Special decoking agent for flue of waste incineration power plant and preparation method of special decoking agent

By using coking decoder of magnesium nitrate and copper nitrate in the flue of waste incineration power plants, combined with composite additives and modified silica microspheres, to form protective films and chemical adsorption, the problems of flue coking and corrosion are solved and high efficiency is achieved Effects of decoking and extending the life of the flue.

CN118931612APending Publication Date: 2024-11-12NINGBO CLARIANT CHEMICAL TECHNOLOGY CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202411234543.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The formation of coke blocks in the flue of waste incineration power plants caused by sudden drop in secondary air temperature during ashes flying, resulting in coking of the furnace, affecting flue gas emissions, and the existing coke decoction agent has corrosion problems, affecting the life of the flue.

Method used

A decoking agent containing magnesium nitrate and copper nitrate is used, and composite additives and modified silica microspheres are added to reduce corrosion and coking and improve decoking efficiency by forming a protective film and chemical adsorption at high temperatures.

Benefits of technology

It significantly improves the decoking efficiency, reduces flue corrosion, extends the working life of the flue, and improves the effect of decoking and ash removal.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005027337900000071
    Figure BDA0005027337900000071
  • Figure BDA0005027337900000081
    Figure BDA0005027337900000081
Patent Text Reader

Abstract

The invention provides a special decoking agent for a flue of a waste incineration power plant. The special decoking agent comprises the following raw materials in parts by weight: 10-25 parts of nitrate, 0.1-0.3 part of a bulking agent, 2.5-10 parts of a composite additive, 2-5 parts of modified silicon dioxide microspheres, 4-5 parts of a catalyst and 50-120 parts of water, wherein the nitrate is a mixture of magnesium nitrate and copper nitrate. The decoking agent special for the flue of the waste incineration power plant is high in decoking efficiency, and the corrosion phenomenon can be effectively reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of decoking agents, and in particular relates to a decoking agent special for flues of garbage incineration power plants and a preparation method thereof. Background Art

[0002] At present, waste incineration power plants operate at high temperatures for a long time and mix industrial waste and stale waste for incineration power generation. The components of domestic waste, industrial waste and stale waste are complex, and the ash melting point is low. When the fly ash encounters a sudden drop in secondary air temperature, it will quickly solidify and become coke, which will cause coking in the furnace. The flue gas and the flue heating surface will stop exchanging heat, causing the ash temperature to drop, and the fly ash will adhere to the surface of the heating surface to form coke. Coking will reduce the inner diameter of the flue and increase the resistance, resulting in the inability to discharge high-temperature flue gas normally, affecting normal production.

[0003] The invention patent with publication number CN105542902A discloses a decoking agent for a waste incinerator and a preparation method thereof. The decoking agent is composed of the following raw materials in parts by weight: 30-45 parts of sodium nitrate, 20-30 parts of sodium carbonate, 12-15 parts of colemanite, 7-12 parts of sodium chloride, 6-10 parts of corundum, and 5-8 parts of copper powder. The decoking agent can be sprinkled into the tuyere and garbage inlet of the waste incinerator at the same time, and covers all coke deposits in the furnace with wind and garbage, reacts with coke at high temperature, and makes the accumulated ash and coke fluffy and softened, which is easy to fall off and remove. Although the decoking agent can improve the decoking effect of the waste incinerator, its use in the decoking of the flue of the waste incineration power plant still needs to be further improved, and the existing decoking agent still has certain corrosion phenomena.

[0004] In view of this, the special decoking agent for flue of waste incineration power plant of the present invention is particularly important. Summary of the invention

[0005] In view of the defects of the prior art, the present invention provides a special decoking agent for flue of a waste incineration power plant and a preparation method thereof. The special decoking agent for flue of a waste incineration power plant provided by the present invention has high decoking efficiency and can effectively reduce corrosion.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0007] On one hand, the present invention provides a special decoking agent for flue of a waste incineration power plant, wherein the special decoking agent comprises the following raw materials in parts by weight: 10 to 25 parts of nitrate, 0.1 to 0.3 parts of a loosening agent, 2.5 to 10 parts of a composite additive, 2 to 5 parts of modified silica microspheres, 4 to 5 parts of a catalyst and 50 to 120 parts of water;

[0008] Wherein, the nitrate is a mixture of magnesium nitrate and copper nitrate.

