Method for recovering valuable metal from aluminum-containing waste power battery ternary positive electrode material

By using the aluminum impurities included in the ternary positive electrode material as a reducing agent, crushing, reducing, alkali leaching, and acid leaching, the problems of high cost and high energy consumption in the existing technology have been successfully solved, and high efficiency and low The recovery rate of valuable metals at cost reaches 98% or above.

CN118932175APending Publication Date: 2024-11-12SHENYANG UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410780655.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing ternary cathode material recycling method, carbon powder, iron sulfide and sodium thiosulfate are used as reducing agents, which are costly and energy-consuming, and have high environmental requirements, low hydrogen utilization rate and great safety hazards, so it is urgently needed. A low cost and low energy consumption process.

Method used

Using the aluminum impurities included in the ternary positive electrode material as a reducing agent, the valuable metals such as nickel, cobalt, lithium are separated through the steps of crushing, reducing, alkali leaching, acid leaching, filtration, precipitation and extraction, reducing the recycling process. cost.

Benefits of technology

It realizes efficient recycling of valuable metals such as nickel, cobalt, and lithium without adding external reducing agents, reducing energy consumption, simplifying operating procedures, low production costs, and a recovery rate of 98% or above.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932175A_ABST
    Figure CN118932175A_ABST
Patent Text Reader

Abstract

The invention relates to a method for recovering valuable metals from an aluminum-containing waste power battery ternary positive electrode material. The method comprises the following steps: crushing and reducing the aluminum-containing ternary positive electrode material by using an aluminum impurity carried by a raw material as a reducing agent; then removing redundant aluminum impurities through alkaline leaching, carrying out acid leaching on alkaline leaching residues, and transferring Li, Co, Ni and Mn elements to a liquid phase; kMnO4 is added into the acid liquor, and MnO2 is precipitated; then adding dimethylglyoxime (DMG) to obtain a nickel dimethylglyoxime precipitate; the cobalt element is extracted from the cobalt-lithium solution, and a lithium-containing solution and a cobalt-containing solution are obtained respectively; and adjusting the pH value of the lithium-containing solution to 6-10, and precipitating aluminum impurities. Filtering, adding a sodium carbonate precipitator, and filtering to obtain a Li2CO3 product; and evaporating, concentrating and crystallizing the cobalt-containing solution to obtain a CoSO4. 7H2O product. According to the method, other types of reducing agents do not need to be added, the reduction reaction is large in heat release and high in spontaneity and does not need to be carried out in an ultra-high-temperature environment, the recovery process cost can be effectively reduced, and good economic benefits and application prospects are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of valuable metal recovery, and in particular to a method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials. Background Art

[0002] Ternary power batteries have a high share (≥35%) in the field of new energy vehicles due to their advantages such as high energy density, low self-discharge rate and high operating voltage. Under normal circumstances, ternary power batteries face retirement after 5 to 8 years of operation. Most retired batteries contain a variety of valuable elements such as nickel, cobalt, manganese, and lithium, and have significant recycling value. Among them, ternary positive electrode materials account for more than 40% of the overall value of the battery, so the recovery of valuable metals in ternary positive electrode materials has become the focus of current attention.

[0003] At present, the methods for recycling ternary positive electrode materials are roughly divided into pyrometallurgy and hydrometallurgy. However, the process that is generally recognized to have the prospect of industrialization is to use the combined treatment technology of pyrometallurgy + hydrometallurgy, which specifically decomposes and reduces the raw materials at high temperature, so that the high-priced nickel, cobalt and manganese elements are reduced to low-priced acid-soluble states, and then leached, and purified and separated by precipitation, extraction and other means.

[0004] CN201711338941.6 discloses a method for recovering valuable metals in waste nickel-cobalt-manganese-oxide lithium ternary battery positive electrode materials, wherein the nickel-cobalt-manganese-oxide lithium ternary battery positive electrode materials are mixed with carbon powder, roasted and reduced, and then acid-leached, filtered, and the pH is adjusted to 7.0-10.0. After filtering and removing impurities, sodium carbonate is added to recover the lithium metal element.

