material plate). The input roller supporting the green strip is unwound, and the carrier web / backing layer is carefully separated from the green strip material. The applicant has discovered that by precisely controlling the separation of the carrier web from the green strip, the green strip exhibits little or no deformation, enabling the production of sintered articles with highly consistent / controlled properties (e.g., thickness, flatness, density, shape, etc.) along its length. In other intended implementations, the green strip may not be mesh-supported and / or may not be on rollers, for example, if the strip is formed in an in-line manner (e.g., along the production line before sintering).
[0127] After the carrier mesh is removed, the self-supporting green strip (comprising particles of inorganic material supported by an organic binder) moves through a binder removal station. Generally, the binder removal station applies heat to the self-supporting green strip, removing the organic binder or causing a chemical change in it, resulting in a non-bonded strip material leaving the binder removal station. By "non-bonded," the applicant means that the binder material has been removed, but the non-bonded strip can still remain together, for example, by burning the binder, by interweaving or bonding between the inorganic particles, or by other means (e.g., electrostatic force, atmospheric pressure). After the organic binder is removed, the non-bonded strip material moves into a sintering station, where heat is applied to it, causing the inorganic particles to sinter (e.g., fully or partially sinter), forming a sintered article leaving the sintering station.
[0128] The applicant was surprised to discover that even after the removal of the organic binder, the inorganic material particles could support themselves as unbonded strip material and / or otherwise support the strips, as described above. However, the unbonded strip material was very delicate or potentially very delicate before sintering after the removal of the organic binder. Therefore, the applicant also identified a novel binder removal and sintering workstation arrangement that allows for the handling of delicate unsupported strip material in a manner that allows for the production of very high-quality sintered articles. (For "unsupported" in the above context, the applicant refers to the absence of organic binder support after the binder has been removed or burned off). Specifically, wide, long, and high-quality sintered articles suitable for roll-to-roll processing were produced without introducing significant deformation or causing article breakage during binder removal or sintering.
[0129] Specifically, the applicant determined that airflow within the binder removal station and / or sintering station (e.g., turbulent airflow due to thermal gradients) could impact the strip material, causing deformation or breakage. Furthermore, the applicant found that highly horizontal processing paths within the binder removal station and / or sintering station reduced or eliminated turbulent airflow, which in turn produced or could produce sintered articles without significant deformation. Additionally, the applicant determined that eliminating airflow-based deformation is particularly important when forming wide sintered articles (e.g., articles wider than 5 mm), as the applicant believes that susceptibility to airflow-based deformation increases with the width of the strip material. Moreover, the applicant determined that eliminating or reducing airflow-based deformation is crucial for achieving roll-to-roll processing, as the applicant found that even minute levels of deformation can lead to breakage of the sintered article or, otherwise, improper winding onto the take-up reel (also known as the take-up roll).
[0130] Given the inorganic green materials and prior sintering techniques, determining the horizontal placement of the strips during binder removal and / or sintering is a surprising finding. For example, some strip sintering may use a downward angled placement of the strip material (e.g., a downward tilt of 12 to 20 degrees) as a way to utilize gravity to pull the fragile strip material through the heating steps of the system, possibly aiming to apply a uniformly distributed force on the strip material to pull the strip material through the heating steps of the process.
[0131] However, the applicant discovered that when the heating section of the sintering system is tilted, vortex airflow may form hot air that rises through the channels of the heating system containing the strip material. Therefore, this airflow impacting the strip material may cause deformation or even breakage. Furthermore, the applicant found that the potential for airflow-based deformation in sintered strips formed using a non-horizontal heating arrangement may increase with the width of the strip material. That is, the technical aspects disclosed herein can be used with systems including non-horizontal heating channels or systems, such as binder removal workstations. Moreover, non-horizontal heating channels or systems can be used to manufacture the technical aspects disclosed herein, such as unique materials and form factors (e.g., garnet or other material strips or geometries).
[0132] The applicant attempted to use a tilted arrangement to sinter wider strips (e.g., strips wider than 5 mm, specifically, 25 micrometer-thick, 32 mm-wide green strips (containing zirconium oxide-3 mol% Y₂O₃ inorganic particles)). For example... Figure 1As shown, when partially sintered at 1250°C, the resulting partially sintered articles exhibit noticeable and periodic deformation or bubbles along the length of the strip. The height of the deformation is approximately greater than 1 mm and is large enough to hinder the winding of the strip onto a core with a diameter of 3-6 inches. The applicant believes that the bubbles form due to the upward flow of hot air from the inclined support surface beneath the strip during the heated phases of strip processing (e.g., during sintering and binder removal).
[0133] In addition to airflow control, the applicant has determined that controlling the heat distribution within the binder removal station and / or sintering station is important or potentially important for forming high-quality sintered articles. Specifically, the applicant has found that when wide strip materials are heated in roll-to-roll processing (e.g., as described herein), the thermal stresses exposed to the strip material (particularly during sintering) should be precisely controlled to limit deformation or breakage; otherwise, at least for at least some of the materials and / or forms disclosed herein (e.g., thin and wide strips of at least some inorganic materials), such deformation or breakage may occur as the strip material shrinks / densifies during sintering. Figure 2 The example shown illustrates a ceramic strip (specifically, an alumina strip) that includes the section where the strip transitions from unsintered to sintered material, utilizing a steep temperature increase within a high-temperature sintering zone. Figure 2 As shown, when the strip experiences a rapid temperature increase in the sintering zone, this steep temperature increase causes or may cause deformation or cross-web shape due to the stress within the strip material. That is, in other embodiments, for example, for different materials (e.g., lithium garnet), a steep temperature increase may be advantageous, for example, by reducing exposure to oxidation or impurities, and deformation can be controlled by other factors (e.g., airflow control and a narrower strip width).
[0134] Therefore, as shown and described below, the applicant has determined that by employing a sintering furnace with independently controlled heating zones and / or multiple independently controlled sintering furnaces, wide and long strip material segments can be sintered at high process yields without significant deformation and / or breakage. Similarly, the binder removal furnace and sintering furnace are designed and positioned relative to each other to limit the thermal shock (e.g., exposure to sharp temperature gradients) exposed to the strip when transitioning between different heating zones within the system described herein.
[0135] After sintering, a wide sintered strip is wound, or a wide sintered strip can be wound onto a take-up reel, to form a roll of sintered strip material. In a contemplated embodiment, the roll is cylindrical or any other shape, for example, when wound around a non-circular geometry (e.g., elliptical, triangular with rounded corners, etc.). Because a high-quality (e.g., low-deformation) strip is formed by the system described herein, in at least some embodiments, the strip can be wound into a roll in a manner that allows for convenient and efficient use of the sintered strip roll in subsequent manufacturing processes (e.g., as a substrate in downstream roll-to-roll manufacturing processes). The applicant has found that the high level of consistency in width, length, thickness, shape, and / or flatness and / or other properties (purity, strength, impermeability, dielectric properties) of the strips or other articles produced by the system described herein enables the winding of the strip onto a take-up reel. Conversely, strips with high levels of deformation or irregularity tend to, or may tend to, break or otherwise form deformed and inconsistent strip rolls, and may not be suitable for being taken onto a reel to form a sintered strip. That is, some anticipated non-horizontal sintering systems (particularly those employing the techniques disclosed herein) can achieve undistorted strips (e.g., if airflow is controlled, the strip is sufficiently thin and stretched, and the sintering rate and temperature are controlled, as described herein).
[0136] Finally, conventional sintered products are formed in the system in which discrete unsintered sheets or green strips are placed on a surface (called a positioning plate) and placed in a furnace where organic binders are burned off and inorganic particles are sintered. The applicant has identified that roll-to-roll forming of sintered products offers many advantages not available with discrete conventional sintered products. For example, wide winding rolls can form sintered products at high throughput rates (e.g., 6 inches per minute or greater). Furthermore, the system / process discussed herein forms wide and thin sinters (e.g., thin ceramics and / or sintered products), enabling the use of sintered products as substrates for the formation of small and low-cost devices (e.g., semiconductor devices, batteries, etc.). Similarly, providing sintered material rolls enables the use of sintered material as input substrate rolls for high-throughput downstream manufacturing processes, further enabling the formation of downstream products at high speed and / or low cost using the sintered products discussed herein.
[0137] System Overview
[0138] See Figure 3This illustrates a system 10 for producing sintered strip articles according to an exemplary embodiment. Generally, green strip material is supplied to system 10 at the input side (separation system 12), and the green strip material moves through system 10 generally in the processing direction 14. In separation system 12, a source 16 of continuous strip material 18 ('continuous' refers to a long length, such as 300 cm or longer as disclosed herein, which may be provided in rolls or strips) is provided and fed into the downstream portion of system 10.
[0139] Generally, the continuous strip material 18 comprises a layer of green strip material 20, which includes particles of sinterable inorganic material bonded to an organic binder (e.g., polyvinyl butyral, dibutyl phthalate, alkyl polycarbonate, acrylic polymer, polyester, silicone, etc.). The green strip material 20 of the continuous strip material 18 is or may be supported on a carrier mesh or backing layer 22. As described in more detail below, in specific embodiments, system 10 is configured to form a long, wide, and / or thin sintered article, and in such embodiments, the green strip material 20 entering system 10 is also relatively long, wide, and / or thin. For example, in specific embodiments, the width of the green strip material 20 is greater than 5 mm, greater than 10 mm, greater than 40 mm, or greater than 125 mm. In specific embodiments, the length of the green strip material 20 is greater than 10 meters (m), specifically greater than 30 m, and more specifically greater than 60 m. In specific embodiments, the thickness of the green strip material 20 is from 3 micrometers to 1 millimeter. Furthermore, the porosity of the input green strip material 20 is greater than the porosity of the sintered product produced by system 10. In other contemplated embodiments, the width of the green strip material 20 may be less than 5 mm, for example, at least 0.5 mm, at least 1 mm, at least 2.5 mm, or less than 0.5 mm in some such embodiments. Similarly, the strip may have other thicknesses and / or lengths and / or porosities. In some embodiments, the strip material 20 may have a non-rectangular cross-section perpendicular to its length, such as circular, elliptical, parallelogram, rhomboid, etc., wherein, perhaps intuitively, the width in such embodiments refers to the maximum cross-sectional dimension perpendicular to the length, while the thickness is the minimum cross-sectional dimension perpendicular to the length.
[0140] The separation system 12 includes a carrier mesh removal station 24. At the carrier mesh removal station 24, carrier mesh 22 is separated from the green strip material 20, and the removed carrier mesh 22 is wound onto, or can be wound onto, a take-up reel 26. Generally, the carrier mesh removal station 24 includes a tension isolator 28 (which may include a vacuum drum) and a stripper 30 that has removed the carrier mesh 22 in a manner that does not cause twisting or compression of the green strip material 20 and isolates the green strip 20 from the tension within the carrier mesh 22 generated by the take-up reel 26. After separation from the carrier mesh 22, the green strip 20 is, or may be, a self-supporting green strip containing particles of inorganic material supported by an organic binder material, but does not contain carrier mesh or other support structures to hold the strip material together during downstream processing through system 10.
[0141] The self-supporting green strip 20 moves into, or can move into, the ultra-low tension control system 32. Generally, the self-supporting green strip 20 is a relatively fragile structure that is pulled through the system 10 by the movement of various spools, rolls, rollers, etc. This pulling action applies tension to the self-supporting green strip 20. The applicant has found that a uniform, low level of tension applied to the self-supporting green strip 20 (e.g., g level, 0.1 g to less than 1 kg; at least 1 g, at least 5 g, and / or no more than 100 g, depending on the strip size and binder strength) is advantageous or potentially advantageous because it improves various properties of the final sintered product, such as shape and flatness in width. However, due to the fragile nature of the self-supporting green strip 20 (which becomes even more fragile after binder removal, as described in more detail below), precise control of the low level of tension ensures that sufficient tension is provided to the strip 20 to limit binder removal / deformation during the sintering process, while also limiting the maximum tension to ensure that the strip 20 does not break. In other intended implementations, in addition to tension due to the weight of the strip itself, greater tension or zero tension is applied, for example, to a stronger strip.
[0142] In one or more embodiments, such as Figure 3 As shown, the tension control system 32 includes an ultra-low tension floating roller 33, which is a lightweight, low-inertia carbon fiber roller. The ultra-low tension floating roller 33 may include air bearings to promote low-friction rotation of the carbon fiber roller of the tension floating roller 33. In other embodiments, a free loop of material or a vacuum box may be used to provide a consistent g-level tension to the strip 20.
[0143] Following the tension control system 32, the self-supporting green strip 20 moves into the binder removal station 34. Generally, the binder removal station 34 includes a plurality of heating elements that transfer heat to channels formed within the station 34. The heat within the binder removal station 34 causes a chemical change and / or removal of at least a portion of the organic binder material of the self-supporting green strip 20, thereby allowing the unbonded strip 36 to leave the binder removal station 34. Generally, the unbonded strip 36 comprises particles of inorganic material with little or no organic binder residue. The applicant has found that even in the absence of organic binder, the unbonded strip 36 retains itself together in a manner that allows it to move into the sintering station 38, for example, through tension control, airflow control, proximity of the binder removal station 34 to the sintering station 38, temperature control between them, and the orientation and alignment of the strip with the stations 34 and 38. Figure 3 As shown.
[0144] Overall, the arrangement and control of the adhesive removal station 34 provides low deformation as the strip 20 passes through it. Furthermore, the adhesive removal station 34 may include a heating element, which enables the removal of volatile organic compounds without applying excessive heat too quickly, which could otherwise ignite the organic adhesive compounds. Ignition can also be controlled by airflow.
[0145] Furthermore, the binder removal station 34 is positioned relative to the sintering station 38 in such a manner that the thermal shock or temperature gradient exposed to the unbonded strip 36 during its movement from the binder removal station 34 into the sintering station 38 is low (e.g., spaced apart, but with linearly aligned paths and correspondingly aligned openings and / or close to each other, e.g., within 1 m, within 10 cm, within 2 cm, and / or closer). The applicant has found that, due to the fragile nature of the unbonded strip 36, limiting the thermal shock experienced by the strip 36 between stations 34 and 38 also provides for the production of flat, consistent, and / or unwarped sintered strips by limiting / eliminating deformation that would otherwise occur due to the temperature gradient experienced between stations 34 and 38.
[0146] In various embodiments, the temperature within workstation 34 is precisely controlled to achieve the desired properties of the strip 36 exiting workstation 34. In various embodiments, the temperature within workstation 34 is between 200 degrees Celsius (or about 200 degrees Celsius) and 500 degrees Celsius (or about 500 degrees Celsius), and the temperature distribution provided along its length by heating workstation 34 results in little or no binder material remaining in the strip material exiting binder removal workstation 34. Furthermore, in some embodiments, some sintering of the inorganic material particles (e.g., shrinkage, increased density, decreased porosity, etc.) may occur during the traversal of binder removal workstation 34.
[0147] After the binder is removed in workstation 34, the unbonded strip 36 moves into sintering workstation 38. Generally, sintering workstation 38 includes one or more heating elements (see, for example, a more detailed discussion below regarding heating elements and their types) that heat sintering workstation 38 to temperatures above 500 °C (e.g., 500 °C (or about 500 °C) to 3200 °C (or about 3200 °C, for example, 3200 °C ± 10%)), resulting in the sintering of the inorganic material particles of the unbonded strip 36. Typically, during sintering, the porosity of the inorganic material decreases. This decrease in porosity may also lead to shrinkage of the strip material (e.g., reduction in width, thickness, length, etc.) when the material is sintered (e.g., in sintering workstation 38). For some materials, during sintering, the elastic modulus increases, the strength increases, and the shape of the pores changes, without a significant decrease in porosity or significant shrinkage. In some embodiments, the sintering workstation 38 transforms the strip 38 into a partially but not fully sintered light yellow material.
[0148] The applicant discovered that the unbonded strip 36 is prone to deformation or breakage as it passes through the sintering station 38, likely due to various forces acting on it during sintering. Specifically, as described above, the applicant found that forces resulting from turbulent airflow through the sintering station 38 are a significant source of deformation, and further found that internal stresses within the strip 36 during sintering are another potential source of significant deformation. Based on these findings, the applicant has arranged and constructed the sintering station 38 in various ways to limit these forces and produce sintered articles with an acceptablely low level of deformation.
[0149] Specifically, such as Figure 3As shown, the sintering workstation 38 is arranged in a substantially horizontal configuration, such that the unbonded strip 36 passes through the workstation 38 in a substantially horizontal orientation. The applicant has found that by maintaining the substantially horizontal arrangement of the sintering workstation 38, vortex airflow can be reduced or minimized, which in turn results in the sintered strip material formed at the output of the sintering workstation 38 having a low level of deformation, a low level of cross-tape shape, and / or flatness. In various embodiments, the applicant believes that for various wide strip materials, low turbulence and therefore low deformation can be achieved by maintaining the angle between the processing path of the strip material and the horizontal plane at less than 10 degrees, specifically less than 3 degrees, and even more specifically less than 1 degree. In some embodiments, the strip can move on a generally horizontal arched path, as described below. In other embodiments, the path through the sintering workstation 38 can be inclined at more than 10 degrees relative to the horizontal, as described above.
[0150] like Figure 3 As shown in the embodiment, the adhesive removal station 34 is also positioned substantially horizontally, so that the turbulent airflow does not cause deformation, cracking, or the like during heating of the adhesive removal station 34. Similarly, the adhesive removal station 34 is aligned vertically with the sintering station 38 (i.e., the corresponding openings are aligned and face each other), so that the unbonded strip 36 remains in a horizontal position when the strip 36 moves from the adhesive removal station 34 to the sintering station 38.
[0151] Furthermore, the applicant discovered that if the unbonded strip 36 is exposed to a temperature distribution with abrupt temperature increases / decreases along the length of the sintering station 38, high levels of stress are generated or potentially generated in the strip 36, which in turn leads to or may lead to deformation or breakage of the strip 36 during the sintering process. Additionally, the applicant found that as the width of the strip 36 increases, the sintering stress increases the risk of deformation. Therefore, based on these findings, the applicant determined that by employing a sintering station 38 with multiple independently controllable heating elements (and potentially multiple sintering furnaces), a temperature distribution along the length of the sintering station 38 can be generated that keeps the stress in the strip 36 below the threshold that the applicant found that tends to cause deformation or breakage based on specific strip configurations.
[0152] After passing through sintering station 38, the partially or fully sintered strip material 40 leaves sintering station 38 and enters output-side take-up system 42. The sintered strip material 40 is wound onto take-up reel 44. Intermediate layer support material 46 is unloaded from reel 48. Support material 46 is wound onto take-up reel 44 such that one layer of support material 46 is located, or may be located, between each layer of sintered strip material 40 on take-up reel 44 or between at least some layers of sintered strip material 40. This arrangement forms a roller or spool of supported sintered strip material 50. In general, support material 46 is a flexible, high-friction material, which enables the sintered strip material 40 to be secured to take-up reel 44 with low winding tension. The flexibility of support material 46 can compensate for any cross-web shape that may exist in the strip 40 (sintered strip material 40). The support material 40 also increases friction between adjacent layers of the strip 40 (sintered strip material 40) on the reel 44, which limits the slippage / impact of the strip 40 (sintered strip material 40) from the reel 44. The applicant believes that without the support material 46, the sintered strip material 40 tends to slip off at least partially from the reel 50 (e.g., impact) because the higher modulus of the sintered strip 40 (sintered strip material 40) limits its ability to stretch under winding tension, which in turn tends to lead to or may lead to poor roll integrity.
[0153] As discussed herein, system 10 is configured to form sintered strip material 40, which, regardless of the width and / or length of the sintered article, exhibits low levels of deformation, low risk of breakage, and consistent properties along its length. The applicant has found that, particularly as the width of the strip increases, the risk of deformation and breakage of the strip may increase at various stages of system 10. For example, in specific embodiments, the sintered strip 40 (sintered strip material 40) has a width greater than 5 mm, greater than 10 mm, greater than 40 mm, or greater than 125 mm, and regardless of the width of the strip material, the various arrangements of system 10 discussed herein limit the risk of deformation or breakage. In other embodiments, the sintered strip has a width less than 5 mm and / or at least 0.5 mm, for example, at least 1 mm, for example, at least 2 mm.
[0154] Furthermore, the various material handling and heating mechanisms of System 10 enable the formation of sintered strips 40 (sintered strip material 40) with high yield. In specific embodiments, it is believed that the production speed of sintered strips achieved by the roll-to-roll processing of System 10 is significantly faster than other sintering processes (e.g., tunnel kiln processing, at least in some cases, e.g., conventional tunnel kiln processing). In specific embodiments, System 10 is configured to produce sintered strips 40 at rates of at least 6 inches per minute, at least 8 inches per minute, at least 19 inches per minute, at least 29 inches per minute, and at least 59 inches per minute. In other embodiments, system 10 is configured to produce sintered strips 40 at rates of at least 3 inches per minute (ipm) for green strips 20 with a width greater than 50 mm; at least 5 inches per minute (ipm) for green strips 20 with a width of 35 mm to 50 mm; at least 9 inches per minute (ipm) for green strips 20 with a width of 15 mm to 35 mm; and at least 10 inches per minute (ipm) for green strips 20 with a width of 5 mm to 15 mm. In other embodiments, system 10 is configured to produce sintered strips 40 at rates of at least 1 inch per minute (ipm) for green strips 20 with a width greater than 50 mm; at least 1.5 inches per minute (ipm) for green strips 20 with a width of 35 mm to 50 mm; at least 2 inches per minute (ipm) for green strips 20 with a width of 15 mm to 35 mm; and at least 3 inches per minute (ipm) for green strips 20 with a width of 5 mm to 15 mm.
[0155] Support wire mesh removal workstation
[0156] Embodiments of forming the sintered articles described herein include applying uniform mesh tension to the green strip material before and after sintering. Separation systems according to one or more embodiments of this disclosure are designed to apply such uniform mesh tension and uniform speed to the green strip material as it separates from the support mesh. Therefore, as disclosed herein, removing the support mesh achieves shape consistency in the green strip material, reduces or eliminates necking or shrinkage of the green strip, and reduces or eliminates the imprinting of features on the surface of the green strip by the equipment, features that would otherwise be present in the sintered strip. That is, the techniques disclosed herein can be used to produce new sintered strips as disclosed herein without a support mesh removal station, wherein the strip may have characteristics attributable to the absence of a support mesh removal station, such as thickness variations, repetitive imprinted surface features, etc.
[0157] As described above, system 10 includes a support mesh removal workstation generally located on the input side of system 10. One aspect of the support mesh removal workstation includes a separation system 12. See also Figure 4The separation system 12 is configured to separate the green strip material 20 from the carrier mesh 22, allowing the green strip material 20 to be processed downstream. In one or more embodiments, a source 16 of the continuous strip material 18 to be separated is provided. Figure 5 As shown more clearly, the continuous strip material 18 includes green strip material 20 supported on the carrier mesh 22. Figure 4 In this embodiment, a source 16 is provided in the form of a spool, which unwinds the continuous strip material 18 to a carrier mesh removal station 24 (including a tension isolator 28 and a stripper 30). In one or more embodiments, the source 16 may include a belt or other form for feeding the continuous strip material. In other contemplated embodiments, the source of the green strip material may be another station on the production line that continuously produces or can continuously produce green material, forming green strips and conditioning them for subsequent processing in the system disclosed herein. Other contemplated embodiments may use green strip material separated by organic material, which is removed by, for example, the adhesive removal station disclosed herein or by any other means.
[0158] According to an exemplary embodiment, the green strip material 20 comprises particles of inorganic material (as described herein), which are sinterable and bonded together with an organic binder. The carrier web 22 may comprise a polymer, paper, or a combination of polymer and paper materials. In some embodiments, the amount of polymer contained in the green strip material is less than the polymer content of the carrier web 22, wherein the polymer content is expressed as a volume percentage of the respective material. According to an exemplary embodiment, the green strip material 20 and the carrier web 22 each have: a respective thickness (t), defined as the distance between a first primary surface and a second primary surface; a respective thickness (W), defined as a first dimension perpendicular to the thickness of one of the first or second surfaces; and a respective length (L), defined as a second dimension perpendicular to both the thickness and width of one of the first or second surfaces, for example, for a green strip having a continuous cross-sectional geometry that is rectangular or elliptical (e.g., where edges may be removed after sintering to form straight sides). In other contemplated embodiments, the sinterable inorganic material strips may be held together by an inorganic binder, for example, after processing in system 10, where the inorganic binder becomes part of the sintered strip. For example, as disclosed herein, in other contemplated embodiments, strips of inorganic material can be held together by causing the inorganic material to self-bond, for example, partially sintered pale yellow strips instead of green strips.
[0159] As will be described herein, according to exemplary embodiments, the carrier mesh 22 provides, or can provide, a contacting main surface for conveying continuous strip material through the separation system 12, and more specifically, conveying the continuous strip material through the carrier mesh removal station 24. In other words, in at least some of these embodiments, it is primarily the carrier mesh 22 that makes contact, such that the green strip material 20 is substantially not in contact, and therefore substantially free of defects or imperfections arising from or potentially arising from contact, such as repeating surface features that may be detectable in the final sintered product due to the surface imprinting of a wheel or roller onto the green strip material. Other embodiments may include such defects or imperfections, for example, when the technical aspects disclosed herein do not include the carrier mesh removal station 24.
[0160] When source 16 is a spool, the continuous strip material has a first tension (which is low, as will be further described herein) and a tendency to unwind at a relatively high speed, even when the continuous material is held at a constant low tension. The separation system 12 acts as a brake, or can act as a brake, to reduce or otherwise control or limit the speed at which the continuous strip material unwinds from source 16.
[0161] According to at least some of these exemplary embodiments, the carrier mesh removal workstation 24 includes a tension isolator 28 (located close to and downstream of source 16) and a stripper 30 (located downstream of tension isolator 28). Tension isolator 28 and stripper 30 separate the carrier mesh 22 from the green strip material 20 without damaging the green strip material. Specifically, tension isolator 28 is designed and used to clamp the carrier mesh and control the pace of the continuous strip material through the separation system. In one or more embodiments, after the carrier mesh 22 has been separated from the green strip material 20, the collection rate of the carrier mesh 22 after separation is controlled to maintain a constant tension in the carrier mesh 22 and consequently, a constant tension in the continuous green strip material 20. In one or more embodiments, tension isolator 28 isolates the carrier mesh 22 separated from the green strip material 20 by mass from the input green strip material 20 from source 16. Without tension isolator 28, any or some inconsistencies in the winding quality of the continuous strip material (i.e., loose winding, which would lead to unwinding or cinching during feeding to stripper 30) would cause variations in the tension and speed of stripper 30.
