Oxidized mineral source fulvic acid chrome-free tanning agent as well as preparation method and application thereof
Through the preparation and application of oxidized ore-source yellow-corrosive acid chrome-free tanning agent, the problems of single cross-linking form and single leather function are solved, and the efficient cross-linking and photothermal performance of leather are achieved, reducing processing steps and Sewage discharge promotes clean energy utilization and environmentally friendly personal thermal management.
Patent Information
- Application Number
- CN202411108354.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-12
AI Technical Summary
The existing chrome-free tanning agent and leather collagen fiber cross-linking form is single, the leather function is single, and it is difficult to replace chrome tanning agent. In addition, traditional insulation methods consume a lot of environmental and resource resources, and poor biocompatible materials limit their personal thermal management. Application in the field.
The preparation method of oxidized ore source chlorine-free tanning agent is adopted, and the oxidized ore source chlorine-free tanning agent is catalyzed by ZrOCl2 to form coordination crosslinking and multi-point hydrogen bond crosslinking to achieve the various combination methods and photothermal properties of leather. Tanning dyeing and photothermal conversion were performed simultaneously.
It improves the cross-linking strength and light-thermal conversion capacity of leather, reduces processing processes and sewage discharge, efficiently utilizes clean energy, reduces dependence on traditional energy, and meets the production requirements of green and environmentally friendly.
Smart Images

Figure CN118932122A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of environmental science and personal thermal management technology, and specifically relates to an oxidized mineral source fulvic acid chrome-free tanning agent and a preparation method and application thereof. Background Art
[0002] Chrome tanning agents are widely used in leather tanning due to their excellent cross-linking properties. 3+ There is a conversion to highly toxic Cr 6+ At present, the development of chrome-free tanning agents mainly uses biomass materials, such as cellulose, chitosan, starch, protein and other materials. However, these chrome-free tanning agents have problems such as single cross-linking form and single function with skin collagen fibers, and it is difficult to replace chrome tanning agents for the time being. Therefore, the development of chrome-free tanning agents with high cross-linking strength and rich functions has gradually become a research hotspot.
[0003] In addition, with the increase of extreme weather on the earth and the increasing shortage of petroleum energy, it is becoming increasingly important to research and develop environmentally friendly materials with enhanced thermal functions. These photothermal materials are expected to achieve optimal personal thermal management, efficiently utilize clean energy and advance the pace of carbon neutrality. At present, traditional insulation methods are mainly through burning coal and central heating with air conditioning. This not only cannot meet the needs of outdoor extreme weather activities, but also leads to greenhouse effects and consumption of limited resources. Inorganic nanomaterials such as copper sulfide compounds, gold, and molybdenum disulfide and organic nanomaterials such as polypyrrole and polyaniline have photothermal conversion efficiency and are widely used in the field of personal thermal management. However, these materials have poor biocompatibility and non-degradability, which limits their application in products and medicines that come into contact with the human body. Therefore, the development of green and ecological thermal management materials is crucial for human health and environmental sustainability. Leather is a renewable biomass resource. It is of great research value to develop leather with photothermal properties based on leather and apply it to the field of personal thermal management. However, there are few research reports in this direction.
[0004] In view of the problems of the existing chrome-free tanning agents having a single cross-linking form with skin collagen fibers and a single leather function, it is urgent to find a new chrome-free tanning agent that can produce multiple bonding modes with skin collagen fibers and give the leather photothermal properties so that it can be used in personal thermal management applications. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a preparation of an oxidized mineral source fulvic acid chrome-free tanning agent and realize the integrated tanning and dyeing and the application of leather in personal thermal management, so as to solve the technical problems that the existing chrome-free tanning agent has a relatively single cross-linking form with leather collagen fibers and a single leather function.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The invention discloses a method for preparing an oxidized mineral-source fulvic acid chrome-free tanning agent, comprising the following steps:
[0008] Dissolve the mineral fulvic acid in deionized water to obtain a mineral fulvic acid solution, then add ZrOCl2 and H2O2, stir for reaction, and freeze-dry to obtain an oxidized mineral fulvic acid chrome-free tanning agent;
[0009] In the process of leather tanning, an oxidized mineral-derived fulvic acid chrome-free tanning agent is added, and the oxidized mineral-derived fulvic acid chrome-free tanning agent forms coordination cross-linking and multi-point hydrogen bond cross-linking with the leather collagen fibers, thereby simultaneously realizing leather dyeing and photothermal conversion.