[0005] CN202310938194.9 discloses a composite sulfur-based reducing agent for selective lithium extraction from waste lithium-ion positive electrode materials and its application. The positive electrode material is mixed with iron sulfide and sodium thiosulfate for reduction roasting, and then leached in water to obtain a lithium-rich solution. The nickel-cobalt-manganese slag is then roasted with sodium persulfate and leached in water to obtain a nickel-cobalt-manganese solution. The nickel-cobalt-manganese solution, the lithium-rich solution and ammonium oxalate are mixed in a molar ratio of 1:1.2:1 and then spray granulated to obtain a nickel-cobalt-manganese spherical regenerated positive electrode material.

[0006] CN201910859941.3 discloses a method for recovering valuable metals from ternary positive electrode materials of waste power batteries, wherein the positive electrode materials are subjected to high-temperature hydrogen reduction treatment, and the lithium-rich solution after water leaching is precipitated to prepare lithium carbonate. After acid leaching of the leached residue, KMnO4 is added to precipitate MnO2. The separated cobalt-nickel solution is extracted to obtain a nickel-containing salt solution and a cobalt-containing salt solution.

[0007] CN202380011867.4 discloses a method for selectively extracting lithium from waste lithium-ion battery powder by aluminum-carbon synergistic reduction, wherein a mixed solid consisting of waste battery powder, carbon powder and aluminum powder is mixed with an alcohol substance and ball-milled; after drying, it is roasted and then carbonated and immersed in water to extract lithium.

[0008] In the above methods, carbon powder, iron sulfide and sodium thiosulfate are used as reducing agents, which are used in large quantities, have high costs and high requirements for the use environment; hydrogen is used as a reducing agent, but has low utilization rate, high energy consumption and great safety hazards. Therefore, it is urgent to find a low-cost, high-efficiency and low-energy lithium-ion battery recycling process. Summary of the invention

[0009] In view of the problems existing in the prior art, the purpose of the present invention is to provide a method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials. The method uses the aluminum impurities in the raw materials as a reducing agent to efficiently reduce the ternary positive electrode materials and reduce the recycling cost; at the same time, it also provides a new idea for pre-treatment of aluminum removal.

[0010] To achieve this object, the present invention adopts the following technical solutions: Step 1: crushing the aluminum-containing ternary positive electrode material; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction; Step 3: alkaline leaching the material in step 2, and separating to obtain alkaline leaching solution and alkaline leaching residue. The main solute component in the alkaline leaching solution is sodium metaaluminate; Step 4: acid leaching the alkali leaching residue in step 3 to obtain an acid leaching solution. The main elements in the acid leaching solution are Li, Co, Ni, and Mn; Step 5: Add KMnO4 to the acid leaching solution in step 4, and filter and separate to obtain a cobalt-nickel-lithium solution and MnO2; Step 6: adding dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution described in step 5 to obtain a cobalt-lithium solution and dimethylglyoxime nickel precipitate; Step 7: extracting the cobalt-lithium solution described in step 6 to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: Adjust the pH of the lithium-containing solution in step 7 to 6-10 to precipitate aluminum impurities. Filter and add sodium carbonate precipitant, and filter to obtain Li2CO3 product; Step 9: The cobalt-containing solution in step 7 is evaporated, concentrated and crystallized to obtain a CoSO4·7H2O product.

[0011] The method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials provided by the present invention utilizes the aluminum impurities in the raw materials as a reducing agent, and does not require the addition of other types of reducing agents, which can greatly reduce the cost of the recovery process. The reduction process reaction formula is: 6LiNi 0.5 Co 0.2 Mn 0.3 O2+2Al→3Li2O+3NiO+1.2CoO+1.8MnO+Al2O3 Li2O+Al2O3→2LiAlO2 The reaction products are mainly metal oxides, a small amount of lithium aluminate, and some unreacted aluminum. Then, alkali leaching is performed to remove most of the aluminum and aluminum oxide. After filtration, acid leaching is performed to efficiently dissolve the solids after alkali leaching. The reaction formula of the acid leaching process is: 2LiAlO2+4H2SO4→Al2(SO4)3+4H2O+Li2SO4 NiO+H2SO4→H2O+NiSO4 CoO+H2SO4→H2O+CoSO4 MnO+H2SO4→H2O+MnSO4 After acid leaching, the valuable elements are transferred to the liquid phase, and then the cobalt-lithium solution is obtained by precipitating manganese and nickel. After extracting cobalt, lithium-containing solution and cobalt-containing solution can be obtained respectively. There is a small amount of aluminum element in the lithium-containing solution. After adjusting the pH to 6-10, it is precipitated in the form of aluminum hydroxide. After filtering, sodium carbonate precipitant is added and filtered to obtain Li2CO3 product. The separated cobalt-containing solution is evaporated, concentrated and crystallized to obtain CoSO4·7H2O product.