[0162] According to exemplary embodiments, continuous strip material 18 is fed into tension isolator 28 with a first tension, and one or more embodiments of the tension isolator have a structure or are configured to apply a second tension greater than the first tension of the continuous strip material 18 to carrier mesh 22 when the continuous strip material 18 is conveyed to stripper 30. In some embodiments, the second tension (i.e., tensile force) is at least 20% greater than the first tension, and / or at least 25 millinewtons (mN) greater than the first tension, for example, at least 100 mN greater, for example, at least 200 mN greater. According to some such embodiments, the second tension is applied to carrier mesh 22, but not, or at least substantially not, to the green strip material. In one or more embodiments, the green strip material 20 maintains the first tension as the continuous strip material moves along tension isolator 28. In one or more embodiments, as the continuous strip material moves along the tension isolator 28, the green strip material contains no or no tension, or contains no or no tension exceeding its own weight, or substantially no or no tension exceeding its own weight, for example, less than 1 Newton (N) exceeding its own weight. Therefore, the tension isolator 28 creates a first tension zone 17 between the tension isolator 28 and the source 16, and a second tension zone 19 between the tension isolator 28 and the stripper 30. The tension applied to the carrier mesh 22 in the first tension zone 17 is less than the tension applied to the carrier mesh 22 in the second tension zone 19. In one or more embodiments, the tension (i.e., tensile stress) applied to the carrier mesh 22 in the second tension zone 19 is about 2.5 pounds per (linear) inch (PLI) or less. For example, in one or more embodiments, the tension applied to the carrier mesh 22 is about 2.4 PLI or less, about 2.3 PLI or less, about 2.2 PLI or less, about 2.1 PLI or less, about 2 PLI or less, about 1.8 PLI or less, about 1.6 PLI or less, about 1.5 PLI or less, about 1.4 PLI or less, about 1.2 PLI or less, or about 1 PLI or less. In one or more embodiments, the first tension is equal to or less than about 50% of the second tension (e.g., about 45% or less, about 40% or less, about 35% or less, about 30% or less, or about 25% or less). In some embodiments, the tension (i.e., tensile force) applied to the carrier mesh 22 in the second tension zone 19 is at least 20% greater than the tension applied to the carrier mesh 22 in the first tension zone 17, and / or at least 25 millinewtons (mN) greater, for example, at least 100 mN greater, for example, at least 200 mN greater. In one or more embodiments, in addition to the tension applied to the green strip material by applying tension on the carrier mesh 28, an additional (nominal) tension is applied to the green strip material.In such embodiments, the tension applied to the carrier mesh can cause the carrier mesh to stretch, which in turn generates some tension in the green strip material, for example, in which the carrier mesh bears the majority of the tension.
[0163] In one or more embodiments, the tension applied to the carrier mesh 22 by the tension isolator 28 is greater than the tension applied to the green strip material 20. In some embodiments, the tension applied to the carrier mesh by the tension isolator is equal to or approximately twice the tension applied to the green strip material as the continuous strip material moves from the source 16 to the stripper 30. In some embodiments, the tension applied to the carrier mesh 22 by the tension isolator 28 is at least 20% greater than the tension applied to the green strip material 20, and / or at least 25 millinewtons (mN), for example, at least 100 mN, for example, at least 200 mN. It may be intuitive that tension as used herein generally refers to the stretching of the material along its length or axial direction, and when units of force are given herein, tension refers to tensile force, and when units of stress are given herein, tension refers to tensile stress, and / or tension as used herein may be given in other units and refers to other relevant parameters, such as pounds per linear inch or metric equivalents.
[0164] exist Figure 4 In the illustrated embodiment, the tension isolator 28 may include a vacuum drum 25. For example... Figure 6 As shown, in one or more embodiments, the vacuum drum 25 rotates, moving the continuous strip material via a drive motor input 27, which is connected to the vacuum drum via a bearing housing 29. Figure 7As shown, the vacuum drum may include an outer surface comprising a plurality of vacuum holes 7 arranged in a uniform distribution. The vacuum holes 7 may be formed along a plurality of axial grooves 8 and / or radial grooves that intersect each other at the vacuum holes 7. A vacuum is applied to the vacuum drum 25 by a vacuum source (e.g., a vacuum blower), which grips the carrier mesh 22 through the vacuum holes 7, thereby facilitating tension of the carrier mesh, as described herein. In one or more embodiments, the distribution of the vacuum holes 7 and the construction of the vacuum drum (including the diameter and vacuum force employed) apply or help apply uniform tension to the carrier mesh along its width. Through this action and construction, the vacuum drum controls the speed of the carrier mesh (and the continuous strip material) as it moves through the separation system 12. In one or more embodiments, a tension isolator pulls the continuous strip material from the source along a first tension zone 17. Any or some inconsistencies in the transfer of the green strip material from the source 16 to the stripper 30 (e.g., loose winding that results in clamping during transfer from the source to the stripper) have no effect or may not affect the separation process. In addition to friction and normal forces proportional to tension, the vacuum drum 25 provides adhesive or attractive forces between the strip material (e.g., carrier mesh) and the vacuum drum 25, thereby increasing adhesive or attractive forces without increasing tension in the strip material. At least due to this advantage, the applicant believes that using a vacuum drum to control the adhesive or attractive forces between the strip material and the rollers (i.e., the vacuum drum) during the step of separating the green strip from the carrier mesh is a unique and effective process for protecting and controlling the shape of potentially particularly fragile green strips. That is, aspects of the technology described herein can be used to produce new sintered products, for example, strips that do exhibit separation marks (e.g., repetitive defects from the rollers, variations in strip thickness, shorter strip lengths, etc.) without using the vacuum drum disclosed herein.
[0165] In one or more embodiments, as the continuous strip material is conveyed to the stripper 30, the tension isolator 28 increases the tension in the continuous strip material (more specifically, in the carrier mesh or primarily in the carrier mesh) along the second tension zone 19. Figure 4 In the illustrated embodiment, the separation system 12 includes a load controller 21 to maintain tension on the carrier mesh. In one or more embodiments, the load controller 21 is also used to regulate the speed of the take-up reel 26 relative to the tension isolator 28.
[0166] In one or more embodiments, the stripper 30 is arranged downstream of the tension isolator 28 and guides the carrier web material 22 in a rewinding direction A and the green strip material 20 in a downstream processing direction B different from the rewinding direction A, such as... Figure 8As shown. In one or more embodiments, the angle C formed by the rewinding direction A and the downstream processing direction is greater than about 90 degrees (e.g., 95 degrees or more, 100 degrees or more, 110 degrees or more, or about 120 degrees or more).
[0167] In one or more embodiments, the peeler 30 includes a sharp blade or edge to create a separation line in the green strip material, for example, located at or near the vertex of corner C, shown as tip 31. In one or more embodiments, the sharp blade or edge creates a separation line in the green strip material, but not in the carrier mesh, just in front of or near tip 31, such as... Figure 8 As shown. In one or more embodiments, the radius of the tip is about 0.05 inches or less (e.g., about 0.04 inches or less, about 0.035 inches or less, about 0.03125 inches or less, about 0.03 inches or less, or about 0.025 inches or less).
[0168] As the continuous strip material passes over the tip 31, the tip 31 separates the carrier web 22 from the green strip material 20. In one or more embodiments, the tip 31 separates the carrier web 22 from the green strip material 20, and then guides the carrier web in a rewinding direction A and the green strip material in a downstream processing direction B. In one or more embodiments, the tip 31 simultaneously separates the carrier web 22 from the green strip material 20 and guides the carrier web in a rewinding direction A and the green strip material in a downstream processing direction B.
[0169] like Figure 4 As shown, the separation system 12 includes a take-up reel 26 for collecting the separated carrier web 22. In the illustrated embodiment, an optional idler roller 23 may be used to further control and maintain the tension in the carrier web 22. In one or more embodiments, as more continuous strip material is conveyed through the separation system, a sensor 15 may also be used to control and maintain the tension in the carrier web, with the diameter of the source 16 decreasing and the diameter of the take-up reel 26 increasing.
[0170] Another aspect of the support mesh removal workstation pertains to a method for separating two materials (e.g., green strip material and carrier mesh). In one or more embodiments, the method includes: feeding a continuous strip material 18 into a tension isolator 28; applying tension to the carrier mesh 22 using the tension isolator 28, which is greater than the tension applied to the green strip material 20; and guiding the carrier mesh to move in a rewinding direction and guiding the green strip material in a downstream processing direction different from the rewinding direction, as described herein. In one or more embodiments, the method includes separating the carrier mesh from the green strip material, and then guiding the carrier mesh in a rewinding direction and guiding the green strip material in a downstream processing direction. In one or more embodiments, the method includes separating the carrier mesh from the green strip material while simultaneously guiding the carrier mesh in a rewinding direction and guiding the green strip material in a downstream processing direction. As taught above, this method is implemented such that the carrier mesh contacts the vacuum drum. In other embodiments, the strip material may have carrier mesh on both sides of the strip, as well as elements of the workstation that can be repeatedly separated and used to remove the two carrier meshes.
[0171] In one or more embodiments, the method includes applying no tension, substantially no tension, or very little tension (as disclosed above) to the green strip material. In one or more exemplary embodiments, the method includes applying no or substantially no tension, or very little tension, to the green strip material as the continuous strip material moves along a first tension zone 17 from source 16 to tension isolator 28. In one or more exemplary embodiments, the method includes applying no or substantially no tension, or very little tension, to the green strip material as the continuous strip material moves along a second tension zone 19 from tension isolator 28 to stripper 30. In one or more exemplary embodiments, the method includes applying no or substantially no tension, or very little tension, to the green strip material 20 as the continuous strip 18 moves (along the first tension zone) from source 16 to tension isolator 28 and (along the second tension zone) to stripper 30. In one or more embodiments, the method includes applying tension to the carrier mesh 22, at least twice the tension applied to the green strip material 20 (at any point along the separation system 12). Selecting a carrier mesh with low elasticity can help the carrier mesh bear most of the bulk of tension applied to the strip material.
[0172] In one or more embodiments, the method includes applying no additional tension to the green strip material other than the tension applied to the green strip material by applying tension on the carrier mesh 28. In such embodiments, since such tension applied to the carrier mesh may cause the carrier mesh to stretch, this in turn creates some tension on the green strip material. In one or more exemplary embodiments, the method includes applying no additional tension to the green strip material as the continuous strip material moves along the first tension zone 17 from the source 16 to the tension isolator 28. In one or more exemplary embodiments, the method includes applying no additional tension to the green strip material as the continuous strip material moves along the second tension zone 19 from the tension isolator 28 to the peeler 30. In one or more exemplary embodiments, the method includes applying no additional tension to the green strip material 20 as the continuous strip 18 moves (along the first tension zone) from the source 16 to the tension isolator 28 and (along the second tension zone) to the peeler 30.
[0173] In one or more embodiments, a method for separating two materials (i.e., green strip material and carrier mesh) includes: feeding continuous strip material into a tension isolator and applying a first tension to the carrier mesh; applying a second tension greater than the first tension to the carrier mesh; and guiding the carrier mesh to move in a rewinding direction, and guiding the green strip material in a downstream processing direction different from the rewinding direction. In one or more embodiments, applying the first tension includes applying no tension or almost no tension, as disclosed herein. In one or more exemplary embodiments, applying the first tension includes applying no or almost no tension to the carrier mesh as the continuous strip material moves along a first tension zone from source 16 to tension isolator 28. In one or more embodiments, the second tension is about 2.5 PLI or less. For example, in one or more embodiments, the tension applied to the carrier mesh 22 is about 2.4 PLI or less, about 2.3 PLI or less, about 2.2 PLI or less, about 2.1 PLI or less, about 2 PLI or less, about 1.8 PLI or less, about 1.6 PLI or less, about 1.5 PLI or less, about 1.4 PLI or less, about 1.2 PLI or less, or about 1 PLI or less. In one or more embodiments, the first tension is equal to or less than about 50% of the second tension (e.g., about 45% or less, about 40% or less, about 35% or less, about 30% or less, or about 25% or less).
[0174] In one or more embodiments, the method includes: after separating the green strip material from the carrier mesh 22, at least partially sintering it (as described in more detail below regarding sintering workstations). In one or more embodiments, the method includes: after separating the carrier mesh 22 from the green strip material 20, winding the carrier mesh 22 onto a take-up reel 26. In one or more embodiments, the method includes: continuously maintaining tension on the carrier mesh 22 along a second tension zone until the carrier mesh is wound onto the take-up reel.
[0175] Adhesive removal workstation
[0176] As mentioned above Figure 3 The system 10 includes a heating workstation configured to remove binder material from the green strip 20. In at least some embodiments, the heating workstation is actively heated and independent of the sintering workstation. In other embodiments, for example, for the firing of the light yellow strips disclosed herein, a heating workstation may not be required. The applicant believes that actively heating the workstation intended for binder removal with its own controllable heat source, independent of the heaters within the sintering furnace, enables better control over the binder removal process and reduces the likelihood of combustion of volatile substances in the binder of the green strip. This is particularly advantageous for wide green strips (e.g., at least 5 mm, at least 10 mm, at least 30 mm, at least 50 mm). Other embodiments include the passively heated binder removal workstation disclosed herein, wherein the workstation uses heat from the sintering furnace and is adjacent to the sintering furnace.
[0177] According to exemplary embodiments, such as Figure 3 As shown, the adhesive removal station 34 receives the green strip 20 from the separation station 12, and then the green strip 20 proceeds through the adhesive removal station 34. See now. Figure 9 A more detailed diagram of the adhesive removal workstation 34 of system 10 is shown and described.
[0178] As described above, the green strip 20 comprises particles of inorganic material bonded by an adhesive (e.g., an organic adhesive) as disclosed herein. An adhesive removal station 34 receives the green strip 20 and, by causing a chemical change in the adhesive and / or removing the adhesive from the green strip 20, leaves particles of inorganic material to form a self-supporting unbonded strip 36, thereby preparing the green strip 20 for sintering. The self-supporting unbonded strip 36 can be moved in processing direction 14 into a sintering station 38, as discussed in more detail below. According to an exemplary embodiment, in an instant (i.e., momentarily), the green strip 20 simultaneously extends toward the station 34, extends into the station 34, extends through the station 34, extends within the station 34, extends near the station 34, and / or extends away from the station 34. Therefore, it will be understood that as the strip material passes through the adhesive removal station 34, the strip material processed in the system 10 simultaneously comprises the green strip 20 continuously connected to the unbonded strip 36.
[0179] According to an exemplary embodiment, the binder of the green strip 20 may be a polymeric binder, and the binder may be chemically changed and / or removed from the green strip 20 by heating it to burn or char it. According to an exemplary embodiment, the binder removal station 34 chars or burns at least a majority of the organic binder from the first portion of the green strip 20 without causing sintering of the inorganic material particles. This can be measured by weighing the green strip before binder removal by station 34 and the inorganic material before the formation of the green strip, then weighing the unbonded strip 36 after the operation of the binder removal station 34, and comparing the differences. If binder residues (e.g., carbon) remain, the applicant believes that subsequent sintering at higher temperatures can generally remove those residues. In other contemplated embodiments, the binder may be removed chemically, for example, by selecting the material to which it is formed, such that it reacts chemically with other materials (e.g., catalysts, gases) passed to the binder removal station before sintering. In other anticipated implementations, the binder may be evaporated or degassed from the green strip 20 at the workstation prior to sintering.
[0180] See still Figure 9According to an exemplary embodiment, the adhesive removal workstation 34 includes an active heater 5120 that, when the green strip 20 comes into contact with the adhesive removal workstation 34, chars or burns at least a majority of the adhesive from the green strip 20 to form a non-bonded strip 36 (e.g., reducing the weight of the non-sintering inorganic material portion of the green strip 20 by more than 50%, such as more than 80%, such as more than 90%, and reducing the overall weight of the green strip 20 by more than 30%, such as more than 50%). The active heater 5120 provides heat to the green strip 20 to burn off the adhesive. In some embodiments, the heater 5120 is an electric heating element or includes an electric heating element (e.g., an induction or resistance heating element). In other embodiments, the heater 5120 is a combustion heating element or includes a combustion heating element (e.g., a gas heating element). In other embodiments, the heater 5120 is a microwave and / or laser or other heating element, or includes a microwave and / or laser or other heating element. Such heating elements can also be used in sintering workstation 38, but to heat to different temperatures, as disclosed herein.
[0181] According to an exemplary embodiment, the active heater 5120 of the binder removal station 34 includes heating zones (e.g., zones 5120A, 5120B, 5120C, 5120D) such that the rate of heat energy received by the green strip 20 increases as it travels through the binder removal station 34. In some embodiments, the rate of heat energy received by the green strip 20 increases non-linearly, for example, initially slowly as the binder decomposes and releases combustible byproducts, and then more rapidly as the potential for flame capture by the green strip 20 decreases. This heating zone scheme, and more specifically, the non-linear scheme, can be particularly useful for the sintering of strips as disclosed herein, where the strip may pass through the production line (e.g., system 10) at a constant rate. According to an exemplary embodiment, in the binder removal station 34, the temperature subjected to the green strip 20 may be at least 200°C, for example at least 250°C, and / or below the sintering temperature of the inorganic particles carried by the green strip 20, for example less than 1200°C (e.g., less than 900°C). In a contemplated embodiment, for at least some of the materials disclosed herein, the binder removal station 34 may sinter the inorganic material of the strip to at least a certain extent, for example, possibly causing individual particles to bond together, which may increase the tensile strength of the strip.
[0182] According to an exemplary embodiment, as the green strip 20 advances through the adhesive removal station 34, the adhesive removal station 34 blows and / or draws gas above and / or below (e.g., above and below) the green strip 20. In some embodiments, the heater 5120 can provide a flow of hot air in exchange for some or all of the heat energy reaching the green strip 20, which may be delivered through a nozzle array, through the walls of the high-pressure chamber, or through a porous wall material. In other embodiments, gas flow is facilitated by a fan or pump adjacent to the adhesive removal station 34, for example, Figure 9 The fan 5122 is shown. A pressurized gas canister can also be used as a source of gas supplied for blowing onto the belt. In some embodiments, the gas is air. In other embodiments, the gas is an inert gas, such as argon.
[0183] In some embodiments, gas is blown and / or drawn onto both the upper and lower sides of the green strip 20, while in other embodiments, gas is guided only on the upper or lower side. In some such embodiments, the green strip 20 is directly supported by a gas bearing and / or a lower surface, and the green strip 20 moves relative to this surface. For example, the green strip 20 may slide along and contact the lower surface (e.g., a surface made of stainless steel). In some embodiments, the gas is heated to a temperature above room temperature (e.g., at least 100°C) before being blown or drawn onto the strip. The applicant has found that this helps prevent thermal shock to the green strip 20, which can affect the properties of the resulting sintered material, such as providing increased strength or flatness due to fewer surface irregularities and stress concentrations.
[0184] Actively blowing or drawing gas (particularly air or oxygen-containing gas) onto the green strip 20 may seem counterintuitive to those skilled in the art, as oxygen could be expected to become fuel and promote flame capture on the strip, potentially causing distortion of the shape of the green strip 20 and / or any other way that compromises the quality of the green strip 20 as it passes through the work station 34. However, the applicant has found that blowing and / or drawing gas (including air in some embodiments) onto the green strip 20 while it is being conveyed through the binder removal work station 34 actually helps prevent flame capture. For example, the applicant has found that the binder is removed and / or charred through the binder removal work station 34 without ignition, but if air is not blown onto the green strip 20, the strip ignites when passing through the work station 34 at the same rate. The applicant anticipates that the risk of fire of the green strip 20 can also be reduced and / or eliminated by: making the green strip 20 move more slowly through the adhesive removal station 34, further spacing the heating zones 5120A, 5120B, 5120C, and 5120D, using flame retardants in the adhesive and increasing ventilation of the adhesive removal station 34, and / or a combination of such techniques.
[0185] While gas can be actively blown and / or drawn onto the green strip 20 and / or onto the unbonded strip 36, the applicant has found that the unbonded strip 36 may be particularly susceptible to damage from vibration and / or out-of-plane bending, depending on how the gas flows. Therefore, in some embodiments, the gas flowing through the binder removal station 34 is and / or includes laminar flow. The airflow may be diffuse and / or may not be directed to the unbonded strip 36. In some embodiments, a gas source or gas actuator (e.g., fan, pump, pressurized supply) delivers gas through the binder removal station 34 at a rate of at least 1 liter per minute, for example through channel 5128 (see...). Figure 10 ).
[0186] According to some embodiments, the green strip 20 travels horizontally rather than vertically through the adhesive removal station 34. This horizontal orientation of the strip can help control the airflow through the adhesive removal station, for example, by reducing the "chimney effect," in which hot gases rise and draw too much air through the adhesive removal station 34, causing the unbonded strip 36 to vibrate. In other anticipated embodiments, air pumps, fans, and ambient air conditions (e.g., high temperatures) counteract and / or control the chimney effect without causing the green strip 20 to be horizontally oriented through the adhesive removal station 34.
[0187] According to an exemplary embodiment, as the green strip 20 travels through workstation 34, the unbonded strip 36 is under positive tension in its length direction. This tension in the green strip 20 helps to secure it in a flat orientation, for example, if the green strip 20 subsequently enters another workstation in the manufacturing system (e.g., sintering workstation 38) for further processing. Without adhesive (e.g., after adhesive removal at workstation 34), the unbonded strip 36 may be weaker than the green strip material 20, for example, having a lower final tensile strength, such as half or less, or even a quarter or less. According to an exemplary embodiment, the tension (i.e., tensile stress) in the unbonded strip 36 in its length direction is less than 500 g / mm. 2 Cross-section. The applicant believes that the green strip 20 is significantly more flexible than the unbonded strip 36, such that the minimum bending radius of the green strip 20 without breaking is less than half that of the unbonded strip 36 (e.g., less than 1 / 4, less than 1 / 8), as measured by ASTM standards (see E290), where the bending radius is the minimum inner radius by which a corresponding portion of the green strip 20 can be bent around a cylinder without breaking.
[0188] In at least some embodiments, after processing by the binder removal station 34, the unbonded strip material 36 moves into the sintering station 38 (discussed in more detail below), which causes the inorganic material of the unbonded strip 36 to be at least partially sintered to form the sintered strip 40. Thus, for continuous processing, in an instant, the green strip 20 is continuously connected to the sintered strip 40 by means of the unbonded strip 36.
[0189] In some such embodiments, the binder removal station 34 is located close to the sintering station 38 such that the distance between them is less than 10 m (e.g., the outlet opening of the binder removal station 34 is close to the inlet opening 106 of the sintering station 38 (see...). Figure 12 The distances between the adhesive removal workstations 34 and 38 are less than 10 mm, 2.5 cm, 5 cm, 10 cm, 25 cm, 100 cm, and 5 m, respectively, thereby reducing the thermal shock that the unbonded strip 36 may experience in the gap between the workstations 34 and 38. This could affect the properties of the resulting sintered material, for example, by providing increased strength or flatness due to smaller surface irregularities and stress concentration points. In the intended embodiment, the adhesive removal workstation 34 is in direct contact with and adjacent to the sintering workstation 38, and / or the adhesive removal workstation 34 and sintering workstation 38 are under a common housing. However, in at least some of these embodiments, an intermediate vent draws away adhesive removal fumes or other byproducts.
[0190] See now Figure 10The adhesive removal workstation 34 includes a wall 5126 defining a channel 5128 having inlet and outlet openings 5130, 5132 at opposite ends of the channel 5128. The channel has a length L between the inlet and outlet openings 5130, 5132, which in some embodiments is at least 5 cm, for example at least 10 cm and / or no more than 10 m. According to an exemplary embodiment, the outlet opening 5132 and / or the inlet opening 5130 is narrow and elongated, for example having a height H and a width W perpendicular to the height H, wherein the height H is less than half the width W, for example less than 1 / 5 of the width W, for example less than 1 / 10 of the width W. In some such embodiments, the height H is less than 5 cm, for example less than 2 cm, for example less than 1 cm and / or at least greater than the thickness of the green strip 20 to be processed therefrom, for example, at least greater than the thickness of the green strip disclosed herein, for example at least greater than 20 μm. The applicant found that the narrow opening improved the performance of the adhesive removal workstation 34 by restricting the circulation of gas (e.g., ambient airflow) at the inlet and outlet openings 5130, 5132. In some embodiments, the channel 5128 is straight, while in other embodiments, the channel is gently arcuate, for example, with a radius of curvature greater than 1 m, wherein the corresponding curvature of the arcuate shape and the strip can help shape or flatten the strip.
[0191] See Figure 11 The processing method of strip 5120 includes the step of advancing the strip through a manufacturing system 5212 (e.g., adhesive removal station 34 or other manufacturing system disclosed herein), wherein, for example, the strip includes a first portion having particles of inorganic material bonded by an adhesive (e.g., green strip 20). The method further includes a step 5214 of preparing the strip for sintering by forming a second portion (e.g., unbonded strip 36) at a station of the manufacturing system, which is achieved by causing a chemical change in the adhesive and / or removing the adhesive from the first portion of the strip, leaving particles of inorganic material, thereby forming the second portion of the strip.
[0192] In some such embodiments, step 5214 of preparing the strip for sintering further includes charring or burning at least a majority of the binder from the first portion of the strip (e.g., as described above), whether or not the inorganic material particles undergo simultaneous sintering. In some embodiments, the workstation of the manufacturing system is a first workstation, and the processing method 5210 further includes the steps of receiving the second portion of the strip at a second workstation 5218, and performing at least partial sintering and / or further sintering 5220 on the inorganic material of the second portion of the strip at the second workstation to form a third portion of the strip.
[0193] In some embodiments, processing method 5210 further includes forward stretching the second portion of the strip as the strip travels forward 5212. In some such embodiments, the forward stretching is such that the tension (i.e., tensile stress) in the second portion of the strip along its length is less than 500 g / mm. 2 Cross-section. In some embodiments, processing method 5210 further includes blowing and / or drawing gas onto the strip while preparing it for sintering 5214. In some embodiments, the strip advancing step 5212 further includes causing the strip to advance horizontally through a workstation, and / or directly supporting the strip via a gas bearing and / or a lower surface, and causing the strip to move relative to the surface and / or relative to the opening 5128.
[0194] Examples of adhesive removal
[0195] The applicant uses a binder removal furnace, similar to binder removal workstation 34, to remove binder from the green strip prior to sintering. In one example, the green strip is a strip of cast zirconia ceramic particles loaded with polymer binder, forming a strip approximately 42 mm wide and 25 μm thick. The green strip is fed at 20 inches per minute through a horizontally configured 6-zone binder removal furnace. The binder removal furnace is set to 325°C inlet to 475°C outlet, with increments of 0 to 25°C for the other four zones. An airflow of approximately 7.5 liters per minute is also provided at temperatures ranging from 0 to 250°C. The airflow is split on both sides of the binder removal furnace. The furnace is 36 inches long and has 18-inch hot zones.
[0196] Sintering workstation
[0197] See Figures 12 to 20 The sintering station 38 is shown and described in more detail. Generally, after the binder material is removed from the green strip 20 in the binder removal station 34, the unbonded strip 36 moves into the sintering station 38.
[0198] In at least one embodiment, sintering station 38 includes sintering furnace 100. Sintering furnace 100 includes an insulating shell 102. Generally, insulating shell 102 includes a plurality of inner walls defining a channel 104 extending through sintering furnace 100 between an inlet (shown as inlet opening 106) and an outlet (shown as outlet opening 108). Adhesive removal station 34 is located adjacent to inlet opening 106, such that green strip material 20 passes through adhesive removal station 34, producing unbonded strip material 36 as described above. Unbonded strip material 36 enters inlet opening 106 and passes through channel 104. While within channel 104, heat generated by heaters (as explained below and above in more detail regarding different types of heating elements) causes unbonded strip 36 to sinter to form sintered strip 40, and sintered strip 40 exits through outlet opening 108 for further processing or collection, such as... Figure 3 As shown. Depending on the temperature distribution exposed to the unbonded strip 36 during sintering, the strip 40 can be fully or partially sintered after leaving the sintering furnace 100. Regardless of whether the strip 40 is partially or fully sintered, due to the sintering occurring within the furnace 100, the porosity of the strip 40 is less than that of the green strip 20. Similarly, in some embodiments, the width of the strip 40 is less than the width of the green strip 20. In some such embodiments and others, the shrinkage of the unbonded strip 36 during sintering can be controlled such that the thickness, width, and / or length of the strip 40 are less than the thickness of the green strip 20.