[0010] Preferably, the usage ratio of mineral fulvic acid: ZrOCl2: H2O2 is (10-30) g: (5-15) mM: (2-6) vol%.
[0011] Preferably, the mass fraction of the mineral-derived fulvic acid in the mineral-derived fulvic acid solution is 5%-15%.
[0012] Preferably, the temperature of the stirring reaction is 45-75°C.
[0013] Preferably, the stirring reaction time is 1-3 h.
[0014] Preferably, the stirring reaction speed is 100-200 rpm / min.
[0015] Preferably, the freeze-drying time is 24-72 hours.
[0016] The invention also discloses an oxidized mineral source fulvic acid chrome-free tanning agent, which is prepared by adopting the preparation method.
[0017] The invention also discloses the use of the oxidized mineral source fulvic acid chrome-free tanning agent prepared by the preparation method in tanning and dyeing and in constructing personal thermal management leather.
[0018] The invention also discloses application of the oxidized mineral source fulvic acid chrome-free tanning agent prepared by the preparation method in clean leather production.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The invention discloses a method for preparing an oxidized mineral-source fulvic acid chrome-free tanning agent, wherein the catalyst ZrOCl2 is used to assist H2O2 in oxidizing the mineral-source fulvic acid. The ZrOCl2 inorganic salt can produce Lewis acid, which enhances the oxidation effect of H2O2. The reaction system is homogeneous catalytic oxidation, which reacts in an aqueous phase, has mild reaction conditions, and is simple. The oxidized mineral-source fulvic acid prepared by the method has a smaller molecular size and more abundant oxygen-containing functional groups. At the same time, the Zr ions in the catalyst can be complexed with the oxidized mineral-source fulvic acid, and when directly applied to the tanning process, the metal ion Zr can generate coordination bonds and cross-link with the leather collagen fibers. The cumbersome process of catalyst recovery and removal is avoided. In addition, based on the dyeing performance and photothermal conversion ability of the mineral-source fulvic acid, the dyeing effect and the excellent photothermal conversion ability of the leather are simultaneously achieved. The processing procedures in the traditional leather processing and manufacturing process are reduced, and the discharge and treatment burden of acid, alkali, salt and dye wastewater are also reduced. The prepared eco-oxidized mineral-source fulvic acid chrome-free tanning agent and constructed photothermal leather are applied in the field of personal thermal management, providing new innovative designs for the clean production of leather and efficient use of clean energy.
[0021] The present invention also discloses an oxidized mineral-source fulvic acid chrome-free tanning agent prepared by the above-mentioned preparation method, and the oxidized mineral-source fulvic acid chrome-free tanning agent has the following advantages: ① excellent physical and chemical properties; the Zr ions and rich oxygen-containing functional groups complexed by the oxidized mineral-source fulvic acid can form coordination bond crosslinking and multi-point hydrogen bond crosslinking with the skin collagen fibers. Compared with the commercially available organic chrome-free tanning agent TWS, the tanned leather has a higher shrinkage temperature and tensile strength. ② reducing the dyeing process; the oxidized mineral-source fulvic acid chrome-free tanning agent contains a quinone group and a conjugated structure, and the appearance is dark black. The dyeing effect can be achieved simultaneously during the tanning process, and the leather is dark black after tanning. The tanning strategy of the invention reduces the dyeing process of the traditional leather industry, which can save manpower and working hours. Reduce the discharge and treatment burden of acid, alkali, salt and dye wastewater. Provide a cleaner and more efficient production method for leather processing and manufacturing ③ efficient use of clean energy; the present invention utilizes the photothermal properties of the oxidized mineral-source fulvic acid to simultaneously give the leather photothermal conversion ability during the tanning stage. Applying leather with photothermal properties in the field of personal thermal management makes efficient use of solar clean energy, reduces dependence on traditional limited energy such as coal and oil, and contributes to promoting carbon neutrality.