[0012] According to the present invention, the aluminum content of the raw material ranges from 12% to 25%; for example, it can be 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, and 25% and specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0013] Preferably, the particle size of the raw material after crushing is 30μm to 75μm; for example, it can be 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 65μm, 70μm, and 75μm, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0014] According to the present invention, the reduction reaction temperature is 400-700°C; for example, it can be 400°C, 500°C, 600°C, and 700°C, as well as specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0015] According to the present invention, the reduction time is 2 to 4 hours; for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, and 4 hours, as well as specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0016] According to the present invention, the alkali leaching stirring speed is 350-550 r / min; for example, it can be 350 r / min, 450 r / min, 550 r / min and specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0017] According to the present invention, the alkali leaching stirring time is 2 to 4 hours; for example, it can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, and 4 hours, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0018] According to the present invention, the solid ratio of the alkali leaching solution is 3:1 to 10:1 ml / g; for example, it can be 3:1 ml / g, 4:1 ml / g, 5:1 ml / g, 6:1 ml / g, 7:1 ml / g, 8:1 ml / g, 9:1 ml / g, and 10:1 ml / g, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0019] According to the present invention, the alkali leaching temperature is 25-80°C; for example, it can be 25°C, 35°C, 45°C, 55°C, 65°C, 75°C, and 80°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0020] Preferably, the alkaline leaching agent is any one of ammonia water, sodium hydroxide or sodium bicarbonate.

[0021] Preferably, the hydroxide ion concentration in the alkaline leaching agent is 2 to 4 mol / L; for example, it can be 2 mol / L, 2.5 mol / L, 3 mol / L, 3.5 mol / L, and 4 mol / L, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0022] According to the present invention, the acid leaching stirring speed is 350-550 r / min; for example, it can be 350 r / min, 450 r / min, 550 r / min and specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0023] According to the present invention, the acid leaching stirring time is 4 to 6 hours; for example, it can be 4 hours, 4.5 hours, 5 hours, 5.5 hours, and 6 hours, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0024] According to the present invention, the solid ratio of the acid leaching solution is 4:1 to 10:1 ml / g; for example, it can be 4:1 ml / g, 5:1 ml / g, 6:1 ml / g, 7:1 ml / g, 8:1 ml / g, 9:1 ml / g, and 10:1 ml / g, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0025] According to the present invention, the pickling temperature is 50-90°C; for example, it can be 50°C, 60°C, 70°C, 80°C, and 90°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0026] Preferably, the acid leaching agent is sulfuric acid.

[0027] Preferably, the sulfuric acid concentration is 1 to 5 mol / L; for example, it can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, and 5 mol / L, as well as specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0028] According to the present invention, in the process of adding KMnO4 in step 5, the molar ratio of KMnO4 to Mn in the solution is 2:3.

[0029] According to the present invention, the reaction time of adding KMnO4 in step 5 is 0.5 to 2 hours; for example, it can be 0.5 hours, 1 hour, 1.5 hours, and 2 hours, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0030] According to the present invention, in the process of adding KMnO4 in step 5, the temperature is 25-50°C; for example, it can be 25°C, 30°C, 40°C, and 50°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0031] According to the present invention, in the process of adding KMnO4 in step 5, the stirring speed is 200-500r / min; for example, it can be 200r / min, 300r / min, 400r / min, 500r / min and specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0032] According to the present invention, in the process of adding dimethylglyoxime in step 6, the molar ratio of dimethylglyoxime to Ni in the solution is 1:2.

[0033] According to the present invention, the reaction time of adding diacetyl oxime in step 6 is 1 to 3 hours; for example, it can be 1 hour, 2 hours, and 3 hours, as well as specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0034] According to the present invention, in the process of adding diacetyl oxime in step 6, the temperature is 25-50°C; for example, it can be 25°C, 30°C, 40°C, and 50°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0035] According to the present invention, in the process of adding diacetyl oxime in step 6, the stirring speed is 200-500 r / min; for example, it can be 200 r / min, 300 r / min, 400 r / min, 500 r / min and specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0036] According to the present invention, in the extraction process in step 7, a multi-step countercurrent extraction is performed using one of P507, P-204, and AD-290.

