Electrode material, electrode for spark plug, and spark plug
By using a composite material structure of high-Ni nickel-based core wire and Cr,Al nickel alloy outer sheath in the spark plug electrode, the problems of insufficient spark wear resistance and oxidation resistance are solved, achieving low specific resistance and good heat dissipation.
Patent Information
- Application Number
- CN202411031957.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2017-05-19
- Filing Date
- 2018-02-07
- Publication Date
- 2024-11-12
AI Technical Summary
Existing spark plug electrode materials are insufficient in terms of spark wear resistance and oxidation resistance, making it difficult to meet the requirements for reducing electrode thickness.
The composite material structure is adopted, in which the core wire is made of nickel-based material with high Ni content, and the outer sheath is made of nickel alloy containing a specific range of Cr and Al. The specific resistivity of the composite material is less than 50 μΩ·cm, and the adhesion between the core wire and the outer sheath is improved through a diffusion layer.
This achieves low specific resistance, good spark wear resistance and oxidation resistance of spark plug electrodes, inhibits oxidation and corrosion, and improves heat dissipation and high-temperature strength.
Smart Images

Figure CN118932217A_ABST
Abstract
Description
[0001] This patent application is a divisional application of the patent application with application number 2018800331937, application date February 7, 2018, and invention name “Electrode material, electrode for spark plug, and spark plug”. Technical Field
[0002] The present invention relates to an electrode material, an electrode for a spark plug, and a spark plug. This application claims priority to Japanese Patent Application No. 2017-100387 filed on May 19, 2017, and the entire contents of the Japanese Patent Application are incorporated herein by reference. Background Art
[0003] A spark plug is an example of an engine component of an automobile, etc. Patent Document 1 discloses an electrode material composed of a nickel alloy having a specific composition as an electrode material suitable for an electrode included in a spark plug.
[0004] Reference List
[0005] Patent Literature
[0006] Patent Document 1: Japanese Unexamined Patent Application Publication No. 2012-069393 Summary of the invention
[0007] [Problems to be solved]
[0008] The electrode material according to the present disclosure comprises:
[0009] A composite material comprising a core wire and a sheath, wherein the core wire comprises 96% by mass
[0010] The above Ni-based material is composed of the outer skin covering the outer peripheral surface of the core wire and not covering the end surface of the core wire but leaving the end surface of the core wire exposed, wherein
[0011] The outer skin is composed of a nickel alloy containing 10 mass % to 30 mass % of Cr and 0.1 mass % to 6 mass % of Al, and
[0012] The specific resistivity of the composite material is less than 50 μΩ·cm.
[0013] The spark plug electrode according to the present disclosure is composed of the electrode material according to the present disclosure.
[0014] A spark plug according to the present disclosure includes the spark plug electrode according to the present disclosure. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] [ Figure 1 ] Figure 1 is a schematic perspective view showing an electrode material according to one embodiment.
[0016] [ Figure 2 ] Figure 2 It is a schematic diagram showing a spark plug including a spark plug electrode composed of the electrode material according to the embodiment, and shows a portion near the electrode.
[0017] [ Figure 3 ] Figure 3 3 is a view showing a sample for evaluating adhesion in Test Example 1.
[0018] [ Figure 4 ] Figure 4 This is a micrograph of a cross section of the wire material of Sample No. 1-1 after the heat cycle test for evaluating adhesion in Test Example 1.
[0019] [ Figure 5 ] Figure 5 This is a micrograph of a cross section of the wire material of Sample No. 1-111 after the heat cycle test for evaluating adhesion in Test Example 1. DETAILED DESCRIPTION
[0020] [Problems to be Solved by the Invention]
[0021] It is desirable that the electrode and the electrode material of the electrode included in the spark plug have both higher spark wear resistance and higher oxidation resistance.
[0022] The electrode material described in Patent Document 1 is composed of a nickel alloy having a specific composition, thereby achieving good high-temperature oxidation resistance and good spark wear resistance. Recently, it is necessary to further reduce the thickness of the electrode of the spark plug (reduce the cross-sectional area). In order to manufacture a spark plug electrode that can meet this demand, an electrode material having both higher spark wear resistance and higher oxidation resistance is desired.
[0023] In view of the above, one object of the present invention is to provide an electrode material having both good spark wear resistance and good oxidation resistance. Another object of the present invention is to provide a spark plug electrode and a spark plug having both good spark wear resistance and good oxidation resistance.
[0024] [Advantageous Effects of the Invention]
[0025] The electrode material, the spark plug electrode, and the spark plug according to the present disclosure have both good spark wear resistance and good oxidation resistance.
[0026] [Description of Embodiments of the Invention]
[0027] First, embodiments according to the present invention will be listed and described.
[0028] (1) The electrode material according to an embodiment of the present invention comprises
[0029] A composite material comprising a core wire and a sheath, wherein the core wire is composed of a nickel-based material containing 96% by mass or more of Ni, the sheath covers the outer peripheral surface of the core wire and does not cover the end surface of the core wire but exposes the end surface of the core wire, wherein
[0030] The outer skin is composed of a nickel alloy containing 10 mass % to 30 mass % of Cr and 0.1 mass % to 6 mass % of Al, and
[0031] The specific resistivity of the composite material is less than 50 μΩ·cm.
[0032] The electrode material is not composed of a single material, but includes a composite material having a multilayer structure composed of a plurality of different materials. In the composite material, the core wire located inside is composed of a nickel-based material with a high Ni content, so it has good conductivity and low specific resistance. In the composite material, the outer skin located outside is composed of a nickel alloy containing a specific range of Cr and Al, so it has good oxidation resistance. Compared with the electrode material having only the composition of the outer skin, the presence of the core wire with low specific resistance can reduce the specific resistance of the composite material. Compared with the electrode material having only the composition of the core wire, the presence of the outer skin with good oxidation resistance makes the composite material have good oxidation resistance. The outer skin exists on the outside of the core wire and can protect the core wire from the external environment. This also makes the composite material have good oxidation resistance. In addition, since both the core wire and the outer skin contain Ni as the main component and contain a common main component, the core wire and the outer skin are easy to adhere to each other. In this electrode material, although the core wire, which is more easily oxidized than the outer skin, is exposed from the end face of the composite material, the oxidation from the end face along the interface between the core wire and the outer skin to the inside of the composite material can be suppressed. This also makes the electrode material have good oxidation resistance. Therefore, according to the above-mentioned electrode material, it is possible to form a spark plug electrode having low specific resistance, good spark wear resistance and good oxidation resistance.
[0033] According to the electrode material, since the core wire is made of a nickel-based material, good thermal conductivity is also achieved. In addition, according to the electrode material, since the core wire is exposed at the end face of the electrode material, heat can be uniformly conducted over the entire length of the composite material compared to the case where the end face is covered by the constituent material of the outer skin. According to the electrode material, heat is not easily accumulated inside the electrode material, the strength reduction caused by the electrode material being kept at a high temperature can be reduced, and the high-temperature strength is also good. Therefore, when a spark plug electrode with a core wire exposed at the end face is formed by using the electrode material, the electrode can be uniformly heat-conducting over its entire length from the end face, and has good heat dissipation capacity. In addition, according to the electrode material, although the core wire has a high Ni content, the electrode material has good corrosion resistance because the outer skin covering the core wire contains a relatively large amount of Cr. As described above, the electrode material has good adhesion between the core wire and the outer skin, and can suppress the progress of corrosion from the end face of the composite material along the interface between the core wire and the outer skin to the inside of the composite material. This also gives the electrode material good corrosion resistance.
[0034] (2) According to an embodiment of the electrode material, in a cross section of the composite material, the area ratio of the cross-sectional area of the outer skin to the cross-sectional area of the composite material is 0.4 or more and 0.7 or less. Hereinafter, the area ratio may be referred to as the outer skin ratio. The cross section refers to the cross section when the composite material is cut along a plane orthogonal to the axial direction of the composite material or the core wire as a cutting surface.
[0035] In the above embodiment, because the sheath ratio is within the above specific range, the composite material has both good oxidation resistance due to the presence of the sheath and good spark wear resistance due to the presence of the core wire in a balanced manner. In the above embodiment, the sheath ratio is not too large, so it has good processability during the manufacturing process, and the composite material also has excellent manufacturability.
[0036] (3) According to an embodiment of the electrode material, the ratio of the grain size of the nickel-based material forming the core wire to the grain size of the nickel alloy forming the sheath is 5 or more. Hereinafter, this ratio may be referred to as a ratio (core wire / sheath).
