Process for improving cleanliness of molten steel for 20CrMnTi

By adopting carbon pre-deoxygenation and carbon-containing ferrochromium deoxygenation alloying during the smelting process of 20CrMnTi gear steel, combined with refining slag modification and micro-calcium treatment, the water nodules and steel matrix scratches caused by Al2O3 inclusions were solved, and the problem of water outlet nodules and steel matrix scratches was achieved. The production of liquid steel with high cleanliness has reduced costs and improved metallurgical effects.

CN118932140AActive Publication Date: 2024-11-12UNIV OF SCI & TECH BEIJING +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410994296.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12
Estimated Expiration
2044-07-24

AI Technical Summary

Technical Problem

In the prior art, the Al2O3 inclusions produced by the aluminum particle deoxidant used in the smelting process of 20CrMnTi gear steel has a high melting point and is not prone to deformation, resulting in water nodules, scratches of the steel matrix and reduced fatigue performance, affecting the smooth progress of production.

Method used

Carbon pre-deoxygenation and carbon-containing ferrochromium deoxygenation alloying during the steel discharge process of converter, combined with the refining slag modification during LF refining, the oxidized chromium element is reduced and re-entered into the liquid steel, replacing the traditional Al deoxygenation process and reducing Al2O3 inclusions The production and optimization of the liquid molten steel composition through micro-calcium treatment and soft blowing operation.

Benefits of technology

It significantly reduces the amount of Al2O3 inclusions and the amount of calcium wire, improves the cleanliness and metallurgical effect of the steel, reduces production costs, extends the life of the water outlet and improves the performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932140A_ABST
    Figure CN118932140A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of ferrous metallurgy, and particularly relates to a molten steel cleanliness improving process for 20CrMnTi. During converter tapping, carbon pre-deoxidation and carbon-containing ferrochrome deoxidation alloying are adopted, refining slag modification is conducted in an LF furnace, and the oxidized chromium element is reduced and enters molten steel again. Compared with a traditional Al deoxidation process, the process has the advantages that the Al consumption can be greatly reduced, so that the generation amount of aluminum oxide type inclusions is reduced, the calcium line feeding amount can be further reduced, and a good metallurgical effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of iron and steel metallurgy, and in particular relates to a process for improving the cleanliness of molten steel of 20CrMnTi. Background Art

[0002] 20CrMnTi gear steel is a carburizing steel with good performance, high hardenability, high strength and toughness, especially high low-temperature impact toughness, good processability, small deformation, good fatigue resistance, and good machinability after normalizing. It is used to manufacture important parts that bear high speed, medium or heavy loads, impact and friction, such as gears, gear rings, gear shaft crosses, etc. At present, the main deoxidizer used in the smelting of gear steel at home and abroad is aluminum particles. The deoxidation product Al2O3 inclusions produced by it have a high melting point and low deformation ability. They belong to the high melting point and non-deformable inclusions. They are easy to gather at the nozzle during the casting process of the tundish, causing nozzle nodules to block, reducing the nozzle life and even affecting the smooth progress of production. In addition, in the subsequent rolling, due to the characteristics of Al2O3 inclusions that are not easy to deform, it will cause scratches on the steel matrix, and the stress is easy to concentrate around the inclusions, thereby forming gaps or cracks, causing the material to be damaged and broken during use, and the fatigue performance is reduced. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to propose a process for improving the cleanliness of molten steel for 20CrMnTi.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A process for improving the cleanliness of molten steel for 20CrMnTi, wherein carbon pre-deoxidation and carbon-containing chromium-iron deoxidation and alloying are performed during the converter steelmaking process, and refined slag is modified during LF refining so that the oxidized chromium element is reduced and re-enters the molten steel.

[0006] As a preferred solution of a process for improving the cleanliness of molten steel for 20CrMnTi according to the present invention, the smelting process comprises the following steps:

[0007] S1. Oxygen determination after converter smelting;

[0008] S2. Steel tapping from converter;

[0009] S3. Carbon pre-deoxidation;

[0010] S4. Deoxidation and primary alloying of carbon-containing ferrochromium;

[0011] S5. Refining slag modification;

[0012] S6.LF secondary alloying;

[0013] S7. Microcalcium treatment;

[0014] S8. Soft blowing.

[0015] As a preferred solution of a process for improving the cleanliness of molten steel of 20CrMnTi described in the present invention, wherein: in the step S1, an oxygen meter is used to determine the oxygen before the converter is tapped.