[0009] Preferably, the mass ratio of the magnesium nitrate to copper nitrate is (3-4):1.

[0010] Further preferably, the mass ratio of the magnesium nitrate to copper nitrate is 3.5:1.

[0011] In some embodiments of the present invention, the preparation steps of the composite additive are as follows:

[0012] (1) Mix glyceryl monostearate and oleic acid, heat in a water bath at 60-70° C., and stir to obtain a mixed solution A;

[0013] (2) Mix zinc nitrate and an equal volume of anhydrous ethanol, add an anhydrous ethanol solution of sodium hydroxide, stir until gel state, add boron nitride, stir and mix, then add starch, heat to 50-60° C., stir and react for 1-3 hours, and obtain a mixed solution B;

[0014] (3) Adding the mixed solution B to the mixed solution A under stirring, and performing ultrasonic dispersion, shearing, filtering, drying and grinding to obtain the composite additive.

[0015] Preferably, the mass ratio of glyceryl monostearate to oleic acid is (6-10):1.

[0016] Further preferably, the mass ratio of glyceryl monostearate to oleic acid is 8:1.

[0017] In some embodiments of the present invention, the mass ratio of glyceryl monostearate in step (1) to zinc nitrate in step (2) is (2-5):1.

[0018] Preferably, the mass ratio of glyceryl monostearate in step (1) to zinc nitrate in step (2) is 3.5:1.

[0019] Preferably, in step (2), the mass ratio of zinc nitrate to sodium hydroxide is 5:(2.1-2.3).

[0020] Further preferably, in step (2), the mass ratio of zinc nitrate to sodium hydroxide is 5:2.2.

[0021] Preferably, in step (2), the concentration of the anhydrous ethanol solution of sodium hydroxide is 0.1 to 0.2 mol / L.

[0022] Further preferably, in step (2), the concentration of the anhydrous ethanol solution of sodium hydroxide is 0.15 mol / L.

[0023] Preferably, in step (2), the amount of boron nitride added is 0.2-0.6% of the mass of zinc nitrate.

[0024] Further preferably, in step (2), the amount of boron nitride added is 0.4% by mass of zinc nitrate.

[0025] In some embodiments of the present invention, in step (2), the mass ratio of starch to zinc nitrate is (10-12):1.

[0026] Preferably, in step (2), the mass ratio of starch to zinc nitrate is 11:1.

[0027] In some embodiments of the present invention, the starch is at least one of corn starch and potato starch.

[0028] Preferably, the starch is potato starch.

[0029] In the prior art, starch is often added to the decoking agent system as a combustion aid to improve the performance. The present invention prepares a composite additive. During the preparation process, inorganic zinc salt is preferably filled into the pores of potato starch colloid to obtain a composite additive of starch-modified zinc oxide. The composite additive can first be evenly dispersed in the decoking agent system. As the decoking agent produces a high-intensity "micro-explosion" at high temperature, the zinc oxide therein is released and dispersed inside the flue, forming a protective film on its low-temperature surface, which effectively reduces corrosion. On the other hand, the residual composite additive can change the thermal expansion coefficient of the deposition layer, making it easier to crack, thereby improving the favorable environment for decoking and cleaning.

[0030] In some embodiments of the present invention, the preparation steps of the modified silica microspheres are as follows:

[0031] 1) Mixing an organic solvent and water, then sequentially adding tetraethyl orthosilicate, hexadecyltrimethylammonium bromide and ammonia water, stirring for 2 to 5 hours, centrifuging, washing, drying and calcining to obtain silica microspheres;

[0032] 2) The modifier and ethanol are mixed, stirred for 20 to 30 minutes, and silica microspheres are added. The mixture is ultrasonically dispersed for 0.5 to 1 hour, magnetically stirred for 2 to 3 days, and then centrifuged, washed and dried to obtain modified silica microspheres.

[0033] In some embodiments of the present invention, the mass ratio of the modifier to the silica microspheres is (0.02-0.05):1.

[0034] Preferably, the mass ratio of the modifier to the silica microspheres is 0.03:1.