[0199] from Figure 12 As can be seen, and unlike typical discrete sheets based on sintering systems, the unbonded strip 36 is a continuous length of material that extends completely through the furnace 100. In this arrangement, a single continuous length of unbonded strip 36 extends into inlet 106, through channel 104, and exits at outlet 108. It will be understood that, since the unbonded strip 36 is continuous throughout the furnace 100, its left edge, its right edge, and its centerline (e.g., positioned parallel to the left and right edges and equidistant from them longitudinal lines) also, or may, extend the entire distance through the furnace 100 between inlet 106 and outlet 108. For example, Figure 14The edges (as edges 130 and 132) mentioned above are shown after leaving the sintering furnace 100. This relationship between the continuous strip 36 and the furnace 100 is believed to be unique to the roll-to-roll sintering process described herein and differs from the physical arrangement of tunnel kiln processing for sintering, in which discrete sheets of material move through the furnace supported by positioning plates, with the positioning plates carrying the sheets to be sintered moving through the furnace. For example, in some embodiments, the strip slides along a surface (e.g., lower surface 126) and / or relative to a surface (e.g., lower surface 126) through the channel 104 of the furnace 100, and is not carried on a locator or conveyor. This can reduce adhesion to the locator and strip adhesive wear associated with the locator, as well as static and dynamic friction and adhesion.
[0200] As stated above, the applicant discovered that the high level of levelness of the unbonded strips 36 within channel 104 and / or channel 104 reduces the impact of the vortex airflow on the strips 36 during sintering. Figure 12 As shown, channel 104, inlet 106, and outlet 108 are located in a substantially horizontal plane. In a specific embodiment, the substantially horizontal plane and / or a gradual arcuate or curved shape (e.g., radius of curvature at least 1 m) is defined by the path defined by the central axis of channel 104, inlet 106, and outlet 108. Similarly, in such embodiments, the non-adhesive strip 36 may also be located in a substantially horizontal plane and / or a gradual arcuate or curved shape (e.g., as shown in the diagram). Figure 13 As shown, the upper surface 124 and / or lower surface 126 of strip 36 are located in a substantially horizontal plane. The substantially horizontal plane of strip 36, as used herein and defined by channel 104, inlet 106, and outlet 108, is one in which the angle formed relative to the horizontal reference plane is 10 degrees or less. In other embodiments, channel 104, inlet 106, and outlet 108 and / or strip 36 within channel 104 are located in even more planar planes, for example, the angle formed by the planes relative to the horizontal reference plane is 3 degrees or less, and more specifically, the angle relative to the horizontal reference plane is 1 degree or less. In other embodiments, channel 104 is not so oriented, and the corresponding sintered strip may have markings associated with a “chimney effect” or irregular heating (e.g., rolled surface blocks or protrusions), for example, if the airflow through channel 104 is vortex-like.
[0201] To further control or limit the vortex airflow exposed to the strip material of system 10 during its passage across system 10, the binder removal station 34 can be positioned relative to sintering station 38 in such a way that the strip material (e.g., the green strip material 20 within the binder removal station and the unbonded strip material 36 within the sintering station) is maintained in a substantially horizontal position as the strips 20 and 36 cross the binder removal station 34 and sintering station 38. In such embodiments, similar to the horizontal arrangement of sintering channel 104, the binder removal station 34 is oriented or can be oriented in a substantially horizontal position, for example, where openings 116 and 118 are aligned such that the line formed therebetween is within 10 degrees of the horizontal.
[0202] In this embodiment, the adhesive removal workstation 34 includes an adhesive burn-off furnace 110. The adhesive burn-off furnace 110 includes an insulating housing 112. Generally, the insulating housing 112 includes a plurality of inner walls defining a channel 114 that extends through the adhesive burn-off furnace 110 between an inlet opening 116 and an outlet opening 118.
[0203] like Figure 12 As shown in the binder burnout furnace 110, channels 114, inlet 116, and outlet 118 are located in a substantially horizontal plane. In a specific embodiment, the substantially horizontal plane is defined by the path defined by the central axis of channel 114, inlet 116, and outlet 118. Similarly, in such embodiments, the green strip 20 within channel 114 may also be located in a substantially horizontal plane. As used herein, the substantially horizontal plane of the green strip 20 and channels 114, inlet opening 116, and outlet opening 118 is such that the angle it forms with respect to a horizontal reference plane is 10 degrees or less. In other specific embodiments, channels 114, inlet opening 116, and outlet opening 118, and / or the green strip 20 within channel 114, are located in even more horizontal planes, for example, the angle formed by the planes with respect to a horizontal reference plane is 3 degrees or less, and more specifically, the angle with respect to a horizontal reference plane is 1 degree or less. In other embodiments, these features may not be so horizontally aligned.
[0204] In addition to maintaining the levelness of the green strip 20 and the unbonded strip 36 in the binder removal furnace 110 and the sintering furnace 100 respectively, the binder removal furnace 110 (also referred to as the binder removal workstation) and the sintering furnace 100 are aligned relative to each other so that the unbonded strip 36 maintains a horizontal position when it transitions from the binder removal furnace 110 to the sintering furnace 100. The applicant found that at this transition point, the unbonded strip 36 is particularly prone to deformation or breakage due to various forces (e.g., forces caused by vortex airflow), since, with most of the organic binder removed, the unbonded inorganic particles of the unbonded strip 36 are held together by weaker forces (e.g., van der Waals forces, electrostatic interactions, small amounts of residual organic binder, frictional interactions / meshing between adjacent particles, binders, plasticizers, liquid carriers, low levels of inorganic matter carried in possible particle-particle bonding, etc.), and thus even smaller forces (e.g., those caused by the interaction of the vortex airflow with the unbonded strip 36) can lead to deformation or breakage.
[0205] Therefore, as Figure 12 As shown, to limit the vortex airflow, the channel 114 of the binder burn-off furnace 110 is aligned vertically with the channel 104 of the sintering furnace 100. Along the strip path passing through the sintering furnace 100 and the binder burn-off furnace 110, the green strip 20 flows horizontally from (as shown in the diagram). Figure 3 The input roller (shown) moves into the binder burn-off inlet 116, through the binder burn-off channel 114, and out of the binder burn-off outlet 118. While within channel 114, the heat generated by the heaters of furnace 110 causes at least a portion of the organic binder material of the green strip 20 to undergo a chemical change and / or be removed, termed "burn-off". Furthermore, the relative positions of the binder burn-off furnace 110 and the sintering furnace 100 ensure that the unbonded strip 36 moves from the binder burn-off furnace 110 into the sintering furnace 100 while always maintaining a horizontal or substantially horizontal position, as described above. Therefore, in at least some embodiments, the vertical alignment between channels 104 and 114 ensures that the unbonded strip 36 maintains substantially the same horizontal plane (i.e., no upward or downward offset between furnaces 110 and 100) as the strip material traverses both furnaces 100 and 110.
[0206] The applicant has determined that the benefits of horizontal binder removal and / or horizontal sintering become more significant as the width of the strip material increases, since wider strip materials are more susceptible to deformation based on airflow vortices. Therefore, the applicant believes that the horizontal arrangement of the sintering furnace 100 and / or binder removal furnace 110 enables the production of wider and / or longer sintered strip materials without significant deformation or breakage, which is believed to be impossible to achieve using existing systems.
[0207] See Figure 13 and Figure 14 In addition to the horizontal arrangement of the binder burn-off furnace 110, sintering furnace 100, and the strip materials (e.g., green strip 20 and unbonded strip 36) within the furnace, the applicant has found that vortex airflow can be limited by providing a sintering channel 104 with a lower height dimension (which in turn involves a lower clearance relative to the unbonded strip 36). The applicant has also found that vortex airflow can be limited by reducing the volume of regions in which thermal gradients are established and which cause air movement, whereas otherwise, the very hot air within the channel 104 might be subjected to such vortex airflow.
[0208] like Figure 13 and 12 As shown, channel 104 is partially defined by a horizontal and generally upward-facing surface 120, which defines at least a portion of the lower surface of channel 104. Similarly, channel 104 is also partially defined by a horizontal and generally downward-facing surface 122, which defines at least a portion of the upper surface of channel 104. The first gap, shown as G1, is the vertical distance between the upward-facing surface 120 and the downward-facing surface 122, and G2 is the vertical distance or gap between the downward-facing surface 122 and the upper surface 124 of the non-adhesive strip 36.
[0209] As described above, in various embodiments, G1 and G2 are relatively small, thus limiting the vortex airflow; however, G1 and G2 should generally be large enough to allow for various processing steps (e.g., through channel 104). In various embodiments, G2 is less than 0.5 inches (less than 12.7 mm), specifically less than 0.375 inches (less than 9.5 mm), and more specifically 0.25 inches (approximately 6.35 mm). It will be understood that G1 is approximately equal to G2 plus the thickness T1 of the unbonded strip 36. Therefore, in various embodiments, because T1 is low (e.g., 3 micrometers to 1 millimeter), G1 is less than 1 inch (less than 25.4 mm), specifically less than 0.75 inches (less than 19 mm), and for thin strip materials it can be less than 0.5 inches (less than 12.7 mm), and for very thin strip materials it can be less than 0.375 inches (less than 9.5 mm).
[0210] Figure 14 The outlet 108 of the sintering furnace 100 is shown, and a small gap G2 relative to the strip 40 is shown according to an exemplary embodiment. In various embodiments, G1 and G2 may represent the maximum gap distance between the relevant surfaces, and in another embodiment, G1 and G2 may represent the average gap distance between the relevant surfaces measured along the length of the channel 104.
[0211] In specific embodiments, surfaces 120 and / or 122 are also substantially horizontal surfaces extending between the inlet 106 and outlet 108 of furnace 100 (as described above). Thus, in such embodiments, surfaces 120 and 122 define a substantially horizontal channel 104. In some embodiments, surfaces 120 and / or 122 may be flat, level surfaces extending between the inlet 106 and outlet 108 of furnace 100. In other embodiments, surfaces 120 and / or 122 may be gradually arcuate or curved as described above, or may be as in the case of an adhesive removal workstation. In specific embodiments, surfaces 120 and / or 122 are substantially horizontal such that the angle formed by the surfaces relative to a horizontal reference plane is less than 10 degrees, specifically less than 3 degrees, and even more specifically less than 1 degree.
[0212] like Figure 13 As shown, the lower surface 126 of the unbonded strip 36 contacts the upper surface 120, so that as the unbonded strip 36 moves forward through the furnace 100, the lower surface 126 of the unbonded strip 36 slides along or relative to the upper surface 120. In a specific embodiment, the sliding contact between the lower surface 126 and the upper surface 120 during sintering produces, or can produce, various longitudinal features (e.g., longitudinally extending marks, grooves, ridges, etc.) formed in the lower surface 126 rather than on the upper surface 124. Therefore, in a specific embodiment, the surface features on the lower surface 126 are different from those on the upper surface 124 that do not come into contact with the opposing surface during sintering. Specifically, this sliding contact is significantly different from the arrangement in some firing processes (e.g., tunnel kiln processes, in which ceramic material is placed on a fixed plate and both move simultaneously through the sintering furnace). In a specific embodiment, surfaces 20 and 122 are alumina or contain alumina, for example, the inner surface of an alumina tube defining channel 104.
[0213] In addition to the location and airflow control arrangements discussed above, the applicant has found that controlling the temperature distribution of the through furnace 100 exposed to the unbonded strip 36 is important for limiting strip deformation or breakage. The applicant has found that excessively rapid temperature increases (e.g., too fast a sintering rate or over too short a distance in the strip) can cause such strip deformation or breakage. See also... Figure 15The furnace 100 may include a plurality of independently controlled heating elements 140 arranged to transfer heat to channels 104 to induce sintering of the unbonded strip 36 as it traverses the furnace 100. While the maximum and minimum sintering temperatures will vary at least in part based on the type of inorganic material carried by the strip 36, generally speaking, the heating elements 140 are configured to generate temperatures of at least 500 degrees Celsius along at least a portion of the channels 104. In some embodiments, for example, for the sintering of ThO2 (thorium oxide) and / or TiO2 (titanium oxide), the channels 104 may be heated to a maximum temperature above 3100 degrees Celsius. Some materials (e.g., carbides, tungsten) have melting points above 3200 degrees Celsius, and in some such embodiments, the temperature range generated by the heaters 140 is between 500 degrees Celsius and higher temperatures (e.g., 3500 degrees Celsius or 3600 degrees Celsius). In a specific embodiment, the heating element 140 may be a U-shaped molybdenum disilicide heating element and / or other heating elements disclosed herein.
[0214] In general, each heating element 140 can be controlled by a control system 142 configured (e.g., through physical arrangement, programming, etc.) to independently control the individual heating elements 140 of the furnace 100, thereby generating a temperature distribution along the length of the channel 104 to provide the desired sintering level in the sintered strip 40 while limiting deformation during the sintering process. In some embodiments, the control system 142 can communicate with one or more temperature sensors 144 that detect the temperature within the channel 104. In such embodiments, the control system 142 can control the heating elements 140 based on input signals received from the sensors 144, thereby maintaining the desired temperature distribution during the continuous sintering of the unbonded strip 36. In some embodiments, the control system 142 can also receive input signals indicating strip movement speed, position, shrinkage, and tension, and control the temperature and / or movement speed based on these signals or other signals (possibly related to these or other strip properties).
[0215] As will be demonstrated in the examples related to the sintering furnace below, the applicant has found that applying a sintering temperature distribution along the length of channel 104 is important, or potentially important, for maintaining low or controlled levels of strip material deformation during sintering. Specifically, the applicant has found that if the temperature rise exposed to the unbonded strip 36 during sintering is too large (e.g., the slope of the temperature distribution is too steep), unacceptably high levels of stress are formed or may form in the strip 36 as the material sinters and shrinks. This, in turn, leads to out-of-plane deformation in the strip 36, such as… Figure 2As shown. Specifically, the applicant has discovered that deformation of strip 36 during sintering can be controlled by controlling the stress at the edges 130 and 132 and / or along the centerline of strip 36. Similar detrimental effects may occur on strip 36 if the transition from the heated portion of system 10 to the room temperature portion of system 10 (e.g., after exiting furnace 100) occurs too abruptly. In other words, the technology of this application can be used to sinter strips without such temperature control or distribution, wherein the resulting new strips or other sintered articles may exhibit deformation or other defects characteristic of this application.
[0216] See Figure 16 and 17 This shows temperature distributions 160 and 170 along the length of the sintering channel 104 generated by the heating element 140 according to an exemplary embodiment. See also Figure 16 Temperature distribution 160 shows that the temperature within channel 104 increases substantially along the length of channel 104 in the processing direction 14. Distribution 160 includes at least three segments: a first segment 162, which represents the temperature in the region of channel 104 adjacent to inlet opening 106; a second segment 164, which represents the temperature of the bulk (e.g., at least 50%, at least 75%, etc.) along the length of channel 104; and a third segment 166, which represents the temperature in the region of channel 104 adjacent to outlet opening 108.
[0217] like Figure 16 As shown, the average slope of the first segment 162 is greater than that of the second segment 164, indicating a relatively rapid increase in temperature within the channel 104 adjacent to the inlet opening 106. The average slope of the second segment 164 is lower (and less than that of the first segment 162). The low average slope of the second segment 164 indicates a gradual increase in temperature experienced by the strip 36 as it moves along most of the length of the channel 104. As described below, this gradual increase is chosen to keep the stress within the strip 36 below a determined threshold for maintaining deformation below the desired level. The average slope of the third segment 166 is a negative slope, representing a cooling section within the channel 104 adjacent to the outlet opening 108, which limits the thermal shock experienced by the strip 36 after it leaves the furnace 100.
[0218] In various embodiments, the gradual temperature increase represented by the low slope of segment 164 can be achieved by controlling the rate of temperature increase along the length of channel 104. In various embodiments, such as Figure 16 As indicated by the x-axis, the length of channel 104 can be substantial, for example, at least 1 meter, at least 50 inches, at least 60 inches, or greater. In modeling and as... Figure 16 In the specific sintering furnace shown, heating channel 104 is 64 inches.
[0219] In various embodiments, the shape of distribution 160 maintains an acceptablely low level of compressive stress within the strip 36 during sintering, thereby avoiding undesirable deformation. The applicant has found that the absence of strip deformation control as described herein is particularly problematic for wide strip materials and high-volume sintering systems. Specifically, wider strips are more susceptible to this type of deformation, and furthermore, deformation in the width direction makes, or may make, difficult or impossible to wind onto a take-up reel. That is, the technical aspects disclosed herein (e.g., carrier separation, tension control, binder removal, etc.) can be practiced and used to produce new materials and products without temperature distribution, for example, where the resulting products are narrow and / or have defects or deformation characteristics associated with such processing.
[0220] Therefore, in various embodiments, the shape of distribution 160 ensures that the compressive stress at the left edge 130 and / or right edge 132 of the unbonded strip 36 remains below the edge stress threshold during sintering, and the compressive stress at the centerline of the unbonded strip 36 remains below the centerline stress threshold during sintering. Generally, the edge stress threshold and centerline stress threshold are defined as compressive stresses above which, during sintering, the unbonded strip 36 experiences out-of-plane (length-width plane) deformation greater than 1 mm. The applicant has found that, for at least some materials and strip widths, by maintaining the edge compressive stress and centerline compressive stress below a threshold of 100 MPa (specifically 75 MPa, and more specifically 60 MPa), out-of-plane deformation during sintering can be limited to less than 1 mm. In a specific implementation, the applicant discovered that, for at least some materials and strip widths, by maintaining a centerline compressive stress below a threshold of 100 MPa (specifically 75 MPa, and more specifically 60 MPa) and an edge stress below a threshold of 300 MPa (specifically 250 MPa, and more specifically 200 MPa), the out-of-plane deformation during sintering can be limited to less than 1 mm.
[0221] In a specific embodiment, the slopes of segments 162 and 166 can be controlled to provide particularly low strip stress at the inlet and outlet of furnace 100. In one such embodiment, control system 142 is configured to control the temperature distribution within segments 162 and 166 in conjunction with controlling the speed of the strip through furnace 100. In this embodiment, this combination of temperature control within segments 162 and 166 and speed control results in uniform sintering shrinkage (strain), thus achieving low stress and low deformation within strip 36 during sintering.
[0222] See Figure 17Another exemplary temperature distribution 170 is shown as a view projected along channel 104. As shown, distribution 170 is displayed in zone 172, increasing to a maximum temperature over approximately 75% of the total length of channel 104. In a specific embodiment, sintering furnace 100 may be constructed of a high thermal conductivity material (e.g., steel or high thermal conductivity ceramic) to reduce the temperature gradient in the cross-sectional mesh (strip / sheet) along the width direction. Figure 17 As shown, there is low or no temperature variation in the width direction. As is generally understood, the temperature distribution of a particular sintering system is based on several factors, including: material type, inorganic particle size, particle density, particle size distribution, porosity, pore size, pore size distribution, sintering atmosphere, stress threshold / permissible deformation of the component (as described above), length of channel 104, production rate, and desired output.
[0223] See Figure 18 This illustrates another embodiment of the sintering workstation 38 according to an exemplary embodiment. In this embodiment, the sintering workstation 38 includes two furnaces 180 and 182 arranged in series with each other. Generally, furnaces 180 and 182 are substantially the same as furnace 100 described above, except that in at least some embodiments, the temperature distribution in furnace 180 differs from the temperature distribution within furnace 182. In this arrangement, an unbonded strip 36 enters the inlet 106 of furnace 180. Inside furnace 180, the unbonded strip 36 is partially sintered to form a partially sintered strip 184, which exits furnace 180 through outlet 108. The partially sintered strip 184 then enters the second furnace 182 through inlet 106 and undergoes additional sintering along the length of channel 104 in furnace 182, thereby sintering strip 40 exits furnace 182 through outlet 108 for reel collection as described above.
[0224] In various embodiments, furnaces 180 and 182 each include multiple independently controllable heating elements, thereby enabling the formation of different and independent temperature distributions within furnaces 180 and 182. In some embodiments, employing two thermally isolated furnaces (e.g., furnaces 180 and 182) provides more precise control over the temperature distribution exposed to the strip material during sintering, compared to a single long furnace with a channel length equal to the total channel length of furnaces 180 and 182. In other anticipated embodiments, the strip may travel back through the same furnace but along different paths and / or be exposed to different temperature distributions for additional sintering.
[0225] Furthermore, in some embodiments, it may be desirable to apply different tensions between furnaces 180 and 182. In such embodiments, a tension control system 186 is located along the sintering path defined by the channel 104 of furnaces 180 and 182. In a specific embodiment, the tension control system 186 is positioned between furnaces 180 and 182 and applies tension to the partially sintered strip 184, such that the tension of the strip 184 in the second furnace 182 is greater than the tension of the unbonded strip 36 in furnace 180. In various embodiments, it may be desirable to increase the tension within the second sintering furnace to provide improved flatness or reduced deformation during the final sintering or subsequent sintering processes in furnace 182. Furthermore, this increased tension may be suitable for application to the partially sintered strip 184, as this partial sintering increases the tensile strength of the strip 184 relative to the lower tensile strength of the unbonded strip 36 in furnace 180.
[0226] See Figure 19 This displays the predicted temperature distribution within furnaces 180 and 182 according to an exemplary embodiment. (Example...) Figure 19 As shown, the heating elements of furnace 180 are controlled to produce temperature distribution 190, and the heating elements of furnace 182 are controlled to produce temperature distribution 192. It will be noted that both distributions 190 and 192 exhibit the same low stress generation and gradual temperature increase, similar to the case of temperature distribution 160 described above. However, distribution 192 is located higher than distribution 190 (e.g., it has a higher average temperature than distribution 190), which results in an additional, higher level of sintering (e.g., additional shrinkage, additional porosity reduction) when the partially sintered strips 184 traverse furnace 182.
[0227] See Figure 20 This illustrates a high-yield sintering system 200 according to an exemplary embodiment. Generally, system 200 includes two parallel systems 10, each sintering strip material. System 200 can be operated to increase the output of a single type of sintered strip material, similar to... Figure 18 The arrangement of the sintered strip material. Alternatively, each system 10 of system 200 can output a different sintered strip material. In various embodiments, system 200 may include three, four, five... parallel systems 10 to further increase the output of sintered strip material.
[0228] Sintering workstation examples and models
[0229] See Figures 21 to 28 Various sintering tests and sintering models are described to confirm the sintering relationships discussed in this paper, such as the relationship between temperature distribution and shrinkage rate, the relationship between temperature distribution and stress in strip materials, the relationship between stress and strip deformation, and the relationship between strip width and sintering deformation risk.
[0230] Example 1 of physical sintering test
[0231] In one embodiment, a horizontal furnace with an actively controlled multi-zone binder removal furnace was tested. In this test, strip-cast "green" zirconia ceramic belts (ceramics loaded with polymer binder) (42 mm wide and approximately 25 micrometers thick) were fed at 20 inches per minute through a horizontal apparatus with a multi-zone binder removal furnace (similar to furnace 38 and binder removal workstation 34 described above). The binder removal furnace was set to 325°C at the inlet and 475°C at the outlet, with increments of 0-25°C for the four central hot zones. An airflow of 7.5 liters per minute was also provided at a temperature of approximately 0°C to approximately 250°C, and the airflow was split between the two sides of the furnace. The furnace was 36 inches long and had 18-inch long hot zones. Inside the furnace, the strip was transported by sliding it along an alumina "D" tube with a tension of 20 grams, and the furnace was set at 1225°C. The sintered zirconia strips, 10-20 feet long, are manufactured and wound onto a 3-inch diameter take-up reel. The sintering shrinkage across the width is approximately 12%.
[0232] Sintering Model 1
[0233] See Figure 21 and Figure 22 The results show the functional relationship between the sintering shrinkage of zirconium oxide and time and temperature. Figure 21 Sintering shrinkage diagrams of zirconia strips at various temperatures and times. Figure 22 This graph shows the mathematical function of sintering shrinkage of zirconia strips at various temperatures and times.
[0234] In order to generate Figure 21 The data points shown represent the casting of approximately 15 mm wide and 25 micrometer thick strips of "green" zirconia ceramic (ceramics loaded with a polymer binder) in the apparatus described in Example 1 of the physical sintering test above, fired at 8 inches per minute in a "bisque" pattern to 1200°C. The bisque-fired strips produced in this manner were then subjected to plucking fire at 1250°C, 1300°C, 1350°C, 1400°C, 1450°C, and 1500°C for 30 seconds, 1 minute, 2 minutes, 3 minutes, and 5 minutes in a narrow-zone furnace. Sintering shrinkage was measured, and these data points are as follows: Figure 21 As shown.
[0235] Based on sintering data, a mathematical curve describing the functional relationship between sintering shrinkage and temperature and time was fitted and extrapolated to lower and intermediate temperatures beyond those tested in actual experiments. This curve fitting and extrapolation are as follows: Figure 22 As shown. Based on Figure 21 and Figure 22The tests and curve fitting shown determined the relationship between sintering shrinkage, sintering time, and temperature for zirconia. The applicant believes that this information can be used to establish a sintering temperature distribution for zirconia to achieve the desired shrinkage rate and reduce stress below the deformation threshold, as described above.
[0236] In one specific implementation, this data is used for... Figure 16 The 64-inch sintering furnace and temperature distribution shown are modeled. For example... Figure 16 As shown, the thermal gradient / distribution 160 starts at 1250°C and ends at 1450°C. The modeling temperatures are as follows: for 0 to 8 inches entering the furnace, the temperature increases from 1250°C to 1300°C; for 8 to 16 inches, it increases from 1300°C to 1312.5°C; for 16 to 24 inches, it increases from 1312.5°C to 1325°C; for 24 to 32 inches, it remains at 1325°C; for 32 to 40 inches, it increases from 1325°C to 1375°C; for 40 to 48 inches, it increases from 1375°C to 1400°C; for 48 to 56 inches, it increases from 1400°C to 1450°C; for 56 to 64 inches, it remains at 1450°C; and then after 64 inches, it cools to below 1000°C.
[0237] Model the functional relationship between contraction and strip transport speed. For example... Figure 16 As shown, the model demonstrates that a faster transport speed (20 inches per minute (ipm)) results in more uniform sintering shrinkage over the length of the hot zone. Therefore, this model confirms that uniform shrinkage over longer lengths is desirable, as shorter distances where sintering strain / shrinkage occurs lead to greater stress in the strip and a greater tendency for bending and out-of-plane plastic deformation.