[0016] As a preferred solution of a process for improving the cleanliness of molten steel of 20CrMnTi described in the present invention, wherein: in the step S2, the tapping temperature is 1610-1650°C, and the tapping time is 3-4 minutes.

[0017] As a preferred solution of the process for improving the cleanliness of molten steel for 20CrMnTi described in the present invention, wherein: in the step S3, during the steel tapping process, carbon powder is added to pre-deoxidize the molten steel, and carbon reacts with free oxygen in the molten steel to generate CO, which then leaves the molten steel system, and the deoxidation product will not pollute the molten steel. The amount of carbon powder added is 0.70-0.95 kg / t 钢 , start adding when the steel output reaches 1 / 4.

[0018] As a preferred solution of a process for improving the cleanliness of molten steel of 20CrMnTi described in the present invention, wherein: in the step S4, when the steel output reaches 1 / 2, carbon-containing ferrochrome is added for deoxidation and alloying; when the carbon-containing ferrochrome is low-carbon ferrochrome, the amount of low-carbon ferrochrome added is 17.5-18.8 kg / t 钢 ; When the carbon-containing ferrochrome is high-carbon ferrochrome and low-carbon ferrochrome, the amount of low-carbon ferrochrome added is 10-12kg / t 钢 , the amount of high carbon ferrochrome added is 4-5kg / t 钢 , and also need to add carbon powder 0.3 ~ 0.5kg / t 钢 .

[0019] As a preferred solution of a process for improving the cleanliness of molten steel of 20CrMnTi described in the present invention, wherein: in the step S4, after deoxidation and alloying, a slag-making agent is added through a silo, and the slag-making agent is selected from synthetic refined slag + lime; the amount of refined synthetic slag added is 5-6 kg / t 钢 , the amount of lime added is 2~3kg / t 钢 ; The synthetic refined slag includes: CaO: 40-50wt%, Al2O3: 30-45wt%; CaO in lime ≥ 95wt%; the basicity of the final refined slag at the end of LF smelting is 5-7, CaO: 50-60wt%, SiO2: 9-13wt%, Al2O3: 25-35wt%, MgO: 3-5wt%, ∑(FeO+MnO)≤1wt%.

[0020] As a preferred solution of a process for improving the cleanliness of molten steel for 20CrMnTi described in the present invention, wherein: in the step S5, after the ladle enters the LF refining process, a modifier is added to the ladle to reduce the oxidizability of the refined slag to produce reducing white slag, and the slag-making modifier is selected from calcium carbide + silicon carbide + aluminum particles; wherein the amount of calcium carbide added is 0.95-1.2 kg / t 钢 , the amount of silicon carbide added is 0.6~0.85kg / t 钢 , the amount of calcium carbide + silicon carbide added ≥ 1.8kg / t 钢 ; At the same time, spread 0.23~0.35kg / t on the slag surface 钢 Aluminum particles are used to assist in rapid deoxidation and aluminum alloying.

[0021] As a preferred solution of a process for improving the cleanliness of molten steel of 20CrMnTi described in the present invention, wherein: in the step S6, after the ladle enters the LF refining process and the slag is modified, silicon manganese and ferrotitanium are added through the feeding bin for secondary alloying.

[0022] As a preferred solution of a process for improving the cleanliness of molten steel for 20CrMnTi described in the present invention, wherein: in the step S7, after alloying, the composition has met the target requirements; considering that the high basicity and high aluminum refined slag system is still used, in order to ensure the castability of the molten steel, the molten steel is subjected to micro-calcium treatment, and the calcium wire feeding amount is 0.35-0.60 m / t 钢 .

[0023] As a preferred solution of a process for improving the cleanliness of molten steel for 20CrMnTi described in the present invention, wherein: in the step S8, after feeding the calcium line, the ladle is subjected to a soft blowing operation for at least 10 minutes before being hoisted to the continuous casting.

[0024] The beneficial effects of the present invention are as follows:

[0025] The invention proposes a process for improving the cleanliness of molten steel for 20CrMnTi. The method adopts the method of carbon pre-deoxidation during steel tapping from a converter and deoxidation and alloying of carbon-containing ferrochrome to replace the traditional Al deoxidation process, thereby reducing the consumption of Al and the amount of inclusions generated. Part of the chromium element in the carbon-containing ferrochrome is oxidized during steel tapping, and the oxidized chromium is reduced and enters the molten steel after entering the LF to make reducing slag. The method can realize the production of high-cleanliness 20CrMnTi gear steel and can reduce the amount of calcium treatment added, thereby saving costs on the one hand and improving the metallurgical effect on the other. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0027] Figure 1 The figure is a schematic flow chart of the process for improving the cleanliness of molten steel of 20CrMnTi according to the present invention.

