Composite material and preparation method thereof, light-emitting device and display device

By using inorganic halogen salts and reducing inorganic salts in nanocrystalline semiconductor luminescent materials, the concentration and reaction conditions of metal ion are adjusted, the fluorescence intensity and luminescence color purity of nanoparticles are improved, and the luminescence color purity after doping rare earth elements is solved. The problem of low efficiency has achieved improved luminous performance.

CN118931539APending Publication Date: 2024-11-12TCL TECHNOLOGY GROUP CORPORATION
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310542504.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After the existing nanocrystalline semiconductor luminescent materials are doped with rare earth elements, the luminescent color purity is low and it is difficult to effectively improve.

Method used

By adding inorganic halogen salts to the cation precursor solution, the halide ions are used to form chemical bonds with metal cations on the surface of nanoparticles, adjust the concentration of metal ions that are not bonded to anions, reduce the half-maximum width of the luminescence peak, improve the luminescence color purity, and High fluorescence intensity composite materials are prepared by adjusting the reaction conditions of reducing inorganic salts and nonionic polymer compounds.

Benefits of technology

A composite material with high luminous purity and fluorescence intensity is achieved, which improves the photoelectric performance and structural stability of the luminous luminous device, and solves the problem of deterioration of luminous purity after doping rare earth elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118931539A_ABST
    Figure CN118931539A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material and a preparation method thereof, a luminescent device and a display device, the preparation method comprises the following steps: providing a cation precursor solution and an anion precursor solution, the cation precursor solution comprising a cation precursor salt, a rare earth metal salt, an inorganic halide salt and a first solvent; and mixing the anion precursor solution with the cation precursor solution to obtain the composite material. According to the preparation method, inorganic halide salt is added into a cation precursor solution, halide ions in the inorganic halide salt can generate a dipole effect with metal cation vacancies on the surfaces of nano-particles to form chemical bonds, and therefore the concentration of the metal ions which do not form bonds with anions in a mixed solution system in the growth stage of the nano-particles is effectively adjusted; therefore, the problem that the half-peak width of a luminescence peak is widened when rare earth elements are doped in the nano-particles to obtain the nano-particles with narrow band gaps can be effectively solved, so that the composite material with high luminescence color purity is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to a composite material, a method for preparing the composite material, and a light-emitting device and a display apparatus comprising the composite material. Background Art

[0002] In recent years, nanocrystalline semiconductor luminescent materials, known as "nanophosphors", have attracted great interest from scientific researchers due to their novel and unusual structures and excellent optical and electrical properties.

[0003] Existing nanocrystalline semiconductor light-emitting materials include single-structure nanocrystals, core-shell structure nanocrystals, and alloy structure nanocrystals. The properties of these nanocrystals, such as the visible light radiation wavelength and radiation lifetime, can change with the change of their own size. These materials can be used to prepare light-emitting devices, such as organic light-emitting diodes (OLEDs) and quantum dot light-emitting diodes (QLEDs).

[0004] Rare earth elements have a unique electronic structure and can emit light covering a spectral region from the ultraviolet region to the near-infrared region. Therefore, the existing technology will dope rare earth elements into nanocrystals to prepare rare earth-doped nanocrystals with high photostability, high chemical stability, long luminescence lifetime (μs-ms), narrow emission band and low toxicity.

[0005] However, the luminescent color purity of rare earth-doped nanocrystals prepared by existing methods is relatively low and needs to be further improved. Summary of the invention

[0006] In view of this, the present application provides a method for preparing a composite material, aiming to improve the problem of low color purity of existing nanocrystalline semiconductor light-emitting materials.

[0007] The embodiment of the present application is implemented as follows: a method for preparing a composite material comprises the following steps:

[0008] Providing a cationic precursor solution and an anionic precursor solution, wherein the cationic precursor solution comprises a cationic precursor salt, a rare earth metal salt, an inorganic halogen salt and a first solvent, and the anionic precursor solution comprises an anionic precursor salt and a second solvent;

[0009] The anion precursor solution is mixed with the cation precursor solution to obtain a composite material. Optionally, in some embodiments of the present application, the cation precursor salt includes one or more of yttrium salt, gadolinium salt, sodium salt, niobium salt, and tantalum salt; and / or

[0010] The rare earth metal salt includes one or more of rare earth metal nitrates, rare earth metal acetates, rare earth metal chlorides, and rare earth metal bromides; and / or

[0011] The rare earth metal salt includes one or more of europium salt, cerium salt, terbium salt, dysprosium salt, samarium salt and ytterbium salt; and / or

[0012] The inorganic halogen salt comprises an alkali metal halide salt; and / or

[0013] The anion precursor salt includes one or more of ammonium vanadate, ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, yttrium chloride, yttrium bromide, and yttrium iodide; and / or

[0014] The first solvent and the second solvent independently include one or more of a water-alcohol solvent, an amine solvent, a sulfur-containing organic solvent, and an ether solvent.

[0015] Optionally, in some embodiments of the present application, the yttrium salt includes one or more of yttrium nitrate, yttrium sulfate, yttrium chloride, and yttrium bromide; and / or

[0016] The gadolinium salt includes one or more of gadolinium nitrate, gadolinium sulfate, gadolinium chloride, and gadolinium bromide; and / or

[0017] The sodium salt includes one or more of sodium nitrate, sodium sulfate, sodium chloride and sodium bromide; and / or

[0018] The niobium salt comprises one or more of niobium nitrate, niobium sulfate, niobium chloride and niobium bromide; and / or

[0019] The tantalum salt comprises one or more of tantalum nitrate, tantalum sulfate, tantalum chloride and tantalum bromide; and / or

[0020] The europium salt includes one or more of europium nitrate, europium acetate, europium chloride, and europium bromide; and / or

[0021] The cerium salt includes one or more of cerium nitrate, cerium acetate, cerium chloride, and cerium bromide; and / or

[0022] The terbium salt includes one or more of terbium nitrate, terbium acetate, terbium chloride, and terbium bromide; and / or

[0023] The dysprosium salt includes one or more of dysprosium nitrate, dysprosium acetate, dysprosium chloride, and dysprosium bromide; and / or

[0024] The samarium salt includes one or more of samarium nitrate, samarium acetate, samarium chloride, and samarium bromide; and / or

[0025] The ytterbium salt includes one or more of ytterbium nitrate, ytterbium acetate, ytterbium chloride, and ytterbium bromide; and / or

[0026] The alkali metal halide salt includes one or more of sodium chloride, sodium bromide, sodium iodide, sodium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, potassium chloride, potassium bromide, potassium iodide, and potassium fluoride; and / or

[0027] The alcohol solvent comprises a short-chain alcohol having 1 to 8 main chain carbon atoms; and / or

[0028] The amine solvent includes one or more of dimethylformamide, dioctylamine, and ethylenediamine; and / or

[0029] The sulfur-containing organic solvent comprises dimethyl sulfoxide; and / or

[0030] The ether solvent includes one or more of tetrahydrofuran, diethyl ether and propylene oxide.

[0031] Optionally, in some embodiments of the present application, in the cationic precursor solution, the concentration of the cation of the cationic precursor salt is 0.005 to 0.05 mmol / ml; and / or

[0032] The molar ratio of the cation in the cationic precursor salt to the rare earth metal salt is (5-20):1; and / or

[0033] The molar ratio of the inorganic halide salt to the cation in the cationic precursor salt is (0.02-0.2):1; and / or

[0034] In the anion precursor solution, the concentration of the anion precursor salt is 0.05 to 1 mmol / ml; and / or

[0035] The molar ratio of the anion in the anion precursor salt to the cation in the cationic precursor salt is (10-20):1.