[0037] According to the present invention, in the extraction process in step 7, 2 to 6 mol / L of sulfuric acid is used for back extraction; for example, it can be 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, and 6 mol / L, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.

[0038] According to the present invention, in the lithium precipitation process in step 8, the precipitation temperature is 95-105°C; for example, it can be 95°C, 100°C, and 105°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0039] According to the present invention, in the lithium precipitation process in step 8, the precipitation time is 0.5 to 2 hours; for example, it can be 0.5 hours, 1 hour, and 2 hours, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0040] According to the present invention, in the lithium precipitation process in step 8, the molar ratio of the amount of sodium carbonate added to the lithium in the solution is 1:2 to 2:1; for example, it can be 1:2, 1:1, and 2:1, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them exhaustively.

[0041] According to the present invention, in the evaporation concentration crystallization process in step 9, the cobalt-containing solution is evaporated to 30% to 60% of the volume of the original solution; for example, it can be 30%, 40%, 50% and 60% and specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.

[0042] According to the present invention, in the evaporation concentration crystallization process in step 9, the crystallization temperature is -10 to 0°C; for example, it can be -10°C, -5°C, and 0°C, as well as specific point values ​​between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.

[0043] According to the present invention, in the evaporation concentration crystallization process in step 9, the amount of CoSO4·7H2O added is 2% to 5% of the total Co molar amount of the solution; for example, it can be 2%, 3%, 4% and 5% and specific points between the above values. Due to space limitations and for the sake of simplicity, the present invention will no longer list them all.

[0044] Compared with the prior art solutions, the present invention has at least the following beneficial effects: (1) The present invention uses aluminum impurities carried by the raw materials as a reducing agent, and does not need to add other types of reducing agents, which can effectively reduce the cost of the recycling process. In addition, the reduction reaction of aluminum impurities as a reducing agent itself releases a large amount of heat and is highly spontaneous, and does not need to be carried out in an ultra-high temperature environment, which can effectively save energy; (2) The whole operation process of the present invention is simple, the production cost is low, and the overall recovery rates of nickel, cobalt, manganese and lithium can reach 98%, 97%, 98% and 93%, respectively, which has good economic benefits and application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0045] Figure 1 The process flow chart adopted by the present invention. DETAILED DESCRIPTION

[0046] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.

[0047] like Figure 1 As shown, the process flow provided by a specific embodiment of the present invention can be: Step 1: crushing the ternary positive electrode material containing 12% to 25% aluminum, and the particle size of the raw material after crushing is 30 μm to 75 μm; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction, wherein the reduction reaction temperature is 400-700° C. and the reduction time is 2-4 hours; Step 3: alkaline leaching the material described in step 2, with an alkali leaching stirring speed of 350-550 r / min, a stirring time of 2-4 h, a liquid-solid ratio of 3:1-10:1 ml / g, and a temperature of 25-80°C. The alkaline leaching agent is any one of ammonia water, sodium hydroxide or sodium bicarbonate, and the hydroxide ion concentration in the alkaline leaching agent is 2-4 mol / L. Alkaline leaching solution and alkaline leaching residue are separated. The main solute component in the alkaline leaching solution is sodium aluminate; Step 4: acid leaching the alkali leaching residue described in step 3 to obtain an acid leaching solution. The acid leaching stirring speed is 350-550r / min, the stirring time is 4-6h, the liquid-solid ratio is 4:1-10:1ml / g, and the temperature is 50-90°C. The acid leaching reagent is sulfuric acid with a concentration of 1-5mol / L. The main elements in the acid leaching solution are Li, Co, Ni, and Mn; Step 5: Add KMnO4 to the acid leaching solution in step 4, with a molar ratio of KMnO4 to Mn in the solution of 2:3. The reaction time is 0.5 to 2 hours, the temperature is 25 to 50°C, and the stirring speed is 200 to 500 r / min. Filter and separate to obtain a cobalt-nickel-lithium solution and MnO2; Step 6: Add dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution in step 5, with a molar ratio of dimethylglyoxime to Ni in the solution of 1:2. The reaction time is 1 to 3 hours, the temperature is 25 to 50° C., and the stirring speed is 200 to 500 r / min. Cobalt-lithium solution and dimethylglyoxime nickel precipitate are obtained; Step 7: extracting the cobalt-lithium solution in step 6, performing multi-step countercurrent extraction with one of P507, P-204, and AD-290, and then stripping with 2-6 mol / L sulfuric acid to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: Adjust the pH of the lithium-containing solution in step 7 to 6-10 to precipitate aluminum impurities. Filter and add sodium carbonate precipitant, the precipitation temperature is 95-105°C, the precipitation time is 0.5-2h, and the molar ratio of sodium carbonate added to lithium in the solution is 1:2-2:1. Filter to obtain Li2CO3 product; Step 9: The cobalt-containing solution in step 7 is evaporated, concentrated and crystallized, and the cobalt-containing solution is evaporated to 30% to 60% of the original solution volume, the crystallization temperature is -10 to 0°C, and the amount of CoSO4·7H2O added is 2% to 5% of the total molar amount of Co in the solution to obtain CoSO4·7H2O product.