[0035] In some embodiments of the present invention, the modifier is 2-mercaptobenzothiazole.

[0036] Preferably, the mass ratio of the tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is (1-2):0.2.

[0037] Further preferably, the mass ratio of the tetraethyl orthosilicate to hexadecyltrimethylammonium bromide is 1.5:0.2.

[0038] Preferably, the concentration of the ammonia water is 25-28 wt %.

[0039] Preferably, the organic solvent is any one of methanol, ethanol and butanol.

[0040] The applicant modifies the silica microspheres, preferably coating and loading them with 2-mercaptobenzothiazole. When the decoking agent containing the modified silica microspheres is atomized and added to the flue of the waste incinerator, on the one hand, the microspheres are dispersed in the ash or coke residue, forming strong chemical adsorption with the flue matrix, and then forming a protective film, which effectively avoids corrosion; on the other hand, the adsorption effect of the modified silica microspheres on the corrosive molten salt leads to less molten salt in contact with the heated surface, which reduces corrosion, reduces high-temperature corrosion together, and extends the working life of the flue.

[0041] In some embodiments of the present invention, the catalyst is a molybdenum catalyst, and the molybdenum content is 10-20 wt%.

[0042] Preferably, the molybdenum content of the molybdenum catalyst is 15 wt%.

[0043] In some embodiments of the present invention, the loosening agent is boric acid or borax.

[0044] Preferably, the loosening agent is boric acid.

[0045] On the other hand, the present invention also provides a method for preparing a special decoking agent for flue of a waste incineration power plant, comprising the following steps: adding nitrate, a loosening agent, a composite additive, modified silica microspheres and a catalyst into water, and stirring and mixing for 10 to 30 minutes to obtain the special decoking agent.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] (1) The special decoking agent provided by the present invention has high decoking efficiency when used for decoking the flue of a waste incineration power plant by adding composite additives and modified silica microspheres, and can effectively reduce the corrosion of the flue.

[0048] (2) The composite additive of starch-modified zinc oxide obtained by filling the pores of potato starch colloid with inorganic zinc salt in the present invention can form a protective film on the low-temperature surface of the flue, effectively reducing corrosion. On the other hand, the residual composite additive can change the thermal expansion coefficient of the deposited layer, making it easier to crack, thereby improving the favorable environment for decoking and cleaning.

[0049] (3) The present invention modifies the silica microspheres and preferably coats and loads them with 2-mercaptobenzothiazole. On the one hand, the silica microspheres are dispersed in the ash or coke residue to form a strong chemical adsorption with the flue matrix, thereby forming a protective film to effectively avoid corrosion. On the other hand, the modified silica microspheres adsorb corrosive molten salts, resulting in less molten salt in contact with the heated surface, thereby alleviating corrosion, and jointly reducing high-temperature corrosion and extending the working life of the flue. DETAILED DESCRIPTION

[0050] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0051] Unless otherwise specified, the reagents used below can be easily obtained from commercial companies.

[0052] Preparation Example 1

[0053] The preparation steps of the composite additive are as follows:

[0054] (1) Mix 8 g of glyceryl monostearate and 1 g of oleic acid, heat in a water bath at 65° C., and stir to obtain a mixed solution A;

[0055] (2) 2.3 g of zinc nitrate and an equal volume of anhydrous ethanol were mixed, and then 169 mL of 0.15 mol / L sodium hydroxide in anhydrous ethanol solution was added, and the mixture was stirred until a gel state was formed. 0.01 g of boron nitride was added, and the mixture was stirred and mixed. Then 25.3 g of potato starch was added, and the mixture was heated to 55° C. and stirred for 2 h to obtain a mixed solution B.

[0056] (3) Adding the mixed solution B to the mixed solution A under stirring, and performing ultrasonic dispersion, shearing, filtering, drying and grinding to obtain a composite additive.

[0057] Preparation Example 2

[0058] The preparation steps of the composite additive are the same as those of Preparation Example 1, except that 4.2 g of zinc nitrate is added in step (2).

[0059] Preparation Example 3

[0060] The preparation steps of the composite additive are the same as those of Preparation Example 1, except that 29.9 g of potato starch is added in step (2).