[0022] The present invention also discloses the application of the above-mentioned oxidized mineral-source fulvic acid chrome-free tanning agent in tanning and dyeing integration and the construction of personal thermal management leather. During the tanning process, the oxidized mineral-source fulvic acid chrome-free tanning agent can simultaneously achieve the dyeing effect of the leather due to the quinone group and conjugated structure it contains, so that the tanned leather presents a dark black color. The photothermal properties of the oxidized mineral-source fulvic acid are utilized to simultaneously give the leather photothermal conversion ability during the tanning stage, thereby producing leather with photothermal effect, which is suitable for the field of personal thermal management. The simultaneous tanning and dyeing are achieved, the dyeing process in the traditional leather industry is reduced, the process flow is simplified, and manpower and working hours are saved. Due to the reduction of the dyeing process, the discharge of acid, alkali, salt and dye wastewater is correspondingly reduced, and the pollution and treatment burden on the environment are reduced. The photothermal conversion ability is given to the leather, so that the leather can efficiently utilize the clean energy of solar energy, reduce the dependence on traditional limited energy, and contribute to the realization of the carbon neutrality goal. The constructed photothermal leather is applied to the field of personal thermal management, which is an innovative technology in the current field of green leather production.
[0023] The present invention also discloses the application of the above-mentioned oxidized mineral-derived fulvic acid chrome-free tanning agent in the clean production of leather. The oxidized mineral-derived fulvic acid chrome-free tanning agent is used in the clean production of leather to replace the traditional chrome-containing tanning agent and reduce the use and emission of harmful substances. The use of chrome-free tanning agent avoids the emission of harmful substances such as chromium, is more environmentally friendly, and meets the requirements of clean production. Leather made with oxidized mineral-derived fulvic acid chrome-free tanning agent has a higher shrinkage temperature and tensile strength, and improves the physical and chemical properties of the leather. The process flow is simplified, the dyeing process and the corresponding energy consumption are reduced, and the production cost is reduced. The adoption of clean production methods is conducive to the sustainable development of the leather industry, reduces the impact on the environment, and is in line with the trend of green production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 The invention discloses a preparation route of the oxidized mineral-derived fulvic acid chrome-free tanning agent;
[0025] Figure 2 The infrared spectra of the mineral-derived fulvic acid, the mineral-derived fulvic acid oxidized by H2O2, and the oxidized mineral-derived fulvic acid chrome-free tanning agent prepared by H2O2-assisted fulvic acid oxidation in Example 4 of the present invention;
[0026] Figure 3 The solid nuclear magnetic spectra of the mineral source fulvic acid, the mineral source fulvic acid oxidized by H2O2 and the oxidized mineral source fulvic acid chrome-free tanning agent prepared by ZrOCl2-assisted H2O2 oxidation of the mineral source fulvic acid in Example 4 of the present invention; wherein a is the mineral source fulvic acid; b is the mineral source fulvic acid oxidized by H2O2; c is the oxidized mineral source fulvic acid chrome-free tanning agent;
[0027] Figure 4This is a nanoparticle size distribution diagram of the mineral source fulvic acid, the mineral source fulvic acid oxidized by H2O2, and the oxidized mineral source fulvic acid chrome-free tanning agent prepared by the oxidized mineral source fulvic acid assisted by H2O2 in Example 4 of the present invention; wherein a is the mineral source fulvic acid; b is the mineral source fulvic acid oxidized by H2O2 and c is the oxidized mineral source fulvic acid chrome-free tanning agent;
[0028] Figure 5 This is a comparison chart of the shrinkage temperature of leather tanned by the mineral source fulvic acid, the mineral source fulvic acid oxidized by H2O2, and the oxidized mineral source fulvic acid chrome-free tanning agent prepared by H2O2-assisted oxidation of mineral source fulvic acid in Example 4 of the present invention, pickled sheepskin and other commercially available chrome-free tanning agents;
[0029] Figure 6 This is a comparison chart of mechanical strength of leather tanned by mineral-derived fulvic acid, H2O2-oxidized mineral-derived fulvic acid, and ZrOCl2-assisted H2O2-oxidized mineral-derived fulvic acid in Example 4 of the present invention, and pickled sheepskin and other commercially available chrome-free tanning agents; wherein a is tensile strength; b is tear strength; c is elongation at break;
[0030] Figure 7 This is a dyeing comparison diagram of leather tanned with mineral-source fulvic acid, mineral-source fulvic acid oxidized with H2O2, and oxidized mineral-source fulvic acid oxidized with ZrOCl2-assisted H2O2 and pickled sheepskin in Example 4 of the present invention;