[0238] Sintering Model 2
[0239] See Figure 23 and 16 The sintering stress is modeled using finite element analysis (FEA) and closure (CF) solutions. For example... Figure 23 and 24It has been confirmed that as the sintering strip becomes wider, extreme sintering stresses greater than -1000 MPa are calculated for a 100 mm wide static strip (single hot zone) and for a 100 mm wide strip (where only two hot zones are present, and the strip is transported at 8 and 16 inches per minute). Conversely, when using 9 hot zones and 2 sinter passes (equivalent to 18 hot zones in a single pass), edge stresses less than approximately -200 MPa are modeled for a 150 mm wide sheet. In the single hot zone and 4 hot zone tests, each hot zone was modeled with a length of 450 mm (18 inches), and the furnace was 900 mm (36 inches), thus in these two modeling embodiments, additional hot zones are equivalent to longer hot zones. For example, a 1-zone 2-pass hot zone is roughly equivalent to a total of 900 mm (36 inches) long hot zones. However, for a 9-zone 2-pass hot zone, it is equivalent to a total of 3660 mm (144 inches) (length) hot zones. Therefore, Figure 23 and 24 It has been confirmed that increasingly wider strips (e.g., greater than 50 mm, 100 mm, 150 mm, 200 mm, 250 mm, etc.) can be achieved by controlling the number of hot zones (e.g., the total length of the sintering hot zones), the temperature distribution exposed to the strip, and the strip's movement rate through the hot zones, thereby maintaining sintering stress at a sufficiently low level to avoid deformation, bending, or cracking.
[0240] Sintering Model 3
[0241] Figure 25 and 26 The model shows a light yellow zirconia strip (i.e., a partially sintered strip) passing twice through a single hot zone with a steep temperature gradient. For the first pass, the hot zone is set at 1250°C, and then for the second pass, it is set at 1400°C. Strip transport speeds of 8 and 16 inches per minute are input. The strip is modeled as 20 micrometers thick and 15 mm and 40 mm wide. Figure 25 Showing the contraction through the hot zone, and Figure 26 The results show that rapid sintering strain generates significant compressive stress in the strips, exceeding 90 MPa for a 40 mm wide strip with an 8 ipm diameter and exceeding 120 MPa for a 40 mm wide strip with a 16 ipm diameter. This is believed to lead to bending and out-of-plane deformation in strips with these widths and thicknesses.
[0242] Sintering Model 4
[0243] Figure 27 and Figure 28 The results show the performance when the model uses a multi-zone furnace with 10 hot zones and two passes, and the temperature set for the second pass is higher than that for the first pass. For both strip transport speeds and strip widths, the stress obtained from the modeling is compared to... Figure 26The stress shown decreased by an order of magnitude. This lower stress is believed to result in much flatter stripes (e.g., smaller deformation). Furthermore, this model confirms the effect of controlled sintering temperature distribution or gradual temperature increase on stress and consequently, deformation during sintering.
[0244] Example 2 of physical sintering test
[0245] In another test embodiment, strips approximately 25 micrometers thick and 15 cm wide of "green" zirconia ceramic tape (ceramics loaded with a polymer binder) were fabricated using a vertically oriented sintering apparatus at a sintering temperature of 1100°C. Approximately 50 feet were produced and wound onto a 3-inch diameter take-up reel. The pale yellow sintering shrinkage width was approximately 10%.
[0246] Then, this 1100℃ "light yellow" stripe passes through a horizontal sintering furnace (basically with...) Figure 12 (As shown below), speeds were approximately 3, 10, 20, 30, 60, and 75 inches per minute, with the furnace set at 1550°C. Sintered strips of 40 feet in length were produced and wound onto a 3-inch diameter take-up reel. During sintering, the tension on the strip was 10 grams, and even at 75 inches per minute, resulting in less than approximately 15 seconds of heat in the hot zone, a porosity of less than 20% was achieved. Slower speeds yielded denser material. Therefore, this test confirms that longer sintering furnaces result in higher density / lower porosity in the sintered strips, and also confirms that higher temperatures result in higher density / lower porosity in the sintered strips.
[0247] Physical Sintering Test Example 3
[0248] In another test embodiment, a strip of approximately 50 micrometers thick was used to cast a "green" alumina ceramic belt (ceramics loaded with a polymer binder) through a feed path of 4–6 inches per minute. Figure 3 The system shown is essentially the same. The binder burn-off furnace is set at 325°C inlet to 475°C outlet, with increments of 0-25°C for the four central hot zones. An airflow of 5-7.5 liters per minute is used at 0-250°C. The sintering furnace is 36 inches long and has an 18-inch hot zone set at 1300°C. Green strips pass through the 18-inch sintering hot zone at 1300°C, producing partially sintered "light yellow" strips. The width of the partially sintered strips is 7% smaller than the width of the green strips.
[0249] Then, the 1300°C "light yellow" strip passes a second time through the sintering furnace at 2 inches per minute, with the furnace set at 1550°C, producing approximately 20 feet of fully sintered alumina strip. The strip is wound onto a 6-inch diameter take-up reel. During sintering, the tension on the strip is approximately 100 grams, and the sintering shrinkage width during the second pass is approximately 15%. After sintering, the strip is translucent to almost transparent. It is readable through when placed on a written document. The particle size is less than approximately 2 micrometers, and the material has a porosity of less than approximately 1%.
[0250] Test Example 4
[0251] In another test embodiment, a strip of approximately 50 micrometers thick was used to cast a "green" zirconia ceramic belt (ceramics loaded with a polymer binder) through a feed path at 6 inches per minute. Figure 3 The system is essentially the same as shown. The binder burn-off furnace is set at 300-475°C with an airflow of -7.5 liters per minute at 200-250°C. The sintering furnace is 36 inches long with an 18-inch hot zone. The temperature gradients are 25°C to 1225°C for the section less than 9 inches, and 1000°C to 1225°C for the section 3-4 inches. Two D-tubes spaced approximately 3 / 8 inch apart are used to restrict air circulation and reduce the temperature gradient. The tension in the strip is 20-60 grams, and the sintering furnace is set at 1225°C. A sintered zirconia strip is produced with a length of 50 feet and wound onto a 3-inch diameter take-up reel. The sintering shrinkage width is approximately 12%.
[0252] To physically model the furnace with a shallow temperature gradient, a "light yellow strip" sintered at 1225°C was passed through a single-zone furnace three times (at progressively higher temperatures). This reduced sintering shrinkage with each pass, minimizing out-of-plane deformation. Specifically, the 1225°C "light yellow" strip was then passed through the furnace a second time at 6 inches per minute, with the furnace set at 1325°C. This process produced 45-foot-long sintered zirconia strips, which were then wound onto a 3-inch diameter take-up reel. During sintering, the tension on the strip was 100-250 grams, and the sintering shrinkage width for this pass was 5-6%.
[0253] The strip is then passed through the furnace a third time at 1325°C at 6 inches per minute, with the furnace set at 1425°C. Approximately 40 feet of sintered zirconia strip is produced and wound onto a 3-inch diameter take-up reel. During sintering, the tension on the strip is 100-250 grams, and the sintering shrinkage width during this pass is 5-6%. After passing through 1425°C, the strip is translucent to almost transparent. It is legible when placed on a written document.
[0254] The 1425°C strip is then passed through the furnace a fourth time at 3-6 inches per minute, with the furnace set at 1550°C. This produces several feet of sintered 1550°C strip, which is then wound onto a 3-inch diameter take-up reel. During sintering, the tension on the strip is 100-300 grams, and the sintering shrinkage (width) during this pass is 0-2%.
[0255] Sintered products
[0256] Embodiments of sintered articles formed using the systems and processes described herein will now be described. Sintered articles can be provided in the form of sintered strips (i.e., continuous sintered articles) or discrete sintered articles. Unless otherwise stated, the term "sintered article" refers to both continuous and discrete sintered articles. Furthermore, "sintering" refers to both partially sintered and fully sintered articles. In one aspect, embodiments of sintered articles include dimensions previously unattainable. In one or more embodiments, the sintered articles also exhibit uniformity of certain properties along these scales. According to another aspect, embodiments of sintered articles exhibiting flattenability indicate that the sintered articles can be flattened or subjected to flattening without imposing significant stress in the sintered articles, thus enabling successful use in downstream processes. Another aspect pertains to embodiments of roll-sintered articles, and another aspect pertains to embodiments of multiple discrete sintered articles. Other aspects include new material compositions or compositions with new microstructures, for example, with regard to unique particle boundaries.
[0257] See Figure 29 A sintered article 1000 according to one or more embodiments includes a first main surface 1010, a second main surface 1020 opposite to the first main surface, and a body 1030 extending between the first and second main surfaces. The body 1030 has: a thickness (t) defined as the distance between the first and second main surfaces, a width (W) defined as a first dimension perpendicular to the thickness of one of the first or second surfaces, and a length (L) defined as a second dimension perpendicular to both the thickness and the width of one of the first or second surfaces. In one or more embodiments, the sintered article includes an opposing subsurface 1040 defining the width (W). In specific embodiments, as described herein, the sintered article 1000 is an example of a sintered strip 40 produced using system 10, but some strips of this technology may be more… Figure 29 The strips shown are longer.
[0258] In one or more embodiments, the sintered article is a continuous sintered article with a width of about 5 mm or more, a thickness of about 3 μm to about 1 mm, and a length of about 300 cm or more. In other embodiments, the width is less than 5 mm, as described above.
[0259] In one or more embodiments, the width of the sintered article is in the following ranges: about 5 mm to about 200 mm, about 6 mm to about 200 mm, about 8 mm to about 200 mm, about 10 mm to about 200 mm, about 12 mm to about 200 mm, about 14 mm to about 200 mm, about 15 mm to about 200 mm, about 17 mm to about 200 mm, about 18 mm to about 200 mm, about 20 mm to about 200 mm, about 22 mm to about 200 mm, about 24 mm to about 200 mm, about 25 mm to about 200 mm, about 30 mm to about 200 mm. 00mm, about 40mm to about 200mm, about 50mm to about 200mm, about 60mm to about 200mm, about 70mm to about 200mm, about 80mm to about 200mm, about 90mm to about 200mm, about 100mm to about 200mm, about 5mm to about 150mm, about 5mm to about 125mm, about 5mm to about 100mm, about 5mm to about 75mm, about 5mm to about 50mm, about 5mm to about 40mm, about 5mm to about 30mm, about 5mm to about 20mm, or about 5mm to about 10mm.
[0260] In some embodiments, the width W of the sintered article is at least 0.5 mm, for example at least 1 mm, for example at least 2 mm, for example at least 5 mm, for example at least 8 mm, for example at least 10 mm, for example at least 15 mm, for example at least 20 mm, for example at least 30 mm, for example at least 50 mm, for example at least 75 mm, for example at least 10 cm, for example at least 15 cm, for example at least 20 cm, and / or not more than 2 m, for example not more than 1 m, for example not more than 50 cm, for example not more than 30 cm. In other embodiments, the sintered article has a different width W.
[0261] In one or more embodiments, the thickness (t) of the sintered article is in the following range: about 3 μm to about 1 mm, about 4 μm to about 1 mm, about 5 μm to about 1 mm, about 6 μm to about 1 mm, about 7 μm to about 1 mm, about 8 μm to about 1 mm, about 9 μm to about 1 mm, about 10 μm to about 1 mm, about 11 μm to about 1 mm, about 12 μm to about 1 mm, about 13 μm to about 1 mm, about 14 μm to about 1 mm, about 15 μm to about 1 mm, about 20 μm to about 1 mm, about 25 μm to about 1 mm, about 30 μm to about 1 mm, about 35 μm to about 1 mm, about 40 μm to about 1 mm, about 45 μm to about 1 mm, about 50 μm to about 1 mm, about 100 μm to about 1 mm, about 200 μm to about 1 mm. Approximately 1 mm, approximately 300 μm to approximately 1 mm, approximately 400 μm to approximately 1 mm, approximately 500 μm to approximately 1 mm, approximately 3 μm to approximately 900 μm, approximately 3 μm to approximately 800 μm, approximately 3 μm to approximately 700 μm, approximately 3 μm to approximately 600 μm, approximately 3 μm to approximately 500 μm, approximately 3 μm to approximately 400 μm, approximately 3 μm to approximately 300 μm, approximately 3 μm to approximately 200 μm, approximately 3 μm to approximately 100 μm, approximately 3 μm to approximately 90 μm, approximately 3 μm to approximately 80 μm, approximately 3 μm to approximately 70 μm, approximately 3 μm to approximately 60 μm, approximately 3 μm to approximately 50 μm, approximately 3 μm to approximately 45 μm, approximately 3 μm to approximately 40 μm, approximately 3 μm to approximately 35 μm, approximately 3 μm to approximately 30 μm, or approximately 3 μm to approximately 30 μm.
[0262] In some embodiments, the thickness t of the sintered article is at least 3 μm, for example at least 5 μm, for example at least 10 μm, for example at least 15 μm, for example at least 20 μm, for example at least 25 μm, for example at least 0.5 mm, for example at least 1 mm, and / or not more than 5 mm, for example not more than 3 mm, for example not more than 1 mm, for example not more than 500 μm, for example not more than 300 μm, for example not more than 100 μm. In other embodiments, the sintered article has a different thickness t.
[0263] In one or more embodiments, the sintered article is continuous and has a length L ranging from the following: about 300 cm to about 500 m, about 300 cm to about 400 m, about 300 cm to about 200 m, about 300 cm to about 100 m, about 300 cm to about 50 m, about 300 cm to about 25 m, about 300 cm to about 20 m, about 350 cm to about 500 m, about 400 cm to about 500 m, about 450 cm to about 500 m, about 500 cm to about 500 m, about 550 cm to... Approximately 500m, approximately 600cm to approximately 500m, approximately 700cm to approximately 500m, approximately 800cm to approximately 500m, approximately 900cm to approximately 500m, approximately 1m to approximately 500m, approximately 5m to approximately 500m, approximately 10m to approximately 500m, approximately 20m to approximately 500m, approximately 30m to approximately 500m, approximately 40m to approximately 500m, approximately 50m to approximately 500m, approximately 75m to approximately 500m, approximately 100m to approximately 500m, approximately 200m to approximately 500m, or approximately 250m to approximately 500m.
[0264] In some embodiments, the sintered article has a continuous, unbroken length L of at least 5 mm: for example, at least 25 mm, for example, at least 1 cm, for example, at least 15 cm, for example, at least 50 cm, for example, at least 1 m, for example, at least 5 m, for example, at least 10 m, and / or not exceeding 5 km, for example, not exceeding 3 km, for example, not exceeding 1 km, for example, not exceeding 500 m, for example, not exceeding 300 m, for example, not exceeding 100 m. In other embodiments, the sintered article has different lengths L. Such continuous long lengths, especially for the materials and qualities disclosed herein, may be surprising to those skilled in the art without the techniques disclosed herein (e.g., controlled separation, tension control, sintering zones, binder removal techniques, etc.).
[0265] In one or more embodiments, the body of the sintered article comprises sintered inorganic material. In one or more embodiments, the inorganic material comprises an interface with a main interface size of less than about 1 mm. As used herein, when applied to inorganic materials, the term "interface" is defined as including chemical heterogeneity or crystal structure heterogeneity, or both.
[0266] Exemplary inorganic materials include ceramic materials and glass-ceramic materials. In some embodiments, inorganic materials may include any one or more of the following: piezoelectric materials, thermoelectric materials, pyroelectric materials, variable resistance materials, or optoelectronic materials. Specific examples of inorganic materials include: zirconium oxide (e.g., yttrium-stabilized zirconium oxide), alumina, spinel, garnet, lithium lanthanum zirconium oxide (LLZO), cordierite, andalusite, perovskite, pyrochlore, silicon carbide, silicon nitride, boron carbide, sodium bismuth titanate, barium titanate, titanium diboride, silicon alumina nitride, aluminum oxynitride, or reactive ceramicized glass-ceramics (glass-ceramics formed through a combination of chemical reaction and devitrification, including in-situ reactions between glass frit and reactant powders).
[0267] In one or more embodiments, the sintered article exhibits compositional uniformity over a specific region. In one or more embodiments, the sintered article includes a region of at least 10 square centimeters along its length having a composition (i.e., relative amounts of chemical substances, by weight percentage (%)), wherein at least one component of the composition varies in this region by less than about 3 wt% (e.g., about 2.5 wt% or less, about 2 wt% or less, about 1.5 wt% or less, about 1 wt% or less, or about 0.5 wt% or less). For example, when the inorganic material comprises alumina, the amount of aluminum may vary by less than about 3 wt% over the at least 10 square centimeter region (e.g., about 2.5 wt% or less, about 2 wt% or less, about 1.5 wt% or less, about 1 wt% or less, or about 0.5 wt% or less). Such compositional uniformity can be at least partially attributed to the novel and unique processes disclosed herein, such as: furnace heating zones with individually controlled elements, careful and gentle loading of green strips, and a stable state of continuous strip processing, etc. In other embodiments, at least some of the novel and inventive strips or other products of the technologies disclosed herein may not have such compositional uniformity.
[0268] In one or more embodiments, the sintered article exhibits crystal structure homogeneity over a specific region. In one or more embodiments, the sintered article includes a region of at least 10 square centimeters along its length having a crystal structure in which the weight percentage variation of at least one phase is less than about 5 percentage points. For illustrative purposes only, the sintered article may include at least one phase constituting 20% by weight of the sintered article, and in the said at least 10 square centimeters region, the amount of this phase is from about 15% to about 25% by weight. In one or more embodiments, the sintered article includes a region of at least 10 square centimeters along its length having a crystal structure in which the weight percentage variation of at least one phase is less than about 4.5 percentage points, less than about 4 percentage points, less than about 3.5 percentage points, less than about 3 percentage points, less than about 2.5 percentage points, less than about 2 percentage points, less than about 1.5 percentage points, less than about 1 percentage point, or less than about 0.5 percentage points. Such crystal structure homogeneity can be at least partially attributed to the novel and unique processes disclosed herein, such as: furnace heating zones with individually controlled elements, careful and gentle handling of green strips, and stable conditions in continuous strip processing, etc. In other embodiments, at least some of the novel and inventive strips or other products of the techniques disclosed herein may not have such crystal structure uniformity.
[0269] In one or more embodiments, the sintered article exhibits porosity uniformity over a specific region. In one or more embodiments, the sintered article includes a region of at least 10 square centimeters along its length, where the porosity variation is less than about 20%. As used herein, the term "porosity" describes a volume percentage (e.g., at least 10 volume% or at least 30 volume%), where "porosity" refers to the volume fraction of the sintered article not occupied by inorganic material. Thus, in one example, the porosity of the sintered article is 10 volume%, and over the said at least 10 square centimeters region, this porosity is greater than about 8 volume% to less than about 12 volume%. In one or more embodiments, the sintered article includes a region of at least 10 square centimeters along its length, where the porosity variation is 18% or less, 16% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, 5% or less, 4% or less, or about 2% or less. Such porosity uniformity can be at least partially attributed to the novel and unique processes disclosed herein, such as: furnace heating zones with individually controlled components, careful and gentle handling of green strips, and stable conditions in continuous strip processing. In other embodiments, the novel and inventive strips or other products of at least some of the techniques disclosed herein may not exhibit such porosity uniformity.
[0270] In one or more embodiments, the sintered article exhibits a granular distribution, for example, when observed under a microscope (e.g. Figure 30A The digital images shown are examples of this type of granular distribution structure, and such as Figure 30B (Conceptual side view shown) It includes particles 1034 that protrude generally outward from the body 1030 and have a height H (e.g., average height) of at least 25 nanometers (nm) and / or no more than 150 micrometers (μm) relative to a recessed portion of the surface at the boundary 1032 between the particles 1034. In one or more embodiments, the height H ranges from about 25 nm to about 125 μm, about 25 nm to about 100 μm, about 25 nm to about 75 μm, about 25 nm to about 50 μm, about 50 nm to about 150 μm, about 75 nm to about 150 μm, about 100 nm to about 150 μm, or about 125 nm to about 150 μm. In one or more embodiments, the height H ranges from about 25 nm to about 125 nm, about 25 nm to about 100 nm, about 25 nm to about 75 nm, about 25 nm to about 50 nm, about 50 nm to about 150 nm, about 75 nm to about 150 nm, about 100 nm to about 150 nm, or about 125 nm to about 150 nm. In other embodiments, the height H can be any other size. In other embodiments, processing conditions (e.g., time, temperature) can cause the sintered material to have a height H that is substantially zero. In some embodiments, for the materials and manufacturing disclosed herein, the product (e.g., strip) includes a particle height H of at least 25 nm, such as at least 50 nm, such as at least 75 nm, such as at least 100 nm, such as at least 125 nm, such as at least 150 nm, and / or no more than 200 μm, such as no more than 150 μm, such as no more than 100 μm, such as no more than 75 μm, such as no more than 50 μm. The techniques disclosed herein can be used to control the size and shape of such microstructures, for example, the rate at which the material passes through the furnace, the furnace temperature and temperature distribution, the composition, particle / particle size and density of the inorganic material in the green strip, and other factors disclosed herein.
[0271] The granular profile is, or can be, an indicator of the manufacturing process used to form the sintered article 1000. Specifically, the granular profile is, or can be, an indicator that the article 1000 is sintered into a thin, continuous article (i.e., as a sheet or strip) rather than cut from a burl, and an indicator that the corresponding surfaces 1010, 1020 are not significantly polished. Furthermore, compared to polished surfaces, the granular profile can provide benefits to the sintered article 1000 in some applications, such as light scattering for backlight units of displays, increasing surface area for better coating adhesion, or for culture medium growth. In a contemplated embodiment, the roughness of surfaces 1010, 1020 is about 10 nm to about 1000 nm, for example, about 15 nm to about 800 nm, over a distance of 10 mm along one dimension of the length of the sintered article. In a contemplated embodiment, either or both of surfaces 1010, 1020 have a roughness of about 1 nm to about 10 μm over a distance of 1 cm along a single axis.
[0272] In one or more embodiments, one or both of surfaces 1010 and 1020 may be polished, resulting in the substantial removal of grain boundary grooves and grain irregularities (or protrusions). In a contemplated embodiment, the sintered article 1000 manufactured according to the process disclosed herein may be polished to a surface similar to, for example... Figures 31A-31B As shown, this depends on the specific intended use of the article. For example, using sintered article 1000 as a substrate may not require an extremely smooth surface, and Figures 30A-30B An unpolished surface may be sufficient; however, if the article is to be used as a mirror or lens, polishing may be necessary, such as... Figures 31A-31B As shown. However, as described herein, polishing can be difficult for particularly thin articles or for those that are thin and have a large surface area. As shown, the substrates disclosed herein can also receive coatings, which can alter surface quality (e.g., smoothness).
[0273] Not limited by theory, it is believed that sintered ceramic sheets or other materials cut from pear-shaped molds may not have easily distinguishable particle boundaries on their surfaces, which is different from... Figures 30A-30BArticles produced by pear-shaped die cuttings are not limited by theory; they can typically be polished to correct rough surfaces resulting from the cutting process, such as grooves from wear. However, surface polishing can be particularly difficult or troublesome for very thin articles of sintered ceramics or other materials, increasing in difficulty as such articles become thinner and their surface area increases. However, sintered articles manufactured according to the techniques disclosed herein are less constrained by such limitations because articles manufactured according to the techniques herein can be produced continuously in long strip lengths. Furthermore, the dimensions of the furnace system, as described herein, can be proportionally determined to accommodate and sinter wider articles, as presented herein.
[0274] In some embodiments (e.g., the sintered article 1000 is in the form of a sheet or strip), surface uniformity is achieved by having fewer surface defects on either or both of the first and second surfaces 1010 and 1020. Here, surface defects are abrasives and / or adhesives with a size of at least 15 μm, 10 μm, and / or 5 μm along the respective surface dimensions. In one or more embodiments, one or both of the first main surface 1010 and the second main surface 1020 have fewer than 15, fewer than 10, and / or fewer than 5 surface defects with a size greater than 15 μm, 10 μm, and / or 5 μm per square centimeter. In one example, on average, one or both of the first main surface 1010 and the second main surface 1020 have fewer than 3 or fewer than 1 such surface defects per square centimeter. In one or more embodiments, one or both of the first and second main surfaces have an area of at least 10 square centimeters with fewer than 100 surface defects with a size greater than 5 μm from adhesion or abrasion. As a supplement or alternative, one of the first and second main surfaces has an area of at least 10 square centimeters with fewer than 100 surface defects larger than 5 μm from adhesion or abrasion, while the other of the first and second main surfaces includes surface defects larger than 5 μm from adhesive or abrasion. Therefore, sintered articles manufactured according to the present invention disclosed herein can have high and consistent surface quality. The applicant believes that the high and consistent surface quality of the sintered article 1000 helps to increase the strength of the article 1000 by reducing stress concentration and / or crack initiation sites.
[0275] Sintered articles can be described as having a flatness of about 0.1 μm (100 nm) to about 50 μm over a 1 cm distance along a uniaxial axis (e.g., along the length or width of the sintered article). In some embodiments, the flatness can be in the following ranges: about 0.2 μm to about 50 μm, about 0.4 μm to about 50 μm, about 0.5 μm to about 50 μm, about 0.6 μm to about 50 μm, about 0.8 μm to about 50 μm, about 1 μm to about 50 μm, about 2 μm to about 50 μm, about 5 μm to about 50 μm, about 10 μm to about 50 μm, about 20 μm to about 50 μm, about 25 μm. The flatness can be approximately 50 μm, 30 μm to 50 μm, 0.1 μm to 45 μm, 0.1 μm to 40 μm, 0.1 μm to 35 μm, 0.1 μm to 30 μm, 0.1 μm to 25 μm, 0.1 μm to 20 μm, 0.1 μm to 15 μm, 0.1 μm to 10 μm, 0.1 μm to 5 μm, or 0.1 μm to 1 μm. This type of flatness, combined with the surface quality, surface consistency, large area, thinness, and / or material properties of the materials disclosed herein, can be particularly useful for a variety of applications, such as tough overlays for displays, high-temperature substrates, flexible separators, and other applications. That is, embodiments may be implemented without this flatness. Flatness is measured using the appropriate national standard (e.g., ASTM A1030).
[0276] In one or more embodiments, the sintered article exhibits a striped profile along the width dimension, such as Figure 32 As shown. In one or more embodiments, the body 1030 has a striped profile, and the thickness along its width is substantially constant. For example, the thickness along the entire width is about 0.9t to about 1.1t (e.g., about 0.95t to about 1.1t, about 0.1t to about 1.1t, about 0.105t to about 1.1t, about 0.9t to about 1.05t, about 0.9t to about t, or about 0.9t to about 0.95t), where t is the thickness value disclosed herein. Figure 32As shown, the striped profile comprises two or more undulations along its width. As used herein, an undulation represents a complete cycle. In some embodiments, the striped profile comprises three or more undulations, four or more undulations, five or more undulations, or ten or more undulations along its entire width, with the upper limit of approximately less than about 20 undulations along its entire width. In one or more embodiments, the stripes can be measured as optical distortion. In one or more embodiments, a sintered article can be placed near a zebra board, which consists of a white board with straight black stripes arranged diagonally on the board. When the zebra board is viewed through the sintered article, the distortion of the black stripes can be visually detected and can be measured using methods and tools known in the art. In one example, the distortion can be measured according to ASTM C1048. In other embodiments, such as for articles disclosed herein formed by polishing or any other means, there may be less distortion or no distortion. In other embodiments, the number and / or magnitude of distortion may be greater.