[0061] Preparation Example 4

[0062] The preparation steps of modified silica microspheres are as follows:

[0063] 1) 40 mL of ethanol and 160 mL of water were mixed, and then 1.5 g of tetraethyl orthosilicate, 0.2 g of hexadecyltrimethylammonium bromide and 1 g of 27 wt % ammonia water were added in sequence, stirred for 3.5 h, centrifuged, washed with ethanol three times, vacuum dried at 60 ° C to constant weight, and calcined at 580 ° C for 4 h to obtain silica microspheres;

[0064] 2) 0.03 g of 2-mercaptobenzothiazole and 100 mL of ethanol were mixed, stirred for 25 min, 1 g of silica microspheres were added, ultrasonically dispersed for 0.7 h, magnetically stirred for 2.5 d, centrifuged, washed with ethanol three times and dried to obtain modified silica microspheres.

[0065] Preparation Example 5

[0066] The preparation steps of modified silica microspheres are the same as those of Preparation Example 4, except that 0.06 g of 2-mercaptobenzothiazole is added in step 2).

[0067] Preparation Example 6

[0068] The preparation steps of silica microspheres are as follows:

[0069] Mix 40 mL of ethanol and 160 mL of water, then add 1.5 g of tetraethyl orthosilicate, 0.2 g of hexadecyltrimethylammonium bromide and 1 g of 27 wt% ammonia water in sequence, stir for 3.5 h, centrifuge, wash with ethanol three times, vacuum dry at 60 ° C to constant weight, and calcine at 580 ° C for 4 h to obtain silica microspheres.

[0070] Unless otherwise specified, the molybdenum catalysts used in the following examples and comparative examples are all ammonium molybdate, with a molybdenum content of 15 wt%.

[0071] Example 1

[0072] A special decoking agent for flue of a waste incineration power plant, comprising the following raw materials in parts by weight: 13.6 parts of magnesium nitrate, 3.9 parts of copper nitrate, 0.2 parts of boric acid, 6.3 parts of composite additives, 3.5 parts of modified silica microspheres, 4.5 parts of molybdenum catalyst and 85 parts of water;

[0073] The composite additive used is obtained from Preparation Example 1, and the modified silica microspheres are obtained from Preparation Example 4;

[0074] The preparation method of the special decoking agent for the flue of a waste incineration power plant in this embodiment comprises the following steps: adding magnesium nitrate, copper nitrate, boric acid, a composite additive, modified silica microspheres and a molybdenum catalyst into water, and stirring and mixing for 20 minutes to obtain the special decoking agent.

[0075] Example 2

[0076] A special decoking agent for flues of waste incineration power plants, comprising the following raw materials in parts by weight: 7.3 parts of magnesium nitrate, 2.2 parts of copper nitrate, 0.1 parts of boric acid, 2.5 parts of composite additives, 2 parts of modified silica microspheres, 4 parts of molybdenum catalysts and 50 parts of water;

[0077] The composite additive used is obtained from Preparation Example 1, and the modified silica microspheres are obtained from Preparation Example 4;

[0078] The preparation method of the special decoking agent for the flue of a waste incineration power plant in this embodiment comprises the following steps: adding magnesium nitrate, copper nitrate, boric acid, a composite additive, modified silica microspheres and a molybdenum catalyst into water, and stirring and mixing for 10 minutes to obtain the special decoking agent.

[0079] Example 3

[0080] A special decoking agent for flue of a waste incineration power plant, comprising the following raw materials in parts by weight: 19.4 parts of magnesium nitrate, 5.6 parts of copper nitrate, 0.3 parts of boric acid, 10 parts of composite additives, 5 parts of modified silica microspheres, 5 parts of molybdenum catalyst and 120 parts of water;

[0081] The composite additive used is obtained from Preparation Example 1, and the modified silica microspheres are obtained from Preparation Example 4;

[0082] The preparation method of the special decoking agent for the flue of a waste incineration power plant in this embodiment comprises the following steps: adding magnesium nitrate, copper nitrate, boric acid, a composite additive, modified silica microspheres and a molybdenum catalyst into water, and stirring and mixing for 30 minutes to obtain the special decoking agent.