[0048] To better illustrate the present invention and facilitate understanding of the technical solution of the present invention, typical but non-limiting embodiments of the present invention are as follows: Example 1 Step 1: crushing the ternary positive electrode material containing 12% aluminum, and the particle size of the raw material after crushing is 30 μm; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction, the reduction reaction temperature is 400°C, and the reduction time is 2h; Step 3: alkaline leaching the material described in step 2, with an alkali leaching stirring speed of 350r / min, a stirring time of 2h, a liquid-solid ratio of 3:1ml / g, and a temperature of 25°C. The alkali leaching reagent is sodium hydroxide, and the hydroxide ion concentration in the alkali leaching reagent is 2mol / L. Alkaline leaching solution and alkali leaching residue are separated. The main solute component in the alkali leaching solution is sodium aluminate; Step 4: Acid leaching the alkali leaching residue described in step 3 to obtain an acid leaching solution. The acid leaching stirring speed is 350r / min, the stirring time is 4h, the liquid-solid ratio is 4:1ml / g, and the temperature is 50°C. The acid leaching reagent is sulfuric acid with a concentration of 1mol / L. Li, Co, Ni, and Mn in the acid leaching solution are 91%, 92%, 92%, and 91% respectively; Step 5: Add KMnO4 to the acid leaching solution in step 4, with a molar ratio of KMnO4 to Mn in the solution of 2:3. The reaction time is 0.5h, the temperature is 25°C, and the stirring speed is 200r / min. Filter and separate to obtain cobalt-nickel-lithium solution and MnO2, and the Mn precipitation efficiency is 95%; Step 6: Add dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution described in step 5, with a molar ratio of dimethylglyoxime to Ni in the solution of 1:2. The reaction time is 1 hour, the temperature is 25°C, and the stirring speed is 200r / min. Cobalt-lithium solution and dimethylglyoxime nickel precipitate are obtained, and the Ni precipitation efficiency is 93%; Step 7: extracting the cobalt-lithium solution in step 6, performing multi-step countercurrent extraction with P507, and then performing back extraction with 2 mol / L sulfuric acid to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: The lithium-containing solution described in step 7 is adjusted to pH 6-10 to precipitate aluminum impurities. Sodium carbonate precipitant is added after filtration, the precipitation temperature is 95°C, the precipitation time is 0.5h, and the molar ratio of sodium carbonate added to lithium in the solution is 1:2. Li2CO3 product is obtained by filtration, and the Li precipitation efficiency is 86%; Step 9: The cobalt-containing solution in step 7 is evaporated, concentrated and crystallized, and the cobalt-containing solution is evaporated to 30% of the original solution volume, the crystallization temperature is -10°C, and the amount of CoSO4·7H2O added is 2% of the total Co molar amount in the solution. CoSO4·7H2O product is obtained, and the Co precipitation efficiency is 90%.