[0277] In one or more embodiments, the sintered article may be flat. In one or more embodiments, a portion of the sintered article or discrete sintered articles (as described herein) may have a three-dimensional shape. For example, in one or more embodiments, a portion of the sintered article or discrete sintered articles may have a saddle shape (having a convex shape along its width and a concave shape along its length, or having a concave shape along its width and a convex shape along its length). In one or more embodiments, a portion of the sintered article or discrete sintered articles may have a c-shape (having a single concave shape along its length). In one or more embodiments, the shape magnitude (which represents the maximum height of a portion of the sintered article or a discrete sintered article as measured from the plane of placement) is less than about 0.75 mm (e.g., about 0.7 mm or less, 0.65 mm or less, 0.6 mm or less, 0.55 mm or less, 0.5 mm or less, 0.45 mm or less, 0.4 mm or less, 0.35 mm or less, 0.3 mm or less, 0.25 mm or less, 0.2 mm or less, 0.15 mm or less, or 0.1 mm or less).
[0278] According to another aspect, embodiments of sintered articles can be described in terms of planarability, or the ability to planarize under standard room temperature (23°C) conditions without heating the sintered article to near its melting or sintering temperature to soften and planarize it. In some embodiments, a portion of the sintered article is planarable. The planarable portion of the sintered article may have a length of about 10 cm or less. In some embodiments, the sintered article may have dimensions described anywhere else herein (e.g., a width of about 5 mm or more, a thickness of about 3 μm to about 1 mm, and a length of about 300 cm or more), and the length of the planarable portion of the sintered article is 10 cm or less. In some embodiments, for example when the sintered article is a discrete sintered article, the entire sintered article is planarable.
[0279] As used herein, flatness is determined by clamping the sintered article (or part of the sintered article) between two rigid parallel surfaces, or by applying surface pressure to the first main surface 1010 of the sintered article (or part of the sintered article) against the rigid surfaces, thereby flattening the sintered article (or part of the sintered article) along a flat plane. Flatness can be measured as the force required to flatten the sintered article (or part of the sintered article) to a distance of 0.05 mm, 0.01 mm, or 0.001 mm from the flattened plane when the sintered article (or part of the sintered article) is clamped between two rigid parallel surfaces. Alternatively, flatness can be measured as the surface pressure applied to the first main surface 1010 to push the sintered article (or part of the sintered article) to a distance of 0.001 mm from the flattened plane when the sintered article (or part of the sintered article) is pushed against the rigid surfaces. Flatness can be measured as the maximum absolute value of the in-plane surface stress (compressive or tensile) on the sintered product (or part of the sintered product) when any flattening method (i.e., sandwiched between or against a rigid parallel surface) is used to flatten the sintered product (or part of the sintered product) to a distance of 0.05 mm, 0.01 mm, or 0.001 mm from the flattened plane. The bending equation σ for thin plate bending can be used. x =Et / 2R(1-ν 2 This stress is determined by [the method described].
[0280] The bending stress equation for thin plates originates from equation σ x =[E / (1-ν 2 )]·(ε x +νε y In the formula, E is the elastic modulus, ν is Poisson's ratio, and ε is the elastic modulus. x and ε yThis represents the strain in the corresponding direction. For a thick beam (where the deflection is much smaller than the beam thickness), ε x It is proportional to the square of the thickness. However, when the beam thickness is significantly smaller than the bending radius (e.g., when a sintered product can have a thickness t of about 20 μm and bend to a bending radius on the order of millimeters), ε y Setting it to 0 is possible. For example... Figure 33 As shown, assume a thin sheet (or sintered product) is bent into a circular ring, where the length L0 of the neutral axis is θxR, where θ is the radius in radians and R is the bending radius, and the length L1 of the outer fiber is θx(R+t / 2), where θ is the radius in radians and R is the bending radius and t is the thickness, and ε on the outer fiber... x It is (L1-L0) / L0, therefore ε x =[θx(R+t / 2)–(θx R)]x 1 / (θx R)=t / 2R. Equation σ x =[E / (1-ν 2 )]·t / 2R becomes the thin plate bending equation above (σ x =Et / 2R(1-ν 2 )).
[0281] In one or more embodiments, when planarized to at least the size described above, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to 25% of the flexural strength of the sintered article (as measured by two-point flexural strength). This stress is defined as the maximum absolute value of the stress determined by the flexural equation of sheet bending, regardless of whether it is compressive or tensile stress. For example, the maximum in-plane stress of the sintered article or a portion thereof may be less than or equal to 24%, 22%, 20%, 18%, 16%, 15%, 14%, 12%, 10%, 5%, or 4% of the flexural strength of the sintered article.
[0282] In one or more embodiments, the sintered article or a portion thereof is planarizable, such that when planarized as described herein, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to 1% of Young's modulus of the sintered article. In one or more embodiments, the maximum in-plane stress of the sintered article may be less than or equal to 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1%, or 0.05% of Young's modulus of the sintered article.
[0283] In one or more embodiments, the sintered article or a portion thereof is planarizable such that when the sintered article or a portion thereof has a thickness of about 40 μm to about 80 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.03 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to 25% of the article's bending strength. In one or more embodiments, the sintered article or a portion thereof is planarizable such that when the sintered article or a portion thereof has a thickness of about 20 μm to about 40 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.015 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to (measured by two-point bending strength) 25% of the article's bending strength. In one or more embodiments, when a sintered article has a thickness of about 3 μm to about 20 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.0075 m, the sintered article or a portion thereof exhibits a maximum in-plane stress (measured by two-point bending strength) less than or equal to 25% of the article's bending strength.
[0284] In one or more embodiments, the sintered article or a portion thereof is planarizable such that when the sintered article or a portion thereof has a thickness of about 80 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.03 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to 25% of the article's bending strength. In one or more embodiments, the sintered article or a portion thereof is planarizable such that when the sintered article or a portion thereof has a thickness of about 40 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.015 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to (measured by two-point bending strength) 25% of the article's bending strength. In one or more embodiments, when the sintered article has a thickness of about 20 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.0075 m, the sintered article or a portion thereof exhibits a maximum in-plane stress (measured by two-point bending strength) less than or equal to 25% of the article's bending strength.
[0285] In one or more embodiments, the sintered article or a portion thereof is planarizable such that when planarized to a distance of 0.05 mm, 0.010 mm, or 0.001 mm from the planarization plane using any planarization method (i.e., sandwiched between or against two rigid parallel surfaces), the sintered article or a portion thereof exhibits a maximum in-plane stress of less than 250 MPa. In one or more embodiments, the maximum in-plane stress may be about 225 MPa or less, 200 MPa or less, 175 MPa or less, 150 MPa or less, 125 MPa or less, 100 MPa or less, 75 MPa or less, 50 MPa or less, 25 MPa or less, 15 MPa, 14 MPa or less, 13 MPa or less, 12 MPa or less, 11 MPa or less, 10 MPa or less, 9 MPa or less, 8 MPa or less, 7 MPa or less, 6 MPa or less, 5 MPa or less, or 4 MPa or less.
[0286] In one or more embodiments, the sintered article or a portion thereof is planarizable such that by clamping it between two rigid parallel surfaces, a force of less than 8N (or 7N or less, 6N or less, 5N or less, 4N or less, 3N or less, 2N or less, 1N or less, 0.5N or less, 0.25N or less, 0.1N or less, or 0.05N or less) is required to planarize the sintered article or a portion thereof to a distance of 0.05mm, 0.010mm, or 0.001mm from planarization.
[0287] In one or more embodiments, the sintered article or a portion thereof is planarizable such that when the sintered article (or a portion thereof) rests against a rigid surface, a pressure of 0.1 MPa or less is required to push the sintered article (or a portion thereof) to a distance of 0.05 mm, 0.010 mm, or 0.001 mm from the planarization plane. In some embodiments, the pressure may be about 0.08 MPa or less, about 0.06 MPa or less, about 0.05 MPa or less, about 0.04 MPa or less, about 0.02 MPa or less, about 0.01 MPa or less, about 0.008 MPa or less, about 0.006 MPa or less, about 0.005 MPa or less, about 0.004 MPa or less, about 0.002 MPa or less, about 0.001 MPa or less, or 0.0005 MPa or less.
[0288] According to another aspect, sintered products can be sintered strip materials rolled into rolls, such as... Figure 34AAs shown. In such embodiments, the rolled sintered article includes a core 1100 and a sintered article 1200 wound around the core (according to one or more embodiments described herein). In one or more embodiments, the core is cylindrical and has a diameter 1240 of less than 60 cm (or about 20 inches). For example, the core may have the following diameters: approximately 55 cm or less, 50 cm or less, approximately 48 cm or less, approximately 46 cm or less, approximately 45 cm or less, approximately 44 cm or less, approximately 42 cm or less, approximately 40 cm or less, approximately 38 cm or less, approximately 36 cm or less, approximately 35 cm or less, approximately 34 cm or less, approximately 32 cm or less, approximately 30 cm or less, approximately 28 cm or less, approximately 26 cm or less, approximately 25 cm or less, approximately 24 cm or less, approximately 22 cm or less, approximately 20 cm or less, approximately 18 cm or less, approximately 16 cm or less, approximately 15 cm or less, approximately 14 cm or less, approximately 12 cm or less, approximately 10 cm or less, approximately 8 cm or less, approximately 6 cm or less, approximately 5 cm or less, approximately 4 cm or less, or approximately 2 cm or less. In other embodiments, the core may be any other shape, and the curvature of the bend around the core may correspond to the diameter scales described above.
[0289] In one or more embodiments, the sintered article wound around the core is continuous and has the dimensions described elsewhere above (e.g., a width of about 5 mm or more, a thickness of about 3 μm to about 1 mm, and a length of about 30 cm or more).
[0290] Winding continuous sintered products (specifically, continuous sintered inorganic materials such as ceramics) onto a core presents several challenges. Firstly, sintered products have a cross-web shape, and the web tension they can tolerate (especially in the binder-free and light yellow states) is extremely low (e.g., g-level tension). Secondly, the modulus of the sintered material can be very high (e.g., up to and including approximately 210 GPa), thus preventing the sintered product from stretching under tension, and potentially resulting in poor roll integrity when wound around the core. Thirdly, during continuous winding, continuous sintered products are prone to agglomeration (i.e., the continuous winding can shift and become misaligned).
[0291] The applicant has discovered that, when a continuously sintered article is wound onto a core, the rolled sintered article of one or more embodiments exhibits excellent integrity through the use of a flexible interlayer support material. In one or more embodiments, the continuously sintered article is arranged on the interlayer support material, and the continuously sintered article and the interlayer support material are wound around the core, such that each continuous winding of the continuously sintered article is separated from each other by the interlayer support material. (Refer to the above) Figure 3The sintered product (or sintered strip material) 40 is wound onto a take-up reel 44. An intermediate layer support material 46 is unwound from or can be unwound from the reel 48, and the intermediate layer support material 46 is wound onto or can be wound onto the take-up reel 44, thereby providing an intermediate layer support material 46 between each layer, between most layers, or between at least some layers of the continuous sintered product 1000 (e.g., sintered product 1200 or sintered strip material 40) on the take-up reel 44. This arrangement forms a roll of sintered material 50.
[0292] See Figure 34B Showing according to an exemplary implementation Figure 34A A specific cross-sectional view of the rolled sintered product 1200 is shown, wherein the sintered product 1200 is rolled twice on the core 1100, and an intermediate layer support material 46 is provided between the sintered product 1200 and the core 1100, and then an intermediate layer support material 46 is provided between the continuous rolls of the sintered product 1200. From Figure 34B Intuitively, when viewed from one end, the sintered article 1200 (in this case, a strip) and the intermediate layer support material 46 form a spiral wound around the core 1100. In other contemplated embodiments, the sintered article may be cut into discrete sheets and still wound around the core, separated from the adjacent winding by the continuous intermediate layer support material 46, for example, when combined, the net length of the sheet is the length L described herein. Figure 34B As shown, in various embodiments, the rolled sintered article according to exemplary embodiments includes an intermediate layer support material 46 between each layer of rolled sintered article (e.g., sintered article 1000, sintered article 1200, or sintered strip material 40). In various embodiments, the intermediate layer support material includes: a first main surface and a second main surface opposite to the first main surface; an intermediate layer thickness (t) defined as the distance between the first and second main surfaces; an intermediate layer width defined as a first dimension perpendicular to the intermediate layer thickness in one of the first or second surfaces; and an intermediate layer length defined as a second dimension perpendicular to both the intermediate layer thickness and the intermediate layer width in one of the first or second main surfaces. In one or more embodiments, the intermediate layer thickness is greater than the thickness of the sintered article. In one or more embodiments, the intermediate layer width may be greater than the width of the rolled sintered article.
[0293] In one or more embodiments, the interlayer support material 46 includes tension (or is under tension) greater than the tension on the continuously sintered article, as measured by a pressure-sensing element. In one or more embodiments, the interlayer support material has a lower modulus (compared to the sintered article), thus stretching under low tension. This is believed to produce higher interlayer roll pressure, improving the integrity of the winding roll. Furthermore, in some embodiments, the tension in the winding roll is controlled by controlling the tension applied to the interlayer support material, and the tension can be gradually reduced as a function of the winding roll diameter. In some such embodiments, the interlayer support material 46 is under tension, while the sintered article (e.g., a strip) is under compression.
[0294] In one or more embodiments, the intermediate support material is thickness-compliant (i.e., its thickness can be reduced by applying pressure to the main surface, and thus can compensate for changes in the cross-web shape or thickness in the sintered article resulting from the sintering process). In some such embodiments, when viewed from the side, the sintered article can be concealed within a roll by the intermediate support material, wherein the intermediate support material contacts adjacent rolls of intermediate support material and at least partially shields and isolates the sintered article, for example, as... Figure 34B As shown, the intermediate layer support material is wider than the sintered article and extends beyond the two edges in the width direction of the sintered article (e.g., strip).
[0295] See Figure 34A In one or more embodiments, the rolled article is situated on a cylindrical core and has a substantially constant diameter 1220 and sidewall width 1230. An intermediate layer of support material enables the continuous or discontinuous sintered article to be wound around the core without causing impact, which increases the sidewall width of the rolled article. In some embodiments, the core includes a circumference and a core centerline along the circumference; the continuous sintered article includes an article centerline along its length and along at least 90% of the length or the entire length of the continuous or discontinuous sintered article; the distance between the core centerline and the article centerline is 2.5 mm or less.
[0296] In one or more embodiments, the frictional forces between the roll article and the continuous or discontinuous sintered article are sufficient to resist lateral impacts from the continuous winding in the coil, even when very low tension is applied to the interlayer support material. A constant tension can be applied to the interlayer support material; however, the tension applied to the inner portion of the roll article toward the core can be greater than the tension applied to the outer portion of the roll article away from the core, because the diameter of the roll article increases from the core to the outer portion as more interlayer support material and continuous sintered article are wound around the core. This compresses or may compress the roll article, preventing or limiting impacts and relative movement between the surfaces of the sintered articles when combined with the friction between it and the interlayer support material and continuous sintered article, thereby at least partially helping to prevent defects.
[0297] In one or more embodiments, the interlayer support material comprises any one or both of a polymer and paper. In some embodiments, the interlayer support material is a combination of a polymer and paper. In one or more embodiments, the interlayer support material may comprise a foamed polymer. In some embodiments, the foamed polymer is closed-cell.
[0298] According to another aspect, the sintered products described herein can be provided as multiple discrete sintered products, as disclosed above, such as... Figure 35 and 36As shown. In one or more embodiments, discrete sintered articles can be formed from roll-shaped or continuous sintered articles, as described herein. For example, discrete sintered articles can be separated from a larger sintered article (which may be a sheet or strip of material) by laser cutting or any other means. In one or more embodiments, each of the plurality of discrete sintered articles has a uniformity or consistency relative to some or all of the other plurality of discrete sintered articles, which may be due to the improved process and material properties described herein. In one or more embodiments, each of the plurality of sintered articles includes: a first main surface, a second main surface opposite to the first main surface, and a body extending between the first and second surfaces. The body comprises sintered inorganic material, and: a thickness (t) defined as the distance between the first and second main surfaces, a width defined as a first dimension perpendicular to the thickness of one of the first or second surfaces, and a length defined as a second dimension perpendicular to both the thickness and the width of one of the first or second surfaces. Intuitively, it can be seen that the discrete sheets or other sintered articles cut from long strips or formed therefrom have a uniform and consistent composition, a uniform and consistent crystal structure, a uniform and consistent thickness, a consistent level of defects, and other properties as disclosed above, which are present or may be present in strips or other elongated articles manufactured using the equipment and processes of the present invention disclosed herein.
[0299] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, as described herein. In one or more embodiments, when planarized, some, most, or each of the plurality of sintered articles exhibit a maximum in-plane stress less than or equal to 25% of the flexural strength of the sintered article (measured by the two-point bending method), defined as the maximum absolute value of the stress determined by the bending equation of sheet bending, regardless of whether it is compressive or tensile stress. For example, the maximum in-plane stress of some, most, or each of the plurality of sintered articles may be less than or equal to 24%, less than or equal to 22%, less than or equal to 20%, less than or equal to 18%, less than or equal to 16%, less than or equal to 15%, less than or equal to 14%, less than or equal to 12%, less than or equal to 10%, less than or equal to 5%, or less than or equal to 4% of the flexural strength of the sintered article.
[0300] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when planarized as described herein, some, most, or each of the plurality of sintered articles exhibits a maximum in-plane stress less than or equal to 1% of the Young's modulus of the sintered article. In one or more embodiments, the maximum in-plane stress of some, most, or each of the plurality of sintered articles may be less than or equal to 0.9%, 0.8%, 0.7%, 0.6%, 0.5%, 0.4%, 0.3%, 0.2%, 0.1%, or 0.05% of the Young's modulus of the respective sintered article.
[0301] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when the sintered article has a thickness of about 40 μm to about 80 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.03 m, the sintered article exhibits a maximum in-plane stress less than or equal to 25% of the article's bending strength. In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when the sintered article has a thickness of about 20 μm to about 40 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.015 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to (measured by two-point bending strength) 25% of the article's bending strength. In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable such that when the sintered article has a thickness of about 3 μm to about 20 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.0075 m, the sintered article or a portion thereof exhibits a maximum in-plane stress less than or equal to (measured by 2-point bending strength) 25% of the article's bending strength.
[0302] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when the sintered article has a thickness of about 80 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.03 m, the sintered article exhibits a maximum in-plane stress less than or equal to 25% of the article's flexural strength. In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when the sintered article has a thickness of about 40 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.015 m, the sintered article exhibits a maximum in-plane stress less than or equal to (measured by two-point flexural strength) 25% of the article's flexural strength. In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable such that when the sintered article has a thickness of about 20 μm (or other thicknesses disclosed herein) and is bent to a bending radius greater than 0.0075 m, the sintered article exhibits a maximum in-plane stress less than or equal to (measured by 2-point bending strength) 25% of the article's bending strength.
[0303] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when planarized to a distance of 0.05 mm, 0.01 mm, or 0.001 mm from the planarization plane using any planarization method (i.e., sandwiched between or against two rigid parallel surfaces), the sintered article exhibits a maximum in-plane stress of less than 250 MPa. In one or more embodiments, the maximum in-plane stress may be about 225 MPa or less, 200 MPa or less, 175 MPa or less, 150 MPa or less, 125 MPa or less, 100 MPa or less, 75 MPa or less, 50 MPa or less, 25 MPa or less, 15 MPa, 14 MPa or less, 13 MPa or less, 12 MPa or less, 11 MPa or less, 10 MPa or less, 9 MPa or less, 8 MPa or less, 7 MPa or less, 6 MPa or less, 5 MPa or less, or 4 MPa or less.
[0304] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable such that when the sintered article is planarized by clamping it between two rigid parallel surfaces to a distance of 0.05 mm, 0.01 mm, or 0.001 mm from the planarization distance, a force of less than 8 N (or 7 N or less, 6 N or less, 5 N or less, 4 N or less, 3 N or less, 2 N or less, 1 N or less, 0.5 N or less, 0.25 N or less, 0.1 N or less, or 0.05 N or less) is required to planarize the sintered article or a portion thereof.
[0305] In one or more embodiments, some, most, or each of the plurality of sintered articles are planarizable, such that when pressed against a rigid surface, a pressure of 0.1 MPa or less is required to push the sintered article to a distance of 0.05 mm, 0.01 mm, or 0.001 mm from the planarization plane. In some embodiments, the pressure may be about 0.08 MPa or less, about 0.06 MPa or less, about 0.05 MPa or less, about 0.04 MPa or less, about 0.02 MPa or less, about 0.01 MPa or less, about 0.008 MPa or less, about 0.006 MPa or less, about 0.005 MPa or less, about 0.004 MPa or less, about 0.002 MPa or less, about 0.001 MPa or less, or 0.0005 MPa or less.
[0306] In one or more embodiments, the thickness of some, most, or each of the plurality of sintered articles is from about 0.7t to about 1.3t (e.g., from about 0.8t to about 1.3t, from about 0.9t to about 1.3t, from about t to about 1.3t, from about 1.1t to about 1.3t, from about 0.7t to about 1.2t, from about 0.7t to about 1.1t, from about 0.7t to about 1t, or from about 0.9t to about 1.1t), where t is the thickness value disclosed herein.
[0307] In one or more embodiments, some, most, or each of the plurality of sintered articles exhibit compositional homogeneity. In one or more embodiments, at least 50% (e.g., about 55% or more, about 60% or more, or about 75% or more) of the plurality of sintered articles comprise regions and compositions in which, (as described herein) at least one component of the composition varies by less than about 3% by weight in said regions. In some embodiments, at least one component of the composition varies by about 2.5% by weight or less, about 2% by weight or less, about 1.5% by weight or less, about 1% by weight or less, or about 0.5% by weight or less in said regions. In one or more embodiments, said region is a sintered article of about 1 square centimeter, or said region is the entire surface area of the sintered article.
[0308] In one or more embodiments, some, most, or each of the plurality of sintered articles exhibit uniform crystal structure. In one or more embodiments, at least 50% (e.g., about 55% or more, about 60% or more, or about 75% or more) of the plurality of sintered articles comprise regions and crystal structures, wherein, in said regions, the weight percentage variation of at least one phase is less than about 5 percentage points (as described herein). For illustrative purposes only, some, most, or each of the plurality of sintered articles may include at least 20% by weight of at least one phase constituting the sintered article, and in at least 50% (e.g., about 55% or more, about 60% or more, or about 75% or more) of the plurality of sintered articles, the amount of this phase present in said regions is about 15% to about 25% by weight. In one or more embodiments, at least 50% (e.g., about 55% or more, about 60% or more, or about 75% or more) of some, most, or each of the plurality of sintered articles comprise regions and crystal structures, wherein, in said regions, the weight percentage variation of at least one phase is less than about 4.5 percentage points, less than about 4 percentage points, less than about 3.5 percentage points, less than about 3 percentage points, less than about 2.5 percentage points, less than about 2 percentage points, less than about 1.5 percentage points, less than about 1 percentage point, or less than about 0.5 percentage points. In one or more embodiments, said region is a sintered article of about 1 square centimeter, or said region is the entire surface area of the sintered article.
[0309] In one or more embodiments, at least 50% (e.g., about 55% or more, about 60% or more, or about 75% or more) of the plurality of sintered articles comprise regions and (as described herein) porosity, the porosity varying by less than about 20%. Thus, in one example, some, most, or each of the plurality of sintered articles has a porosity of 10% by volume, and in at least 50% of the plurality of sintered articles, in the region, this porosity is greater than about 8% by volume and less than about 12% by volume. In one or more specific embodiments, at least 50% of the plurality of sintered articles comprises regions and porosity, in which the porosity varies by 18% or less, 16% or less, 15% or less, 14% or less, 12% or less, 10% or less, 8% or less, 6% or less, 5% or less, 4% or less, or about 2% or less. In one or more embodiments, the region is a sintered article of about 1 square centimeter, or the region is the entire surface area of the sintered article.
[0310] Examples 5-6 and Comparative Examples 7-8
[0311] Examples 5-6 and Comparative Examples 7-8 are discrete sintered products formed from continuous sintered products of quadrilateral or zirconium tetroxide polycrystalline materials. Examples 5-6 were formed according to the processes and systems described herein, while Comparative Examples 7-8 were formed using other processes and systems that do not include at least some of the techniques disclosed herein (e.g., tension control, zoned sintering furnace, airflow control). Examples 5-6 and Comparative Examples 7-8 each have a length of 55.88 mm, a width of 25.4 mm, a thickness of 0.04 mm, and a corner radius of 2 mm. Examples 5-6 and Comparative Examples 7-8 each have a Young's modulus of 210 GPa, a Poisson's ratio (ν) of 0.32, and a g / cm³ of 6 g / cm³. 3 The density (ρ).
[0312] like Figure 35 The illustrated embodiment 5 has a c-shape and a shape size of 0.350 mm. As... Figure 36 The illustrated embodiment 6 has a saddle shape and a size of 0.350 mm. (As shown...) Figure 37 As shown, Comparative Example 7 has a gull-wing shape and a size of 0.350 mm. Figure 38 As shown, Comparative Example 8 has a gull-wing shape and a size of 0.750 mm. Figure 39 The image shows a comparison of the shape and size of each sintered product relative to the plane before planarization.
[0313] The planarability of the embodiments was evaluated using two loading methods described elsewhere in this document (i.e., clamping the sintered article between two rigid parallel surfaces, or applying surface pressure to one of the main surfaces of the sintered article to push the sintered article against a rigid surface, thereby causing the sintered article to planarize along a planarization plane).
[0314] Figure 40 The diagram shows the force (in N) required to flatten each of the sintered articles of Examples 5-6 and Comparative Examples 7-8 to a distance of 0.001 mm from the flattened plane by clamping them between two rigid parallel surfaces. Figure 40 As shown, Examples 5-6 require significantly less force to planarize the sintered articles, indicating greater planarability. Furthermore, the ability to planarize sintered articles with such low force suggests that such articles can be manipulated in downstream processing or subjected to downstream processing without breakage, cracking, or any other form of defect. Downstream processing may include, for example, applying a coating, which may be conductive or non-conductive. This same planarability is also confirmed by measuring the pressure required to planarize each of the sintered articles of Examples 5-6 and Comparative Examples 7-8 to a distance of 0.001 mm from the planarized plane by pushing the sintered articles against a rigid surface. The results are as follows... Figure 41 As shown, this confirms that the planarization required in Examples 5-6 was significantly less than that in Comparative Examples 7-8. Figure 42 The maximum in-plane surface stress in the planarized sintered articles of Examples 5-6 and Comparative Examples 7-8 is shown. Examples 5-6 exhibit stresses less than 11 MPa, while Comparative Examples 7-8 exhibit stresses more than 20 times higher, indicating that the sintered articles of Comparative Examples 7-8 are more likely to fracture, crack, or have defects during downstream processing. The stress locations in Example 5 are shown below. Figure 43A As shown (bottom surface stress when flattened) and as... Figure 43B As shown (top surface stress when planarized). The stress locations in Example 6 are as follows. Figure 44A As shown (bottom surface stress when flattened) and as... Figure 44B As shown (top surface stress when planarized). The stress location in Comparative Example 7 is as follows. Figure 45A As shown (bottom surface stress when flattened) and as... Figure 45B As shown (stress on the top surface when planarized). In Comparative Example 7, on the bottom surface, the central portion exhibits a tensile stress of 208.6 MPa, with compressive stresses of -254.6 MPa on both sides. Correspondingly, on the front surface, the central portion experiences a compressive stress of approximately -208.6 MPa, and tensile stresses of 254.6 MPa on both sides. The stress locations in Comparative Example 8 are shown below. Figure 46AAs shown (bottom surface stress when flattened) and as... Figure 46B As shown (top surface stress when planarized). In Comparative Example 8, on the bottom surface, the central portion exhibits a tensile stress of 399.01 MPa, with compressive stresses of -473.63 MPa on both sides. Correspondingly, on the front surface, the central portion experiences a compressive stress of approximately -399.08 MPa, and tensile stresses of 473.60 MPa on both sides. The high stress at point X in Comparative Examples 7-8 indicates that these sintered articles may fracture along the high-stress location.