[0037] In the above embodiment, the nickel-based material forming the core wire contains relatively coarse grains, and the nickel alloy forming the outer skin contains relatively fine grains. Because the core wire has a coarse crystal structure, the specific resistance is easily reduced. Because the outer skin has a fine crystal structure, the oxidation resistance is easily improved. That is, the specific resistance of the core wire can be reduced not only in terms of composition but also in terms of structure; and the oxidation resistance of the outer skin can be improved not only in terms of composition but also in terms of structure. Therefore, the above embodiment has low specific resistance, higher spark wear resistance and higher oxidation resistance.
[0038] (4) According to an embodiment of the electrode material, the electrode material includes a diffusion layer between the core wire and the sheath, wherein the Ni content of the diffusion layer changes in a gradient manner. The details of the diffusion layer will be described below.
[0039] Due to the presence of the diffusion layer, the above embodiment has better adhesion between the core wire and the outer sheath. Therefore, as described above, the above embodiment is more likely to suppress the progress of oxidation and corrosion to the inside, and thus has higher oxidation resistance.
[0040] (5) According to an embodiment of the electrode material, at least one of the nickel-based material forming the core wire and the nickel alloy forming the sheath contains a rare earth element in an amount of 0.01 mass % to 0.7 mass % both inclusive in total.
[0041] Since the above embodiment contains the rare earth element (which may be one element or two or more elements) within the above specific range, the oxidation resistance of the core wire and the sheath can be further improved.
[0042] (6) According to an embodiment of the electrode material, the nickel alloy forming the outer skin comprises, in terms of mass %,
[0043] 0.1 mass % to 1.5 mass % of Si,
[0044] 0.1 mass % to 0.6 mass % of Mn,
[0045] 10 mass % or more and 30 mass % or less of Cr,
[0046] 0.1 mass % to 6 mass % of Al,
[0047] 0.01 mass % to 12 mass % of Fe, and
[0048] The content of Ti is 0.01 mass % or more and 0.6 mass % or less, and the balance is Ni and inevitable impurities.
[0049] Since the above embodiment includes the sheath composed of the nickel alloy containing Si, Mn, Fe, and Ti within the above-mentioned specific ranges in addition to Cr and Al, the oxidation resistance is further improved.
[0050] (7) According to the embodiment of the electrode material,
[0051] In terms of mass %, the nickel-based material forming the core wire comprises
[0052] 0.01 mass % to 1.5 mass % of Si,
[0053] 0 mass % or more and 1.5 mass % or less of Mn,
[0054] 0.001 mass% to 1.5 mass% of Cr,
[0055] 0.001 mass % to 0.5 mass % of Al,
[0056] 0.01 mass % to 1.5 mass % of Fe, and
[0057] The content of Ti is 0 mass % or more and 0.5 mass % or less, and the balance is Ni and inevitable impurities.
[0058] Since the above embodiment includes a core wire composed of a nickel-based material containing Si, Cr, Al, Fe and optionally Mn and Ti within the above-mentioned specific ranges, an increase in specific resistance and a decrease in thermal conductivity due to the mixing of the above-mentioned elements are suppressed, thereby providing good spark wear resistance and good thermal conductivity, and oxidation resistance is also improved to a certain extent, thereby obtaining higher oxidation resistance.
[0059] (8) A spark plug electrode according to an embodiment of the present invention is composed of the electrode material according to any one of (1) to (7) above.
[0060] Since the spark plug electrode is composed of an electrode material including the above-mentioned specific composite material, the spark plug electrode also has a low specific resistance of less than 50 μΩ·cm, good spark wear resistance, and good oxidation resistance as described above. In the spark plug electrode, the core wire included in the composite material can be exposed at the end face of the electrode. Even when the core wire is exposed at the end face, as described above, the adhesion between the core wire and the outer skin covering the outer peripheral surface of the core wire is good, so oxidation is difficult to proceed to the inside. Therefore, the spark plug electrode has good oxidation resistance.
[0061] Furthermore, according to the spark plug electrode, when the core wire is exposed at the end face of the electrode, as described above, heat can be uniformly conducted over the entire length of the electrode from the end face, and good heat dissipation capability is also achieved. Furthermore, as described above, since the core wire is covered with the outer skin and the adhesion between the core wire and the outer skin is good, the spark plug electrode also has good corrosion resistance.
[0062] (9) A spark plug according to an embodiment of the present invention includes the spark plug electrode according to (8) above.
[0063] Since the spark plug includes the above-described spark plug electrode, the spark plug also has good spark wear resistance and good oxidation resistance as described above.
[0064] [Detailed description of embodiments of the present invention]
[0065] Now, embodiments according to the present invention will be described in detail with reference to the accompanying drawings as required. Unless otherwise specified, the content of an element is expressed in mass %.
[0066] [Electrode materials]
[0067] (summary)
[0068] like Figure 1 As shown, the electrode material 1 according to the embodiment is a metal wire having a double-layer structure including an inner layer and an outer layer. The electrode material 1 is used for a spark plug 2 ( Figure 2 ) included in the electrode 20 (same), wherein the spark plug 2 is used in the engine of an automobile or the like. The electrode material 1 according to the embodiment includes a composite material 10, which includes a core wire 11 and a sheath 12, the sheath 12 covering the outer peripheral surface of the core wire 11 and not covering the end surface of the core wire 11 but leaving the end surface of the core wire 11 exposed. Although the core wire 11 and the sheath 12 are composed of metals with different compositions, the core wire 11 and the sheath 12 each contain Ni as a main component (the component with the highest content by mass). The core wire 11 is composed of a nickel-based material containing more than 96% by mass of Ni. The sheath 12 is composed of a nickel alloy containing more than 10% by mass and less than 30% by mass of Cr and more than 0.1% by mass and less than 6% by mass of Al. In the electrode material 1 according to the embodiment, the composite material 10 has a specific resistance of less than 50μΩ·cm.
[0069] (composition)
[0070] In the composite material 10 forming the electrode material 1, both the core wire 11 and the sheath 12 contain Ni as a main component. Therefore, it is not easy to form a heterogeneous phase near the interface between the core wire 11 and the sheath 12, so that good adhesion between the core wire 11 and the sheath 12 is achieved. In particular, because the Ni content of the nickel-based material forming the core wire 11 is 96% by mass or more, the nickel-based material has a low specific resistance and contributes to reducing the specific resistance of the composite material 10. The high Ni content provides good thermal conductivity, can improve the heat dissipation ability of the composite material 10, provides good plastic workability, and contributes to the manufacture of the composite material 10 having a double-layer structure. On the other hand, because the nickel alloy forming the sheath 12 contains Cr and Al within a specific range (Cr and Al contribute to improving oxidation resistance), the nickel alloy contributes to improving the oxidation resistance of the composite material 10. In the electrode material 1 according to the embodiment, the core wire 11 with poor oxidation resistance is covered with the sheath 12, thereby suppressing the oxidation of the core wire 11, and the above-mentioned effects due to the presence of the core wire 11 are appropriately achieved. In addition, although the Cr content of the sheath 12 included in the electrode material 1 according to the embodiment is slightly high and tends to have a high specific resistance, good spark wear resistance is achieved by adjusting (for example) the composition of the sheath 12 and the ratio of the sheath 12 in the composite material 10 (the sheath ratio described below) within a range where the specific resistance of the composite material 10 satisfies less than 50 μΩ·cm.
[0071] <Core Wire>
[0072] Examples of the nickel-based material forming the core wire 11 include nickel alloys with various compositions or pure nickel having a Ni content of 96 mass % or more. As the Ni content increases, the specific resistance tends to decrease. The Ni content may be 96.5 mass % or more, and further may be 97 mass % or more.
[0073] An example of the nickel-based material forming the core wire 11 is a nickel alloy having the following composition (1). The effects achieved by introducing each element will be described below (for Cr and Al, see the section of the sheath). As the content of each element listed below decreases, the specific resistance tends to decrease, and the thermal conductivity tends to increase. As the content thereof increases, (for example) oxidation resistance and high-temperature strength tend to increase (the same applies to each element contained in the nickel alloy forming the sheath 12 described below).
[0074] Composition (1): The nickel alloy comprises 0.01 mass % to 1.5 mass % Si, 0 mass % to 1.5 mass % Mn, 0.001 mass % to 1.5 mass % Cr, 0.001 mass % to 0.5 mass % Al, 0.01 mass % to 1.5 mass % Fe and 0 mass % to 0.5 mass % Ti, with the remainder being Ni and unavoidable impurities.
[0075] The nickel alloy may further contain a total of 0.01 mass % to 0.7 mass % of rare earth elements. Examples of rare earth elements include Y and lanthanide elements (e.g., La, Ce, and Yb), and may contain one or two or more elements (the same applies to the nickel alloy forming the outer skin 12 described below).