[0049] Example 2 Step 1: crushing the ternary positive electrode material containing 25% aluminum, and the particle size of the raw material after crushing is 30 μm; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction, the reduction reaction temperature is 700° C., and the reduction time is 4 h; Step 3: alkaline leaching the material described in step 2, with an alkali leaching stirring speed of 550r / min, a stirring time of 4h, a liquid-solid ratio of 10:1ml / g, and a temperature of 80°C. The alkali leaching reagent is sodium hydroxide, and the hydroxide ion concentration in the alkali leaching reagent is 4mol / L. Alkaline leaching solution and alkali leaching residue are separated. The main solute component in the alkali leaching solution is sodium aluminate; Step 4: Acid leaching the alkali leaching residue described in step 3 to obtain an acid leaching solution. The acid leaching stirring speed is 550r / min, the stirring time is 6h, the liquid-solid ratio is 10:1ml / g, and the temperature is 90°C. The acid leaching reagent is sulfuric acid with a concentration of 5mol / L. Li, Co, Ni, and Mn in the acid leaching solution are 99%, 98%, 99%, and 98% respectively; Step 5: Add KMnO4 to the acid leaching solution in step 4, with a molar ratio of KMnO4 to Mn in the solution of 2:3. The reaction time is 2 hours, the temperature is 50°C, and the stirring speed is 500r / min. Filter and separate to obtain cobalt-nickel-lithium solution and MnO2, with a Mn precipitation efficiency of 98%; Step 6: Add dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution described in step 5, with a molar ratio of dimethylglyoxime to Ni in the solution of 1:2. The reaction time is 3 hours, the temperature is 50°C, and the stirring speed is 500r / min. Cobalt-lithium solution and dimethylglyoxime nickel precipitate are obtained, and the Ni precipitation efficiency is 98%; Step 7: extracting the cobalt-lithium solution in step 6, performing multi-step countercurrent extraction with P507, and then performing back extraction with 4 mol / L sulfuric acid to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: The lithium-containing solution described in step 7 is adjusted to pH 6-10 to precipitate aluminum impurities. Sodium carbonate precipitant is added after filtration, the precipitation temperature is 105°C, the precipitation time is 2 hours, and the molar ratio of sodium carbonate added to lithium in the solution is 2:1. Li2CO3 product is obtained by filtration, and the Li precipitation efficiency is 93%; Step 9: The cobalt-containing solution in step 7 is evaporated, concentrated and crystallized, and the cobalt-containing solution is evaporated to 60% of the original solution volume, the crystallization temperature is -10°C, and the amount of CoSO4·7H2O added is 5% of the total molar amount of Co in the solution. CoSO4·7H2O product is obtained, and the Co precipitation efficiency is 98%.

[0050] Comparative Example 1 Step 1: crushing the ternary positive electrode material containing 5% aluminum, and the particle size of the raw material after crushing is 30 μm; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction, the reduction reaction temperature is 700° C., and the reduction time is 4 h; Step 3: alkaline leaching the material described in step 2, with an alkali leaching stirring speed of 550r / min, a stirring time of 4h, a liquid-solid ratio of 10:1ml / g, and a temperature of 80°C. The alkali leaching reagent is sodium hydroxide, and the hydroxide ion concentration in the alkali leaching reagent is 4mol / L. Alkaline leaching solution and alkali leaching residue are separated. The main solute component in the alkali leaching solution is sodium aluminate; Step 4: Acid leaching the alkali leaching residue described in step 3 to obtain an acid leaching solution. The acid leaching stirring speed is 550r / min, the stirring time is 6h, the liquid-solid ratio is 10:1ml / g, and the temperature is 90°C. The acid leaching reagent is sulfuric acid with a concentration of 5mol / L. Li, Co, Ni, and Mn in the acid leaching solution are 60%, 68%, 49%, and 58%, respectively; Step 5: Add KMnO4 to the acid leaching solution in step 4, with a molar ratio of KMnO4 to Mn in the solution of 2:3. The reaction time is 2 hours, the temperature is 50°C, and the stirring speed is 500r / min. Filter and separate to obtain cobalt-nickel-lithium solution and MnO2, with a Mn precipitation efficiency of 98%; Step 6: Add dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution described in step 5, with a molar ratio of dimethylglyoxime to Ni in the solution of 1:2. The reaction time is 3 hours, the temperature is 50°C, and the stirring speed is 500r / min. Cobalt-lithium solution and dimethylglyoxime nickel precipitate are obtained, and the Ni precipitation efficiency is 98%; Step 7: extracting the cobalt-lithium solution in step 6, performing multi-step countercurrent extraction with P507, and then performing back extraction with 4 mol / L sulfuric acid to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: The lithium-containing solution described in step 7 is adjusted to pH 6-10 to precipitate aluminum impurities. Sodium carbonate precipitant is added after filtration, the precipitation temperature is 105°C, the precipitation time is 2 hours, and the molar ratio of sodium carbonate added to lithium in the solution is 2:1. Li2CO3 product is obtained by filtration, and the Li precipitation efficiency is 93%; Step 9: The cobalt-containing solution in step 7 is evaporated, concentrated and crystallized, and the cobalt-containing solution is evaporated to 60% of the original solution volume, the crystallization temperature is -10°C, and the amount of CoSO4·7H2O added is 5% of the total molar amount of Co in the solution. CoSO4·7H2O product is obtained, and the Co precipitation efficiency is 98%.