[0036] Optionally, in some embodiments of the present application, the rare earth metal salt is a europium salt, and the cationic precursor solution also includes a reducing inorganic salt.

[0037] Optionally, in some embodiments of the present application, the reducing inorganic salt includes one or more of sulfite, selenite, tellurite, thiosulfate, thioselenate, and thiotellurate; and / or

[0038] The molar ratio of the reducing inorganic salt to the rare earth metal salt is (0.5-10):1.

[0039] Optionally, in some embodiments of the present application, the cationic precursor solution also includes a non-ionic polymer compound.

[0040] Optionally, in some embodiments of the present application, the non-ionic polymer compound includes one or more of polyvinyl pyrrolidone, polypropylene pyrrolidone, and polybutylene pyrrolidone; and / or

[0041] The molar ratio of the nonionic polymer compound to the cation in the cationic precursor salt is (0.05-0.1):1.

[0042] Correspondingly, an embodiment of the present application further provides a composite material, comprising nanoparticles and rare earth metal elements doped in the nanoparticles, wherein the surface of the nanoparticles is connected to a halogen ligand.

[0043] Optionally, in some embodiments of the present application, the composite material is composed of the nanoparticles and rare earth metal elements doped in the nanoparticles, wherein halogen ligands are connected to the surfaces of the nanoparticles.

[0044] Optionally, in some embodiments of the present application, the material of the nanoparticles includes one or more of YVO4, NaFY4, NaClY4, NaBrY4, NaIY4, YNbO4, YTaO4, GdCl3, and GdBr3; and / or

[0045] The rare earth metal elements include Eu 3+ 、Eu 2+ 、Ce 3+ , Tb 3+ One or more of; and / or

[0046] The halogen ligand includes one or more of Cl, Br, I, and F; and / or

[0047] In the composite material, the molar ratio of the rare earth metal element to the nanoparticles is (0.005-0.185):1.

[0048] Correspondingly, an embodiment of the present application further provides a light-emitting device, comprising a stacked anode, a light-emitting layer and a cathode, wherein the material of the light-emitting layer comprises the composite material prepared by the above-mentioned preparation method.

[0049] Optionally, in some embodiments of the present application, the anode and the cathode are independently selected from a doped metal oxide particle electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal element electrode or an alloy electrode, the material of the doped metal oxide particle electrode includes one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, tin-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode includes AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, the material of the metal element electrode includes one or more of Ag, Al, Cu, Mo, Au, Pt, Ca, Mg and Ba; and / or

[0050] The light-emitting device further comprises a hole transport layer between the anode and the light-emitting layer, wherein the material of the hole transport layer comprises 4,4'-N,N'-dicarbazolyl-biphenyl, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), N,N'-bis(3 -methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(N-vinylcarbazole) and its derivatives, N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1'-biphenyl-4- 4'-diamine, spiro NPB, poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], 1,3-bis(carbazol-9-yl)benzene, polyaniline, polypyrrole, poly(p-)phenylene vinylene, aromatic tertiary amines, polynuclear aromatic tertiary amines , 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO; and / or

[0051] The light-emitting device further comprises an electron transport layer between the light-emitting layer and the cathode, wherein the material of the electron transport layer comprises one or more of metal oxides, doped metal oxides, Group 2-6 semiconductor materials, Group 3-5 semiconductor materials and Group 1-3-6 semiconductor materials, wherein the metal oxides may include but are not limited to one or more of ZnO, TiO2, SnO2 and Ta2O3; the metal oxides in the doped metal oxides comprise one or more of ZnO, TiO2 and SnO2, and the doping elements comprise one or more of Al, Mg, Li, In and Ga; the Group 2-6 semiconductor materials comprise one or more of ZnS, ZnSe and CdS; the Group 3-5 semiconductor materials comprise one or more of InP and GaP; the Group 1-3-6 semiconductor materials comprise one or more of CuInS and CuGaS; and / or

[0052] The light-emitting device also includes a hole injection layer located between the anode and the light-emitting layer, and the material of the hole injection layer includes one or more of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, a derivative of PEDOT:PSS doped with s-MoO3, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0053] Correspondingly, an embodiment of the present application further provides a display device, which includes the above-mentioned light-emitting device.

[0054] The preparation method of the composite material described in the present application, adds an inorganic halogen salt to the cationic precursor solution, and the halogen ions in the inorganic halogen salt can form a chemical bond with the metal cation vacancies on the surface of the nanoparticles by a dipole effect, thereby effectively adjusting the concentration of metal ions that are not bonded to anions in the mixed solution system during the nanoparticle growth stage, for example, reducing the concentration of metal ions that are not bonded to anions in the mixed solution system, so that the problem of widening the half-peak width of the luminescence peak caused by doping rare earth elements in nanoparticles to obtain nanoparticles with narrow band gaps can be solved, thereby solving the problem of poor luminescence color purity caused by doping rare earth elements in nanoparticles, and then obtaining a composite material with high luminescence color purity; in addition, the halogen ions in the inorganic halogen salt can form a chemical bond with the metal cation vacancies on the surface of the nanoparticles by a dipole effect, thereby passivating the surface of the nanoparticles, thereby increasing the fluorescence intensity of the nanoparticles, thereby improving the luminescence performance of the device. Further, the surface of the nanoparticles doped with rare earth metal elements has fewer defects and higher structural stability, thereby having better luminescence performance, thereby improving the luminescence performance of the device. BRIEF DESCRIPTION OF THE DRAWINGS

[0055] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without paying any creative work.

[0056] Figure 1 is a flow chart of a method for preparing a composite material provided in an embodiment of the present application;

[0057] Figure 2 is a schematic structural diagram of a light-emitting device provided in an embodiment of the present application;

[0058] Figure 3 is a schematic structural diagram of another light-emitting device provided in an embodiment of the present application;

[0059] Figure 4 is a structural schematic diagram of another light-emitting device provided in an embodiment of the present application;

[0060] Figure 5 is a structural schematic diagram of another light-emitting device provided in an embodiment of the present application;

[0061] Figure 6 is a structural schematic diagram of another light-emitting device provided in an embodiment of the present application;

[0062] Figure 7 is a TEM image of the composite material of Example 1 of the present application;

[0063] Figure 8 is a TEM image of the composite material of Example 2 of the present application;

[0064] Fig. 9 is a TEM image of the composite material of Example 3 of the present application;

[0065] Fig.10 is a chromatogram of light emitted by the light emitting device of device embodiment 1 of the present application;

[0066] Fig.11 This is a chromatogram of light emitted by the light-emitting device of comparative example 2 of the present application.

[0067] Reference numerals:

[0068] Light-emitting device 100 ; anode 10 ; light-emitting layer 20 ; cathode 30 ; hole transport layer 40 ; electron transport layer 50 ; hole injection layer 60 . DETAILED DESCRIPTION

[0069] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0070] In this application, unless otherwise stated, directional words such as "upper" and "lower" generally refer to the upper and lower parts of the device in actual use or working state, specifically the drawing direction in the accompanying drawings; while "inner" and "outer" refer to the outline of the device. In addition, in the description of this application, the term "including" means "including but not limited to". The terms first, second, third, etc. are used only as labels and do not impose numerical requirements or establish an order.

[0071] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0072] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0073] In the present application, when a layer is formed "on" another layer, the so-called "on" is a broad concept, which may indicate that the formed another layer is adjacent to the certain layer, or may indicate that there are other spacing structural layers between the another layer and the certain layer. For example, when a second electrode is formed "on" the first carrier functional layer, the so-called "on" may indicate that the formed second electrode is adjacent to the first carrier functional layer, or may indicate that there are other spacing structural layers between the second electrode and the first carrier functional layer, such as a light-emitting layer.