[0076] In the nickel alloy having the above composition (1), Mn, Ti and rare earth elements are not essential. The specific resistance of the nickel alloy forming the core wire 11 is low because the number of essential elements as described above is small and the content of each element is slightly lower than that of the sheath 12 described below. In addition, since the nickel alloy contains the above elements within the above specific range, the oxidation resistance is also good to a certain extent.
[0077] The contents of the elements in the nickel alloy having the composition (1) may be as described below, while, for example, a decrease in specific resistance and improvements in thermal conductivity and oxidation resistance can be expected.
[0078] Si: 0.03 mass % to 1.3 mass %, further 0.05 mass % to 1.2 mass %
[0079] Mn: 0.01 mass % to 1.3 mass %, further 0.1 mass % to 1.2 mass % Cr: 0.001 mass % to 1.4 mass %, further 0.001 mass % to 1.3 mass %
[0080] Al: 0.001 mass % to 0.4 mass %, further 0.001 mass % to 0.3 mass %
[0081] Fe: 0.02 mass % to 1.3 mass %, further 0.03 mass % to 1.2 mass %
[0082] Ti: 0.01 mass % to 0.5 mass %, further 0.03 mass % to 0.3 mass %
[0083] Rare earth elements: 0.05 mass % to 0.68 mass % in total, further 0.08 mass % to 0.65 mass % in total
[0084] <Outer Skin>
[0085] The nickel alloy forming the sheath 12 contains Cr and Al as essential elements. The nickel alloy contains more than 50 mass %, typically 60 mass % or more Ni, and contains Ni as a main component, but the Ni content of the nickel alloy is lower than the Ni content of the nickel-based material forming the core wire 11.
[0086] Chromium (Cr) has an antioxidant effect, particularly an effect of suppressing internal oxidation, and is less likely to increase specific resistance than Al. Therefore, the Cr content of the nickel alloy forming the outer skin 12 is 10 mass % or more, and contains a slightly large amount of Cr. Chromium further has an effect of improving corrosion resistance. As the Cr content increases, oxidation resistance and corrosion resistance improve. The Cr content may be 12 mass % or more, and further may be 13 mass % or more and 14 mass % or more. When the Cr content is 30 mass % or less, the increase in specific resistance decreases.
[0087] As the Cr content decreases, the specific resistance is easily reduced. The Cr content may be 29% or less, further 28% or less, and 27% or less.
[0088] Aluminum (Al) is an element with a high antioxidant effect. In the case of containing Al, when the spark plug electrode composed of the electrode material 1 is used as a spark plug, an oxide (oxide film) containing Al is subsequently generated on the surface of the electrode. The oxide film easily inhibits oxidation to the inside of the electrode. When Si and Al are contained together, an oxide film containing Al and Si is easily formed, and the antioxidant effect can be further improved. When the Al content is 0.1% by mass or more, a high antioxidant effect is exhibited. As the Al content increases, the oxidation resistance increases. The Al content may be 0.2% by mass or more, and further 2.5% by mass or more. When the Al content is 6% by mass or less, the increase in resistivity and the peeling, damage, etc. of the oxide film caused by the increase in the thickness of the oxide film can be reduced, and the antioxidant effect caused by the presence of the oxide film is easily exhibited. As the Al content decreases, the resistivity is easily reduced, and (for example) the increase in the thickness of the oxide film is easily reduced. Therefore, the Al content may be 5.5% by mass or less, and further 5% by mass or less.
[0089] An example of the nickel alloy forming the outer skin 12 is a nickel alloy having the following composition (2).
[0090] Composition (2): The nickel alloy contains 0.1 mass % to 1.5 mass % Si, 0.1 mass % to 0.6 mass % Mn, 10 mass % to 30 mass % Cr, 0.1 mass % to 6 mass % Al, 0.01 mass % to 12 mass % Fe and 0.01 mass % to 0.6 mass % Ti, with the remainder being Ni and unavoidable impurities.
[0091] The nickel alloy may further contain 0.01 mass % or more and 0.7 mass % or less of rare earth elements in total.
[0092] In the nickel alloy having the composition (2), Si, Mn, Fe, and Ti are essential in addition to Cr and Al. The nickel alloy forming the sheath 12 contains an increased number of essential elements, and the amount of each element contained is slightly larger than that of each element in the core wire 11. Therefore, the nickel alloy has good oxidation resistance.
[0093] The contents of the elements in the nickel alloy having the composition (2) may be as described below, while, for example, a decrease in specific resistance and improvements in thermal conductivity and oxidation resistance can be expected.
[0094] Si: 0.15 mass % to 1.3 mass %, further 0.2 mass % to 1.2 mass %, Mn: 0.2 mass % to 0.55 mass %, further 0.3 mass % to 0.5 mass %, Fe: 0.02 mass % to 11.5 mass %, further 0.03 mass % to 11 mass %
[0095] Ti: 0.02 mass % to 0.55 mass %, further 0.03 mass % to 0.5 mass %
[0096] Rare earth elements: 0.1% to 0.65% by mass in total, further 0.2% to 0.6% by mass in total
[0097] <Effects of adding each element>
[0098] Silicon (Si) is an element with a high antioxidant effect and can improve oxidation resistance. As described above, silicon will then produce an oxide film and easily inhibit oxidation to the inside of the electrode. As the Si content increases, it is easy to obtain the antioxidant effect due to the formation of the oxide film. By setting the Si content to below the upper limit, the increase in resistivity and the peeling, damage, etc. of the oxide film caused by the increase in the thickness of the oxide film can be reduced.
[0099] Manganese (Mn) has an antioxidant effect, particularly an effect of inhibiting internal oxidation. When Mn is included in the above range, the oxidation resistance can be improved. As the Mn content increases, the oxidation resistance is easily improved. By setting the Mn content to below the upper limit, the increase in specific resistance can be reduced.
[0100] When Fe is included, hot workability is improved, thereby providing good manufacturability. As the Fe content increases, hot workability is easily improved. By setting the Fe content to below the upper limit, the increase in resistivity can be reduced, and the decrease in strength of the spark plug at operating temperature can be reduced.
[0101] Titanium (Ti) contained in the above range provides a crystal refining effect. The fine crystal structure can increase the total length of the grain boundary, easily suppress internal oxidation, and easily improve oxidation resistance. When the outer skin 12 is composed of a nickel alloy containing Ti, the outer skin 12 is likely to have a fine crystal structure, and the oxidation resistance is easily improved. In addition, because Ti suppresses the generation of Al nitride (AlN), the oxidation resistance is easily improved. This is because the damage to the oxide film caused by the generation of Al nitride in the oxide film can be suppressed, thereby easily maintaining the oxide film. As the Ti content increases, the oxidation resistance is easily improved. By setting the Ti content to below the upper limit, the increase in resistivity can be reduced.
[0102] The rare earth elements contained in the above range provide a crystal refining effect. As described above, internal oxidation is easily suppressed, and oxidation resistance is easily improved by reducing the grain size. When the outer skin 12 is composed of a nickel alloy containing rare earth elements, the outer skin 12 is likely to have a fine crystal structure, and oxidation resistance is easily improved. As the content of rare earth elements increases, oxidation resistance is easily improved. When the content of rare earth elements is below the upper limit, the increase in resistivity can be reduced, and the reduction in plastic workability is suppressed, thereby achieving good manufacturability of the composite material 10 and the electrode.
[0103] In addition to the above elements, the nickel-based material forming the core wire 11 and the nickel alloy forming the sheath 12 may contain carbon (C). The C content may be greater than 0 mass % and less than or equal to 0.1 mass %. When the C content is within the above range, the high temperature strength can be improved while suppressing the reduction of plastic workability. As the C content increases, the high temperature strength can be further improved. As the C content decreases, the plastic workability is improved, and the manufacturability of the composite material 10 and the electrode is also improved. The C content of the sheath 12 that needs to have high temperature strength may be 0.01 mass % or more and 0.09 mass % or less, and further 0.02 mass % or more and 0.08 mass % or less. When the C content of the nickel alloy forming the sheath 12 is higher than the C content of the core wire 11, the high temperature strength is easily improved. The C content of the core wire 11 may be 0.001 mass % or more and 0.09 mass % or less, and further 0.005 mass % or more and 0.08 mass % or less.