Claims

1. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials, It is characterized in that The method is: Step 1: crushing the aluminum-containing ternary positive electrode material; Step 2: subjecting the raw materials described in step 1 to a full reduction reaction; Step 3: alkali leaching the material in step 2, and separating to obtain alkali leaching solution and alkali leaching residue, wherein the main solute component in the alkali leaching solution is sodium aluminate; Step 4: acid leaching the alkali leaching residue described in step 3 to obtain an acid leaching solution, wherein the main elements in the acid leaching solution are Li, Co, Ni, and Mn; Step 5: Add KMnO to the acid leaching solution described in step 4. 4 , filter and separate to obtain cobalt-nickel-lithium solution and MnO 2 ; Step 6: adding dimethylglyoxime (DMG) to the cobalt-nickel-lithium solution described in step 5 to obtain a cobalt-lithium solution and dimethylglyoxime nickel precipitate; Step 7: extracting the cobalt-lithium solution described in step 6 to obtain a lithium-containing solution and a cobalt-containing solution; Step 8: The lithium-containing solution described in step 7 is adjusted to pH 6-10 to precipitate aluminum impurities, filtered, added with sodium carbonate precipitant, and filtered to obtain Li 2 CO 3 product; Step 9: The cobalt-containing solution described in step 7 is evaporated, concentrated and crystallized to obtain CoSO 4 7H 2 O product.

2. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In step 1, the aluminum content of the raw material is in the range of 12% to 25%; preferably, the particle size of the raw material after crushing is 30 μm to 75 μm.

3. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In the step 2, the reduction reaction temperature is 400-700° C., and the reduction time is 2-4 hours.

4. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In step 3, the alkali leaching stirring speed is 350-550 r / min, the stirring time is 2-4 h, the liquid-solid ratio is 3:1-10:1 ml / g, and the temperature is 25-80° C.; preferably, the alkali leaching agent is any one of ammonia water, sodium hydroxide or sodium bicarbonate; preferably, the hydroxide ion concentration in the alkali leaching agent is 2-4 mol / L.

5. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In step 4, the acid leaching stirring speed is 350-550 r / min, the stirring time is 4-6 h, the liquid-solid ratio is 4:1-10:1 ml / g, and the temperature is 50-90° C.; preferably, the acid leaching reagent is sulfuric acid; preferably, the sulfuric acid concentration is 1-5 mol / L.

6. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In step 5, KMnO is added 4 Process, KMnO 4 The molar ratio of Mn to the solution is 2:3, the reaction time is 0.5 to 2 hours, the temperature is 25 to 50°C, and the stirring speed is 200 to 500 r / min.

7. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In the process of adding diacetyl oxime in step 6, the molar ratio of diacetyl oxime to Ni in the solution is 1:2, the reaction time is 1 to 3 hours, the temperature is 25 to 50° C., and the stirring speed is 200 to 500 r / min.

8. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In the extraction process of step 7, after multi-step countercurrent extraction with one of P507, P-204, and AD-290, back extraction is performed with 2-6 mol / L sulfuric acid.

9. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In the lithium precipitation process in step 8, the precipitation temperature is 95-105° C., the precipitation time is 0.5-2 h, and the molar ratio of the amount of sodium carbonate added to the lithium in the solution is 1:2-2:

1.

10. A method for recovering valuable metals from aluminum-containing waste power battery ternary positive electrode materials according to claim 1, It is characterized in that In the evaporation, concentration and crystallization process in step 9, the cobalt-containing solution is evaporated to 30% to 60% of the original solution volume, and the crystallization temperature is -10 to 0°C. CoSO 4 7H 2 The amount of O added is 2% to 5% of the total molar amount of Co in the solution.

Citation Information

Cited By

  • Method for synergistically reducing and recovering lithium carbonate from aluminum-containing waste power battery ternary positive electrode material

    CN119592798A

  • Method for recycling valuable metal from aluminum-containing waste ternary battery positive electrode powder by using hazelnut shell powder

    CN120158606A

  • Method for recovering valuable metals from aluminum-containing waste ternary battery positive electrode powder by using bamboo poles

    CN120158609A