[0031] Figure 8 The oxidized ore-source fulvic acid chrome-free tanning agent prepared by oxidizing the ore-source fulvic acid with H2O2 and ZrOCl2-assisted H2O2 to tan and pickle sheepskin under simulated sunlight of 1000w·m -2 Comparison of the light and thermal properties of tanned leather. DETAILED DESCRIPTION
[0032] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0033] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0034] The present invention is further described in detail below in conjunction with the accompanying drawings:
[0035] The invention discloses a method for preparing an oxidized mineral-source fulvic acid chrome-free tanning agent, comprising the following steps:
[0036] 1) dissolving a certain amount of mineral fulvic acid in deionized water to obtain a mineral fulvic acid solution;
[0037] 2) adding catalyst ZrOCl2 and H2O2 into the ore-derived fulvic acid solution, and using the catalyst ZrOCl2 to assist H2O2 in oxidizing the ore-derived fulvic acid;
[0038] 3) The solution of the reaction system is heated to react for a certain period of time. After the reaction is complete, the reaction solution is collected and freeze-dried to obtain an oxidized mineral-derived fulvic acid chrome-free tanning agent.
[0039] The oxidized mineral source fulvic acid chrome-free tanning agent is applied to the leather tanning process, and leather dyeing and construction of leather with light and heat properties are simultaneously achieved during the tanning process. The leather is pickled sheepskin, pickled cowhide or pickled pigskin.
[0040] Preferably, the usage ratio of mineral fulvic acid: ZrOCl2: H2O2 is (10-30) g: (5-15) mM: (2-6) vol%.
[0041] Preferably, in step 1), the mass fraction of the mineral-source fulvic acid in the mineral-source fulvic acid solution is 5%-15%.
[0042] Preferably, in step 2), the amount of catalyst ZrOCl2 used is 5-15mM.
[0043] Preferably, in step 2), the amount of H2O2 used is 2 vol%-6 vol%.
[0044] Preferably, in step 3), the stirring reaction temperature is 45-75° C., the time is 1-3 h, and the rotation speed is 100-200 rpm / min.
[0045] Preferably, in step 3), the drying process adopts freeze drying method, and the drying time is 24-72 hours.
[0046] Preferably, the molar concentration of the catalyst ZrOCl2 is 10 mM; the volume fraction of H2O2 is 4 vol%; the stirring reaction temperature is 60°C, the time is 2 h, and the rotation speed is 175 rpm / min.
[0047] The invention also discloses an oxidized mineral source fulvic acid chrome-free tanning agent prepared by the method.
[0048] The present invention also discloses the application of the above-mentioned oxidized mineral source fulvic acid chrome-free tanning agent in the clean production of leather, which simultaneously achieves the dyeing effect and gives the leather photothermal conversion performance. The prepared tanning agent is an ecological organic tanning agent, which is more environmentally friendly than traditional tanning agents. At the same time, the dyeing effect of the tanning agent avoids the dyeing section in leather processing, reduces the use of processes and dyes, and conforms to the concept of clean production. Photothermal conversion utilizes solar energy, which is a clean energy source. The entire application and the final function of the leather conform to the concepts of cleanliness, greenness and environmental protection.
[0049] Example 1
[0050] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0051] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 45°C for heating; then add 5mM of catalyst ZrOCl2 and 2vol% of H2O2; react for 1h under mechanical stirring at a speed of 100rpm / min; after the reaction, take out the solution and freeze-dry it for 24h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0052] Example 2
[0053] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0054] Take 30g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 15%; place the three-necked flask in an oil pan at 75°C for heating; then add 15mM of catalyst ZrOCl2 and 6vol% of H2O2; react for 3h under mechanical stirring at a speed of 200rpm / min; after the reaction, take out the solution and freeze-dry it for 72h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0055] Example 3
[0056] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0057] Take 20g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 10%; place the three-necked flask in an oil pan at 60°C for heating; then add 10mM of catalyst ZrOCl2 and 4vol% H2O2; react for 1h under mechanical stirring at a speed of 150rpm / min; after the reaction, take out the solution and freeze-dry it for 48h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0058] Example 4
[0059] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0060] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 60°C for heating; then add 10mM of catalyst ZrOCl2 and 4vol% of H2O2; react for 2h under mechanical stirring at a speed of 175rpm / min; after the reaction, take out the solution and freeze-dry it for 48h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0061] A method for preparing H2O2-oxidized ore-derived fulvic acid (OMFA-0), comprising:
[0062] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a 5% mass fraction of mineral humic acid solution; place the three-necked flask in an oil pan at 60°C for heating; then add 4vol% H2O2; react for 2h under mechanical stirring at a speed of 175rpm / min; after the reaction, take out the solution and freeze-dry it for 48h to obtain OMFA-0.