[0104] (structure)
[0105] The nickel-based material forming the core wire 11 and the nickel alloy forming the sheath 12 generally each have a crystal structure. For the sheath 12, as the grain size decreases, the total length of the grain boundary increases, and it becomes difficult for oxygen to enter the inside, so the oxidation resistance is easily improved, wherein the sheath 12 is arranged on the outside, and in the use state of the electrode for the spark plug composed of the electrode material 1 according to the embodiment, the sheath 12 is exposed to the external environment. On the contrary, for the core wire 11 arranged on the inside of the sheath 12 in the above-mentioned use state, as the grain size increases, the electrical conductivity becomes better, thereby easily reducing the specific resistance, and the thermal conductivity also becomes better to provide better heat dissipation ability, and heat is not easy to accumulate inside. In this embodiment of the electrode material 1, the ratio of the grain size of the nickel-based material forming the core wire 11 to the grain size of the nickel alloy forming the sheath 12 (core wire / sheath) is 5 or more. When the ratio of the grain size (core wire / sheath) is 5 or more, the nickel-based material forming the core wire 11 has a relatively large grain size so that the specific resistance is easily reduced, and further, the nickel alloy forming the sheath 12 has a relatively small grain size so that good oxidation resistance is provided. As the ratio of the grain size (core wire / sheath) increases, for example, when the ratio is greater than 5, further 6 or more, 7 or more, and 8 or more, the specific resistance is more easily reduced, and the oxidation resistance is more easily improved. By adjusting not only the composition of the core wire 11 and the sheath 12, but also the structure of the core wire 11 and the sheath 12, it is possible to obtain an electrode material 1 having higher spark wear resistance and higher oxidation resistance.
[0106] The crystal grain size of the nickel-based material forming the core wire 11 is, for example, about 50 μm to about 500 μm, and further about 100 μm to about 400 μm. The crystal grain size of the nickel alloy forming the sheath 12 is, for example, about 10 μm to about 100 μm, and about 20 μm to about 60 μm.
[0107] Examples of methods for adjusting the grain size include adjusting the above composition and adjusting the heat treatment conditions during the manufacturing process. For example, the introduction of an element having a crystal refining effect (such as Ti or a rare earth element) is likely to reduce the grain size, but this depends on the manufacturing conditions. Alternatively, for example, in the case of heat treatment during the manufacturing process, the grain size is likely to be reduced by setting the heat treatment temperature to a slightly lower temperature, but this depends on the composition.
[0108] (State of the interface)
[0109] The inventors of the present invention have found that when a diffusion layer 13 in which the Ni content changes in a gradient manner is included between the core wire 11 and the sheath 12, the adhesion is further improved. Typically, the diffusion layer 13 is a region in which the Ni content decreases from the core wire 11 to the sheath 12 compared to the nickel-based material forming the core wire 11, and the Ni content increases from the sheath 12 to the core wire 11 compared to the nickel alloy forming the sheath 12. The region in which the Ni concentration changes in a gradient manner is generated by diffusing the components constituting the core wire 11 and the sheath 12 near the interface between the core wire 11 and the sheath 12. Herein, this region is referred to as the diffusion layer 13.
[0110] The composition of the diffusion layer 13 is different from the composition of the nickel-based material forming the core wire 11, and is different from the composition of the nickel alloy forming the outer skin 12. Therefore, the diffusion layer 13 can be determined as follows: the composition of the composite material 10 is analyzed by an appropriate method, the composition near the above-mentioned interface, the composition of the central part of the core wire 11, and the composition on the surface side of the outer skin 12 are compared, and the area with different Ni contents is extracted as the diffusion layer. The "composition of the central part of the core wire 11" may be the composition at the center of gravity of the contour shape of the core wire 11. For example, when the contour of the core wire 11 is as follows Figure 1 When the composite material 10 is a rectangle as shown, the composition near the intersection of the diagonal lines of the rectangle can be defined as "the composition of the central part of the core wire 11". The composition of the surface side of the outer skin 12 can be, for example, a composition located at a position from the outermost surface of the outer skin 12 to about 20% of the thickness of the outer skin 12. An example of a simple method for extracting the diffusion layer 13 is as follows. A cross section of the composite material 10 is prepared, and an area near the interface between the core wire 11 and the outer skin 12 is observed with a microscope. Due to the different compositions, the colors presented by the diffusion layer 13, the core wire 11, and the outer skin 12 are different from each other. The area with different colors located between the core wire 11 and the outer skin 12 is extracted as the diffusion layer 13.
[0111] The diffusion layer 13 generally exists in a tubular shape along the interface between the core wire 11 and the outer skin 12. When the average thickness t of the diffusion layer 13 13 When the average thickness is greater than 1 μm, the adhesion is improved. 13 When the average thickness t is 1.2 μm or more, and further 1.5 μm or more, the adhesion is further improved. 13 When the thickness is about 10 μm or less, and further about 8 μm or less, the reduction of the core 11 and the outer skin 12 due to the formation of the diffusion layer 13 can be reduced. The average thickness t can be determined by extracting the diffusion layer 13 on the cross section of the composite material 10, determining five or more measurement points of the diffusion layer 13 at equal intervals along the circumferential direction of the core 11, and calculating the average value of the thickness at these measurement points. 13 .
[0112] In order to form the diffusion layer 13, for example, processing conditions, heat treatment conditions, etc. may be adjusted during the manufacturing process. The details of the manufacturing conditions will be described below.
[0113] (Specific resistance)
[0114] In the electrode material 1 according to the embodiment, the specific resistance of the composite material 10 at room temperature (generally about 20° C.) is less than 50 μΩ·cm. As the specific resistance of the composite material 10 decreases, that is, to 48 μΩ·cm or less, further to 46 μΩ·cm or less, particularly to 30 μΩ·cm or less, 25 μΩ·cm or less, 20 μΩ·cm or less, and 15 μΩ·cm or less, higher spark wear resistance is provided.
[0115] Although the composite material 10 includes a skin 12 with a slightly higher specific resistance, as described above, because the composite material 10 also includes a core wire 11 with a slightly lower specific resistance, the composite material 10 has a low specific resistance as a whole. The specific resistance of the composite material 10 is changed by the composition of the core wire 11, the composition of the skin 12, the ratio of the grain size (core wire / skin), the skin ratio described below, etc. In the electrode material 1 according to the embodiment, the composition, ratio, skin ratio, etc. are adjusted so that the specific resistance of the composite material 10 satisfies less than 50μΩ·cm. For example, by using a nickel-based material with a higher Ni content as the core wire 11, increasing the ratio (core wire / skin) to a certain extent, or further reducing the skin ratio, it is easy to reduce the specific resistance.
[0116] (Skin Ratio)
[0117] As described above, the ratio of the sheath 12 to the core wire 11 in the composite material 10 can be adjusted within the range where the resistivity of the composite material 10 satisfies less than 50 μΩ·cm. In the embodiment of the electrode material 1, in the cross section of the composite material 10, the area ratio of the cross-sectional area of the sheath 12 to the cross-sectional area of the composite material 10 (skin ratio) is 0.4 or more and 0.7 or less. When the skin ratio is 0.4 or more, the reduction in oxidation resistance due to the excessively high ratio of the core wire 11 can be suppressed, and the oxidation resistance is easily improved. As the ratio of the sheath 12 increases, that is, when the skin ratio is 0.45 or more, and further 0.5 or more, the oxidation resistance is further improved. When the skin ratio is 0.7 or less, the increase in resistivity due to the excessively high ratio of the sheath 12 can be suppressed, and the resistivity is easily reduced. As the ratio of the sheath 12 decreases, that is, when the skin ratio is 0.65 or less, and further 0.6 or less, the resistivity is more easily reduced.
[0118] During the manufacturing process, the ratio of the thickness of the material that will eventually serve as the sheath 12 to the thickness of the material that will eventually serve as the core wire 11 may be adjusted, or the processing conditions may be adjusted so that the sheath ratio is within a predetermined range. Note that the sheath ratio is selected within a range where the resistivity of the composite material 10 satisfies less than 50 μΩ·cm, depending on the composition of the material.
[0119] (Shape and size)
[0120] Examples of the electrode material 1 according to the embodiment include square wires having a rectangular cross-sectional shape ( Figure 1 ) and a round wire having a circular cross-sectional shape. The outer shape of the electrode material 1 (which is the outer shape of the composite material 10 and also the outer shape of the outer skin 12) can be appropriately changed by performing plastic processing such as wire drawing and rolling on the electrode material 1 during the manufacturing process. When the outer skin 12 is a tubular shape having a uniform thickness in its circumferential direction, the core wire 11 has a cross-sectional shape similar to the outer shape of the electrode material 1.
[0121] The size (such as cross-sectional area or wire diameter) of the electrode material 1 may be appropriately selected. When the electrode material 1 is a square wire, the thickness t of the electrode material 1 may be about 1 mm or more and about 3 mm or less, and the width w may be about 2 mm or more and about 4 mm or less. When the electrode material 1 is a round wire, the wire diameter of the electrode material 1 may be about 2 mm or more and about 6 mm or less. The size of the core wire 11 (same as above) and the thickness of the sheath 12 may be within the range corresponding to the above-mentioned sheath ratio.