[0315] In some semiconductor packages and similar packages containing light-emitting diodes (LEDs), a significant portion of the electrical energy supplied to or through the package may be lost or dissipated as heat. The heat dissipation capability of these semiconductor packages and similar packages may be a limiting factor when attempting to supply additional electrical energy (or current) through the package. Furthermore, in at least some LED-containing packages, the brightness of the LED may be limited by the heat dissipation capability of the LED-containing package. It may be desirable to reduce or maintain the component temperature within the semiconductor package, for example, from approximately 75°C to approximately 85°C.
[0316] In one or more embodiments and see Figure 47 The sintered articles described herein (e.g., sintered article 1000, sintered article 1200, or sintered strip material 40) are directly or indirectly bonded, adhered, connected, or otherwise attached to the substrate 1500 to form a package 2000. The sintered article 1000 may serve as the dielectric in the package 2000. In some embodiments, the package 2000 is a semiconductor package, an electronic package, a power delivery package, a light-emitting diode (LED) package, or the like. Compared to conventional packages, the package 2000 of this disclosure provides improved performance (e.g., heat dissipation, lower thermal resistance, etc.). In other such embodiments, the sintered articles described herein (e.g., sintered article 1000, sintered article 1200, or sintered strip material 40) are the substrate 1500 or another substrate 1500.
[0317] In some embodiments, package 2000 includes an intermediate layer 1300 between substrate 1500 and sintered article 1000. Intermediate layer 1300 may include materials that are bonded, adhered, connected, or otherwise attached to or facilitate attachment of the substrate 1500 and sintered article 1000. Intermediate layer 1300 may include multiple discrete layers bonded or joined together to form intermediate layer 1300. In some embodiments, intermediate layer 1300 is a material with high thermal conductivity, so that heat generated by electronic components (e.g., semiconductor devices or chips) or metal-based layers is conducted through intermediate layer 1300 to substrate 1500. In some embodiments, intermediate layer 1300 has a thermal conductivity greater than that of sintered article 1000. In some embodiments, intermediate layer 1300 has a thermal conductivity less than that of substrate 1500. The intermediate layer 1300 may have a thermal conductivity greater than about 8 W / m·K to about 20 W / m·K, greater than about 8 W / m·K to about 16 W / m·K, or greater than about 8 W / m·K to about 13 W / m·K, or greater than about 9 W / m·K to about 12 W / m·K, for example 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, or 20 W / m·K, including all ranges and subranges therein. In some embodiments, the intermediate layer 1300 is an adhesive-like material. In some embodiments, the intermediate layer 1300 is a compliant material configured to deform and / or withstand shear forces arising from the difference in coefficients of thermal expansion (CTE) between the substrate 1500 and the sintered article 1000 as a result of heating and cooling of the encapsulation 2000.
[0318] In some embodiments, the intermediate layer 1300 comprises a matrix of polyimide, epoxide, or a combination thereof. In some embodiments, the matrix 130 of the intermediate layer may comprise non-conductive particles (e.g., boron nitride), conductive particles (e.g., silver, copper, etc.), or a combination thereof. The conductive and / or non-conductive particles may be uniformly or non-uniformly distributed throughout the intermediate layer matrix 130. In some embodiments, the intermediate layer 1300 is associated with the metal-based layer 1350 and component 1401 (…). Figure 50 (e) The heat is conducted and transferred to the substrate 1500. In some embodiments, the length (L) and width (W) of the intermediate layer 1300 may be substantially similar to one or both of the substrate 1500 and / or the sintered article 1000. In some embodiments, the intermediate layer may have a thickness (t2) of about 0.1 μm to about 100 μm, or about 10 μm to about 75 μm, or about 15 μm to about 35 μm, or even about 20 μm to about 40 μm, for example 5, 10, 15, 20, 25, 30, 35, or 40 μm, including all ranges and subranges therein.
[0319] In one or more embodiments, the substrate 1500 includes: a first main surface 1510, a second main surface 1520 opposite to the first main surface, and a body 1530 extending between the first and second surfaces 1510, 1520. The sintered article 1000 may be directly or indirectly joined, bonded, connected, or otherwise attached to the first main surface 1510 or the second main surface 1520 of the substrate 1500. The body 1530 has: a thickness (t1) defined as the distance between the first main surface 1510 and the second main surface 1520; a width (W1) defined as a first dimension perpendicular to the thickness of one of the first or second surfaces; and a length defined as a second dimension perpendicular to both the thickness and the width of one of the first or second surfaces. In one or more embodiments, the substrate 1500 includes an opposing subsurface 1540 defining the width (W1). In some embodiments, the length and width of the sintered article 1000 and the substrate 1500 are substantially equal (e.g., their lateral dimensions are within 5% of each other). In some embodiments, the thickness (t1) of the substrate 1500 is greater than the thickness (t) of the sintered article 1000 (e.g., the thickness (t) of the sintered article 1000 disclosed herein). In some embodiments, the thickness (t1) of the substrate 1500 is about 25%, about 50%, about 75%, about 100%, about 200%, about 500%, or more greater than the thickness (t) of the sintered article 1000. In some embodiments, the thickness (t1) of the substrate 1500 is about 0.5 mm to about 5.0 mm, or about 1.0 mm to about 2.0 mm, or about 1.0 mm to about 1.6 mm, or even about 1.2 mm to about 1.5 mm. In some embodiments, the substrate 1500 serves as a heat sink for the package 2000. In some embodiments, the substrate 1500 comprises a conductive metal, such as aluminum, copper, or a combination thereof.
[0320] Figure 47 and 48A cross-sectional view of an exemplary package 2000 in which an intermediate layer 1300 bonds a substrate 1500 and a sintered article 1000. A metal-based layer 1350 may be provided on the main surface of the sintered article 1000 opposite to the main surface to which the intermediate layer 1300 is bonded. That is, the sintered article 1000 may include an intermediate layer 1300 on one main surface and a metal-based layer 1350 on the opposite main surface. The intermediate layer 1300 may be applied to one or both of the substrate 1500 and the sintered article 1000. Subsequently, the substrate 1500 and the sintered article 1000 may be assembled or bonded together, with the intermediate layer 1300 located between each of the main surfaces. The intermediate layer 1300 may be activated by thermal energy, photochemical wavelengths, pressure, or other similar methods, thereby bonding, adhesively attaching, joining, or otherwise attaching the substrate 1500 to the sintered article 1000 via the intermediate layer 1300.
[0321] like Figure 47 As shown, one or both of the main surfaces 1510 and 1520 of the substrate 1500 may be patterned to include a groove 1325. The groove 1325 helps to bond the intermediate layer 1300 to the substrate 1500. The groove 1325 also helps to minimize the shear stress experienced by the intermediate layer 1300 due to CTE results between the substrate 1500 and the sintered article 1000. In some embodiments, the groove 1325 covers at least a portion of the main surface of the substrate 1500. The groove 1325 may have a depth of about 0.1 μm to about 1 mm or about 10 μm to about 50 μm in the main surface of the substrate 1500. The intermediate layer 1300 may extend at least partially within the groove 1325 of the substrate 1500. The cross-section of the groove 1325 may be rectangular, square, circular, triangular, or other similar shapes or combinations thereof, and may extend continuously, linearly, or in any other manner on the main surface of the sintered article 1000.
[0322] The metal-based layer 1350 can be directly or indirectly bonded to the sintered article 1000 by electroplating, printing, physical vapor deposition, chemical vapor deposition, sputtering, or other suitable techniques. The metal-based layer 1350 is a conductive material capable of conducting or providing electrical energy (or current) through or through the package 2000. In some embodiments, the metal-based layer is configured to minimize resistance and heat generated along its length. In some embodiments, the metal-based layer 1350 includes copper, nickel, gold, silver, brass, lead, tin, and combinations thereof. The metal-based layer 1350 can be indirectly bonded to the sintered article 1000 via a seed layer 1375. That is, the seed layer 1375 can provide a basis for bonding the metal-based layer 1350 to the sintered article 1000. In some embodiments, bonding the metal-based layer 1350 to the seed layer 1375 of the sintered article 1000 is performed by "reflow" in a reflow oven, thereby electrically connecting the metal-based layer 1350 to other electronic components in the package 2000. In some embodiments, the seed layer 1375 comprises tin, titanium, tungsten, lead, or a combination thereof. The seed layer 1375 can be applied to the main surface of the sintered article 1000 by electroplating, printing, physical vapor deposition, chemical vapor deposition, sputtering, or other suitable techniques.
[0323] In some embodiments, the metal-based layer 1350 may be directly or indirectly bonded to the sintered article 1000 before, during, or after bonding it to the substrate 1500. In some embodiments, the metal-based layer 1350 is a continuous, semi-continuous, or discontinuous array or "loop" on the main surface of the sintered article 1000. In some embodiments, before applying the metal-based layer 1350 and / or seed layer 1375 to the sintered article 1000, portions of one or both main surfaces of the sintered article 1000 may be masked or covered to prevent the application of the metal-based layer 1350 and / or seed layer 1375 to the masked portions of the sintered article 1000. That is, the masked portions of one or both main surfaces of the sintered article 1000 may be used to form a continuous, semi-continuous, or discontinuous array or "loop" of the metal-based layer 1350 and / or seed layer 1375 on the main surface of the sintered article 1000. After applying the metal-based layer 1350 to the unmasked portion of the main surface of the sintered article 1000, the mask can be removed to expose the portion of the main surface where there was previously a mask (on which there is no metal-based layer and / or seed layer). Figure 47 and 49An example of a metal-based layer 1350 as an array on the main surface of a sintered article is provided. The metal-based layer 1350 has a thickness (t3) of about 0.1 μm to about 1 mm or about 2 μm to about 100 μm, about 5 μm to about 70 μm or even about 5 μm to about 50 μm.
[0324] In one or more embodiments, package 2000 includes a semiconductor device or chip 1400. In some embodiments, the semiconductor device 1400 is directly or indirectly bonded, adhered, connected, or otherwise attached to a first main surface 1010 or a second main surface 1020 of substrate 1000. The semiconductor device 1400 may be indirectly bonded to sintered article 1000 via a seed layer 1375, such as... Figure 49 As shown. Semiconductor device 1400 may include one or more light-emitting diodes (LEDs). In some embodiments, semiconductor device 1400 is connected to metal-based layer 1350 via one or more wires 1450. Wires 1450 may be rigid or flexible wires or electrical connectors (e.g., similar to metal-based layer 1350) that electrically connect semiconductor device 1400 and metal-based layer 1350. Figure 47 and 49 The conductive wire 1450 bridges the distance between the semiconductor device 1400 and the metal-based layer 1350. Of course, in one or more embodiments, the conductive wire 1450 may travel along or contact the surface of the sintered article 1300. The conductive wire 1450 may provide electrical power between the metal-based layer 1350 and the semiconductor device 1400. In some embodiments, electrical power operating through the metal-based layer 1350 is transmitted to the semiconductor device 1400 via the conductive wire 1450. In some embodiments, the electrical power provided to the semiconductor device 1400 powers an LED thereon, which emits one or more light wavelengths (λ). The semiconductor device 1400 may include one or more lenses 1405 to amplify or guide the light from the LED thereon. The semiconductor device 1400 may also include a phosphor material 1475, via which it filters and transmits specific wavelengths (λ) of light emitted from the LED.
[0325] In one or more embodiments, a method of manufacturing package 2000 includes providing a sintered article 1000. The sintered article 1000 may be in a roll comprising a circular or cylindrical core with a diameter less than 60 cm, around which a continuous sintered article is wound. The sintered article 1000 may also be provided as a discrete, flat length. In one or more embodiments, a method of manufacturing package 2000 includes providing a carrier or temporary substrate 1499 (see...). Figure 50This can be on a roller or as a large, flat sheet. In some embodiments, the length of the sintered article 1000 is joined, bonded, connected, or otherwise attached to the length of a carrier or temporary substrate 1499 to form a precursor package 1999. The carrier or temporary substrate 1499 can support the sintered article 1000 for subsequent winding onto a core. In some embodiments, the carrier or temporary substrate 1499 supports the sintered article 1000 during subsequent processes that may damage, degrade, or harm the substrate 1500. In some embodiments, the carrier or temporary substrate 1499 comprises glass, a polymer, or a combination thereof. In some embodiments, the carrier or temporary substrate 1499 is a polymer strip or a polyamide strip.
[0326] In some embodiments, the precursor encapsulation 1999 includes a precursor interlayer 1299 between the sintered article 1000 and the temporary substrate 1499. Figure 50 The precursor intermediate layer 1299 may include a material that bonds, adheres, connects, or otherwise attaches the temporary substrate 1499 and the sintered article 1000. In some embodiments, the precursor intermediate layer 1299 is a high-temperature resistant adhesive. The precursor intermediate layer 1299 may be activated by thermal energy, photochemical wavelengths, pressure, or other similar methods to bond, adhere, connect, or otherwise attach the temporary substrate 1499 to the sintered article 1000. In some embodiments, the precursor intermediate layer 1299 may be deactivated by a method similar to or different from activation, thereby separating or disconnecting the sintered article 1000 from the temporary substrate 1499. In some embodiments, the precursor intermediate layer 1299 and the temporary substrate 1499 are configured to withstand subsequent processing (without degradation) of the precursor package 1999, including the application of a metal-based layer 1350, a seed layer 1375, a semiconductor device 1400, a wire 1450, and / or other similar components.
[0327] Figure 50 This illustrates the method of forming package 2000 from precursor package 1999. Figure 50 Step (a) in the diagram shows the precursor encapsulation 1999 after applying a metal-based layer 1350 to the main surface opposite the surface of the sintered article 1000 to which the precursor intermediate layer 1299 is bonded. Figure 50 Step (a) also shows the removal of the mask (e.g., between metal-based layers 1350) from the sintered article 1000 after the preform package 1999 has been removed. A seed layer 1375 may be applied to the sintered article 1000 before or after step (a). Figure 50Step (b) shows the application of components of assembly 1401 (i.e., semiconductor device 1400 and wire 1450) to the sintered article 1000, thereby electrically connecting the semiconductor device 1400 and the metal-based layer 1350. In some embodiments, the carrier or temporary substrate 1299 and the precursor intermediate layer 1299 are configured to support the sintered article 1000 and are completed, possibly at high temperatures (e.g., up to or greater than 320°C). Figure 50 No degradation or deformation occurs during steps (a) and (b) shown. Figure 50 Step (c) shows the separation of the sintered article 1000 (including the metal-based layer 1350, the semiconductor device 1400, and the wires 1450 thereon) from the temporary substrate 1499. In some embodiments, step (c) can be performed by deactivating the precursor intermediate layer 1299 using thermal energy, photochemical wavelengths, dragging, or other similar methods. In some embodiments, the sintered article 1000 (including the metal-based layer 1350, the semiconductor device 1400, and the wires 1450 thereon) is pulled away from the temporary substrate 1499 by machine or by hand. In some embodiments, step (c) is performed in a reflow oven when the seed layer 1375 or solder electrically connects the components of the assembly 1401. The precursor intermediate layer 1299 may be transported together with the sintered article 1000, the temporary substrate 1499, or both (a portion of each). Figure 50 Step (c) shows an embodiment in which the precursor intermediate layer 1299 is transported together with the temporary substrate 1499. In some embodiments, the precursor intermediate layer 1299 may become intermediate layer 1300 during subsequent processing (e.g., heating) or by bonding or contacting with the substrate 1500. Figure 50 Step (d) shows the bonding of the sintered article 1000 and the substrate 1500, with the intermediate layer 1300 located therebetween. In some embodiments, the precursor intermediate layer 1299 may be the same as the intermediate layer 1300. Figure 50 Step (e) shows the application of other components of assembly 1401 (e.g., lens 1405 and phosphor 1475) to sintered article 1000. In some embodiments, components of assembly 1401 can be applied at lower temperatures (e.g., <150°C) so that the intermediate layer 1300 and substrate 1500 do not degrade or deform during the completion of assembly 1401. Figure 50 The package 2000 shown in step (e) may include one or more of the components 1401.
[0328] Figure 51 Another illustrative method for forming package 2000 from precursor package 1999 is provided. Figure 51 Step (a) shows the sintered product 1000, which is provided from the rolled core as a flat sheet or in any other manner, and is planarized. Figure 51 Step (b) shows the joining of the planarized sintered article 1000 and the carrier or temporary substrate 1499 to form a precursor package 1999. A precursor intermediate layer 1299 or a similar layer may be located between the sintered article 1000 and the carrier or temporary substrate 1499. The precursor package 1999 may be rolled onto a core and stored, shipped, or sold for subsequent processing. Figure 51 Step (c) shows the application of a metal-based layer 1350 and components of the light-emitting assembly 1401 (e.g., semiconductor device 1400, wire 1450, lens 1405, phosphor 1475, etc.) to the sintered article 1000. Step (c) may include several stages of electrically connecting the metal-based layer 1350 to the semiconductor device 1400 and any LEDs thereon on the sintered article 1000. Step (c) also includes a solder reflow operation in a solder oven, thereby electrically connecting all components of the assembly 1401. Figure 51 Step (d) illustrates the separation or detachment of the sintered article 1000 (including component 1401) from the temporary substrate 1499. Step (d) can be accomplished by pulling the sintered article 1000 (including component 1401) away from the temporary substrate 1499 by machine or by hand. Step (d) can be catalyzed by heat, exposure to photochemical wavelengths, cooling, exposure to solvents, or other similar methods. Of course, if present, the precursor intermediate layer 1299 can be transported together with the sintered article 1000, the temporary substrate 1499, or both (a portion of each). Figure 51 Step (e) shows the sintered article 1000 (including component 1401) being bonded to the substrate 1500 to form the package 2000. In some embodiments, the sintered article 1000 (including component 1401) and the substrate 1500 may be bonded to the package 2000 via an intermediate layer 1300 or a similar layer therebetween. Figure 51 Step (f) shows cutting the package 2000 at different points along its length L4 into multiple segments 2001. The package 2000 can be cut into segments 2001 along its length L4 using localized cutting pressure, laser energy (e.g., UV ablation laser), or similar techniques. In some embodiments, each segment 2001 includes at least one or more components 1401. The segments 2001 of the package 2000 can be used in a variety of applications, including filaments for light bulbs, electronic devices, handheld devices, head-mounted displays, vehicle dashboards, etc.
[0329] Figures 52-54This diagram shows a cross-sectional view of package 2000, which includes a flip-chip configuration of sintered article 1000 and semiconductor device 1400. In these embodiments, a section of package 2000 may include apertures 1501 in substrate 1500. Apertures 1501 can be formed by drilling, cutting, or partially removing substrate 1500. Apertures 1501 can also be formed by spacing two substrates 1500 on a main surface of sintered article 1000. In some embodiments, a metal-based layer 1350 may be bonded, adhered, joined, or otherwise attached to the same main surface of sintered article 1000 as substrate 1500.
[0330] Figure 52 Showing an exemplary cross-sectional view of package 2000, which includes a sintered article 1000 bonded to a substrate 1500. In some embodiments, a metal-based layer 1350 is provided in apertures 1501. That is, the metal-based layer 1350 is bonded to the main surface of the sintered article 1000, which is the same as the substrate 1500. In some embodiments, a seed layer 1375 is applied to the metal-based layer 1350 and bonding occurs. The seed layer 1375 helps bond the metal-based layer 1350 and the semiconductor device 1400 in a "flip-chip" configuration. In one or more embodiments, the seed layer 1375 comprises tin, titanium, tungsten, lead, or alloys thereof. In some embodiments, the seed layer 1375 is conductive and eliminates the need for wires to electrically connect the metal-based layer to the semiconductor device 1400. In some embodiments, a volume 1485 may be formed between the sintered article 1000 and the semiconductor device 1400. Together with the metal-based layer 1350 and / or seed layer 1375, volume 1485 can be sealed between the sintered article 1000 and the semiconductor device 1400. In some embodiments, the LED on the semiconductor device 1400 is the opposite volume 1485 and is located within the aperture 1501. In some embodiments, the LED on the semiconductor device 1400 is within volume 1485. Phosphor material 1475 may be provided within volume 1485. Figure 52 and 53In this embodiment, the sintered article 1000 may be translucent or substantially transparent, allowing light wavelengths (λ) emitted from the LED on the semiconductor device 1400 to propagate through the sintered article 1000. In some embodiments, the sintered article 1000 may transmit some, most, or all of about 35% to about 95%, or about 45% to about 85%, or about 55% to about 75% of the visible light wavelengths (λ) emitted from the LED or transmitted through the phosphor 1475, for example, 35%, 40%, 50%, 60%, 65%, 75%, 85%, 90%, 95%, or more up to 99%, including all ranges and subranges therein.
[0331] The total light transmittance (T) through 1000 of the sintered product can be defined by the following Equation 1:
[0332] T = Φ e t / Φ e i
[0333] In the formula,
[0334] Φ e t It is the radiative flux transmitted through the surface; and
[0335] Φ e i It is the radiant flux received by the surface.
[0336] The measurements of these parameters are described in ASTM standard test method D1003-13.
[0337] Although similar to Figure 52 ,but Figure 53 The intermediate layer 1300 shown is located between the sintered product 1000 and the substrate 1500. Figure 53 It also shows such an implementation, wherein, (e.g.) Figure 52 At least a portion of the pore 1501 (as shown) is blocked by the substrate 1500, which may be isolated from or connected to adjacent portions of the substrate 1500. In other embodiments, at least a portion of the pore 1501 is blocked by a filler (e.g., epoxide, plastic, polymer material, etc.) to seal the chip 1400 and the metal-based layer 1350 within the package 2000. Figure 53 In this embodiment, the substrate 1500 contacts the semiconductor device 1500, thereby conducting heat generated when electrical power is supplied to the package 2000 from the semiconductor device 1400. In some embodiments, the sintered article 1000 includes holes 1490 extending through its thickness. For example... Figure 53 and 55As shown, the hole 1490 in the sintered product 1000 intersects with the volume 1485. The hole 1490 allows cooling of the phosphor material 1475 within the volume 1485 via ambient convection. The hole 1490 also allows light of the wavelength (λ) from the LED within the volume 1485 to be emitted from the package 2000. Figure 54 As shown, a reflector 1480 may be included in volume 1485 and / or aperture 1490 to amplify or reflect the light wavelength (λ) emitted from the LED on semiconductor device 1400. The reflector 1480 may have a conical, hemispherical, tapered, or curved shape. In some embodiments, the reflector 1480 may be coated with a coating to amplify the light wavelength (λ) emitted from the LED on semiconductor device 1400. Figure 55 This shows another possible construction.
[0338] In one or more embodiments, the sintered articles described herein can be used in microelectronic applications or articles. For example, such microelectronic articles may include sintered articles (according to one or more embodiments described herein) comprising a first main surface and a second main surface opposite the first main surface. In one or more embodiments, the microelectronic articles may include continuous sintered articles (e.g., long strips as described herein) or discrete sintered articles (e.g., sheets cut or segmented from strips). In one or more embodiments, the microelectronic articles include continuous or discrete sintered articles with a width of about 1 mm or more, about 1 cm or more, about 5 cm or more, or about 10 cm or more. In one or more embodiments, the microelectronic articles include sintered articles with a length of about 1 m or more, about 5 m or more, or about 10 m or more. In one or more embodiments, the microelectronic articles include continuous or discrete sintered articles with a thickness of less than 1 mm, about 0.5 mm or less, or 300 micrometers or less, about 150 micrometers or less, or about 100 micrometers or less. In one or more embodiments, the microelectronic article includes a sintered article having a crystalline ceramic content of about 10% or more, about 25% or more, about 50% or more, about 75% or more, or about 90% or more.
[0339] In one or more embodiments, the sintered article includes one or more channels (e.g., holes, pores, wells, tubes, channels, connectors; see also) arranged along a given region of a first main surface of the sintered article. Figure 53(1490) In one or more embodiments, the channels extend partially or completely through the thickness of the sintered article. In one or more embodiments, the channels may be arranged in a repeating or periodic pattern, for example, wherein the channels are formed along a strip using a continuous roll-to-roll process, wherein the strip may later be segmented to form individual components, such as for semiconductors or other electronic devices. In one or more embodiments, the channels are spaced apart such that there is a distance of about 0.5 m or less, 10 cm or less, or 5 cm or less between the channels (e.g., at least some, most, or each channel and its nearest neighbor). In some embodiments, such channel spacing may exist in sintered articles with a thickness of less than 1 mm, about 0.5 mm or less, or 300 micrometers or less, about 150 micrometers or less, or about 100 micrometers or less. In one or more specific embodiments, such channel spacing may exist in sintered articles with a thickness of about 50 micrometers or less. Channels can be cut using lasers, masking and etchants, punching, or other methods; for example, before sintering, during sintering (e.g., during partial sintering), or after sintering. Forming channels after sintering can help to accurately place and determine the dimensions of the channels; however, due to the consistency of the processes and materials described herein, channels can be formed, for example, in green strips or partially sintered strips, and the accuracy of placement, size, wall geometry, etc., can be within the tolerances required for some applications.
[0340] In one or more embodiments, the sintered article includes a conductive layer (e.g., copper, aluminum, or other conductive layer; see also) disposed on a first main surface, a second main surface, or simultaneously on both the first and second main surfaces. Figure 47Layer 1350). In one or more embodiments, the conductive layer partially or completely covers the main surface on which it is disposed, for example, overlapping at least 20%, such as 40%, at least 60%, or at least 80%, of the corresponding surface. In other words, the conductive layer may form a continuous layer over the entire area of the surface on which it is disposed, or it may form a discontinuous layer on the surface on which it is disposed. The conductive layer may form a repeating or periodic pattern, for example, forming undivided semiconductor components on a strip. In one or more embodiments, the sintered article may include one or more additional layers disposed on top of the conductive layer or disposed between the conductive layer and the sintered article and / or between the conductive layer and the strip (or other sintered article disclosed herein). Such one or more additional layers may partially or completely cover the surface on which it is disposed (i.e., the main surface of the sintered article or the conductive layer), for example, according to the percentage described above with respect to the conductive layer. In other words, the one or more additional layers may form a continuous layer over the entire area of the surface on which it is disposed, or it may form a discontinuous layer on the surface on which it is disposed. The one or more additional layers may form a pattern that may be repeating or periodic. In some embodiments, the one or more additional layers may also be conductive layers, dielectric layers, sealing layers, adhesive layers, smooth surface layers, or other functional layers. In some embodiments, the conductive layer and optionally the one or more additional layers may be present in sintered articles with a thickness of less than 1 mm, about 0.5 mm or less, or 300 micrometers or less, about 150 micrometers or less, about 100 micrometers or less, or about 50 micrometers or less. Therefore, the layers and sintered articles may be flexible and / or may be wound onto rollers or reels, as described herein.
[0341] In some embodiments, the sintered article may include two or more of a plurality of channels, conductive layers, and one or more additional layers.