[0063] See also Figure 1 The present invention discloses a preparation route of an oxidized mineral-source fulvic acid chrome-free tanning agent; as can be seen from the figure, the preparation of an oxidized mineral-source fulvic acid chrome-free tanning agent includes the following steps: first dissolving mineral-source fulvic acid in deionized water; then adding catalyst ZrOCl2 and H2O2 to the mineral-source fulvic acid solution, and using catalyst ZrOCl2 to assist H2O2 in oxidizing the mineral-source fulvic acid; heating the solution of the reaction system for a certain period of time, and after the reaction is complete, collecting and freeze-drying the reaction solution to obtain oxidized mineral-source fulvic acid. The oxidized mineral-source fulvic acid is applied to the tanning process of sheep acid hides, and leather dyeing and construction of leather with photothermal properties can be achieved simultaneously during the tanning process.
[0064] See also Figure 2 The infrared spectra of the mineral fulvic acid (MFA), the mineral fulvic acid oxidized with H2O2 (OMFA-0) and the oxidized mineral fulvic acid chrome-free tanning agent (OMFA) prepared by the oxidized mineral fulvic acid with the assistance of ZrOCl2 in Example 4 of the present invention are shown in FIG. 1 . As can be seen from the figure, at 3000-3700 cm -1 The broad characteristic peak at 1707cm is attributed to the -OH in the carboxyl group or phenolic hydroxyl group. -1 The stretching vibration peak at 1412cm belongs to the C=O in the carboxyl group, aldehyde group or carbonyl group. -1 The symmetric stretching vibration peak at -COO - OMFA is located in the hydrogen bonding region and 1705 cm -1 There is a broader and stronger absorption peak at the oxidized OMFA, which indicates that the oxidized OMFA contains more oxygen-containing functional groups such as carboxyl and phenolic hydroxyl.
[0065] See also Figure 3 The solid nuclear magnetic spectrum of the oxidized mineral fulvic acid chrome-free tanning agent prepared by mineral fulvic acid, H2O2 oxidation of mineral fulvic acid and ZrOCl2-assisted H2O2 oxidation of mineral fulvic acid in Example 4 of the present invention; wherein, a is mineral fulvic acid (MFA); b is H2O2 oxidation of mineral fulvic acid (OMFA-0); c is oxidized mineral fulvic acid chrome-free tanning agent (OMFA); it can be seen that the aromatic carbon peak intensity (100-150ppm) of OMFA-0 and OMFA is significantly weaker than that of MFA. The relative contents of aromatic carbon in MFA, OMFA-0 and OMFA are 41.28%, 31.47% and 26.8%, respectively. It shows that the H2O2-ZrOCl2 catalytic oxidation system has a stronger oxidizing ability than H2O2, which promotes the opening of the benzene ring. The oxygen-bonded aromatic carbon corresponds to the phenolic hydroxyl group (151.91-156.14ppm). Compared with MFA (1.85%) and OMFA-0 (3.50%), OMFA has the highest phenolic hydroxyl content of 4.02%. At the same time, the relative content of carboxyl in OMFA is 12.32%, which is much higher than that of MFA. In addition, the carbonyl content of OMFA also increases. Therefore, ZrOCl2-assisted H2O2 oxidation can promote the depolymerization of molecules and increase the content of carboxyl, phenolic hydroxyl and carbonyl.