[0122] In the electrode material 1 according to the embodiment, the core wire 11 is exposed at the end surface of the electrode material 1. Figure 2 As shown, by using such an electrode material 1, an electrode 20 in which the core wire 11 is exposed from the end surface 20e can be formed.
[0123] (Method for producing electrode material)
[0124] For example, the following embedding method can be used to manufacture the electrode material 1 according to the embodiment. The embedding method used in this article refers to a method comprising: preparing a raw material wire that will eventually serve as the core wire 11, and performing plastic processing such as wire drawing and rolling in a state where the outer skin raw material that will eventually serve as the outer skin 12 is embedded in the raw material wire. An example of the embedding method includes the following preparation steps, embedding steps, and processing steps. When the method further includes a heat treatment step for performing heat treatment after the processing step, a composite material 10 including the above-mentioned diffusion layer 13 can be manufactured.
[0125] (Preparation Step) A step of arranging a sheath raw material around a raw material wire to prepare a preliminary material in which the outer periphery of the raw material wire is covered with the sheath raw material.
[0126] (Fitting Step) A step of performing plastic working on the preliminary material to fasten the preliminary material, thereby producing a fitting material in which the sheath raw material is fitted on the outer periphery of the raw material wire.
[0127] (Processing Step) A step of plastically processing the fitting material so as to have a predetermined size and a predetermined shape, thereby producing a processed material including the core wire 11 and the sheath 12 provided on the outer periphery of the core wire 11.
[0128] Hereinafter, each step will be described.
[0129] <Preparation steps>
[0130] In this step, a raw wire material and a sheath material having a predetermined composition (which has been described in the section of the composition of the core wire 11 and the sheath 12) are prepared. Materials in various forms such as strips, sheets, wires, and tubes can be used as the sheath material. The wire material forming the raw wire material and the sheath material can be manufactured by, for example, melting → casting → hot working (such as rolling, forging, and extrusion) → cold working (such as wire drawing and rolling) and then optionally performing heat treatment. For the manufacture of the raw wire material and the sheath material, reference can be made to a known method for manufacturing a metal wire material, a metal plate material, a metal sheet material, or a metal tube material.
[0131] Examples of a method for arranging the sheath raw material on the outer periphery of the raw material wire material include the following method.
[0132] (a) A strip, sheet or wire of a sheath material is wound around a raw material wire.
[0133] (b) The raw material wire is inserted and arranged in the tube forming the outer sheath raw material.
[0134] (c) The wire material forming the sheath material is arranged around the raw material wire material in the axial direction so as to extend longitudinally.
[0135] After the sheath material is arranged on the periphery of the raw material wire, the edges of the plurality of wires, sheets, etc. forming the sheath material can be joined to each other, or the raw material wire and the sheath material, etc. can be joined to each other by a connection method such as welding or soldering as needed. In this case, misalignment between the raw material wire and the sheath material is less likely to occur, and the subsequent fitting step is easy to perform.
[0136] When manufacturing the raw material wire and the sheath raw material, for example, the atmosphere during melting and casting can be a low oxygen atmosphere having an oxygen concentration lower than that of the air atmosphere (for example, an oxygen concentration of 10% by volume or less). In this case, oxidation of the raw materials, particularly rare earth elements, can be easily suppressed.
[0137] In addition, by performing rolling as cold working after wire drawing, the outer shape of the drawn wire material can be changed from a round wire to a square wire or the like, for example.
[0138] When heat treatment is performed after cold working, the workability of the obtained heat-treated material is improved, so it is easy to perform plastic working in the subsequent processing step. As the conditions of this heat treatment, known conditions (for example, Patent Document 1) can be referred to.
[0139] In addition, the shape and size (such as external dimensions and thickness) of the raw material wire and the outer skin raw material can be selected according to the cross-sectional shape of the composite material 10, the degree of processing and processing state in subsequent processing steps, etc., so as to obtain a composite material 10 that meets the final shape, final external dimensions and a predetermined outer skin ratio.
[0140] <Matching Steps>
[0141] In the fitting step, the preparation material, in particular the outer skin raw material, is tightened from the outside of the preparation material so that the raw material wire and the outer skin raw material are integrated, thereby manufacturing the fitting material. Plastic processing such as wire drawing and rolling can be used for tightening. In this article, plastic processing can be a process in which the outer skin raw material is tightened to the extent that the outer skin raw material can be in close contact with the raw material wire. For example, the plastic processing can be a process in which the processing degree (area reduction rate) of each processing is relatively high, specifically, it can be a process in which the area reduction rate is greater than 20%.
[0142] <Processing steps>
[0143] In the processing step, the integrated chimeric material is subjected to plastic processing such as wire drawing and rolling, so that the raw wire material and the sheath raw material are formed into a core wire 11 and a sheath 12 having a predetermined shape and a predetermined size, respectively. The plastic processing may be cold processing. In the processing step, the processing may be repeatedly performed until the final shape and the final size are obtained. In this case, the method may optionally include an intermediate heat treatment step, in which heat treatment is performed between processing and processing. The object to be processed is softened by the intermediate heat treatment, and subsequent processing can be easily performed.
[0144] <Heat treatment step>
[0145] In this step, the processed material manufactured in the processing step is heat-treated to form the above-mentioned diffusion layer 13 near the interface between the core wire 11 and the sheath 12. As described above, the formation of the diffusion layer 13 further improves the adhesion between the core wire 11 and the sheath 12. The heat treatment conditions depend on the composition of the core wire 11, the composition of the sheath 12, the degree of processing, etc. However, the heating temperature may be from about 150°C to about 1,200°C, and the heating time may be from about 1 second to about 20 hours. Although the heat treatment conditions depend on the composition, degree of processing, etc. of the core wire 11 and the sheath 12, in the case where the heating temperature is a relatively low temperature of, for example, about 150°C, the heating time can be made slightly longer within the above range, and in the case where the heating temperature is a relatively high temperature of, for example, about 1,200°C, the heating time can be made slightly shorter within the above range. Although these conditions depend on the composition, degree of processing, etc. of the core wire 11 and the sheath 12, under the condition that the degree of processing is increased to a certain extent and the heating temperature is set at a slightly lower temperature within the above range, or under the condition that the degree of processing is reduced to a certain extent and the heating temperature is set at a slightly higher temperature within the above range, it is easy to form a diffusion layer 13 with an average thickness greater than 1 μm. In addition, it is also expected that the heat treatment can provide an effect of reducing the specific resistance of the composite material 10 (improving spark wear resistance) by eliminating the processing strain introduced in the processing step, and provide an effect of making the material easy to process into an electrode 20 having a predetermined shape (improving processability). In addition, the size of the crystal grains can be adjusted to a certain extent by the above-mentioned heat treatment conditions. Although the crystal grain size depends on the composition, degree of processing, etc., when the heating temperature is set to a slightly lower temperature, the crystal grain size tends to be easily reduced. In the case where the composite material 10 includes a core wire 11 having a composition (1) and a sheath 12 having a composition (2), and in the case where the composition (1) and the composition (2) further contain a rare earth element within the above range, the heating temperature can be 800°C or higher, and further 850°C or higher and 1,200°C or lower (refer to Test Example 1).
[0146] (use)
[0147] The electrode material 1 according to the present embodiment can be used as a material of an electrode included in a spark plug 2 used in an engine of an automobile such as a four-wheel vehicle or a motorcycle, for example.
[0148] (Main Advantages)
[0149] Due to the presence of the core wire 11 composed of a nickel-based material having a high Ni content, the electrode material 1 according to the embodiment has low specific resistance and good spark wear resistance, and due to the presence of the outer skin 12 composed of a nickel alloy containing Cr and Al within a specific range, the electrode material 1 according to the embodiment also has good oxidation resistance. The outer peripheral surface of the core wire 11 is covered with the outer skin 12, so that in the core wire 11, only the end face is a region substantially exposed to the external environment, so the electrode material 1 has a structure that is easy to suppress oxidation of the core wire 11. This also makes the electrode material 1 according to the embodiment have good oxidation resistance. Because the core wire 11 and the outer skin 12 contain a common main component (Ni), the core wire 11 and the outer skin 12 can be closely attached to each other, and oxidation is not easy to proceed from the end face of the electrode material 1 along the interface between the core wire 11 and the outer skin 12 to the inside of the electrode material 1. This also makes the electrode material 1 according to the embodiment have good oxidation resistance. These advantages will be specifically described in the following Test Example 1.