[0074] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0075] The technical solution of this application is as follows:

[0076] First, see Figure 1 The present invention provides a method for preparing a composite material, comprising the following steps:

[0077] Step S11: providing a cationic precursor solution and an anionic precursor solution, wherein the cationic precursor solution comprises a cationic precursor salt, a rare earth metal salt, an inorganic halogen salt and a first solvent, and the anionic precursor solution comprises an anionic precursor salt and a second solvent;

[0078] Step S12: mixing the anion precursor solution and the cation precursor solution, and crystallizing them to obtain a composite material, wherein the composite material includes nanoparticles and rare earth metal elements doped in the nanoparticles, and the surfaces of the nanoparticles are connected with halogen ligands.

[0079] The preparation method of the composite material described in the present application, adds an inorganic halogen salt to the cationic precursor solution, and the halogen ions in the inorganic halogen salt can form a chemical bond with the metal cation vacancy on the surface of the nanoparticle by a dipole effect and connect to the surface of the nanoparticle as a ligand, thereby effectively adjusting the concentration of metal ions that are not bonded to anions in the mixed solution system (it can be understood that the mixed solution system here includes the liquid and the nanoparticles) during the nanoparticle growth stage, for example, reducing the concentration of metal ions that are not bonded to anions in the mixed solution system, so that the problem of widening the half-peak width of the luminescence peak caused by doping rare earth elements in nanoparticles to obtain nanoparticles with narrow band gaps can be effectively solved, thereby solving the problem of poor luminescence color purity caused by doping rare earth elements in nanoparticles, and then obtaining a composite material with high fluorescence intensity and high luminescence color purity. In addition, the halogen ions in the inorganic halogen salt can form a chemical bond with the metal cation vacancy on the surface of the nanoparticle by a dipole effect, thereby passivating the surface of the nanoparticles, and then improving the fluorescence intensity and corresponding photoelectric properties of the nanoparticles. Furthermore, the surface of the nanoparticles doped with rare earth metal elements has fewer defects and higher structural stability, thus having better luminescence performance.

[0080] In the step S11:

[0081] The cation precursor salt may include, but is not limited to, one or more of yttrium salt, gadolinium salt, sodium salt, niobium salt, and tantalum salt. The cation precursor salt may provide stable cations for the nanoparticles, and the cations are not easily reduced, which may effectively improve the stability of the nanoparticles.

[0082] In some embodiments, the yttrium salt may include, but is not limited to, one or more of yttrium nitrate, yttrium sulfate, yttrium chloride, and yttrium bromide.

[0083] In some embodiments, the gadolinium salt may include, but is not limited to, one or more of gadolinium nitrate, gadolinium sulfate, gadolinium chloride, and gadolinium bromide.

[0084] In some embodiments, the sodium salt may include, but is not limited to, one or more of sodium nitrate, sodium sulfate, sodium chloride, and sodium bromide.

[0085] In some embodiments, the niobium salt may include, but is not limited to, one or more of niobium nitrate, niobium sulfate, niobium chloride, and niobium bromide.

[0086] In some embodiments, the tantalum salt may include, but is not limited to, one or more of tantalum nitrate, tantalum sulfate, tantalum chloride, and tantalum bromide.

[0087] The rare earth metal salt may include but is not limited to one or more of rare earth metal nitrates, rare earth metal acetates, rare earth metal chlorides, and rare earth metal bromides. The rare earth metal salt can be well dissolved to form a rare earth metal element solution, which is conducive to preparing nanoparticles with good doping effect.

[0088] The rare earth metal salt may include, but is not limited to, one or more of europium salts, cerium salts, terbium salts, dysprosium salts, samarium salts, and ytterbium salts.

[0089] In some embodiments, the europium salt may include, but is not limited to, one or more of europium nitrate, europium acetate, europium chloride, and europium bromide.

[0090] In some embodiments, the cerium salt may include, but is not limited to, one or more of cerium nitrate, cerium acetate, cerium chloride, and cerium bromide.

[0091] In some embodiments, the terbium salt may include, but is not limited to, one or more of terbium nitrate, terbium acetate, terbium chloride, and terbium bromide.

[0092] In some embodiments, the dysprosium salt may include, but is not limited to, one or more of dysprosium nitrate, dysprosium acetate, dysprosium chloride, and dysprosium bromide.

[0093] In some embodiments, the samarium salt may include, but is not limited to, one or more of samarium nitrate, samarium acetate, samarium chloride, and samarium bromide.

[0094] In some embodiments, the ytterbium salt may include, but is not limited to, one or more of ytterbium nitrate, ytterbium acetate, ytterbium chloride, and ytterbium bromide.

[0095] The inorganic halide salt includes but is not limited to alkali metal halide salts, and the alkali metal halide salt includes but is not limited to one or more of sodium chloride, sodium bromide, sodium iodide, sodium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, potassium chloride, potassium bromide, potassium iodide, and potassium fluoride.

[0096] The inorganic halogen salt can ionize halogen ions, and the halogen ions can form chemical bonds with metal cation vacancies on the surface of nanoparticles by dipole effect and connect to the surface of nanoparticles as ligands, thereby passivating the surface of nanoparticles, and then improving the fluorescence intensity and corresponding photoelectric performance of nanoparticles. The halogen ions form chemical bonds with metal cation vacancies on the surface of nanoparticles by dipole effect, and can also effectively adjust the concentration of metal ions of different valence states in the mixed solution during the nanoparticle growth stage, such as reducing the concentration of free metal cations in the mixed solution system, so that the problem of widening of the half-peak width of the luminescence peak caused by doping rare earth elements in nanoparticles to obtain nanoparticles with narrow band gaps can be effectively solved, thereby solving the problem of poor luminescence color purity caused by doping rare earth elements in nanoparticles, and then obtaining a composite material with high fluorescence intensity and high luminescence color purity.

[0097] The first solvent is a solvent that can provide a reaction environment for crystal growth, for example, it may include but is not limited to one or more of water, alcohol solvents, amine solvents, sulfur-containing organic solvents, and ether solvents.

[0098] The alcohol solvent includes but is not limited to short-chain alcohols having 2 to 8 main chain C atoms, and the short-chain alcohols having 2 to 8 main chain C atoms are selected from one or more of methanol, ethanol, propanol, butanol, isopropanol, isobutanol and ethylene glycol.

[0099] The amine solvent includes, but is not limited to, one or more of dimethylformamide, dioctylamine, and ethylenediamine.

[0100] The sulfur-containing organic solvent includes but is not limited to dimethyl sulfoxide.

[0101] The ether solvent includes, but is not limited to, one or more of tetrahydrofuran, diethyl ether, and propylene oxide.

[0102] In some embodiments, in the cationic precursor solution, the concentration of the cation of the cationic precursor salt is 0.005-0.05 mmol / ml, for example, 0.01-0.03 mmol / ml, 0.015-0.035 mmol / ml, 0.02-0.04 mmol / ml, 0.025-0.045 mmol / ml, etc. Within the concentration range, the rate of the crystallization reaction can be within an appropriate range, which is conducive to the preparation of nanoparticles with good size uniformity.

[0103] In some embodiments, the molar ratio of the cation in the cationic precursor salt to the rare earth metal salt is (5-20): 1, for example, (6-13): 1, (7-14): 1, (8-15): 1, (9-16): 1, (10-17): 1, (11-18): 1, (12-19): 1, (13-19.5): 1. Within the molar ratio range, nanoparticles with a suitable rare earth metal element doping amount can be prepared to achieve a better doping effect.