[0028] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0029] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] The present invention provides a process for improving the cleanliness of molten steel for 20CrMnTi (such as Figure 1 As shown in the figure, the method of carbon pre-deoxidation of converter steel + carbon-containing chromium iron deoxidation and alloying is adopted to replace the Al deoxidation process, which can not only reduce the consumption of deoxidation alloy, but also reduce the amount of calcium wire feed and the generation of inclusions, and has a good metallurgical effect.

[0031] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0032] Example 1

[0033] This embodiment is a process for improving the cleanliness of molten steel for 20CrMnTi, using a 100t top and bottom combined blowing converter for smelting, and includes the following steps:

[0034] S1. Oxygen determination after converter smelting, oxygen value 484ppm;

[0035] S2. After the oxygen fixation is completed, the converter starts to rotate and start to tap steel;

[0036] S3. Carbon pre-deoxidation, add 65kg carbon powder when the steel output is 1 / 4;

[0037] S4. Carbon-containing ferrochrome deoxidation alloying, when the steel output is 1 / 2, 1795kg of low-carbon ferrochrome deoxidation alloying is added, and then 520kg of synthetic refined slag (CaO: 45wt%, Al2O3: 39wt%) is added through the silo, and 240kg of lime is added;

[0038] S5. Refining slag modification, the ladle enters the LF station and starts smelting after power is turned on, 105kg of calcium carbide and 75kg of silicon carbide are added to the slag surface, and 26kg of aluminum particles are spread on the slag surface;

[0039] S6.LF secondary alloying, after the slag modification, 890kg silicon manganese and 86kg titanium iron were added for secondary alloying;

[0040] S7. Calcium treatment: After the alloy composition meets the requirements, in order to ensure the smooth casting of molten steel, feed the calcium line 45m;

[0041] S8. Soft blowing. After wire feeding, the ladle is transferred to the soft blowing area for soft blowing. The soft blowing time is 12 minutes. Through on-site sampling, after the soft blowing, the inclusions in the molten steel are shown in Table 1:

[0042] Table 1 Inclusions in molten steel after soft blowing

[0043] type Al-O CaO Ca-Al-O CaS-containing <![CDATA[Quantity (pcs / (50mm 2 ))]]> 28 6 25 165 Average size (μm) 3.78 3.66 4.02 3.52

[0044] Example 2

[0045] This embodiment is a process for improving the cleanliness of molten steel for 20CrMnTi, using a 100t top and bottom combined blowing converter for smelting, and includes the following steps:

[0046] S1. Oxygen determination after converter smelting, the oxygen value is 520ppm;

[0047] S2. After the oxygen fixation is completed, the converter starts to rotate and start to tap steel;

[0048] S3. Carbon pre-deoxidation, add 75kg carbon powder when the steel output reaches 1 / 4;

[0049] S4. Carbon-containing ferrochrome deoxidation alloying, when the steel output is 1 / 2, 1820kg low-carbon ferrochrome deoxidation alloying is added; then 545kg synthetic refined slag (CaO: 45wt%, Al2O3: 39wt%) is added through the silo, and 250kg of lime is added;

[0050] S5. Refining slag modification, the ladle enters the LF station and is powered on to start smelting, 110kg of calcium carbide and 75kg of silicon carbide are added to the slag surface, and 25kg of aluminum particles are spread on the slag surface;

[0051] S6.LF secondary alloying, after the slag modification, 880kg silicon manganese and 80kg titanium iron are added for secondary alloying;

[0052] S7. Calcium treatment: After the alloy composition meets the requirements, in order to ensure the smooth casting of molten steel, feed 50m of calcium wire;

[0053] S8. Soft blowing. After feeding the wire, the ladle is transferred to the soft blowing area for soft blowing. The soft blowing time is 13 minutes. Through on-site sampling, after the soft blowing, the inclusions in the molten steel are shown in Table 1:

[0054] Table 2 Inclusions in molten steel after soft blowing

[0055] type Al-O CaO Ca-Al-O CaS-containing <![CDATA[Quantity (pcs / (50mm 2 ))]]> 35 6 28 174 Average size (μm) 3.74 3.76 4.04 3.48

[0056] Comparative Example 1

[0057] A 20CrMnTi gear steel smelting process, using a 100t top and bottom combined blowing converter for smelting, comprises the following steps:

[0058] S1. Oxygen determination, oxygen value 498ppm;

[0059] S2. Steel tapping: After oxygen fixation is completed, the converter rotates and steel tapping begins.