[0150] In addition, the electrode material 1 according to the embodiment includes the core wire 11 having a high Ni content and good thermal conductivity, the core wire 11 is exposed at the end surface of the electrode material 1 to uniformly conduct heat over the entire length of the electrode material 1, and the electrode material 1 has good heat dissipation capability. Therefore, heat is not easily accumulated inside the electrode material 1, and (for example) it is also possible to reduce the reduction in high temperature strength.
[0151] [Electrode for spark plug]
[0152] The electrode 20 according to the embodiment is used as Figure 2 In the spark plug 2 shown, the electrode 20 is composed of the electrode material 1 according to the above embodiment. Since the electrode 20 substantially maintains the characteristics such as the composition, structure and specific resistance of the electrode material 1, the electrode 20 has a low specific resistance of less than 50 μΩ·cm, good spark wear resistance and good oxidation resistance.
[0153] In the electrode 20 according to the embodiment, both the core wire 11 and the outer skin 12 are usually exposed at the end face 20e. Because the electrode 20 is composed of the electrode material 1 according to the embodiment (including the above-mentioned specific composite material 10), although the core wire 11 is exposed at the end face 20e, the electrode 20 still has good oxidation resistance and good corrosion resistance. This is because, as described above, the adhesion between the core wire 11 and the outer skin 12 is good, so it is easy to suppress oxidation and corrosion from the end face 20e of the electrode 20 along the interface between the core wire 11 and the outer skin 12 to the inside of the electrode 20. In the case where the electrode 20 includes a diffusion layer 13, the progress of oxidation and corrosion is further suppressed. In addition, because the core wire 11 is exposed at the end face 20e of the electrode 20, heat can be uniformly conducted over the entire length of the electrode 20 from the end face 20e of the electrode 20, and the electrode 20 also has good heat dissipation capabilities. In this article, as described above, the core wire 11 has a high Ni content. Therefore, when the core wire 11 is excessively kept at a high temperature, the core wire 11 may soften and deform, such as bend. Since the electrode 20 has good heat dissipation capability and heat is not easily accumulated, softening and deformation can be prevented. The electrode 20 includes the sheath 12 having good high temperature strength. Therefore, even if the core wire 11 softens, the sheath 12 can prevent the electrode 20 from deforming.
[0154] The electrode 20 according to the embodiment can be manufactured by cutting the electrode material 1 according to the embodiment to have an appropriate length and forming the cut wire into a predetermined shape. The electrode 20 according to the embodiment composed of the electrode material 1 according to the embodiment can be used as the center electrode 21 or the ground electrode 22, or as both. Figure 2 An example of a ground electrode 22 composed of the electrode material 1 according to this embodiment is shown. The ground electrode 22 is easily exposed to, for example, high-temperature gas compared to the center electrode 21. Therefore, the electrode material 1 according to the embodiment is suitable for the material of the ground electrode 22.
[0155] [spark plug]
[0156] The spark plug 2 according to the embodiment is included in an engine of an automobile or the like and is used for ignition of, for example, a fuel mixed gas, and includes the electrode 20 according to the embodiment. The spark plug 2 generally includes a rod-shaped center electrode 21, an insulator 25 that holds the center electrode 21 in a state where the front end of the center electrode 21 protrudes, a metal shell 26 that holds the insulator 25 in a state where the front end of the insulator 25 protrudes, and an L-shaped ground electrode 22 joined to the end surface of the metal shell 26 by welding or the like. One end of the ground electrode 22 is joined to the metal shell 26, and a region of the other end of the ground electrode 22 is bent so as to be opposed to the end surface of the center electrode 21. Spark discharge is generated between the ground electrode 22 and the center electrode 21. Ignition is performed by this discharge.
[0157] Since the spark plug 2 according to the embodiment includes the electrode 20 composed of the electrode material 1 according to the above embodiment, the spark plug 2 has both good spark wear resistance and good oxidation resistance. In addition, the spark plug 2 has good corrosion resistance and good heat dissipation capability as described above.
[0158] [Test Example 1]
[0159] Electrode materials having various compositions and structures were produced, and the characteristics of the electrode materials were evaluated.
[0160] Samples No. 1-1 to 1-18 are wires each formed of a composite material having a double-layer structure, the composite material comprising a core wire and a sheath covering the outer peripheral surface of the core wire. Each wire is manufactured by the above-mentioned embedding method. In general, a raw material wire as a core wire and a sheath raw material as a sheath are prepared, the sheath raw material is embedded on the periphery of the raw material wire, and then cold working (in this article, cold working is wire drawing and rolling) is performed. After the cold working, heat treatment is performed.
[0161] Sample Nos. 1-101 and 1-102 are each formed of a single wire composed of a nickel alloy having a composition shown in Table 1, rather than a composite material having a double-layer structure.
[0162] Each of the raw material wire rod, sheath raw material and single wire described above is manufactured through the steps of melting → casting → hot working → cold working, and optionally heat treatment thereafter.
[0163] Herein, a molten metal of a nickel alloy (sheath or single wire) having a composition shown in Table 1 and a molten metal of a nickel-based material (core wire) having a composition shown in Table 2 are prepared by using a typical vacuum melting furnace. Commercially available pure Ni and particles of various additive elements can be used as raw materials for the molten metal. The molten metal is refined to reduce or remove impurities and inclusions. Herein, the degree of refining is adjusted so that the C (carbon) content reaches the amount shown in Table 1 or Table 2.
[0164] The composition is expressed in mass %.
[0165] In the table, "BAL." represents the balance, and the balance herein is Ni and inevitable impurities.
[0166] In the table, "rare earth" means a rare earth element. Compositions containing only Y or containing Y and Yb are shown herein.
[0167]
Table 1
[0168]
[0169]
Table 2
[0170]
[0171] The outer skin raw material is arranged around the obtained raw material wire, and plastic processing is performed to fasten the outer skin raw material and the raw material wire, thereby producing an integrated chimeric material, and the chimeric material is cold processed. As a cold processing, cold rolling is performed here after cold drawing. The processing degree of cold drawing is selected so that the double-layer structure drawn wire obtained after the cold drawing process becomes a round wire with an outer diameter of 1mmφ to 3mmφ. The processing degree of cold rolling is selected so that the round wire becomes a square wire with an outer dimension of 0.5mm to 2.0mm in width and 1.5mm to 3.0mm in length. The size, processing degree, etc. of the raw material wire and the outer skin raw material produced are adjusted so that for the double-layer structure composite material finally produced and including the core wire and the outer skin, in the cross-section of the double-layer structure composite material, the area ratio of the cross-sectional area of the outer skin to the cross-sectional area of the composite material and the area ratio of the cross-sectional area of the core wire to the cross-sectional area of the composite material are the cross-sectional area ratios shown in Table 2.
[0172] The square wire was subjected to final heat treatment, and the resulting heat-treated material was used as a sample of an electrode material. In the final heat treatment of Samples No. 1-1 to 1-18 and 1-111 in Table 3, the heating temperature was selected from the range of 800° C. to 1,200° C., and the retention time was selected from the range of one second to two hours. The atmosphere was a nitrogen atmosphere or a hydrogen atmosphere.
[0173] In Table 3, Samples No.1-1, 1-111 and 1-112 are samples using raw wires and sheath raw materials having the same composition and the same size, and only the conditions of the final heat treatment are changed. Samples No.1-2 and 1-6 are samples whose conditions of the final heat treatment are different from those of Sample No.1-1. In this article, the retention time is the same, and the heating temperature is changed. More specifically, assuming that the heating temperature of Sample No.1-1 is standard, the heating temperature of Sample No.1-111 is the lowest (below 850°C in this article), the heating temperature of Sample No.1-6 is reduced to a certain extent (above 850°C in this article), and the heating temperature of Sample No.1-2 is increased to a certain extent. The heating temperature of No.1-112 is the highest and is outside the above-mentioned heating temperature range (above 1200°C and below 1300°C). The conditions of the final heat treatment in Sample No.1-4 are the same as those of Sample No.1-1.
[0174] <Composition>
[0175] The composition of the electrode material of the sample was detected by using an inductively coupled plasma (ICP) atomic emission spectrometer. According to the results, the composition is the same as that shown in Tables 1 and 2, and the electrode material contains the elements shown in Tables 1 and 2, and the balance is composed of Ni and unavoidable impurities. In the electrode materials of each sample No. 1-1 to 1-18, 1-111 and 1-112, the Ni content of the core wire is more than 96% by mass. In Tables 1 and 2, "- (hyphen)" or "0" means that the content is less than the detection limit and the element is substantially not contained. For composition analysis, for example, atomic absorption spectrophotometry can be used.