[0104] In some embodiments, the molar ratio of the inorganic halide salt to the cation in the cationic precursor salt is (0.02-0.2):1, for example, (0.04-0.16):1, (0.06-0.18):1, (0.08-0.2):1, (0.1-0.14):1, (0.12-0.19):1, etc. Within the molar ratio range, the metal cation vacancy defects on the surface of the nanoparticles can be effectively passivated, achieving excellent passivation effect, which is conducive to preparing nanoparticles with excellent photoelectric properties.

[0105] In some embodiments, when the rare earth metal salt is a europium salt, since only trivalent europium salt exists and trivalent europium emits red light, when it is necessary to dope divalent europium that emits blue light in the nanoparticles, the cationic precursor solution also includes a reducing inorganic salt. The reducing inorganic salt can reduce the trivalent europium in the europium salt to divalent europium to prepare a composite material with better blue light emitting color.

[0106] The reducing inorganic salt may include, but is not limited to, one or more of sulfites, selenites, tellurites, thiosulfates, thioselenates, and thiotellurates.

[0107] In some embodiments, the sulfite includes, but is not limited to, one or more of sodium sulfite, cadmium sulfite, lead sulfite, indium sulfite, and silver sulfite.

[0108] In some embodiments, the selenite includes, but is not limited to, one or more of sodium selenite, cadmium selenite, lead selenite, indium selenite, and silver selenite.

[0109] In some embodiments, the tellurite includes, but is not limited to, one or more of sodium tellurite, cadmium tellurite, lead tellurite, and silver tellurite.

[0110] In some embodiments, the thiosulfate salt includes, but is not limited to, one or more of sodium thiosulfate, cadmium thiosulfate, lead thiosulfate, and silver thiosulfate.

[0111] In some embodiments, the thioselenate includes, but is not limited to, one or more of sodium thioselenate and cadmium thioselenate.

[0112] In some embodiments, the thiotellurate includes but is not limited to sodium thiotellurate.

[0113] The molar ratio of the reducing inorganic salt to the rare earth metal salt is (0.5-10):1, for example, (1-6):1, (2-7):1, (3-8):1, (4-9):1, etc. Within the molar ratio range, the trivalent europium ions can be effectively reduced, and the cationic precursor solution can have an appropriate pH range, which is conducive to the growth of crystals.

[0114] In some embodiments, the cationic precursor solution further includes a nonionic polymer compound, which can effectively increase the viscosity of the cationic precursor solution, reduce the speed of the crystallization reaction, and make the size uniformity of the prepared nanoparticles better.

[0115] The non-ionic polymer compound may include, but is not limited to, one or more of polyvinylpyrrolidone (PVP), polypropylenepyrrolidone, and polybutylenepyrrolidone.

[0116] In some embodiments, the molar ratio of the nonionic polymer compound to the cation in the cationic precursor salt is (0.05-0.1):1, for example, 0.06:1, 0.07:1, 0.08:1, 0.09:1, etc. Within the molar ratio range, it is beneficial to prepare a cationic precursor solution with a suitable viscosity, thereby effectively controlling the reaction rate and preparing nanoparticles with relatively uniform size.

[0117] In some embodiments, the method for preparing the cationic precursor solution comprises:

[0118] A. providing a cationic precursor salt and a third solvent, mixing them to obtain a cationic precursor salt solution;

[0119] B. providing a rare earth metal salt and a fourth solvent, mixing them to obtain a rare earth metal salt solution;

[0120] C. Mixing the cationic precursor salt solution and the rare earth metal salt solution at room temperature, and stirring for 5 to 15 minutes under vacuum or inert atmosphere to obtain a mixed solution;

[0121] D. Adding an inorganic halide salt to the mixed solution and stirring for 5 to 15 minutes under vacuum or inert atmosphere to obtain the cationic precursor solution.

[0122] In some embodiments, the reducing inorganic salt and / or the non-ionic polymer compound are added to the mixed solution at the same time as the inorganic halide salt is added.

[0123] In some embodiments, after adding an inorganic halide to the mixed solution and stirring for 5 to 15 minutes under vacuum or inert atmosphere, and before obtaining the cationic precursor solution, the process further includes: adding a nonionic polymer compound to the mixed solution system and stirring at room temperature for 1 to 3 hours.

[0124] The third solvent and the fourth solvent independently include, but are not limited to, one or more of water, a short-chain alcohol having 2 to 8 main chain carbon atoms, dimethylformamide, dimethyl sulfoxide, and tetrahydrofuran. The short-chain alcohol having 2 to 8 main chain carbon atoms is selected from one or more of methanol, ethanol, propanol, butanol, isopropanol, isobutanol, and ethylene glycol.

[0125] The inert atmosphere may include, but is not limited to, one or more of nitrogen, argon, and helium.

[0126] In the step S12:

[0127] The anion precursor solution includes anion precursor salt and a second solvent.

[0128] The anion precursor salt may include, but is not limited to, one or more of ammonium vanadate, ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, yttrium chloride, yttrium bromide, and yttrium iodide.

[0129] The second solvent is a solvent that can provide a reaction environment for crystal growth, for example, it can include but is not limited to one or more of water, alcohol solvents, amine solvents, sulfur-containing organic solvents, and ether solvents. The alcohol solvents, amine solvents, sulfur-containing organic solvents, and ether solvents are described above and will not be described in detail here.

[0130] In some embodiments, in the anion precursor solution, the concentration of the anion precursor salt is 0.05-1 mmol / ml, for example, 0.1-0.6 mmol / ml, 0.2-0.7 mmol / ml, 0.3-0.8 mmol / ml, 0.4-0.9 mmol / ml, 0.5-0.95 mmol / ml, etc. Within the concentration range, the rate of the crystallization reaction can be within an appropriate range, which is conducive to preparing nanoparticles with good size uniformity.

[0131] The molar ratio of the anion in the anionic precursor salt to the cation in the cationic precursor salt is (10-20):1, such as (11-16):1, (12-17):1, (13-18):1, (14-19):1, (15-19.5):1, etc. Within the molar ratio range, it is beneficial to prepare nanoparticles with uniform size and excellent fluorescence efficiency.

[0132] In some embodiments, the anion precursor solution is injected into the cationic precursor solution in a one-time addition manner, or the anion precursor solution is injected into the cationic precursor solution in a stepwise addition manner.

[0133] The preparation method of the composite material described in the present application is simple to operate and easy to repeat. It effectively solves the problem of widening of the half-width of the luminescence peak caused by doping rare earth elements into nanoparticles to obtain nanoparticles with a narrow band gap, thereby solving the problem of deterioration of luminescence color purity caused by doping rare earth elements into nanoparticles, and further obtaining a composite material with high fluorescence intensity and high luminescence color purity.

[0134] In a second aspect, an embodiment of the present application further provides a composite material prepared by the composite material preparation method described above, wherein the composite material comprises nanoparticles and rare earth metal elements doped in the nanoparticles, and the surface of the nanoparticles is connected to a halogen ligand.

[0135] In some embodiments, the composite material consists of the nanoparticles and rare earth metal elements doped in the nanoparticles, wherein halogen ligands are connected to the surfaces of the nanoparticles.

[0136] The material of the nanoparticles may include, but is not limited to, one or more of YVO4, NaFY4, NaClY4, NaBrY4, NaIY4, YNbO4, YTaO4, GdCl3, and GdBr3.