[0060] S3. Deoxidation and alloying: when the output of steel reaches 1 / 3, add 100 kg of aluminum blocks and add 1373 kg of low-carbon ferrochrome and 889 kg of silicon manganese in sequence through the alloy silo.

[0061] S4. Slag making, after adding the deoxidizer, 395kg lime and 310kg synthetic refined slag (CaO: 45wt%, Al2O3: 40wt%) are added through the silo. After the steel is tapped, the ladle car leaves the tapping position and enters the LF station;

[0062] S5. Slag modification: After the ladle enters the LF station, it is powered on and smelting begins. 95kg of calcium carbide and 60kg of silicon carbide are added to the slag surface.

[0063] S6. Fine-tuning the alloy: after the modification of the refined slag is completed, 100 kg of low-carbon ferrochrome, 78 kg of silicon manganese and 80 kg of ferrotitanium are added to the molten steel through the alloy silo to adjust the composition of the molten steel to the target range of the process card;

[0064] S7. Feed wire. After alloying, in order to ensure the smooth casting of molten steel, feed 110m of calcium wire;

[0065] S8. Soft blowing. After feeding the wire, the ladle is transferred to the soft blowing area for soft blowing. The soft blowing time is 10 minutes. Through on-site sampling, after the soft blowing, the inclusions in the molten steel are shown in Table 3:

[0066] Table 3 Inclusions in molten steel after soft blowing

[0067] type Al-O CaO Ca-Al-O CaS-containing <![CDATA[Quantity (pcs / (50mm 2 ))]]> 70 38 87 367 Average size (μm) 4.05 4.07 3.96 4.74

[0068] Comparative Example 2

[0069] A 20CrMnTi gear steel smelting process, using a 100t top and bottom combined blowing converter for smelting, comprises the following steps:

[0070] S1. Oxygen determination, oxygen value 533ppm;

[0071] S2. Steel tapping: after oxygen fixation, the converter rotates and steel tapping begins;

[0072] S3 deoxidation alloying, the amount of steel reached 1 / 3 when adding aluminum block 100kg and through the alloy silo sequentially added low carbon ferrochrome 1388kg, silicon manganese 878kg;

[0073] S4. Slag making, after adding deoxidizer, add 400kg lime and 315kg synthetic refined slag (CaO: 44wt%, Al2O3: 37wt%) through the silo. After the steel is tapped, the chartered car just leaves the tapping position and enters the LF station;

[0074] S5. Slag modification: After the ladle enters the LF station, it is powered on and smelting begins. 90kg of calcium carbide and 65kg of silicon carbide are added to the slag surface.

[0075] S6. Fine-tuning the alloy: after finishing the modification of the refined slag, add 105kg of low-carbon ferrochrome, 85kg of silicon manganese and 80kg of ferrotitanium to the molten steel through the alloy silo to adjust the composition of the molten steel to the target range of the process card;

[0076] S7. Feed wire. After alloying, in order to ensure the smooth casting of molten steel, feed 110m of calcium wire;

[0077] S8. Soft blowing. After wire feeding, the ladle is transferred to the soft blowing area for soft blowing. The soft blowing time is 10 minutes. Through on-site sampling, after the soft blowing, the inclusions in the molten steel are shown in Table 4:

[0078] Table 4 Inclusions in molten steel after soft blowing

[0079] type Al-O CaO Ca-Al-O CaS-containing <![CDATA[Quantity (pcs / (50mm 2 ))]]> 71 35 86 603 Average size (μm) 4.08 4.06 3.98 4.86