[0176] <Structure>
[0177] For the electrode material of each sample, the ratio of the grain size of the nickel-based material forming the core wire to the grain size of the nickel alloy forming the outer skin (core wire / outer skin) was detected. Table 3 shows the results. In this article, the cross section of the sample was observed with an optical microscope. For the obtained microscopic observation image, the average grain size of the core wire and the average grain size of the outer skin were determined by using the intersection method (straight line method). In this article, the observation magnification, etc. are adjusted so that the number of grains cut by one measuring line is more than 10. For each core wire and outer skin, more than five measuring lines are drawn on a cross section, a total of more than 50 grains are extracted, and the average value of the grain size is determined. The average grain size of the core wire / the average grain size of the outer skin is determined as the ratio of the grain size (core wire / outer skin). Table 3 shows the measurement results of some samples.
[0178] When the ratio (core wire / sheath) of the electrode material is less than 5, the ratio is small, and both the core wire and the sheath are considered to have a coarse crystal structure, etc., and the electrode material is evaluated as B. When the ratio (core wire / sheath) of the electrode material is 5 or more and less than 10, the ratio is large, and the core wire is considered to have a relatively large crystal structure, and the sheath has a relatively fine crystal structure, and the electrode material is evaluated as G. When the ratio (core wire / sheath) of the electrode material is 10 or more, the ratio is larger, and the core wire is considered to have a relatively larger crystal structure, and the sheath has a relatively finer crystal structure, and the electrode material is evaluated as VG. The evaluation results are also shown in Table 3. In this test, in each of the electrode materials of Samples No. 1-1 to 1-18, the grain size of the core wire is about 50 μm or more and about 500 μm or less, and the grain size of the sheath is about 10 μm or more and about 100 μm or less.
[0179] For the electrode material of each sample, a cross section was prepared, and the cross section was observed with a scanning electron microscope (SEM) to detect the average thickness (μm) of the diffusion layer present between the core wire and the outer skin. Table 3 shows the results. In this article, in the SEM observation image, the area between the core wire and the outer skin and whose color is different from the color of the core wire and the outer skin is defined as the diffusion layer. In the SEM observation image, five or more measurement points are determined at equal intervals along the circumferential direction of the core wire, and the thickness of the diffusion layer at each measurement point is determined, and the average value of these thicknesses is defined as the average thickness of the diffusion layer. Table 3 shows the measurement results of some samples.
[0180] For the regions showing different colors, elemental analysis was performed using, for example, an energy dispersive X-ray spectrometer (EDX) connected to a SEM, and the results showed that the Ni content changed in a gradient manner from the core side to the sheath side. The diffusion layer was extracted by elemental analysis, so that the thickness of the diffusion layer could be measured with high accuracy. The use of SEM observation images can simply and easily measure the thickness of the diffusion layer.
[0181] <Specific resistance>
[0182] The specific resistance (μΩ·cm) of the electrode material of each sample was measured. The results are shown in Table 3. The specific resistance (room temperature) was measured by a DC four-terminal method using a resistance measuring device. Here, the gauge length GL was 100 mm.
[0183] <Spark wear resistance>
[0184] Among the electrode materials of the samples, the electrode materials having a specific resistance (room temperature) of 50 μΩ·cm or more were considered to have poor spark wear resistance and were rated as B. The electrode materials having a specific resistance of less than 50 μΩ·cm were considered to have good spark wear resistance and were rated as G. The electrode materials having a specific resistance of less than 30 μΩ·cm were considered to have very good spark wear resistance and were rated as VG. The evaluation results are also shown in Table 3.
[0185] <Antioxidant Properties>
[0186] The electrode material of each sample was subjected to the following thermal cycle test, and the mass change before and after the test was detected. Table 3 shows the results. In this article, the mass change (%) is determined as ((W1-W0) / W0)×100, where W0 represents the mass of the sample before the thermal cycle test, and W1 represents the mass of the sample after the thermal cycle test. When the sign of the mass change is negative (-), the result means that the mass after the test is reduced. When the sign of the mass change is positive (only numerical values are described in Table 3), the result means that the mass after the test is increased.
[0187] <<Thermal Cycle Test>>
[0188] A thermal cycle of heating at 1100° C. for 30 minutes and then cooling at room temperature for 30 minutes was defined as one cycle, and this cycle was repeated 100 times.
[0189] When the change in mass is a decrease (when the sign of the change is negative), it is considered that (for example) an oxide film is excessively formed and the oxide film is detached. This electrode material is considered to have poor oxidation resistance and is rated as B. When the change in mass is an increase of more than 5% and less than or equal to 10%, it is considered that an oxide film is properly formed. This electrode material is considered to have good oxidation resistance and is rated as G. When the mass change is 0% or more and less than 5%, it is considered that an oxide film is more properly formed. This electrode material is considered to have very good oxidation resistance and is rated as VG. The evaluation results are also shown in Table 3.
[0190] <Adhesion>
[0191] The above-mentioned thermal cycle test was performed on the electrode material of each sample, and the degree of oxidation along the interface between the core wire and the outer skin was detected. Table 3 shows the results. Figure 3 As shown, a square wire was prepared as a sample S, and the above-mentioned thermal cycle test (100 cycles) was performed, wherein the square wire was the electrode material of each sample, and in the square wire, the core wire 11 and the sheath 12 were exposed at the end face of the square wire, and the outer peripheral face of the core wire 11 was covered with the sheath 12. Subsequently, the length of the oxide formed along the interface between the core wire 11 and the sheath 12 from the end face of the sample S was measured.
[0192] Here, after the thermal cycle test, a plane parallel to the axial direction of the core wire 11 is obtained in the sample S (see Figure 3 The longitudinal section obtained by cutting along the cutting plane line aa in the figure was observed by SEM. The length of the oxide along the interface (oxidation progress length, μm) was measured on the SEM observation image. The results are shown in Table 3. Figure 4 A SEM observation image of sample No. 1-1 is shown. Figure 5 The SEM observation image of sample No.1-111 is shown. Figure 4 and 5In the SEM observation image shown, the region between the core wire 11 and the sheath 12 and showing a color different from the colors of the core wire 11 and the sheath 12 is defined as an oxide 15. With regard to the above inclusions, it can be identified as an oxide by performing elemental analysis using, for example, the above SEM-EDX spectrometer. By extracting the oxide by elemental analysis, the length of the oxide can be measured with higher accuracy. The use of the SEM observation image can simply and easily measure the length of the oxide. An observation image obtained by a metallographic microscope can be used instead of the SEM observation image for the measurement of the length of the oxide. A metallographic microscope can also be used to confirm the color difference between the core wire and the sheath.
[0193] When the length of the oxide is 500 μm or more, it is considered that the adhesion between the core wire and the sheath is poor, and the area near the interface is easily oxidized, and this electrode material is rated as B. When the length of the oxide is less than 500 μm, the adhesion between the core wire and the sheath is considered to be good, and this electrode material is rated as G. When the length of the oxide is less than 100 μm, the adhesion between the core wire and the sheath is considered to be very good, and this electrode material is rated as VG. The evaluation results are also shown in Table 3.
[0194] <Overall Evaluation>
[0195] In the above evaluation, when the result includes at least one B, the durability characteristics are considered to be poor, and this electrode material is rated as B. When the result does not include B, and includes VG and G, the durability characteristics are considered to be good, and this electrode material is rated as G. When the results of all items are VG, the durability characteristics are considered to be very good, and this electrode material is rated as VG. This comprehensive evaluation is also shown in Table 3.
[0196]
Table 3
[0197] Table 3 shows that the electrode materials of each sample No. 1-1 to 1-18 formed of a composite material including a core wire and a sheath (hereinafter, may be referred to as a composite material sample group) have both good spark wear resistance and good oxidation resistance compared to each sample No. 1-101 and 1-102 formed of a single wire. Herein, the composite material sample group has good spark wear resistance due to low specific resistance, and has good oxidation resistance due to small mass change (increase) after thermal cycle test.
[0198] One reason why the above results are obtained is considered to be as follows.
[0199] Sample No. 1-101 formed of a single wire with a high Ni content has a low specific resistivity, but the mass changes greatly, so the oxidation resistance is poor. Sample No. 1-102 is formed of a single wire composed of a nickel alloy with a slightly higher Cr content. The mass of Sample No. 1-102 has basically not changed and has good oxidation resistance, but has an extremely high specific resistivity. That is, it is difficult for a single wire to have both good spark wear resistance and good oxidation resistance. In contrast, the composite material sample group includes a composite material including a core wire with a high Ni content and a sheath composed of a nickel alloy containing a specific range of Cr and Al. Therefore, it is believed that the specific resistivity can be reduced by the core wire and the oxidation resistance can be improved by the sheath.