[0137] The rare earth metal element may include but is not limited to Eu 3+ 、Eu 2+ 、Ce 3+ , Tb 3+ One or more of .

[0138] The halogen ligands include, but are not limited to, one or more of Cl, Br, I, and F.

[0139] In the composite material, the molar ratio of the rare earth metal element to the nanoparticle is (0.005-0.185):1, for example, (0.01-0.11):1, (0.02-0.12):1, (0.03-0.13):1, (0.04-0.14):1, (0.05-0.15):1, (0.06-0.16):1, (0.07-0.17):1, (0.08-0.18):1, (0.06-0.08):1, (0.07-0.09):1, etc. Within the ratio range, the composite material can have excellent photoelectric properties.

[0140] In a third aspect, an embodiment of the present application provides a film, wherein the film includes the composite material described above.

[0141] It can be understood that the film can be a luminescent film.

[0142] Fourth, please refer to Figure 2 The embodiment of the present application further provides a light emitting device 100, comprising an anode 10, a light emitting layer 20 and a cathode 30 stacked in sequence. The material of the light emitting layer 20 comprises the composite material described above.

[0143] See also Figure 3 In one embodiment, the light emitting device 100 further includes a hole transport layer 40 between the anode 10 and the light emitting layer 20. In other words, the light emitting device 100 includes the anode 10, the hole transport layer 40, the light emitting layer 20 and the cathode 30 stacked in sequence.

[0144] See also Figure 4 In one embodiment, the light emitting device 100 further includes an electron transport layer 50 between the light emitting layer 20 and the cathode 30. In other words, the light emitting device 100 includes an anode 10, a light emitting layer 20, an electron transport layer 50 and a cathode 30 stacked in sequence.

[0145] See also Figure 5 In one embodiment, the light emitting device 100 includes an anode 10, a hole transport layer 40, a light emitting layer 20, an electron transport layer 50 and a cathode 30 which are stacked in sequence.

[0146] See also Figure 6 In one embodiment, the light emitting device 100 further includes a hole injection layer 60 between the anode 10 and the hole transport layer 40. In other words, the light emitting device 100 includes an anode 10, a hole injection layer 60, a hole transport layer 40, a light emitting layer 20, an electron transport layer 50 and a cathode 30 stacked in sequence.

[0147] The anode 10 and the cathode 30 are anodes and cathodes for light-emitting devices known in the art, and can be independently, but not limited to, doped metal oxide particle electrodes, composite electrodes, graphene electrodes, carbon nanotube electrodes, metal single-substance electrodes or alloy electrodes. The material of the doped metal oxide particle electrode can be, but not limited to, one or more of indium-doped tin oxide (ITO), fluorine-doped tin oxide (FTO), antimony-doped tin oxide (ATO), aluminum-doped zinc oxide (AZO), gallium-doped zinc oxide (GZO), tin-doped zinc oxide (ZTO), indium-doped zinc oxide (IZO), magnesium-doped zinc oxide (MZO) and aluminum-doped magnesium oxide (AMO). The composite electrode is a composite electrode in which metal is sandwiched between doped or undoped transparent metal oxide particles, such as AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, etc., wherein " / " represents a stacked structure, for example, AZO / Ag / AZO represents a composite electrode including an AZO layer, an Ag layer and an AZO layer stacked in sequence. The material of the metal single substance electrode may include but is not limited to one or more of Ag, Al, Cu, Mo, Au, Pt, Ca, Mg and Ba.

[0148] The material of the hole transport layer 40 may also be a material known in the art for a hole transport layer, for example, it may include but is not limited to 4,4'-N,N'-dicarbazolyl-biphenyl (CBP), poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine (α-NPD), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine (TPD), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) (Poly-TPD), N ...1-naphthyl)-1,1'-biphenyl-4,4"-diamine (α-NPD), (3-methylphenyl)-N,N'-bis(phenyl)-spiro(spiro-TPD), N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine (DNTPD), 4,4',4'-tri(N-carbazolyl)-triphenylamine (TCTA), 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))] (TFB), poly(N-vinylcarbazole) (PVK) and its derivatives, N,N'-di(1-naphthyl)-N,N'-diphenyl -1,1'-biphenyl-4-4'-diamine (NPB), spiro NPB, poly(phenylene vinylene) (PPV), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene] (MEH-PPV), poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene] (MOMO-PPV), 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene (spiro-omeTAD), 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline] (TAPC), 1,3-bis(carbazol-9-yl)benzene (MCP ), polyaniline, polypyrrole, poly(p-)phenylene vinylene, aromatic tertiary amine, polynuclear aromatic tertiary amine, 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compound, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO. One or more.

[0149] The material of the electron transport layer 50 is a material known in the art for electron transport layers, for example, it may include but not limited to one or more of metal oxides, doped metal oxides, 2-6 group semiconductor materials, 3-5 group semiconductor materials and 1-3-6 group semiconductor materials. Specifically, the metal oxide may include but not limited to one or more of ZnO, TiO2, SnO2, Ta2O3; the metal oxide in the doped metal oxide may include but not limited to one or more of ZnO, TiO2, SnO2, and the doping element may include but not limited to one or more of Al, Mg, Li, In, and Ga. For example, the doped metal oxide may be aluminum zinc oxide (AZO), lithium-doped zinc oxide (LZO), and magnesium-doped zinc oxide (MZO). The 2-6 semiconductor group material may include but not limited to one or more of ZnS, ZnSe, and CdS; the 3-5 semiconductor group material may include but not limited to one or more of InP and GaP; the 1-3-6 group semiconductor material may include but not limited to one or more of CuInS and CuGaS.

[0150] In at least one embodiment, the material of the electron transport layer 50 is ZnO particles modified by a free radical scavenger.

[0151] The material of the hole injection layer 60 can also be a material known in the art for the hole injection layer, for example, it can include but is not limited to one or more of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HAT-CN), PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO3 derivatives (PEDOT:PSS:s-MoO3), 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine (m-MTDATA), tetracyanoquinodimethane (F4-TCQN), copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0152] It is understandable that the light-emitting device may also be provided with some functional layers conventionally used in light-emitting devices to help improve the performance of the light-emitting device, such as an electron blocking layer, a hole blocking layer, an electron injection layer, an interface modification layer, etc.

[0153] It can be understood that the materials of each layer of the light-emitting device can be adjusted according to the light-emitting requirements of the light-emitting device.

[0154] In some embodiments, the light emitting device 100 further includes a substrate, and the substrate is disposed on a surface of the anode 10 away from the light emitting layer 20 , or the substrate is disposed on a surface of the cathode 30 away from the light emitting layer 20 .

[0155] The substrate may be a rigid substrate or a flexible substrate. In some embodiments, the material of the substrate may include but is not limited to one or more of glass, silicon wafer, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyethylene naphthalate, polyamide and polyether sulfone.

[0156] It can be understood that the light emitting device 100 can be a positive light emitting device or an inverted light emitting device. The light emitting device 100 can be a quantum dot light emitting device or an organic light emitting device.

[0157] The light-emitting layer 20 of the light-emitting device 100 described in the present application includes the composite material described above, and thus has higher light-emitting efficiency and longer lifespan.

[0158] The present application also relates to a display device, which includes the light-emitting device 100 .

[0159] The display device can be any electronic product with a display function, including but not limited to smart phones, tablet computers, laptops, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, among which smart wearable devices can be, for example, smart bracelets, smart watches, virtual reality (VR) helmets, etc.

[0160] The present application is described in detail below through specific embodiments. The following embodiments are only partial embodiments of the present application and are not limitations of the present application.