[0083] Example 4

[0084] A special decoking agent for flue of a waste incineration power plant and a preparation method thereof, wherein the specific implementation steps are the same as those of Example 1, except that the composite additive used is obtained from Preparation Example 2.

[0085] Example 5

[0086] A special decoking agent for flue of a waste incineration power plant and a preparation method thereof, wherein the specific implementation steps are the same as those of Example 1, except that the composite additive used is obtained from Preparation Example 3.

[0087] Example 6

[0088] A special decoking agent for flue of a waste incineration power plant and a preparation method thereof, wherein the specific implementation steps are the same as those of Example 1, except that the modified silica microspheres are obtained from Preparation Example 5.

[0089] Comparative Example 1

[0090] A decoking agent specially used for flue of a waste incineration power plant and a preparation method thereof, wherein the specific implementation steps are the same as those of Example 1, except that an equal amount of zinc oxide is added to replace the composite additive.

[0091] Comparative Example 2

[0092] A decoking agent specially used for flue of a waste incineration power plant and a preparation method thereof. The specific implementation steps are the same as those in Example 1, except that an equal amount of silica microspheres obtained in Preparation Example 6 are added to replace the modified silica microspheres.

[0093] Performance Test 1:

[0094] The following performance tests were performed on the special decoking agents prepared in the above Examples 1-6 and Comparative Examples 1-2. The specific test results are shown in Table 1:

[0095] (1) Decoking effect: 0.03 wt % of each special decoking agent prepared in Examples 1-6 and Comparative Examples 1-2 was added to the flue of the waste incineration power plant. The addition of each special decoking agent was at least 2 days apart. The 24-hour average flue gas temperature in the middle of the flue half an hour after the decoking agent was added was recorded to characterize the decoking effect. When no special decoking agent was added, the 24-hour average flue gas temperature in the middle of the flue was 717.6° C.;

[0096] (2) Coke removal rate: Coke removal rate = [(W2-W3) / (W2-W1)] × 100%, where the flue weighs W1, the flue is used normally, baked at 1200°C for 1 hour, weighed W2, left at room temperature for 2 hours, then rinsed with a sponge under running hot water, dried, weighed W3, and the coke removal rate is calculated;

[0097] (3) Corrosion performance: Visually observe whether there is corrosion in the flue after rinsing with a sponge under running hot water and drying in performance test (1).

[0098] Table 1

[0099]

[0100] As can be seen from Table 1, the special decoking agent provided by Examples 1 to 3 of the present invention has a better decoking effect, no corrosion, and excellent performance; Example 4 changes the mass ratio of zinc nitrate and glyceryl monostearate, which affects the stability of the composite additive system, and Example 5 changes the mass ratio of zinc nitrate and potato starch, which affects the dispersibility of the composite additive. Comparative Example 1 replaces the composite additive with an equal amount of zinc oxide. The above embodiments and Comparative Example 1 have different degrees of adverse effects on the decoking effect and anti-corrosion effect of the special decoking agent, and the flue gas temperature (24h average) in the middle of the flue is too high; Example 6 changes the preparation ratio of modified silica microspheres, which affects the adsorption effect of the modified silica microspheres and has a greater impact on the anti-corrosion effect of the special decoking agent; Comparative Example 2 directly adds unmodified silica microspheres, which is affected by the agglomeration effect, and the comprehensive performance of the decoking agent is poor.

[0101] Performance Test 2

[0102] A waste power plant in Guangdong: 3 600t / d mechanical grate waste incinerators, with a daily waste processing capacity of 1800t. The selected location was the middle and upper part of the second flue, and the decoking was continued for 1.5 days. Every day, 8 barrels of the special decoking agent prepared in Example 1 were added continuously (the addition rate was 20-25min / barrel, 25kg per barrel, 2 barrels on each side in the morning and afternoon), and the temperature data before and after decoking were recorded, as shown in Table 2:

[0103] Table 2 (Unless otherwise specified, the following data are all 24-hour averages)

[0104]

[0105] It should be noted that the data on day 0 are the average values ​​of the 7 consecutive days of operation before adding the decoking agent.