[0200] exist Figure 4 In the SEM observation image of sample No. 1-1, the gray area on the lower right side is the core wire 11, the central band-shaped gray area is the outer skin 12, the dark gray area is the oxide 15, and the black area on the left is the background (the same applies to the following Figure 5 SEM observation image of sample No.1-111). Figure 4 As shown, on the surface of the sheath 12, there is only a dark gray area with a very small thickness. This indicates that the sheath 12 is not easily oxidized and has good oxidation resistance. On the contrary, in the portion of the core wire 11 exposed from the sheath 12, there is a dark gray area with a certain degree of thickness. This indicates that oxidation is likely to occur at a high Ni content.
[0201] In addition, the composite material sample group contains a common main component of the core wire (Ni) and a main component of the sheath (Ni), and has good adhesion between the core wire and the sheath. This is also considered to be the reason for improving the oxidation resistance. Figure 4 and 5 Describe the adhesion. Figure 4 As shown in the SEM observation image of , in sample No. 1-1, although the oxide 15 is formed along the interface between the core wire 11 and the outer skin 12 from the end face of the electrode material, the formation length of the oxide 15 from the end face is short, specifically, it is less than 300 μm. The short formation length of the oxide 15 is one basis for proving the good adhesion between the core wire 11 and the outer skin 12. On the contrary, Figure 5As shown in the SEM observation image in, in sample No. 1-111, the formation length of oxide 15 is relatively long, specifically, more than 500 μm. This shows that in sample No. 1-111, the core wire 11 and the sheath 12 are not sufficiently close to each other, and oxygen and the like easily enter through the interface from the end faces of the core wire 11 and the sheath 12. In this electrode material, oxygen and the like enter from the interface between the core wire and the sheath over time, forming oxides, and thus the core wire and the sheath are separated from each other. It is presumed that it is therefore difficult to fully obtain the effects brought about by the presence of the core wire and the sheath. Therefore, in order to satisfactorily obtain the effects of exhibiting both good spark wear resistance and good oxidation resistance for a long time, it is preferred to improve the adhesion between the core wire and the sheath.
[0202] Furthermore, this experiment showed the following conclusions.
[0203] (1) Even when the composition of the sheath is the same and the sheath ratio is the same, the spark wear resistance and oxidation resistance can be changed by changing the composition of the core wire (for example, refer to Samples No. 1-1 to 1-3 and compare them, and refer to Samples No. 1-8 and 1-9 and compare them).
[0204] (2) When the rare earth element is contained in at least one of the core wire and the sheath, particularly in the core wire, the change in mass (increased amount) is small, and the oxidation resistance tends to improve (for example, refer to Sample Nos. 1-4 and 1-5 and compare therebetween, and refer to Samples Nos. 1-10 to 1-12 and compare therebetween). As the content of the rare earth element increases, the oxidation resistance tends to improve (for example, refer to Sample Nos. 1-11 and 1-12 and compare therebetween).
[0205] (3) As the skin ratio increases, the change in mass (increase amount) is small, and the antioxidant property tends to improve (for example, refer to samples No. 1-1, 1-4 and 1-6 and compare with samples No. 1-10, 1-13 and 1-15, refer to samples No. 1-8 and 1-17, and compare with each other, and refer to samples No. 1-9 and 1-18).
[0206] (4) When the ratio of the grain size (core / sheath) is large, the specific resistance tends to decrease easily (for example, refer to Sample No. 1-1 and 1-2 and compare them). One reason for this is considered to be that the grains of the core are relatively large. When the ratio (core / sheath) is large, the core has relatively large grains and therefore has good thermal conductivity. In view of this, the ratio (core / sheath) is preferably a large ratio, which is 5 or more in this article, and further more than 5. According to this test, although the ratio (core / sheath) depends on the composition, degree of processing, etc., the ratio (core / sheath) can be adjusted to a certain extent by changing the heat treatment conditions. Herein, as the heating temperature during the heat treatment decreases, the ratio (core / sheath) tends to increase easily (for example, refer to Sample No. 1-6, 1-1 and 1-112 and compare them). For Sample No. 1-112, it is considered that the grains of both the core and the sheath become coarse by the high heating temperature during the heat treatment, and therefore, the ratio (core / sheath) is 1.
[0207] (5) The diffusion layer formed between the core wire and the outer skin can further improve the adhesion. For example, the comparison between Sample No. 1-1, 1-111 and 1-112 shows that as the average thickness of the diffusion layer increases, the length of oxide formation decreases. From these results, it can be expected that by adjusting the thickness of the diffusion layer, the adhesion between the core wire and the outer skin is further improved, and therefore, the oxidation resistance is further improved, and as mentioned above, good oxidation resistance can be maintained for a long time. In this test, although the average thickness of the diffusion layer depends on the composition, degree of processing, etc., the average thickness of the diffusion layer can be adjusted by changing the heat treatment conditions. As the heating temperature during the heat treatment increases, the average thickness tends to increase.
[0208] The test shows that an electrode material including a composite material having a double-layer structure including a core wire having a high Ni content and an outer sheath composed of a nickel alloy containing a specific range of Cr and Al has low specific resistance, good spark wear resistance, and good oxidation resistance. It is expected that a spark plug electrode composed of the electrode material and a spark plug including the spark plug electrode have both good spark wear resistance and good oxidation resistance.
[0209] The scope of the present invention is not limited to the embodiments but is defined by the appended claims, and is intended to cover all modifications within the meaning and scope equivalent to the claims.
[0210] For example, the composition, shape, size, etc. of the electrode material described in Experimental Example 1 may be appropriately changed.
[0211] Reference numerals list
[0212] 1. Electrode Materials
[0213] 10. Composite Materials
[0214] 11 core wire
[0215] 12 skins
[0216] 13Diffusion layer
[0217] 15 Oxide
[0218] 2 Spark plugs
[0219] 20 electrodes
[0220] 20e end face
[0221] 21 Central Electrode
[0222] 22 Grounding Electrode
[0223] 25 Insulator
[0224] 26 Metal Shell
[0225] S specimen
Claims
1. An electrode material, comprising: A composite material comprising a core wire and a sheath, wherein the core wire is composed of a nickel-based material containing 96% by mass or more of Ni, the sheath covers the outer peripheral surface of the core wire and does not cover the end surface of the core wire but exposes the end surface of the core wire, wherein The outer skin is composed of a nickel alloy containing 10 mass % to 30 mass % of Cr and 0.1 mass % to 6 mass % of Al, and The composite material has a specific resistance of less than 50 μΩ·cm, The oxidation proceeds from the end surface of the composite material along the interface between the core wire and the outer skin toward the inside of the composite material over a length of less than 300 μm. 2 . The electrode material according to claim 1 , wherein in a cross section of the composite material, an area ratio of a cross-sectional area of the outer skin to a cross-sectional area of the composite material is 0.4 or more and 0.7 or less. 3 . The electrode material according to claim 1 , wherein a ratio of a grain size of the nickel-based material forming the core wire to a grain size of the nickel alloy forming the outer skin is 5 or more. 4 . The electrode material according to claim 1 , comprising a diffusion layer between the core wire and the sheath, wherein a Ni content of the diffusion layer changes in a gradient manner. 5 . The electrode material according to claim 1 , wherein at least one of the nickel-based material forming the core wire and the nickel alloy forming the sheath contains a rare earth element in a total amount of 0.01 mass % to 0.7 mass % both inclusive.
6. The electrode material according to any one of claims 1 to 5, wherein the nickel alloy forming the outer skin comprises, in mass %, 0.1 mass % to 1.5 mass % of Si, 0.1 mass % to 0.6 mass % of Mn, 10 mass % or more and 30 mass % or less of Cr, 0.1 mass % to 6 mass % of Al, 0.01 mass % to 12 mass % of Fe, and The content of Ti is 0.01 mass % or more and 0.6 mass % or less, and the balance is Ni and inevitable impurities.
7. The electrode material according to any one of claims 1 to 6, wherein the nickel-based material forming the core wire comprises, in mass %, 0.01 mass % to 1.5 mass % of Si, 0 mass % or more and 1.5 mass % or less of Mn, 0.001 mass% to 1.5 mass% of Cr, 0.001 mass % to 0.5 mass % of Al, 0.01 mass % to 1.5 mass % of Fe, and The content of Ti is 0 mass % or more and 0.5 mass % or less, and the balance is Ni and inevitable impurities. 8 . A spark plug electrode, comprising the electrode material according to claim 1 . 9 . A spark plug comprising the spark plug electrode according to claim 8 .