[0161] Example 1

[0162] Take 10 ml of an aqueous solution containing 0.1 mmol of yttrium nitrate, 0.01 mmol of europium nitrate and 0.01 mmol of cerium nitrate, mix them, and stir them for 10 min under a nitrogen atmosphere; then, add 0.02 mmol of NaCl to the system and stir for 10 min; then, add 0.01 mmol of polyvinyl pyrrolidone to the system and stir vigorously for 5 min to obtain a cationic precursor solution;

[0163] Take 10 ml of 0.1 mmol ammonium vanadate solution (anion precursor solution), add the ammonium vanadate solution dropwise to the cationic precursor solution until a white flocculent precipitate appears in the solution, stop adding, then centrifuge and wash the precipitate to obtain Eu 3+ and Ce 3+ The composite material is prepared by co-doping YVO4 nanoparticles.

[0164] In the composite material of this embodiment, Eu 3+ The doping amount is Eu 3+The molar ratio of Ce to YVO4 is 0.075:1. 3+ The doping amount is Ce 3+ The molar ratio with YVO4 is 0.05:1.

[0165] Example 2

[0166] Take 10 ml of 0.1 mmol of yttrium nitrate aqueous solution and 0.01 mmol of europium nitrate solution, mix them, and stir them for 10 min under nitrogen atmosphere; then, add 0.08 mmol of Na2SO3 to the system, and then add SO3 2- The reduction of Eu 3+ Reduction to Eu 2+ , then add 0.02 mmol of NaCl to the system and stir for 10 min; then add 0.01 mmol of polypropylene pyrrolidone to the system and stir vigorously for 5 min to obtain a cationic precursor solution;

[0167] Take 10 ml of 0.1 mmol ammonium vanadate solution (anion precursor solution), add the ammonium vanadate solution dropwise to the cationic precursor solution until a white flocculent precipitate appears in the solution, stop adding, then centrifuge and wash the precipitate to obtain Eu 2+ By doping YVO4 nanoparticles, a composite material is prepared.

[0168] In the composite material of this embodiment, Eu 2+ The doping amount is Eu 2+ The molar ratio with YVO4 is 0.05:1.

[0169] Example 3

[0170] Take 10 ml of a 0.1 mmol sodium sulfate aqueous solution, 0.01 mmol cerium nitrate and 0.01 mmol terbium nitrate solution, mix them, and stir them for 10 min under a nitrogen atmosphere; then, add 0.02 mmol NaCl to the system and stir for 10 min; then add 0.01 mmol polypropylene pyrrolidone to the system and stir vigorously for 5 min to obtain a cationic precursor solution;

[0171] Take 10 ml of 0.1 mmol ammonium fluoride and 0.1 mmol yttrium chloride solution, add the anion precursor solution dropwise to the cationic precursor until a white flocculent precipitate appears in the solution, stop adding, and then centrifuge and wash the precipitate to obtain Ce 3+ and Tb 3+ The composite material is prepared by co-doping NaYF4 nanoparticles.

[0172] In the composite material of this embodiment, Ce 3+The doping amount is Ce 3+ The molar ratio of Tb to NaYF4 is 0.05:1. 3+ The doping amount is Tb 3+ The molar ratio with NaYF4 is 0.08:1.

[0173] Example 4

[0174] This example is substantially the same as Example 1, except that the amount of cerium nitrate used in this example is 0.03 mmol.

[0175] In the composite material of this embodiment, Eu 3+ The doping amount is Eu 3+ The molar ratio of Ce to YVO4 is 0.075:1. 3+ The doping amount is Ce 3+ The molar ratio to YVO4 is 0.075:1.

[0176] Example 5

[0177] This example is substantially the same as Example 1, except that the amount of cerium nitrate used in this example is 0.05 mmol.

[0178] In the composite material of this embodiment, Eu 3+ The doping amount is Eu 3+ The molar ratio of Ce to YVO4 is 0.075:1. 3+ The doping amount is Ce 3+ The molar ratio with YVO4 is 0.1:1.

[0179] Example 6

[0180] This embodiment is substantially the same as embodiment 2, except that the amount of europium nitrate used in this embodiment is 0.03 mmol.

[0181] In the composite material of this embodiment, Eu 2+ The doping amount is Eu 2+ The molar ratio to YVO4 is 0.07:1.

[0182] Example 7

[0183] This embodiment is substantially the same as embodiment 2, except that the amount of europium nitrate used in this embodiment is 0.05 mmol.

[0184] In the composite material of this embodiment, Eu 2+ The doping amount is Eu 2+ The molar ratio to YVO4 is 0.095:1.

[0185] Example 8

[0186] This embodiment is substantially the same as embodiment 3, except that the amount of cerium nitrate used in this embodiment is 0.03 mmol.

[0187] In the composite material of this embodiment, Ce 3+ The doping amount is Ce 3+ The molar ratio of Tb to NaYF4 is 0.08:1. 3+ The doping amount is Tb 3+ The molar ratio with NaYF4 is 0.08:1.

[0188] Example 9

[0189] This embodiment is substantially the same as embodiment 3, except that the amount of terbium nitrate used in this embodiment is 0.03 mmol.

[0190] In the composite material of this embodiment, Ce 3+ The doping amount is Ce 3+ The molar ratio of Tb to NaYF4 is 0.05:1. 3+ The doping amount is Tb 3+ The molar ratio with NaYF4 is 0.1:1.

[0191] Example 10

[0192] 10 ml of an aqueous solution containing 0.1 mmol of gadolinium nitrate, 0.01 mmol of europium nitrate and 0.01 mmol of cerium nitrate were mixed and stirred for 10 min under a nitrogen atmosphere; then, 0.02 mmol of NaCl was added to the system and stirred for 10 min; then, 0.01 mmol of polyvinyl pyrrolidone was added to the system and stirred vigorously for 5 min to obtain a cationic precursor solution;

[0193] Take 10 ml of 0.1 mmol ammonium chloride solution (anion precursor solution), add the ammonium chloride solution dropwise to the cationic precursor solution until a white flocculent precipitate appears in the solution, stop adding, then centrifuge and wash the precipitate to obtain Eu 3+ and Ce 3+ The composite material is prepared by co-doping GdCl3 nanoparticles.

[0194] In the composite material of this embodiment, Eu 3+ The doping amount is Eu 3+ The molar ratio of Ce to GdCl3 is 0.05:1. 3+ The doping amount is Ce 3+ The molar ratio with GdCl3 is 0.06:1.

[0195] Comparative Example 1

[0196] YVO4:Sm was synthesized by sol-gel method. 3+ ,Eu 3+ Nanocrystals (i.e. Sm 3+ and Eu 3+ co-doped YVO4 nanocrystals).

[0197] First, weigh 0.01mmol of Eu2O3 (99.99%), 0.025mmols of Sm2O3 (99.99%) and 0.465mmol of Y2O3 (99.99%) and dissolve them in 2mol / L nitric acid solution respectively and heat to form Eu(NO3)3, Sm(NO3)3 and Y(NO3)3 solutions. When these raw materials are fully dissolved, mix them evenly in a beaker, add 1mmol of NH4VO3(AR) and 6mmols of citric acid, add ammonia water to adjust the pH value to 6, then put the mixed solution into a water bath at 80℃ and heat it until the solution becomes a sol, then put the sol into an oven and bake it at 120℃ for 24 hours to turn the sol into a dry gel, then transfer the dry gel into a small crucible and pre-sinter it in a muffle furnace at 700℃ in air atmosphere for 2 hours; after the sample is cooled, put it into a muffle furnace and calcine it at 1000℃ in air atmosphere for 4 hours to finally obtain white powdery YVO4:Sm 3+ ,Eu 3+ Nanocrystalline composite materials.