[0106] As shown in Table 2, after 6 months of continuous operation, the evaporation capacity of the waste heat boiler is basically 60t / h. After 1.5 days of decoking, the second and third flues have obvious decoking effects. Under the premise that the evaporation capacity is increased from 60.13t / h (7d average) before decoking to 64.03t / h (1-3d average) after decoking, the temperature in the middle of the third flue is reduced from 716.2℃ (7d average) before decoking to 699.9℃ (1-3d average) after decoking. At the same time, the steam production per ton of garbage is increased from 2.15t / t (7d average) to 2.25t / t (1-3d average). During this stage, the negative pressure difference of the flue before and after the evaporator is gradually decreasing, and the pressure difference is reduced from 25Pa (7d average) to 9Pa. At the same time, after the micro-explosion of the horizontal flue on the 3rd day, on-site observations found that the amount of ash in the scraper of the horizontal flue was significantly increased compared with the usual micro-explosion. This indicates that the special decoking agent prepared in the present invention has excellent decoking performance and significant decoking effect.

[0107] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A special decoking agent for flue of waste incineration power plant, characterized in that: The special descorching agent comprises the following raw materials in parts by weight: 10 to 25 parts of nitrate, 0.1 to 0.3 parts of loosening agent, 2.5 to 10 parts of composite additives, 2 to 5 parts of modified silica microspheres, 4 to 5 parts of catalyst and 50 to 120 parts of water; Wherein, the nitrate is a mixture of magnesium nitrate and copper nitrate.

2. The special decoking agent for flue of waste incineration power plant according to claim 1, characterized in that: The preparation steps of the composite additive are as follows: (1) Mix glyceryl monostearate and oleic acid, heat in a water bath at 60-70° C., and stir to obtain a mixed solution A; (2) Mix zinc nitrate and an equal volume of anhydrous ethanol, add an anhydrous ethanol solution of sodium hydroxide, stir until gel state, add boron nitride, stir and mix, then add starch, heat to 50-60° C., stir and react for 1-3 hours, and obtain a mixed solution B; (3) Adding the mixed solution B to the mixed solution A under stirring, and performing ultrasonic dispersion, shearing, filtering, drying and grinding to obtain the composite additive.

3. The special decoking agent for flue of waste incineration power plant according to claim 2, characterized in that: The mass ratio of glyceryl monostearate in step (1) to zinc nitrate in step (2) is (2-5):

1.

4. The special decoking agent for flue of waste incineration power plant according to claim 2, characterized in that: In step (2), the mass ratio of starch to zinc nitrate is (10-12):

1.

5. The special decoking agent for flue of waste incineration power plant according to claim 2, characterized in that: The starch is corn starch and / or potato starch.

6. The special decoking agent for flue of waste incineration power plant according to claim 1, characterized in that: The preparation steps of the modified silica microspheres are as follows: 1) Mixing an organic solvent and water, then sequentially adding tetraethyl orthosilicate, hexadecyltrimethylammonium bromide and ammonia water, stirring for 2 to 5 hours, centrifuging, washing, drying and calcining to obtain silica microspheres; 2) The modifier and ethanol are mixed, stirred for 20 to 30 minutes, and silica microspheres are added. The mixture is ultrasonically dispersed for 0.5 to 1 hour, magnetically stirred for 2 to 3 days, and then centrifuged, washed and dried to obtain modified silica microspheres.

7. The special decoking agent for flue of waste incineration power plant according to claim 6, characterized in that: The mass ratio of the modifier to the silica microspheres is (0.02-0.05):

1.

8. The special decoking agent for flue of waste incineration power plant according to claim 6, characterized in that: The modifier is 2-mercaptobenzothiazole.

9. The special decoking agent for flue of waste incineration power plant according to claim 1, characterized in that: The catalyst is a molybdenum catalyst, and the molybdenum content is 10-20wt%.

10. A method for preparing a special decoking agent for flue of a waste incineration power plant according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: adding nitrate, a loosening agent, a composite additive, modified silicon dioxide microspheres and a catalyst into water, and stirring and mixing for 10 to 30 minutes to obtain the special decoking agent.

Citation Information

Patent Citations

  • Decoking agent for garbage incinerator and preparation method thereof

    CN105542902A