[0342] In one or more embodiments, the system 10 for producing sintered strip articles may include a manufacturing system for further processing the green strips, partially sintered articles, and / or sintered articles described herein for use in microelectronic articles. In one or more embodiments, the manufacturing system may be arranged downstream of the binder removal furnace 110 but upstream of the sintering station 38 to process binder-free strips, or after the sintering station 38 to process partially sintered articles, or before the furnace 110 to process the green strips, which are then sintered as described elsewhere herein. In one or more embodiments, the manufacturing system may be arranged downstream of the sintering station 38 but upstream of the take-up system 42 to process sintered articles. In one or more embodiments, the manufacturing system may be arranged downstream of the take-up reel 44 but upstream of the reel 48 to process sintered articles. In one or more embodiments, the manufacturing system may be arranged downstream of the reel 48 to process sintered articles. In such embodiments, the manufacturing system processes green strip material, partially sintered products, or sintered products as they are processed continuously (not discretely). Other configurations may process sintered products as discrete products.
[0343] In one or more embodiments, the manufacturing system may expose at least a portion of the green strip material, a partially sintered article, or a sintered article to a mechanism for forming channels, such as laser energy or drilling. One or more embodiments of the manufacturing system using laser energy to generate channels may include a hub drum with surface curvature (see also...). Figure 6 The vacuum drum 25, wherein the drum pulls the green strip material, the partially sintered article, or the sintered article to match its curvature, thereby facilitating the formation of channels on the main surface of the sintered article. In one or more embodiments, the drum helps to focus a laser beam onto the main surface of the green strip material, the partially sintered article, or the sintered article.
[0344] In one or more embodiments, the channels can be created by mechanical means. For example, the manufacturing system may include a flat plate on which green strip material, partially sintered articles, or fired articles are temporarily fixed. In this way, a main surface of the green strip material, partially sintered articles, or fired articles is in contact with the flat plate. The green strip material, partially sintered articles, or fired articles can be transferred to the manufacturing system using stepping and repetitive movement, acceleration or deceleration, or continuous speed to temporarily fix a portion of the sintered article to the flat plate. In one or more embodiments, a vacuum can be used to temporarily fix a portion of the green strip material, partially sintered articles, or fired articles to the flat plate.
[0345] In one or more embodiments, the manufacturing system can form channels by mechanically separating a portion of the green strip material, partially sintered article, or fired article. In one or more embodiments, the manufacturing system may include using a photolithography solvent or acid to remove a portion of the green strip material, partially sintered article, or fired article. In such embodiments, when the manufacturing system is applied to the green strip material or partially sintered article, the manufacturing system may include a control mechanism to control the size of the holes and the pattern size because the green strip material or partially sintered article shrinks when fully sintered. For example, the control mechanism may include a sensor at the exit of the sintering workstation 38 that measures the distance between channels and the spacing between channels and feeds this information back to the manufacturing system for adjustment. For example, if a manufacturing system forms channels with a diameter of approximately 75 micrometers and a spacing or pitch between the channels of 500 micrometers, and assuming the total sintering shrinkage from green strip material to sintered product is 25%, the manufacturing system can be adjusted to form channels with a pitch of 667 micrometers and a diameter of approximately 100 micrometers in the green strip material. After processing, if the total sintering shrinkage is measured to be 23%, the manufacturing system can then be further adjusted to the correct channel spacing in the green strip material, which would be 649 micrometers, to accommodate the 23% total sintering shrinkage. In some embodiments, the widest cross-sectional dimension of the channel (coplanar with the surface of the sheet or strip) is at least 250 nm, for example, at least 1 μm, for example, at least 10 μm, for example, at least 30 μm, for example, at least 50 μm and / or no more than 1 mm, for example, no more than 500 μm, for example, no more than 100 μm. In some embodiments, the channels are filled with a conductive material, for example, copper, gold, aluminum, silver, alloys thereof, or other materials. Channels can be formed by laser cutting, laser and etchant, mechanical drilling, or any other method. Channels can be arranged in a repeating pattern along a sheet or strip, which can then be divided into individual electronic components.
[0346] Figure 104 This is an example of a cross-section of a stacked arrangement 810 of ceramic sheets 812 with channels 814 extending into the metal layer 816. A reference 818 helps align the sheets 812.
[0347] The system 10 described herein provides other methods for controlling the channel spacing during the sintering process. For example, during sintering, tension in the processing direction 14 can stretch the sintered article and cause a bias in sintering shrinkage. This tension can increase the channel spacing in the processing direction 14, effectively reducing sintering shrinkage in the processing direction 14. When tension is applied, different sintering is observed in the processing direction 14 relative to the direction perpendicular to the processing direction 14, and the range is from about 2% to about 3%. Therefore, some other rounded channels can be oval or elliptical.
[0348] The size and shape of the channel can be controlled and adjusted by the following combination: sintering shrinkage in a direction parallel to the processing direction 14, sintering shrinkage in a direction perpendicular to the processing direction 14, tension in these two directions, and the shape of the sintering workstation 38, and / or by using air bearings to transport green strip material, partially sintered products, or sintered products during sintering or when hot.
[0349] In one or more embodiments, ceramic material can be added at any step within system 10 to reduce sintering shrinkage. Ceramic material can be added via an inkjet printhead, which can uniformly apply such ceramic material to a porous partially sintered article or sintered article having open porosity. In one or more embodiments, a small amount of ceramic material can be added to a porous partially sintered article or sintered article via printing. Laser, photolithography, inkjet, atomic layer deposition, and some printing and other processing methods can be used, either from the inner radius of a bent air bearing or by utilizing a segmented drum with open areas (for exposing a partially sintered article or sintered article to processing equipment). Therefore, a portion of the strips or other articles disclosed herein can be or may include two or more co-fired inorganic materials (e.g., ceramics or phases), such that one material permeates and fills the pores of another material. In the contemplated embodiments, the filling / permeating material can be chemically identical to the porous material, but can be distinguished by crystal content (e.g., grain size, phase).
[0350] In one or more embodiments, channels can be formed on a sintered article having a pattern of conductive layers on one or both sides. The conductive layer can be printed or patterned (screen printing, electrodeposition, etc.) after the channels are formed and final sintering. In one or more embodiments, the conductive layer can also be printed or deposited before the final sintering of the sintered article. In some sintering processes where only discrete (not continuous) pieces (e.g., length and width dimensions of approximately 20 cm by 20 cm) are sintered, the conductive layer is printed after channel formation and / or only on the green strip material. For multilayer substrates, up to 30-40 green strip layers are used, such that individual green strip layers are aligned and stacked with some multilayer substrates. Copper-based conductors, alumina, and tungsten, molybdenum, or platinum conductors can be co-sintered to form a low-sintering ceramic encapsulation based on cordierite (glass ceramic). In some embodiments described herein, the conductive layer can be formed prior to the final sintering step (i.e., by printing or deposition), and the techniques disclosed herein can help control the size of the channels and conductor patterns during the sintering step.
[0351] Furthermore, the continuous sintering process and system 10 provide a means of controlling the channel spacing and patterning, as well as the conductive layer patterning in terms of spacing, during the sintering process. During sintering, tension in the processing direction can stretch the green strip material, the partially sintered product, or the sintered product and / or cause sintering shrinkage bias, as disclosed above. This tension can increase the channel spacing and patterning, as well as the conductive layer patterning, in the processing direction, effectively reducing sintering shrinkage in the processing direction. The range of sintering in the processing direction versus the direction perpendicular to the processing direction can be from about 2% to about 3%, for example, when the strip is stretched in the processing direction or the length direction.
[0352] A controlled curvature sintering workstation 38 or a bending air bearing can be used to transport green strip material, partially sintered products, or sintered products in the processing direction 14, and can prevent excessive curvature in the width of the green strip material, partially sintered products, or sintered products. If a moderate on-strip or sheet curvature exists, tension in a direction parallel to the processing direction can provide some tension perpendicular to the processing direction to control or limit deformation.
[0353] Applying tension in a direction perpendicular to the processing direction 14 would be difficult, especially for sintered products that are plastically deformable and / or for sintered products that are plastically deformable at the temperatures during sintering. In such areas of system 10 (or more specifically, sintering workstation 38), rollers angled relative to a direction parallel to the processing direction 14 (see, for example) Figure 88B A tension can be applied perpendicular to the processing direction 14 (e.g., the width direction of the strip). This tension can increase the spacing of the channels perpendicular to the processing direction 14, effectively reducing sintering shrinkage perpendicular to the processing direction 14.
[0354] Alignment reference marks can be manufactured using lasers, mechanical methods, or chemical methods (e.g., slight compositional changes with visible results). These marks aid in alignment for further processing steps, such as conductor printing, patterning, and / or lamination.
[0355] Another aspect of this disclosure pertains to multilayer sintered articles having a width of about 1 mm or more, about 1 cm or more, 5 cm or more, 10 cm or more, or 20 cm or more, and a length of 1 m or more, 3 m or more, 5 m or more, 10 m or more, or 30 m or more, wherein the sintered article has a thickness of less than 1 mm, less than about 0.5 mm, less than about 300 micrometers, less than about 150 micrometers, or less than about 100 micrometers. In one or more embodiments, the sintered article has a crystalline ceramic content of more than 10% by volume, more than 25% by volume, more than 50% by volume, more than 75% by volume, or more than 90% by volume. The article has at least two sintered articles and may have more than 40 such layers. The thickness of the sintered article layers is 150 micrometers or less, 100 or less, 75 or less, 50 or less, 25 or less, 20 or less, 15 or less, 10 or less, 5 or less, and / or, for example, at least 3 micrometers (i.e., at least 3 micrometers). In one or more embodiments, the sintered product layers do not need to be of the same composition, and some of these layers include glass. In some embodiments, such glass layers may include 100% glass, such as at least 100% amorphous silicate glass.
[0356] In one or more embodiments, the multilayer sintered article includes multiple channels, conductive layers, and / or optional additional layers, as described herein with respect to microelectronic articles.
[0357] In one or more embodiments, system 10 may include processes and equipment for manufacturing such multilayer sintered articles. Multilayers can be manufactured by casting or meshing multiple layers of green strip material (i.e., ceramic particles with a polymer binder) onto each other. The multilayer green strip material structure can then be processed using system 10 as described herein. In one or more embodiments, the multilayer green strip material structure can also be formed by continuously stacking multiple green strips containing ceramic particles at near room temperature, and then feeding the stacked strips into system 10. Partially sintered articles can also be stacked together under low pressure in a sintering station 38. Pressure can be induced by having a moderate curvature in the sintering station 38, through which the partially sintered articles are drawn. Each partially sintered article may have its own tension and output speed control mechanism. Each partially sintered article may have reference marks to aid in article alignment. Tension and output speed can be used to match sintering shrinkage between articles, thereby aligning the channels and conductors between articles. If the reference marks are not aligned when the multilayer product leaves the furnace, the layer output speed and / or tension can be adjusted to bring the layers back to alignment. Additional pressure perpendicular to the length and width of the multilayer product can be provided using rollers at high temperature, as described above.
[0358] Because the conductors and ceramic materials in multilayer electronic substrates may not have the same coefficient of thermal expansion, some designs can be provided for overall stress reduction (balancing) from the "top" side to the "bottom" side of the multilayer sintered product. Generally, such designs have similar amounts of metal or ceramic on the top and bottom of the multilayer, for example, making the layers mirror images of the center plane in the corresponding stack. For thin ceramic layers, structures with unbalanced stress / CTE may experience ceramic deformation and / or curling of the entire stack structure.
[0359] In one or more embodiments, the electronic circuit board includes a sintered article as described herein, on which conductors are patterned. The conductors for the circuit board can be printed directly onto a green strip material, a partially sintered article, or a sintered article, and / or can be printed onto a coating or layer bonded to the green strip material, the partially sintered article, or the sintered article, such as an adhesion-promoting layer, a surface-smoothing layer, and / or other functional layers. Printing can be from direct screen printing, electrodeposition and patterning, photolithography, using a silicone carrier located between pattern formation and the application of the pattern onto the sintered article via a gravure patterning roller and / or other processes.
[0360] Conductors for circuit boards can be printed directly onto partially sintered products, and / or onto coatings thereon, after intermediate sintering steps but before final sintering. The porosity of partially sintered products or sintered products can improve the adhesion of conductor printing or patterns. Printing can be performed via direct screen printing, photolithography, or using a silicone carrier positioned between pattern formation and the application of the pattern onto the ceramic via gravure patterning rollers or other processes.
[0361] One aspect of the process and equipment is the simultaneous patterning of long, continuous porous ceramic strips or sheets using a drum. The drum pulls the ceramic strip or sheet to match the curvature of the drum surface, making the printing of the conductor pattern less difficult. Photolithography can also be performed on the drum to etch or wash away some of the conductor pattern on the green strip or sheet using solvents or acids before final sintering. When patterning conductors before final sintering, it is recommended to use patterns, sizes, gauges, or pitches that control sintering shrinkage. Unfortunately, the sintering shrinkage of ceramic strips or sheets can vary by a percentage or more between one continuous green strip (or sheet) and sometimes even within a single green strip or strip. One method to ensure accurate spacing of the conductor patterns is to have sensors at the exit of the final sintering step and measure the spacing between the conductor patterns. This information can be fed into the method of patterning (e.g., laser, drilling, punching, etching systems) and the method of photolithography exposure (e.g., radiation or light source, masking) to adjust the conductor pattern in the strip or sheet before final sintering to match existing sintering shrinkage. (The length of the strip or sheet between the measuring device and the “patterning” device may not be perfectly precise; however, it can be more accurate than batch sintering in a periodic furnace or using a tunnel furnace (e.g., where inaccuracies could lead to significant losses of the final product).
[0362] Continuous sintering (e.g., continuous firing of ceramics via roll-to-roll sintering) provides another way to control the channel spacing during the sintering process. Tension applied in the roll transport direction (i.e., the length direction of the strip) during sintering can stretch the sintered product (e.g., strip or sheet) and / or bias sintering shrinkage. This tension can increase the spacing of the conductor patterns in the strip or sheet transport direction, effectively reducing sintering shrinkage in the strip transport direction. When tension is applied, a difference in sintering is observed between the strip transport direction and the direction perpendicular to the strip transport direction, up to 2-3%.
[0363] Photolithography, inkjet printing, atomic layer deposition, some printing, and other processing methods can be performed by bending the inner radius of the air bearing or by using segmented drums with open areas (used to expose ceramic strips or strips to conductor patterning equipment).
[0364] Using copper-based conductors, alumina and tungsten, molybdenum or platinum conductors can be co-sintered with other inorganic materials disclosed herein to form low-sintering ceramic encapsulations based on cordierite (glass ceramic).
[0365] In some such embodiments, the ceramic strip or roll with a conductor pattern being pulled through or onto a kiln device or a bending air bearing with a controlled curvature can keep the ceramic strip or sheet with the conductor pattern from excessive curvature over a short length of the strip perpendicular to the direction of bag transport.
[0366] Applying tension in a direction perpendicular to the belt transport direction (the transverse direction of the roll) can be difficult, especially at temperatures where the ceramic strip with a conductor pattern is plastically deformable or sintered and plastically deformable. In the hot zone of the furnace, rollers angled relative to the belt transport direction can apply tension perpendicular to it. This tension increases the channel spacing perpendicular to the belt transport direction, effectively reducing sintering shrinkage perpendicular to the belt transport direction. The size and pitch of the conductor pattern can be controlled and adjusted by a combination of: sintering shrinkage along the direction parallel to the belt transport direction (the length of the ceramic strip), sintering shrinkage perpendicular to the belt transport direction, tension in both directions, the shape of the furnace, and / or air bearings on which the ceramic strip or sheet rests during sintering or when heated.
[0367] Alignment reference marks can be manufactured using lasers, mechanical methods, or chemical methods (e.g., slight compositional changes with visible results). These marks aid in aligning further processing steps, such as conductor printing / patterning and lamination.
[0368] Multilayer structures with ceramic and conductor can be bonded at high temperatures, from a final sintered conductor plus a ceramic sheet or strip with fewer layers, or even from a sheet with only a single ceramic plus a conductor layer.
[0369] Stress balancing from top to bottom is advantageous for thin circuit boards with ceramic insulation. This can be achieved by printing material patches or patterns on the sides that are opposite to the desired conductor pattern, which can alleviate the coefficient of thermal expansion (CTE) or thermal expansion-related stress between the conductor and the ceramic (and sometimes the sintering differential stress between the conductor and the ceramic). This can also be achieved by using a second conductor layer with similar material thickness and mass on the bottom of the board, which balances the CTE stress (and sintering differential stress) from top to bottom, resulting in a nearly flat rather than curled circuit board.
[0370] As multilayer structures and / or circuit boards become thicker, they become more rigid after complete sintering. Specifically, for ceramic and conductor structures with thicknesses of 1 mm, 0.5 mm, and 250 micrometers, winding the product onto small rollers with diameters of 30 to 7.5 cm becomes problematic. Methods for cutting continuously sintered products using lasers, diamond saws, abrasive jetting, water jetting, and other techniques can be used in continuous sintering equipment, where individual structures or groups of structures can be cut into sheets. Cutting equipment can be added to the exit of the final sintering furnace, and the cutting device can move or come into contact with, for example, long products as they leave the furnace.
[0371] See Figure 56 and 57This illustrates the process of initiating the sintering and threading of the preform strip 20A via a binder removal station 34A and a sintering station 38A in a system 1500A for producing sintered strip articles, according to an exemplary embodiment. In general, system 1500A is substantially the same as and performs substantially the same function as system 10 described above, differing only in slightly different alternating reel arrangements / positions in the separation system 12A, tension control system 32A, and take-up system 42A.
[0372] To initiate the roll-to-roll transfer of strip material from source reel 16A to take-up reel 44A, the green strip 20A needs to thread through the channel of binder removal station 34A and through sintering station 38A, thereby connecting the green strip 20A to the take-up reel 44A, which applies tension to pull the green strip through binder removal station 34A and through sintering station 38A. Similarly, if the strip material breaks during operation of binder removal station 34A and sintering station 38A (which may occur after binder removal), the strip material needs to thread through binder removal station 34A and then through sintering station 38A, which is done when these stations are at full operating temperature. The applicant determines that this thread-through will be particularly difficult (especially when binder removal station 34A and sintering station 38A are at high temperatures) because it is difficult to (e.g.) Figure 3 The unbonded strip 36 (i.e., the self-supporting strip material after the organic binder has been removed) passes through the sintering workstation 38A after the binder has been removed. Therefore, it should be understood that while the passing process and system discussed herein primarily concern the passing of the green strip 20A, the passing process can be used to pass various strip materials (including, for example,...) through the sintering workstation 38A. Figure 3 The unbonded strip 36 and / or partially sintered strip material (as shown) pass through the sintering system (e.g., system 10 or system 1500A).
[0373] As discussed in more detail below, the applicant has developed a process that uses threading material or a leader to draw a green strip 20A through an adhesive removal station 34A and a sintering station 38A, thereby initiating the roll-to-roll processing described above. In this embodiment, the threading material passes through the sintering station 38A and the adhesive removal station 34A, and the leader is connected to the green strip 20A upstream of or at the inlet side of the adhesive removal station 34A.
[0374] Then, tension is applied to the green strip 20A via a lead wire from the take-up reel 44A to initiate the process of moving the green strip 20A through the binder removal station 34A and through the sintering station 38A. While various schemes for the green strip to pass through the binder removal station 34A and through the sintering station 38A could allow for sintering of the green strip (e.g., manual passing), the applicant has determined that the lead wire-based passing process discussed herein provides high quality / low warpage in the sintered strip material, even at the leading edge of the sintered material. This improved product quality reduces product waste, improves process efficiency by eliminating the need to handle / remove warpage segments on the green strip, and improves the winding integrity of the sintered material on the take-up reel 44A due to the shape consistency along the length of the sintered strip material. Furthermore, in cases of heat penetration (e.g., when the binder removal station 34A and the sintering station 38A are at a certain temperature), the applicant has found that the lead-based process described herein provides an efficient way to support and pull the strip material after it leaves the binder removal station 34A (e.g., as...). Figure 3 The leading edge of the fragile, unbonded portion of the non-bonded strip 36 (shown and described above) is sintered until it passes through the sintering workstation 38Ad.
[0375] In such Figure 56 and 57 In the illustrated embodiment, the threading material (shown as lead wire 1502A) passes from the take-up reel 44A through the channels of both the sintering station 38A and the adhesive removal station 34A in opposite directions, such that the first segment of lead wire 1502A (shown as end segment 1504A) is located outside the inlet opening 116A of the adhesive removal station 34A. Figure 56 As shown, in this arrangement, lead 1502A is a single adjacent sheet of material, which is positioned such that lead 1502A extends the entire distance from take-up reel 44A through sintering workstation 38A and adhesive removal workstation 34A.
[0376] The green strip 20A moves from the source reel 16A (e.g., by unwinding the green strip 20A from the reel described above) toward the inlet opening 116A of the adhesive removal station 34A, such that the front section 1506A of the green strip 20A is adjacent to and overlaps with the end section 1504A of the lead wire 1502A. Figure 57As shown, after placing the front section 1506A of the green strip 20A and the end section 1504A of the lead wire 1502A adjacent to each other, the front section 1506A and the end section 1504A of the green strip 20A are joined or bonded together, located upstream of the adhesive removal station (e.g., in the processing direction 14A, between the inlet opening 116A of the adhesive removal station and the source reel 16A). This forms a joint or bond between the lead wire 1502A and the green strip 20A at the overlapping section.
[0377] Once the lead wire 1502A is connected to the green strip 20A, a force is applied to the portion of the lead wire 1502A located outside (e.g., downstream) of the binder removal station 34A and the sintering station 38A, thereby pulling the lead wire 1502A and the green strip 20A through the binder removal station 34A and the sintering furnace 38A in the processing direction 14A. Figure 56 In the specific embodiment shown, a second end or downstream end 1508A of the lead wire 1502A is connected to a take-up reel 44A, and the force generated by the rotation of the take-up reel 44A provides the force for moving / pulling the lead wire 1502A and the green strip 20A through the adhesive removal station 34A and the sintering furnace 38A. In some embodiments, the applicant has found that a processing speed of approximately 3 inches per minute (e.g., the speed at which the strip material moves through system 1500A) is used during the thread-up process, and in a specific embodiment, this speed can be increased to approximately 6 inches per minute for sintering once the bond between the lead wire 1502A and the green strip 20A has passed through the adhesive removal station 34A and the sintering furnace 38A.
[0378] Therefore, by using lead wire 1502A, the downstream or rewinding side of system 1500A is initially connected to the upstream or unwound side of system 1500A, enabling roll-to-roll sintering of the green strip 20A. Furthermore, by providing initial passage between the binder removal station 34A and sintering station 38A via the connection between the same unwound and take-up systems, which allows the green strip 20A to advance during sintering, the lead-based passage process described herein establishes suitable tension and speed for the entire length of the green strip 20A traversing the binder removal station 34A and sintering station 38A (including the front end 1506A of the green strip 20A at the overlapping position). Moreover, by providing a horizontal pulling force via lead wire 1502A, the lead-based process described herein achieves a passage through the horizontally oriented binder removal station 34A and sintering station 38A, which would otherwise be difficult (especially considering the fragile nature of the strip material after binder removal).
[0379] As specifically described above regarding System 10, the binder removal station 34A is heated to remove or burn off the binder from the green strip 20A, and the sintering station 38A is heated to induce sintering of the inorganic material of the green strip 20A. In one potential use of the passing process described herein, the binder removal station 34A and / or the sintering station 38A are already at their respective operating temperatures when the lead wire 1502A passes through. This is the case when the lead wire 1502A is used to pass through the green strip 20A after material breakage during reel-to-reel sintering. In another potential use of the passing process described herein, the binder removal station 34A and / or the sintering station 38A are at low temperatures (e.g., below their respective operating temperatures, at room temperature, etc.) when the lead wire 1502A passes through. This is the case when the lead wire 1502A is used to pass through the green strip 20A during the initial startup process of System 1500A.
[0380] As discussed in more detail above, after the initial movement of the junction or overlap between the lead wire 1502A and the front end 1506A of the green strip 20A through the adhesive removal workstation 34A and sintering furnace 38A, the green strip 20A is continuously unwound from source 16A and moved through workstations 34A and 38A to form the length of sintered material as described above. After sintering, the sintered material is wound onto a take-up reel 44A. In one embodiment, the lead wire 1502A is detached from the sintered strip material once the front end 1506A of the green strip 20A leaves the sintering workstation 38A and before the sintered strip material is wound onto the take-up reel 44A. In another embodiment, the lead wire 1502A is wound onto the take-up reel 44A together with the sintered strip material to form the innermost layer of the reel including the sintered material.
[0381] In various embodiments, lead 1502A is an elongated and flexible sheet of material capable of withstanding the high temperatures of the adhesive removal station 34A and the sintering station 38A. In such... Figure 57 In the connection process shown, the front section 1506A of the green strip 20A overlaps with the end section 1504A of the lead wire 1502A, forming an overlapping section 1512A. In this arrangement, the lower surface of the green strip 20A faces and contacts the upper surface of the lead wire 1502A. In this arrangement, by placing the green strip 20A on top of the lead wire 1502A, the lead wire 1502A serves to support the front section 1506A of the green strip 20A through the adhesive removal workstation 34A and the sintering furnace 38A.
[0382] In some embodiments, an adhesive material 1510A is used to form an adhesive bond between the lead 1502A and the green strip 20A. For example... Figure 57As shown, in some such embodiments, the binder material 1510A is located on the upper surface of the lead 1502A and forms an adhesive with the lower surface of the green strip 20A. As discussed in more detail below, in various embodiments, the applicant has determined that matching of various properties (e.g., the coefficients of thermal expansion (CTE) of the materials forming the binder 1510A, lead 1502A, and green strip 20A) helps maintain the bond between the lead 1502A and the strip material, particularly during the high-temperature process across the sintering workstation 38A. Furthermore, the strong bond between the lead 1502A and the green strip 20A allows the desired level of tension to be applied to the lead 1502A and transferred to the green strip 20A via the bond provided by the binder 1510A. As described herein, the applicant has found that low (e.g., gram level) but consistent tension applied to the strip material during sintering reduces warpage that might otherwise form across the width of the strip during sintering.
[0383] In various embodiments, the applicant determined that the volume of the adhesive material 1510A used and the shape of the adhesive material 1510A applied to the lead 1502A affect the nature of the bond formed between the lead 1502A and the green strip 20A. In specific embodiments, the adhesive material 1510A is a small volume (e.g., about 0.1 mL of alumina-based adhesive material). In one embodiment, the adhesive 1510A is used to bond the lead 1502A to the unsintered green strip material 20A, and in such embodiments, the applicant found that the rounded shape of the adhesive 1510A works well. The applicant hypothesizes that the rounded geometry helps to disperse the thermal and mechanical stresses induced by adhesive and strip shrinkage and CTE mismatch (if present) between the materials of the lead 1502A, the adhesive 1510A, and the green strip 20A. In another embodiment, adhesive 1510A is used to bond lead 1502A to a portion of the sintering material strip, and in such embodiments, the applicant believes that the line of adhesive 1510A extending across the width of lead 1502A works well. The applicant speculates that the line geometry plays a role in applying uniform constraint to the roll as it moves through the sintering workstation.