[0198] Comparative Example 2

[0199] This embodiment is substantially the same as Embodiment 1, except that no inorganic halogen salt NaCl is added in this embodiment.

[0200] The composite materials of Examples 1 to 3 were subjected to TEM tests, and the results were Figures 7 to 9 TEM image shown. Figures 7 to 9 It can be seen that the composite material of the present application has good particle size uniformity and dispersibility, and there is no agglomeration phenomenon.

[0201] The composite materials of Examples 1 to 10 and the composite materials of Comparative Examples 1 to 2 were tested for fluorescence intensity. The fluorescence intensity was tested by direct testing with a fluorescence tester. The test results are shown in Table 1.

[0202] Table 1:

[0203] Fluorescence intensity (au) Example 1 5.2E4 Example 2 7.5E4 Example 3 6.3E4 Example 4 8.2E4 Example 5 9.9E4 Example 6 4.3E4 Example 7 3.7E4 Example 8 5.6E4 Example 9 5.0E4 Example 10 6.4E4 Comparative Example 1 4.1E3 Comparative Example 2 4.7E3

[0204] It can be seen from Table 1 that the composite materials of Examples 1 to 10 have higher fluorescence intensities than the composite materials of Comparative Examples 1 to 2. It can be seen that the preparation method of the composite material of the present application can prepare a composite material with higher fluorescence intensity.

[0205] Device Example 1

[0206] The patterned ITO substrate is placed in acetone, washing liquid, deionized water and isopropanol for ultrasonic cleaning in sequence. Each ultrasonic step needs to last for about 15 minutes. After the ultrasonic cleaning is completed, the ITO substrate is placed in a clean oven for drying. After the ITO substrate is dried, the surface of the ITO substrate is treated with ultraviolet-ozone for 5 minutes to further remove organic matter attached to the surface of the ITO substrate and improve the work function of ITO.

[0207] Depositing PEDOT:PSS material on the surface of the ITO substrate, and then heating on a heating table at 150° C. for 30 minutes to obtain a hole injection layer 60 with a thickness of 30 nm;

[0208] In a nitrogen atmosphere, a TFB material is spin-coated on the hole injection layer 60 , and then heated on a heating table at 150° C. for 30 minutes to obtain a hole transport layer 40 with a thickness of 30 nm;

[0209] The composite material in Example 1 is deposited on the hole transport layer 40, and then heated on a heating table at 100°C for 10 minutes to obtain a light-emitting layer 20 with a thickness of 30 nm;

[0210] Depositing ZnO material on the light-emitting layer 20, and then heating on a heating table at 80°C for 30 minutes to obtain an electron transport layer 50 with a thickness of 30 nm;

[0211] Ag is evaporated on the electron transport layer 50 to obtain a cathode 30 with a thickness of 80 nm;

[0212] The light emitting device 100 is packaged using ultraviolet curing adhesive.

[0213] Device Examples 2 to 10

[0214] Device Examples 2 to 10 are substantially the same as Device Example 1, except that Device Examples 2 to 10 use the composite materials of Examples 2 to 10 to replace the composite materials in Device Example 1, respectively.

[0215] Device Comparison Examples 1 to 2

[0216] Device Comparative Examples 1-2 are substantially the same as Device Example 1, except that the composite materials in Device Example 1 are replaced by the composite materials in Comparative Examples 1-2.

[0217] The half-peak width of the light emitted by the light-emitting devices of device embodiment 1 and device comparison example 2 is tested. The testing method is: using Ocean Optic USB2000+ spectrometer to test the light color of the light-emitting devices of device embodiment 1 and device comparison example 2, to obtain a light emission chromatogram of the light-emitting device, and draw a straight line parallel to the bottom of the peak from the midpoint of the peak height of the chromatogram. The distance between the two points where this straight line intersects with the two sides of the peak is the half-peak width.

[0218] Fig.10 and Fig.11 The following are spectra of the light emitted by the light emitting devices of device embodiment 1 and device comparative example 2, respectively. Fig.10 and Fig.11 It can be seen that the half-peak width of the light emitted by the light-emitting device of device embodiment 1 is 24nm, and the half-peak width of the light emitted by the light-emitting device of device comparative example 2 is 40nm. It can be seen that the composite material prepared by the preparation method of the embodiment of the present application has a narrower half-peak width of light emission, and thus has a higher color purity.

[0219] The light emitting devices of device embodiments 1 to 10 and device comparative examples 1 to 2 were subjected to the lighting voltage, 40 mA / cm 2 Voltage, CIE coordinates, and external quantum efficiency EQE test under current density. See Table 2 for test results.

[0220] The test method for the start-up voltage is as follows: the voltage value when the brightness reaches 1 nit is obtained in the efficiency test system built by Keithley 6485, which is the start-up voltage.

[0221] 40mA / cm 2 The test method of voltage and CIE under current density is: use FPD optical property measurement equipment to measure voltage, current, brightness, luminous spectrum and other parameters, and calculate that 40mA / cm 2 The voltage under current density and luminescence spectrum data can directly read the CIE coordinates.

[0222] The detection method of external quantum efficiency EQE is: using FPD optical property measurement equipment from Foster, controlling the efficiency test system built by QE PRO spectrometer, Keithley 2400, and Keithley 6485 through LabView, measuring parameters such as voltage, current, brightness, and luminescence spectrum, and calculating the external quantum efficiency EQE.

[0223] Table 2:

[0224]

[0225] From Table 2 we can see that:

[0226] Compared with the light-emitting devices of device comparison examples 1 to 2, the light-emitting devices of device embodiments 1 to 10 have lower turn-on voltages. It can be seen that the composite material prepared by the method for preparing the composite material of the present application can effectively reduce the turn-on voltage of the light-emitting device.

[0227] Compared with the light-emitting devices of device comparative examples 1 to 2, the light-emitting devices of device embodiments 1 to 10 have a power consumption of 40 mA / cm 2 The voltage under the current density is lower, which shows that the composite material prepared by the preparation method of the composite material of the present application can effectively reduce the operating voltage of the light-emitting device. The reason may be that the composite material described in the present application has good electrical conductivity.

[0228] It can be seen from the CIE coordinate values ​​of Examples 1 to 10 that the color coordinates of the light-emitting device prepared from the composite material described in the present application cover a wider area and can achieve full-spectrum luminescence. The reason may be that rare earth-doped nanocrystals can obtain a series of CIE-varying materials by changing the proportion of rare earth elements, thereby obtaining a full spectrum.

[0229] The composite materials and preparation methods thereof, light-emitting devices and display devices provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A method for preparing a composite material, characterized in that: The steps include: Providing a cationic precursor solution and an anionic precursor solution, wherein the cationic precursor solution comprises a cationic precursor salt, a rare earth metal salt, an inorganic halogen salt and a first solvent, and the anionic precursor solution comprises an anionic precursor salt and a second solvent; The anion precursor solution and the cationic precursor solution are mixed to obtain the composite material.

2. The preparation method according to claim 1, characterized in that: The cationic precursor salt includes one or more of yttrium salt, gadolinium salt, sodium salt, niobium salt, and tantalum salt; and / or The rare earth metal salt includes one or more of rare earth metal nitrates, rare earth metal acetates, rare earth metal chlorides, and rare earth metal bromides; and / or The rare earth metal salt includes one or more of europium salt, cerium salt, terbium salt, dysprosium salt, samarium salt and ytterbium salt; and / or The inorganic halogen salt comprises an alkali metal halide salt; and / or The anion precursor salt includes one or more of ammonium vanadate, ammonium fluoride, ammonium chloride, ammonium bromide, ammonium iodide, yttrium chloride, yttrium bromide, and yttrium iodide; and / or The first solvent and the second solvent independently include one or more of water, alcohol solvents, amine solvents, sulfur-containing organic solvents, and ether solvents.