[0080] It can be seen from the above embodiments and comparative examples that at the end of 20CrMnTi converter smelting, the oxygen content in the molten steel is still about 500ppm. The traditional Al deoxidation process is adopted. When the traditional Al deoxidation process is adopted, aluminum blocks are added to the molten steel for deoxidation (Comparative Examples 1-2). Aluminum and oxygen combine to form a large amount of Al2O3 inclusions. Although the refined slag can adsorb and remove most of the aluminum oxide inclusions, some of them will still remain in the molten steel, affecting the castability of the molten steel. At present, calcium treatment is usually used to deform and treat Al2O3 inclusions, but excessive calcium treatment will affect the cleanliness of the molten steel. Excessive calcium combines with sulfur in the molten steel to generate too many CaS inclusions, especially for 20CrMnTi gear steel, which is difficult to control. The present invention adopts the method of carbon pre-deoxidation + carbon-containing chromium iron deoxidation alloying in converter steel tapping, replacing the traditional Al deoxidation process, which can significantly reduce the number of Al2O3 inclusions and also greatly reduce the amount of calcium wire used for modifying Al2O3 inclusions. The present invention can realize the production of high-cleanliness 20CrMnTi gear steel on the one hand, and reduces the consumption of aluminum blocks and calcium wires on the other hand, thereby reducing the cost of production and helping enterprises to improve their benefits.

[0081] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A process for improving the cleanliness of molten steel for 20CrMnTi, characterized in that: Carbon pre-deoxidation + carbon-containing ferrochromium deoxidation and alloying are carried out during the converter steelmaking process, and the refining slag is modified during LF refining so that the oxidized chromium element is reduced and re-enters the molten steel.

2. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 1, characterized in that: The smelting process comprises the following steps: S1. Oxygen determination after converter smelting; S2. Steel tapping from converter; S3. Carbon pre-deoxidation; S4. Deoxidation and primary alloying of carbon-containing ferrochromium; S5. Refining slag modification; S6.LF secondary alloying; S7. Microcalcium treatment; S8. Soft blowing.

3. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In step S2, the tapping temperature is 1610-1650° C., and the tapping time is 3-4 minutes.

4. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In step S3, during the steel tapping process, carbon powder is added to pre-deoxidize the molten steel, and the amount of carbon powder added is 0.70-0.95 kg / t 钢 , start adding when the steel output reaches 1 / 4.

5. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In the step S4, when the steel output reaches 1 / 2, carbon-containing ferrochrome is added for deoxidation and alloying; when the carbon-containing ferrochrome is low-carbon ferrochrome, the amount of low-carbon ferrochrome added is 17.5-18.8 kg / t 钢 ; When the carbon-containing ferrochrome is high-carbon ferrochrome and low-carbon ferrochrome, the amount of low-carbon ferrochrome added is 10-12kg / t 钢 , the amount of high carbon ferrochrome added is 4-5kg / t 钢 , and also need to add carbon powder 0.3 ~ 0.5kg / t 钢 .

6. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In the step S4, after deoxidation and alloying, a slag-making agent is added through the silo, and the slag-making agent is selected from synthetic refined slag + lime, and the amount of refined synthetic slag added is 5-6 kg / t 钢 , the amount of lime added is 2~3kg / t 钢 .

7. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In step S5, after the ladle enters the LF refining process, a modifier is added to the ladle to reduce the oxidizability of the refined slag to produce reducing white slag, and the modifier is selected from calcium carbide + silicon carbide + aluminum particles; wherein the amount of calcium carbide added is 0.95-1.2 kg / t 钢 , the amount of silicon carbide added is 0.6~0.85kg / t 钢 , calcium carbide + silicon carbide addition amount ≥ 1.8kg / t 钢 ; At the same time, spread 0.23~0.35kg / t on the slag surface 钢 of aluminum particles.

8. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In the step S6, after the slag is refined to produce reducing white slag, silicon manganese and ferrotitanium are added through an alloy silo for secondary alloying.

9. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In step S7, the molten steel is subjected to micro-calcium treatment, and the feeding amount of calcium wire is 0.35-0.6 m / t 钢 .

10. The process for improving the cleanliness of molten steel for 20CrMnTi according to claim 2, characterized in that: In step S8, after the calcium wire is fed, the ladle is subjected to a soft blowing operation for at least 10 minutes before being hoisted to the continuous casting.

Citation Information

Patent Citations

  • Smelting method for improving cutting performance of round steel for machinery

    CN105567899A

  • Smelting process for reducing TiN inclusion of gear steel 20CrMnTi

    CN107619983A

  • Method for solving clogging of continuous casting nozzle of 20CrMnTiH gear steel

    CN109628680A

  • Control method for steel bar titanium nitride inclusions for 35MnB series engineering machinery

    CN111961950A

  • High-cleanliness steel production method of LF-VD process route

    CN118272607A