[0384] In a specific embodiment, the adhesive removal station 34A operates to remove liquid and / or organic components from the adhesive 1510A (and from the green strip 20A) as the overlapping segment 1512A between the lead 1502A and the green strip 20A traverses the adhesive removal station 34A. The applicant believes that the various properties of the adhesive material 1510A and the green strip 20A are related to the likelihood of breakage of the bond formed by the adhesive material 1510A during traversal through the adhesive removal station 34A and the sintering station 38A. The applicant speculates that the temperature distribution through the adhesive removal station 34A causes the organic material in the green strip 20A to soften and even melt before evolving into a strip, which can help limit the stress intensity around the adhesive joint as individual components begin to change shape / size due to shrinkage and thermal expansion. The applicant speculates that allowing the green strip to "deform" or "reshape" around the location of the adhesive 1510A before losing its elastic / plastic properties helps reduce defects and improves the quality of the bond formed by the adhesive 1510A. Similarly, this elastic / plastic property also allows for the expulsion of liquids and organic materials from the adhesive, which would otherwise lead to increased pressure between the lead 1502A and the green strip 20A. This increased pressure could cause bond failure, or the accumulated gas could cause the green strip 20A to crack.
[0385] In a specific embodiment, the tension applied during the process of pulling the lead wire 1502A and the green strip 20A at the overlap or joint can vary or increase as the overlap segment 1512A traverses the binder removal station 34A and / or the sintering station 38A. In a specific embodiment, a low level of tension (e.g., less than 25 grams) is initially provided as the overlap segment 1512A traverses the binder removal station 34A, and then the tension increases as the overlap segment 1512A traverses the sintering station 38A. In a specific embodiment, once the overlap segment 1512A and the binder material 1510A reach the center of the sintering station 38A, a tension of approximately 25 grams or greater is applied. The applicant believes that at this point, the tension can be increased without causing the bond between the lead wire 1502A and the green strip 20A to separate, because sintering of the material of the green strip 20A has already occurred at this point. The applicant believes that applying high levels of tension prematurely before the opportunity to build up strength usually leads to the failure of the bond formed by adhesive 1510A.
[0386] In various embodiments, the connection and / or support between the lead wire 1502A and the green strip 20A are enhanced by varying levels of overlap between them. Figure 57It can be seen that the greater the overlap between lead wire 1502A and green strip 20A, the greater the amount of support provided by lead wire 1502A to green strip 20A. Similarly, the level of overlap between lead wire 1502A and green strip 20A is related to the amount of friction-based connection between lead wire 1502A and green strip 20A, which can complement the bonding provided by adhesive 1510A. In embodiments employing adhesive 1510A, the applicant has found that overlap segments 1512A with a length of 1 to 5 inches measured in the processing direction 14A perform well. In some embodiments, the connection between lead wire 1502A and green strip 20A can be provided solely by friction (e.g., without adhesive 1510A), and in such cases, the length of overlap segment 1512A in the processing direction 14A can be greater than 5 inches, such as greater than 10 inches, 10 inches to 30 inches, approximately 24 inches, etc.
[0387] In various embodiments, the applicant has provided multiple material combinations of the through-type / functional lead 1502A, green strip 20A, and binder 1510A as described herein. Generally, the lead 1502A is formed of a material different from the green strip 20A in at least one respect. In some such embodiments, the lead 1502A is formed of the same type of material as the inorganic particles of the green strip 20A, but has a different (e.g., higher) degree of sintering than the inorganic material of the green strip 20A. In some such embodiments, the lead 1502A is an elongated strip of sintered ceramic material, and the green strip 20A carries unsintered or less sintered particles of the same type of ceramic material.
[0388] In some other embodiments, lead 1502A is formed of an inorganic material of a different type than the inorganic particles of green strip 20A. In a specific embodiment, lead 1502A is formed of a ceramic material of a different type than the inorganic particles of green strip 20A. In some other embodiments, lead 1502A is formed of a metallic material, while the inorganic particles of green strip 20A are ceramic inorganic materials.
[0389] The applicant discovered that Figure 57The connection level between the lead wire 1502A and the green strip 20A provided by the connection arrangement shown and described herein allows for good transmission of force / tension from the lead wire to the green strip 20A without significant risk of detachment. Furthermore, the applicant has found that by selecting materials for the inorganic particulate materials of the lead wire 1502A, the binder 1510A, and the green strip 20A that have relatively similar coefficients of thermal expansion (CTE), the risk of detachment and warping due to sintering can be reduced. In various embodiments, the CTE of the material of the lead wire 1502A is within ±50% of the CTE of the inorganic material of the green strip 20A, specifically within ±40% of the CTE of the inorganic material of the green strip 20A, and more specifically within ±35% of the CTE of the inorganic material of the green strip 20A. Similarly, in various embodiments, the CTE of the lead 1502A material is within ±50% of the CTE of the adhesive material 1510A, specifically within ±40% of the CTE of the adhesive material 1510A, and more specifically within ±35% of the CTE of the adhesive material 1510A.
[0390] Lead 1502A can be formed from a variety of suitable materials. In some embodiments, lead 1502A is formed from a sintered ceramic material, and in other embodiments, lead 1502A is formed from a metallic material. In some embodiments, the applicant has found that using a porous ceramic material increases the ability of the adhesive material 1510A to bond to lead 1502A. The applicant believes that the porosity of lead 1502A makes it easier to bond the adhesive material 1510A compared to leads with fewer holes or polished surfaces. In specific embodiments, lead 1502A can be a platinum ribbon or a fully sintered ceramic material (e.g., alumina or yttrium-stabilized zirconia (YSZ)).
[0391] In a specific embodiment, the dimensions of lead wire 1502A enable processing and connection to the green strip 20A. In a specific embodiment, the width of lead wire 1502A substantially matches the width of the green strip 20A (e.g., within ±10%). In a specific embodiment, the thickness of lead wire 1502A is from 5 μm to 500 μm, and more specifically, from 20 to 40 μm. Furthermore, the length of lead wire 1502A is sufficient to extend from the take-up reel 44A through both the sintering workstation 38A and the adhesive removal workstation 34A, thus the length of lead wire 1502A varies with the dimensions of system 1500A.
[0392] Although Figure 56 and 57Lead 1502A is generally shown as a long, thin, flat segment of sintered ceramic material, but lead 1502A can have other forms. For example, in one embodiment, lead 1502A can be a ceramic plate having the length of a platinum wire bonded to a green strip. In another embodiment, lead 1502A can be the length of a ceramic fiber rope or a ceramic fiber twist.
[0393] Adhesive material 1510A can be formed from a variety of suitable materials. In some embodiments, adhesive material 1510A is a ceramic adhesive material. In a specific embodiment, adhesive material 1510A is an alumina-based adhesive material, for example, alumina-based adhesive #C4002 purchased from Zircar Ceramics.
[0394] See Figures 58-65 This document shows and describes various systems and processes for bending the unbonded strip 36B in the longitudinal or length direction during sintering. In general, the applicant identified an unforeseen challenge when sintering wide, thin, and continuous lengths of the unbonded strip 36B: ensuring a high level of flatness in the width direction of the final sintered strip 40B. A high level of flatness in the width direction is desirable when using the sintered strip material described herein in several applications, such as substrates for thin-film circuits, thick-film circuits, and solid-state lithium-ion batteries.
[0395] Some continuous strip sintering processes may be prone to certain flatness distortions (e.g., bowing in the width direction, edge wrinkling, bubble formation, etc.), believed to be due to in-plane stresses generated within the strip material during sintering. For example, the applicant has found that various factors (e.g., ceramic particle density in the unbonded strip 36B, large temperature differences in the strip material along the system length (e.g., potentially exceeding 1000 degrees Celsius due to the continuous nature of the system and process described herein), processing speed, etc.) lead to in-plane stresses generated during sintering, which in turn may induce bending in a manner that releases these in-plane stresses without the application of counteracting forces.
[0396] For example, alumina strips continuously sintered via the system described herein may simultaneously have regions at room temperature and at the maximum sintering temperature. The strips may also have regions with minimal shrinkage at the start of the sintering process, and regions nearing completion where sintering is nearing completion and shrinkage exceeds 8% or even 10% linearly. Shrinkage and temperature gradients can be sources of complex biaxial stresses that can induce distortion, for example, causing curling and wrinkling, even for strips entering the sintering station with a certain degree of flatness. Such distortions may then become frozen into the sintered strip after cooling, thus degrading its potential use.
[0397] As discussed in detail below, the applicant has determined that stresses that could lead to flatness distortion can be at least partially offset by inducing longitudinal or longitudinal bending in the strip during sintering. During sintering, the strip material undergoes plastic relaxation and deforms into the induced longitudinal bending shape, which generates forces within the strip material that tend to reduce otherwise present in-plane stresses, and as a result, can produce sintered strips with a high level of flatness in the width direction. The applicant believes that despite variations in the particle density of the green strip and high production rates, relatively flat strips can be produced by employing longitudinal bending during the sintering process.
[0398] Furthermore, in at least some embodiments, the planarization process described herein produces flat and thin sintered articles while avoiding / limiting surface contact and the resulting surface defects and scratches, which is common for contact / pressure-based planarization devices, for example, when material is pressed between cover plates during sintering. As shown below, the applicant has developed several systems and processes for inducing longitudinal bending, resulting in at least one main surface of a strip that does not touch during sintering, and some processes resulting in both upper and lower (main) surfaces of a strip that does not touch during sintering. The applicant believes that other ceramic sintering processes cannot achieve a high level of flatness in the width direction during continuous sintering, or have the limited degree of surface contact provided by the systems and processes described herein.
[0399] See Figure 58 This demonstrates the processes and systems used to produce sintered continuous strips with high flatness. Specifically, Figure 58 This illustrates a system 1600B for producing sintered strip articles according to an exemplary embodiment. Generally, system 1600B is identical to and functions the same as system 10 described above, except that system 1600B includes a sintering workstation 38B, which includes a bending system 1602B located within the sintering workstation 38B. In general, the bending system 1602B is configured or arranged to induce a radius of curvature along the length direction or longitudinal axis of the unbonded strip 36B when the strip 36B is sintered within the sintering workstation 38B at a high temperature (e.g., above 500 degrees Celsius). The applicant has determined that, during sintering, inducing longitudinal bending in the strip material by bending can improve the shape across the width of the final sintered strip 40B via the mechanism described herein.
[0400] exist Figure 58In the specific embodiment shown, the bending system 1062B includes an upwardly convex bending surface 1604B that defines at least a portion of the lower channel surface passing through the sintering workstation 38B. The upwardly convex bending surface 1604B defines at least one radius of curvature (shown as R1B), which in this specific embodiment is a radius of curvature ranging from 0.01 m to 13000 m or includes a radius of curvature ranging from 0.01 m to 13000 m. Generally, the unbonded strip 36B moves through the sintering workstation 38B (as described above), and the gravity and / or tensile tension in the strip cause the strip to bend to at least partially conform to the bending surface 1604B, inducing longitudinal bending in the strip during sintering at elevated temperatures. In this specific embodiment, the tension applied to the unbonded strip 36B is at least 0.1 grams of force per linear inch of the width of the unbonded strip 36B, and the movement speed through the sintering workstation 38B is 1 to 100 inches of strip length per minute.
[0401] like Figure 58 As shown, the curved surface 1604B is about an axis parallel to the width of the unbonded strip 36B (and perpendicular to the width axis). Figure 58 The axis of the unbonded strip 36B is bent (as shown in the attached drawing plane). Therefore, in this embodiment, the path of the unbonded strip 36B through the sintering station 38B is generally defined by the channel 104B, and the convex curved surface 1604B defines the curved section of the path through the sintering station 38B. During sintering, when the unbonded strip 36B passes through the curved section of the path defined by the convex curved surface 1604B, bending is induced in the unbonded strip 36B because its shape conforms to the curved surface 1604B.
[0402] exist Figure 58 In the specific embodiment shown, the curved surface 1604B forms a continuous curved surface with a single radius of curvature that extends the entire length of the channel 104B between the inlet and outlet of the sintering workstation 38B. In this type of embodiment, the radius of curvature of the surface 1604B, which needs to simultaneously achieve a sufficient level of curvature and extend the entire length of the sintering workstation 38B, can vary based on the length of the sintering workstation. Thus, for a given maximum rise H1B of the curved surface 1604B (e.g., ...), the radius of curvature can vary. Figure 60As shown, a shorter sintering workstation 38B can have a smaller R1B than a longer sintering workstation 38B. As a specific example, a sintering workstation 38B at least 1 m long can have a curved surface 1604B with an R1B of 1 m to 130 m. As a specific example, a sintering workstation 38B at least 3 m long can have a curved surface 1604B with an R1B of 10 m to 1130 m. As a specific example, a sintering workstation 38B at least 6 m long can have a curved surface 1604B with an R1B of 40 m to 4500 m. As a specific example, a sintering workstation 38B at least 10 m long can have a curved surface 1604B with an R1B of 120 m to 13000 m. In such embodiments, regardless of length, H1B can be from 1 mm to 10 cm, resulting in the R1B range described above.
[0403] As described above regarding system 10, the sintering workstation 38B is arranged such that the planes intersecting the inlet and outlet of the sintering workstation form an angle of less than 10 degrees relative to the horizontal plane. As described above, this generally horizontal sintering arrangement allows the unbonded strip 36B to move through the sintering workstation 38B in a generally horizontal position. In such embodiments, the curved surface 1604B defines the lower surface of the path through which the strip 36B traverses between the inlet and outlet of the sintering workstation 38B. The applicant believes that by using a horizontal sintering arrangement (as described above, reducing the thermal gradient based on airflow) and forming a longitudinally curved shape in the strip during sintering, sintered strips with the high level of flatness described herein can be produced and / or can be produced rapidly (far faster than other sintering systems). It should be understood that while the applicant believes that the curvature during sintering combined with the horizontal sintering workstation 38B provides a high level of flatness, in other embodiments, the sintering workstation 38B can be arranged at any angle from horizontal to vertical. In such non-horizontal implementations, the size and location of the curved surface 1604D are sufficient to achieve the desired level of flatness.
[0404] like Figure 58As shown, in the processing arrangement of system 1600B, the adjacent length of the strip material (e.g., unbonded strip 36B) moves into a heating station (e.g., sintering station 38B). In this arrangement, a portion of the adjacent strip (shown as unbonded strip 36B) is located upstream of the inlet 106B entering the sintering station 38B. After sintering, the sintered portion of the adjacent strip (e.g., sintered strip 40B) is located downstream of the outlet 108B of the sintering station 38B. As is generally understood, at any given time, the adjacent strip includes a third portion of the strip being sintered at the sintering station 38B. This third portion of the adjacent strip is located between the unbonded unsintered strip 36B (located upstream of the sintering station 38B) and the sintered portion 40B of the adjacent strip (located downstream of the sintering station 38B). The portion of the adjacent strip being sintered (shown as strip portion 1606B) is located in sintering workstation 38B, where it is being heated to the required sintering temperature (e.g., a temperature greater than 500 degrees Celsius).
[0405] Typically, the strip portion 1606B has a direction of machining (e.g., in the machining direction). Figure 58 The orientation (from right to left) indicates a decrease in porosity or an increase in sintering degree. For example... Figure 58 As shown, strip portion 1606B is bent into a conforming upward convex curved surface 1604B, thereby strip portion 1606B typically adopts a curved shape, the radius of curvature of which matches R1B. As described above, longitudinal tension can be applied to adjacent strips, thereby bending strip portion 1606B into a conforming upward convex curved surface 1604B.
[0406] As can be understood from the above description of the unwound and retracted portions of system 10, system 1600B provides continuous spool-to-spool processing of the long adjacent length of the strip. In this way, the entire adjacent length of the strip being processed can be moved continuously and sequentially through sintering station 38B, such that during the passage through sintering station 38B, the entire adjacent length of the processed strip is bent into a radius of curvature R1B of an upwardly convex curved surface 1604B.
[0407] See Figure 59 This shows details of a sintering workstation 38B including a bending system 1602B according to an exemplary embodiment. Figure 59 In the illustrated embodiment, the sintering workstation channel 104B is defined by a tube 1608B (e.g., the alumina tube described above). In this embodiment, the upwardly convex curved surface 1604B is defined by the upwardly facing surface of a device or insert 1610B placed within the tube 1608B. Figure 59As shown, the length of device 1610B is at least 80%, more specifically at least 90%, and even more specifically at least 95% of the length of channel 104B. In some embodiments, the length of device 1610B is greater than the length of channel 104B such that when it enters and exits sintering workstation 38B, the entry and exit segments of the strip are supported by the upwardly convex curved surface 1604B.
[0408] As would be commonly understood, in various embodiments, the radius of curvature defining the continuous convex curved surface 1604B is a function of the maximum elevation H1B and the longitudinal length L2B (e.g., Figure 60 the distance in the horizontal orientation of ) of surface 1604. In a specific embodiment, when the convex curved surface 1604B extends the entire length of sintering workstation 38B, the longitudinal length of surface 1604B is substantially equal to the longitudinal length of sintering workstation 38B. Thus, in such embodiments, the radius of curvature R1B of the convex curved surface 1604B is defined as R1B = H1B+(L2B^2) / H1B, and in various embodiments, 0.1 mm < H1B < 100 mm and 0.1 m < L2...
Claims
1. A method for manufacturing a ceramic strip, the method comprising: Sintering a ribbon comprising a polycrystalline ceramic until the porosity of the polycrystalline ceramic is less than 20 volume percent by exposing particles of the polycrystalline ceramic to a heat source to induce sintering between the particles, wherein the strip is particularly thin, such that the thickness of the strip is less than 500 μm, thereby promoting rapid sintering via heat penetration, and The strip is at least 5 mm wide and at least 300 cm long.
2. The method of claim 1, further comprising subjecting the strip to positive stretching in the length direction during the sintering process.
3. The method of claim 1 further comprising moving the strip toward a heat source and then away from the heat source during sintering.
4. The method according to any one of claims 1 to 3, wherein: The amount of sintering time is particularly short, less than 2 hours in total, helping to maintain small particle sizes in the ceramic strips.
5. The method of claim 4, wherein: The sintering time is less than 1 hour in total, and wherein, after sintering, the density of the polycrystalline ceramic is greater than 95 volume % dense.
6. The method of claim 4, wherein: After sintering, the strip comprises closed pores.
7. The method of claim 1, wherein: The ribbon comprises a volatile component which evaporates during the sintering process, wherein the volatile component is inorganic, and wherein the ribbon comprises at least 1 volume % more of the volatile component before sintering than after sintering.
8. A strip comprising: a body comprising particles of an inorganic material sintered together, the body extending between first and second major surfaces, wherein the body has a thickness defined as the distance between the first and second major surfaces, a width defined as a first dimension of the first major surface perpendicular to the thickness, and a length defined as a second dimension of the first major surface perpendicular to both the thickness and the width, wherein the strip is long, having a length of about 300 cm or more; wherein the strip is thin, having a thickness of about 3 μm to about 1 mm; and Therein, the strips are particularly wide, having a width of approximately 5 mm or more.
9. The strip of claim 8, wherein: The geometric consistency of the strip is as follows: the width of the strip varies by less than 100 μm when measured at positions in the length direction spaced 1 m apart; and the thickness of the strip varies by less than 10 μm when measured at positions in the length direction spaced 1 m apart along the center of the width direction of the strip.
10. The strip of claim 8, wherein: The strip is flat or flattenable such that a 10 cm length of the strip pressed between parallel flat surfaces flattens to contact with the parallel flat surfaces or to within 0.05 mm of contact with the parallel flat surfaces without cracking.
11. The strip of claim 10, exhibiting a maximum in-plane stress of no more than 1% of its Young's modulus when flattened into contact with said parallel planar surfaces and / or within 0.05 mm of said parallel planar surfaces.
12. The strip of claim 8, wherein: The first and second major surfaces of the strip have a granular profile, wherein the grains are ceramic, and wherein at least some individual grains of mutually adjacent ceramic have little to no intervening amorphous material, such that the thickness of the amorphous material between two adjacent grains is less than 5 nm.
13. The strip of claim 8, wherein: The body has a porosity of less than 10 volume percent.
14. The strip of claim 13, wherein: The body has a closed hole.
15. The strip of claim 13, wherein: The particles include lithium, and wherein, The ionic conductivity of the main body is greater than 5x10 -5 S / cm.
16. The strip of claim 8, wherein: The main body has a particularly fine particle size, which is 5 μm or less.
17. The strip of claim 8, further comprising a conductive metal connected to the first major surface of the body.
18. The strip of claim 17, wherein: The body includes a repeating pattern of holes, and wherein the conductive metal is arranged in a repeating pattern.
19. The strip of claim 18, wherein: The first and second major surfaces have a granular profile, and the strip further includes a coating overlying the granular profile of the first major surface, wherein an outwardly facing surface of the coating is less rough than the granular profile of the first surface, and wherein the conductive metal is connected to the first major surface by bonding to the outwardly facing surface of the coating.
20. The strip of claim 8, wherein: The viscosity of the inorganic material at a temperature greater than 900° C. is 12.5 poise.
21. A coil of strip as claimed in any one of claims 8 to 20, wherein The strip is wrapped around itself and overlapped, bending to a radius of less than 30 cm.
22. A plurality of sheets cut from a strip as claimed in any one of claims 8 to 20.
23. A strip comprising: a body comprising mutually sintered ceramic particles, the body extending between first and second major surfaces, wherein the body has a thickness defined as the distance between the first and second major surfaces, a width defined as a first dimension of the first major surface perpendicular to the thickness, and a length defined as a second dimension of the first major surface perpendicular to both the thickness and the width; wherein the strip is thin, having a thickness of about 3 μm to about 1 mm; and wherein the first and second major surfaces of the strip have a granular profile, and Therein, at least some individual grains of the ceramic that are adjacent to one another have little to no intervening amorphous material, such that the thickness of the amorphous material between two adjacent grains is less than 5 nm.
24. A strip comprising: a body comprising mutually sintered ceramic particles, the body extending between first and second major surfaces, wherein the body has a thickness defined as the distance between the first and second major surfaces, a width defined as a first dimension of the first major surface perpendicular to the thickness, and a length defined as a second dimension of the first major surface perpendicular to both the thickness and the width; wherein the strip is thin, having a thickness of about 3 μm to about 1 mm; wherein the first and second major surfaces of the strip have a granular profile; wherein the particles contain lithium, and the body has a mass greater than 5 x 10 -5 S / cm ionic conductivity.
25. An article comprising: A body comprising mutually sintered inorganic material particles, wherein the particles comprise lithium manganese oxide, lithium cobalt oxide, lithium iron phosphate or a combination thereof, wherein the thickness of the body between the first main surface and the second main surface thereof is in the range of 3 μm to 100 μm, wherein the first major surface and the second major surface have an unpolished granular profile such that the profile includes particles protruding outward from the respective major surfaces and having a height of at least 25 nm and not more than 150 μm relative to the recessed portions of the respective major surfaces at the boundaries between the respective particles.
26. The article of claim 25, wherein the body has a porosity of less than 10% by volume.
27. The article of claim 25, wherein the body has a length of at least 10 m.
28. The article of claim 25, wherein the body has a thickness greater than 5×10 -5 S / cm ionic conductivity.
29. The article of claim 25, wherein the particles comprise LiCoO2.
30. The article of claim 25, wherein the height is at least 150 nm.
31. The article of claim 25, wherein the height does not exceed 80 μm.
32. The article of claim 25, wherein the body has a width of 5 mm or greater.
33. The article of claim 25, wherein the particles have an average particle size of 5 μm or less.
34. The article of claim 25 wherein there are fewer than 10 pinholes having a cross-sectional area of at least one square micron per square millimeter of surface extending through the body.
35. A coil of the article of claim 25 wound on a spool.
36. A sintered product comprising: a first major surface, a second main surface opposite to the first main surface, a body extending between the first and second major surfaces, the body comprising a sintered ceramic, wherein the first and second major surfaces have a granular profile, the granular profile comprising grains of the sintered ceramic, the grains having a height of 25 nm to 150 μm relative to a recessed portion of the respective major surface at a boundary between the grains; wherein the body has a thickness defined as the distance between the first and second major surfaces, wherein the thickness is in the range of 3 μm to 1 mm; wherein the body has a width defined as a first dimension of the first major surface perpendicular to the thickness, wherein the width is greater than 40 mm; and The sintered article has a flatness in the range of about 100 nm to about 50 μm over a one centimeter distance in a length direction thereof, wherein the length is defined as a second dimension of the first major surface that is perpendicular to both the thickness and the width.
37. The sintered product according to claim 36, wherein the sintered product is a ceramic tape, wherein the length of the body is 10m or more.
38. The sintered article of claim 36, wherein the ceramic comprises doped zirconia.
39. The sintered article of claim 38, wherein the dopant comprises yttrium oxide (Y2O3), and wherein Y2O3 comprises 3 mol% of the ceramic.
40. The sintered article of claim 38, wherein the zirconium oxide comprises tetragonal zirconium oxide.
41. The sintered article of claim 36, wherein the first major surface comprises an area of at least ten square centimeters having fewer than one hundred surface defects greater than 5 μm in size from adhesion or wear.
42. Sintered products, including: a first major surface, a second major surface opposite to the first major surface, a body extending between the first and second major surfaces, the body comprising a sintered ceramic, wherein the first and second major surfaces have a granular profile, the granular profile comprising grains of the sintered ceramic, the grains having a height of 25 nm to 150 μm relative to a recessed portion of the respective major surface at a boundary between the grains; wherein the body has a thickness defined as the distance between the first and second major surfaces, wherein the thickness is in the range of 3 μm to 1 mm; wherein the body has a width defined as a first dimension of the first major surface perpendicular to the thickness, wherein the width is greater than 40 mm; and wherein the body is flattenable without cracking as determined by pressing the body between rigid parallel surfaces at 23°C such that the body covers or is within 0.05 mm of a flat surface.
43. The sintered article of claim 42, wherein the body has a porosity of less than 10% by volume.
44. The sintered article of claim 42, wherein the width is greater than 125 mm.
45. The sintered article of claim 42, wherein the sintered article is a ceramic tape, wherein the length of the body is 10 m or more.
46. The sintered article according to claim 42, wherein the sintered article has a roughness of about 1 nm to about 10 μm over a distance of 1 cm in the length direction.
47. A sintered product comprising: a first major surface, a second main surface opposite to the first main surface, a body extending between the first and second major surfaces, the body comprising a sintered ceramic, wherein the first and second major surfaces have a granular profile, the granular profile comprising grains of the sintered ceramic, the grains having a height of 25 nm to 150 μm relative to a recessed portion of the respective major surface at a boundary between the grains; wherein the body has a thickness defined as the distance between the first and second major surfaces, wherein the thickness is in the range of 3 μm to 1 mm; wherein the body has a width defined as a first dimension of the first major surface perpendicular to the thickness, wherein the width is greater than 40 mm; and The sintered product is a ceramic tape, wherein the length of the main body is 10 m or more.
48. A sintered article according to claim 47, wherein the width is greater than 125 mm.
49. A system comprising: a bobbin having a continuous strip material wound thereon, the continuous strip material comprising a green strip material and a backing layer; Collect the scroll; a heating station including at least one furnace, the heating station configured to receive an unwound length of the continuous strip; The heating workstation comprises: a first bending section such that the continuous strip of material is bent; and at least two rollers defining said first bending section over which said continuous strip of material is bent, The heating station is controlled to provide an air-free atmosphere to at least a portion of the heating station, wherein the air-free atmosphere is at least one of vacuum, hydrogen or helium.
50. The system of claim 49, wherein: For green strip material having a width greater than 50 mm, the system is configured to move the continuous strip material at a rate of at least 1 inch / minute.