3. The preparation method according to claim 2, characterized in that: The yttrium salt includes one or more of yttrium nitrate, yttrium sulfate, yttrium chloride, and yttrium bromide; and / or The gadolinium salt includes one or more of gadolinium nitrate, gadolinium sulfate, gadolinium chloride, and gadolinium bromide; and / or The sodium salt includes one or more of sodium nitrate, sodium sulfate, sodium chloride and sodium bromide; and / or The niobium salt comprises one or more of niobium nitrate, niobium sulfate, niobium chloride and niobium bromide; and / or The tantalum salt comprises one or more of tantalum nitrate, tantalum sulfate, tantalum chloride and tantalum bromide; and / or The europium salt includes one or more of europium nitrate, europium acetate, europium chloride, and europium bromide; and / or The cerium salt includes one or more of cerium nitrate, cerium acetate, cerium chloride, and cerium bromide; and / or The terbium salt includes one or more of terbium nitrate, terbium acetate, terbium chloride, and terbium bromide; and / or The dysprosium salt includes one or more of dysprosium nitrate, dysprosium acetate, dysprosium chloride, and dysprosium bromide; and / or The samarium salt includes one or more of samarium nitrate, samarium acetate, samarium chloride, and samarium bromide; and / or The ytterbium salt includes one or more of ytterbium nitrate, ytterbium acetate, ytterbium chloride, and ytterbium bromide; and / or The alkali metal halide salt includes one or more of sodium chloride, sodium bromide, sodium iodide, sodium fluoride, lithium chloride, lithium bromide, lithium iodide, lithium fluoride, potassium chloride, potassium bromide, potassium iodide, and potassium fluoride; and / or The alcohol solvent comprises a short-chain alcohol having 1 to 8 main chain carbon atoms; and / or The amine solvent includes one or more of dimethylformamide, dioctylamine, and ethylenediamine; and / or The sulfur-containing organic solvent comprises dimethyl sulfoxide; and / or The ether solvent includes one or more of tetrahydrofuran, diethyl ether and propylene oxide.

4. The preparation method according to claim 1, characterized in that: In the cationic precursor solution, the concentration of the cation of the cationic precursor salt is 0.005 to 0.05 mmol / ml; and / or The molar ratio of the cation in the cationic precursor salt to the rare earth metal salt is (5-20):1; and / or The molar ratio of the inorganic halide salt to the cation in the cationic precursor salt is (0.02-0.2):1; and / or In the anion precursor solution, the concentration of the anion precursor salt is 0.05 to 1 mmol / ml; and / or The molar ratio of the anion in the anion precursor salt to the cation in the cationic precursor salt is (10-20):

1.

5. The preparation method according to claim 1, characterized in that: The rare earth metal salt is a europium salt, and the cationic precursor solution also includes a reducing inorganic salt.

6. The preparation method according to claim 5, characterized in that: The reducing inorganic salt includes one or more of sulfite, selenite, tellurite, thiosulfate, thioselenate, and thiotellurate; and / or The molar ratio of the reducing inorganic salt to the rare earth metal salt is (0.5-10):

1.

7. The preparation method according to claim 1 or 5, characterized in that: The cationic precursor solution also includes non-ionic polymer compounds.

8. The preparation method according to claim 7, characterized in that: The non-ionic polymer compound includes one or more of polyvinyl pyrrolidone, polypropylene pyrrolidone and polybutylene pyrrolidone; and / or The molar ratio of the nonionic polymer compound to the cation in the cationic precursor salt is (0.05-0.1):

1.

9. A composite material, characterized in that: The invention comprises nanoparticles and rare earth metal elements doped in the nanoparticles, wherein the surfaces of the nanoparticles are connected with halogen ligands.

10. The composite material according to claim 9, characterized in that: The composite material consists of the nanoparticles and rare earth metal elements doped in the nanoparticles, wherein the surfaces of the nanoparticles are connected with halogen ligands.

11. The composite material according to claim 9 or 10, characterized in that: The material of the nanoparticles includes one or more of YVO4, NaFY4, NaClY4, NaBrY4, NaIY4, YNbO4, YTaO4, GdCl3, and GdBr3; and / or The rare earth metal elements include Eu 3+ 、Eu 2+ 、Ce 3+ , Tb 3+ One or more of; and / or The halogen ligand includes one or more of Cl, Br, I, and F; and / or In the composite material, the molar ratio of the rare earth metal element to the nanoparticles is (0.005-0.185):

1.

12. A light emitting device comprising a stacked anode, a light emitting layer and a cathode, characterized in that: The material of the light-emitting layer includes the composite material prepared by the preparation method according to any one of claims 1 to 8, or the material of the light-emitting layer includes the composite material according to any one of claims 9 to 11.

13. The light emitting device according to claim 12, characterized in that: The anode and the cathode are independently selected from a doped metal oxide particle electrode, a composite electrode, a graphene electrode, a carbon nanotube electrode, a metal single substance electrode or an alloy electrode. The material of the doped metal oxide particle electrode includes one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, tin-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide. The composite electrode includes AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS. The material of the metal single substance electrode includes one or more of Ag, Al, Cu, Mo, Au, Pt, Ca, Mg and Ba. And / or The light-emitting device further comprises a hole transport layer between the anode and the light-emitting layer, wherein the material of the hole transport layer comprises 4,4'-N,N'-dicarbazolyl-biphenyl, poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine], N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), N,N'-bis(3 -methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine, 4,4',4'-tri(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(N-vinylcarbazole) and its derivatives, N,N'-di(1-naphthyl)-N,N'-diphenyl-1,1'-biphenyl-4- 4'-diamine, spiro NPB, poly(phenylene vinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylene vinylene], poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylene vinylene], 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene, 4,4'-cyclohexylbis[N,N-di(4-methylphenyl)aniline], 1,3-bis(carbazol-9-yl)benzene, polyaniline, polypyrrole, poly(p-)phenylene vinylene, aromatic tertiary amines, polynuclear aromatic tertiary amines , 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraarylbenzidine, PEDOT:PSS and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO; and / or The light-emitting device further comprises an electron transport layer between the light-emitting layer and the cathode, wherein the material of the electron transport layer comprises one or more of metal oxides, doped metal oxides, Group 2-6 semiconductor materials, Group 3-5 semiconductor materials and Group 1-3-6 semiconductor materials, wherein the metal oxides may include but are not limited to one or more of ZnO, TiO2, SnO2 and Ta2O3; the metal oxides in the doped metal oxides comprise one or more of ZnO, TiO2 and SnO2, and the doping elements comprise one or more of Al, Mg, Li, In and Ga; the Group 2-6 semiconductor materials comprise one or more of ZnS, ZnSe and CdS; the Group 3-5 semiconductor materials comprise one or more of InP and GaP; the Group 1-3-6 semiconductor materials comprise one or more of CuInS and CuGaS; and / or The light-emitting device also includes a hole injection layer located between the anode and the light-emitting layer, and the material of the hole injection layer includes one or more of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, a derivative of PEDOT:PSS doped with s-MoO3, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

14. A display device, characterized in that: The display device comprises the light emitting device according to any one of claims 12 to 13.