[0066] See also Figure 4The nanoparticle size distribution diagram of the oxidized mineral fulvic acid chrome-free tanning agent prepared by mineral fulvic acid, H2O2 oxidized mineral fulvic acid and ZrOCl2 assisted H2O2 oxidized mineral fulvic acid in Example 4 of the present invention; wherein a is mineral fulvic acid (MFA); b is H2O2 oxidized mineral fulvic acid (OMFA-0); c is oxidized mineral fulvic acid chrome-free tanning agent (OMFA); it can be seen from the figure that the average particle size of MFA is 796nm. The average particle sizes of OMFA-0 and OMFA are 180nm and 157nm respectively (see Figure 4 (b) and (c)). This indicates that the H2O2-ZrOCl2 system has better depolymerization performance. The smaller molecular size allows the tanning agent to penetrate more fully and evenly.
[0067] See also Figure 5 This is a comparison chart of the shrinkage temperatures of leather tanned by the mineral source fulvic acid, the oxidized mineral source fulvic acid prepared by H2O2 oxidation of mineral source fulvic acid, and the oxidized mineral source fulvic acid chrome-free tanning agent prepared by H2O2-assisted oxidation of mineral source fulvic acid in Example 4 of the present invention, and pickled sheepskin and other commercially available chrome-free tanning agents; as can be seen from the figure, the crust leather tanned by OMFA has the highest shrinkage temperature, indicating that the chrome-free tanning agent prepared by H2O2 oxidation of mineral source fulvic acid with the assistance of ZrOCl2 has the best tanning effect.
[0068] See also Figure 6 This is a comparison chart of the mechanical strength of leather tanned with mineral fulvic acid, H2O2-oxidized mineral fulvic acid, and ZrOCl2-assisted H2O2-oxidized mineral fulvic acid in Example 4 of the present invention, among which a is tensile strength; b is tear strength; c is elongation at break; it can be seen from the figure that the tensile strength of the crust leather tanned with OMFA is the best, and the tear strength and elongation at break are slightly lower than those of the commercially available organic chrome-free tanning agent TWS.
[0069] See also Figure 7 This is a dyeing comparison diagram of leather tanned with mineral fulvic acid, mineral fulvic acid oxidized with H2O2, and chrome-free tanning agent prepared by oxidizing mineral fulvic acid with the aid of H2O2 and ZrOCl2 in Example 4 of the present invention, and pickled sheepskin; as can be seen from the figure, mineral fulvic acid oxidized with H2O2 (OMFA-0) and chrome-free tanning agent (OMFA) prepared by oxidizing mineral fulvic acid with the aid of H2O2 and ZrOCl2 have smaller molecular sizes and penetrate more evenly, and the tanned leather presents a uniform dark black color.
[0070] See also Figure 8 The oxidized ore-source fulvic acid chrome-free tanning agent prepared by oxidizing the ore-source fulvic acid with H2O2 and ZrOCl2-assisted H2O2 to tan and pickle sheepskin under simulated sunlight of 1000w·m -2The following is a comparison of the photothermal properties of tanned leather; it can be seen from the figure that compared with the acid-soaked sheepskin (PS), the surface temperature of the tanned leather reached about 50°C under simulated sunlight for 300s, and the temperature increased by nearly 20°C.
[0071] Example 5
[0072] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0073] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 45°C for heating; then add 10mM of catalyst ZrOCl2 and 4vol% of H2O2; react for 2h under mechanical stirring at a speed of 200rpm / min; after the reaction, take out the solution and freeze-dry it for 24h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0074] Example 6
[0075] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0076] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 45°C for heating; then add 10mM of catalyst ZrOCl2 and 6vol% H2O2; react for 2h under mechanical stirring at a speed of 150rpm / min; after the reaction, take out the solution and freeze-dry it for 48h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0077] Example 7
[0078] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0079] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 45°C for heating; then add 15mM of catalyst ZrOCl2 and 2vol% of H2O2; react for 1h under mechanical stirring at a speed of 125rpm / min; after the reaction, take out the solution and freeze-dry it for 36h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0080] Example 8
[0081] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0082] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 60°C for heating; then add 15mM of catalyst ZrOCl2 and 4vol% of H2O2; react for 2h under mechanical stirring at a speed of 100rpm / min; after the reaction, take out the solution and freeze-dry it for 72h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0083] Example 9
[0084] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0085] Take 10g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 5%; place the three-necked flask in an oil pan at 75°C for heating; then add 15mM of catalyst ZrOCl2 and 6vol% H2O2; react for 3h under mechanical stirring at a speed of 200rpm / min; after the reaction, take out the solution and freeze-dry it for 24h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0086] Example 10
[0087] A method for preparing an oxidized mineral-derived fulvic acid chrome-free tanning agent comprises the following steps:
[0088] Take 15g of mineral humic acid and add it into a three-necked flask, then add 200mL of deionized water to fully dissolve the mineral humic acid to obtain a mineral humic acid solution with a mass fraction of 7.5%; place the three-necked flask in an oil pan at 65°C for heating; then add 12mM of catalyst ZrOCl2 and 3vol% of H2O2; react for 1.5h under mechanical stirring at a speed of 160rpm / min; after the reaction, take out the solution and freeze-dry it for 60h to obtain an oxidized mineral humic acid chrome-free tanning agent.
[0089] The present invention first deoxidizes mineral-derived fulvic acid through a ZrOCl2-H2O2 catalytic oxidation system, and the prepared oxidized mineral-derived fulvic acid has a smaller molecular size and richer oxygen-containing functional groups. At the same time, the Zr ions in the catalyst ZrOCl2 exist in the form of complexation with the oxidized mineral-derived fulvic acid. Then, the prepared oxidized mineral-derived fulvic acid is applied to the leather tanning process. The oxidized mineral-derived fulvic acid can form coordination crosslinking and multi-point hydrogen bond crosslinking with leather collagen fibers. Finally, based on the dyeing and photothermal properties of the oxidized mineral-derived fulvic acid, the tanning and dyeing are integrated and the application of leather in personal thermal management is realized. The present invention utilizes the properties of mineral-derived fulvic acid to realize the construction of tanning and dyeing integrated and leather with photothermal properties, providing a new approach for the innovative design of ecological leather manufacturing and efficient use of clean energy. In summary, the oxidized mineral-derived fulvic acid chrome-free tanning agent prepared by the method of the present invention has good tanning effect, dyeing effect and photothermal conversion ability, and the raw materials and products are environmentally friendly, the preparation method is simple and easy to implement, and is suitable for large-scale production.
[0090] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing an oxidized ore-derived fulvic acid chrome-free tanning agent, characterized in that: The following steps are involved: Dissolve the mineral fulvic acid in deionized water to obtain a mineral fulvic acid solution, then add ZrOCl2 and H2O2, stir for reaction, and freeze-dry to obtain an oxidized mineral fulvic acid chrome-free tanning agent; In the process of leather tanning, an oxidized mineral-derived fulvic acid chrome-free tanning agent is added, and the oxidized mineral-derived fulvic acid chrome-free tanning agent forms coordination cross-linking and multi-point hydrogen bond cross-linking with the leather collagen fibers, thereby simultaneously realizing leather dyeing and photothermal conversion.
2. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: The usage ratio of the mineral source fulvic acid: ZrOCl2: H2O2 is (10-30) g: (5-15) mM: (2-6) vol%.
3. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: In the mineral source fulvic acid solution, the mass fraction of the mineral source fulvic acid is 5%-15%.
4. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: The temperature of the stirring reaction is 45-75°C.
5. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: The stirring reaction time is 1-3h.
6. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: The rotation speed of the stirring reaction is 100-200 rpm / min.
7. The method for preparing the oxidized ore-derived fulvic acid chrome-free tanning agent according to claim 1, characterized in that: The freeze-drying time is 24-72h.
8. An oxidized mineral-derived fulvic acid chrome-free tanning agent, characterized in that: The method is prepared by any one of claims 1 to 7.
9. Application of the oxidized mineral-derived fulvic acid chrome-free tanning agent obtained by the preparation method described in any one of claims 1 to 7 in integrated tanning and dyeing and in the construction of personal thermal management leather.
10. Use of the oxidized mineral-derived fulvic acid chrome-free tanning agent obtained by the preparation method according to any one of claims 1 to 7 in clean leather production.
Citation Information
Patent Citations
Epoxy modified collagen polypeptide based organic chrome-free tanning agent as well as preparation method and application thereof