Method and device for high-concentration carbon doping on refractory metal surface and inner surface layer

By heating the carbon source at high temperatures, generating high-energy carbon atoms and diffusing them to the refractory metal surface and inner surface layer, the problem of difficult to achieve high concentration carbon doping in the prior art is solved, and the material's sputter resistance is improved Ability and wear resistance extend the life of the system.

CN118932275APending Publication Date: 2024-11-12XIAN BAOHENG ELECTRONIC TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123064.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to achieve high concentration carbon doping on the surface and inner surface layer of refractory precious metal materials, resulting in poor resistance to the material under bombardment and radiation of low-energy particles, and the carburizing layer is uneven, making it impossible to effectively fill the internal cavity.

Method used

Heat the carbon source at high temperature to generate high-energy carbon atoms, allowing them to diffuse to the surface and inner surface layer of the refractory metal. Through the design of the closed cavity and vacuum chamber, the carbon atoms enter the inside of the material with a high diffusion coefficient and fill the holes. and unit cell spaces, a uniform high concentration carbon doped layer is formed.

Benefits of technology

Achieve high concentration carbon doping on the surface and inner surface layer of refractory metal, improve the material's sputtering resistance and wear resistance, extend the system's life and reliability, and ensure the uniform distribution of carbon atoms within the material and Stable existence.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932275A_ABST
    Figure CN118932275A_ABST
Patent Text Reader

Abstract

The invention discloses a method and a device for performing high-concentration carbon doping on a refractory metal surface and an inner surface layer. The method comprises the following steps: placing a refractory noble metal material in a closed cavity, putting or introducing a carbon source, heating the refractory noble metal material in the closed cavity to 800-1200 DEG C, and keeping for 3-20 hours to complete carbon doping. According to the method, carbon atoms are cracked out at a high temperature, the carbon atoms are diffused from the surface of a refractory metal material to a body with a certain thickness below the surface at a high migration rate by utilizing the high energy and activity of the high-temperature carbon atoms, and the carbon atoms can be diffused in refractory precious metal at a high speed due to the fact that the carbon atoms obtain large energy at the high temperature, so that the refractory precious metal is more stable. And the number of carbon atoms entering metal in unit time is huge and can reach 1019 / cm < 2 > or above, so that a large number of carbon atoms can stably enter unit cell gaps of the material, grain boundaries of the material and holes in the material for a long time, and the material is fully filled with the carbon atoms.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal processing and relates to a method and a device for high-concentration carbon doping on the surface and inner surface layer of a refractory metal. Background Art

[0002] Refractory precious metal materials, also known as high-melting-point rare metal materials, have many important applications in numerous engineering and technical fields, playing an extremely important, critical and irreplaceable role. However, in many cases, because these materials are not hard enough, the diameter of the atoms in the materials is large and the gaps are large, in some electronics and special applications, they have poor resistance to low-energy particle bombardment or low-energy particle radiation. Under high-density, high-dose low-energy particle irradiation, various damages occur, triggering atomic migration, causing the material to crack or break, and perforate, resulting in a decrease in the life or reliability of various components made of this material, causing the entire system to be scrapped prematurely.

[0003] During the processing of refractory precious metal materials, there are many cavities inside, such as Figure 1 As shown in the figure, such voids exist between the grain interfaces of the material, changing the continuity of the material and the close contact between the grain interfaces to varying degrees, affecting both the mechanical properties of the material and the electronic properties of the material at the microscopic structure, making it difficult to obtain a complete surface of the material during processing. Especially in the process of electronic applications, the presence of voids destroys the uniformity of the electric field and forms tiny tips on the surface, resulting in concentrated field strength at the tip, making it easier to discharge at the tip, producing a microscopic electric spark effect, and thus causing early failure of the material.

[0004] At present, the existing traditional process equipment and methods are used to dope metal materials with carbon: the metal material is heated to about 900℃, and placed in liquid high-carbon organic oil. At a temperature of about 900℃, the high temperature of the workpiece causes the organic material to crack, and the carbon atoms decomposed from the organic matter enter the metal surface and penetrate from the workpiece surface to a surface layer of a certain thickness below the surface. This method can be defined as immersion medium-temperature liquid-solid carburizing. As the metal is immersed in the organic liquid, the surface temperature of the metal material continues to drop, the overall temperature of the material is also dropping, and the number of carbon atoms in the organic carbon source is also decreasing with the decrease in temperature. After a short period of time, the temperature of the workpiece becomes low, and the carbon atoms can no longer be decomposed, and the carburizing of the workpiece is basically completed. Since the carburizing process is also a cooling process, the high temperature time is short, the temperature of the workpiece gradually decreases, the energy obtained by the carbon atoms is small, the diffusion coefficient of the carbon atoms in the metal is low, the amount of carbon atoms entering the metal material per unit time is small, and the carbon atoms are concentrated in the shallow surface layer of the metal material.

[0005] Even if the carburized metal material is heated twice or multiple times and carburized multiple times, a uniform and continuous carburized layer will not be formed in the metal working body.

[0006] For many critical applications of refractory precious metals, it is required to form a carbon-doped layer with roughly uniform distribution of carbon atoms on the surface and in the body of a certain thickness below the surface layer. This immersion medium-temperature liquid-solid carburizing process method cannot meet the technical requirements for a certain carburizing depth.

[0007] For the uniform doping of high-concentration carbon atoms in refractory precious metals, when the temperature is low, the solid solubility of carbon atoms in the material is not high, and the carbon atoms can only be deposited on the surface of the metal material at a lower concentration. It is difficult to enter the material body of a certain thickness below the surface of the material. Since the number of carbon atoms entering the material body is not enough, and the atoms entering the unit cell voids within the material grains are not many, the carbon atoms are not enough to fill the voids or pores within the material body of a certain thickness below the internal surface layer of the material, and the carburized layer is limited to the surface of the metal material.

[0008] When the carburizing temperature of refractory precious metals is low, carbon atoms exist in the shallow surface layer of the material in the form of interstitial filling. They fail to constitute or form a carbon-doped layer of sufficient thickness. Also, due to the low temperature, they cannot form a good ceramic phase with the metal material. Their wear resistance is limited, and their ability to resist low-energy particle bombardment under strong fields is insufficient, resulting in unsatisfactory anti-sputtering ability of the material. Summary of the invention

[0009] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and to provide a method and device for high-concentration carbon doping on the surface of refractory metal and the inner surface layer of a certain thickness below the surface, which can achieve high-concentration carbon doping on the surface of refractory metal and the material body of a certain thickness below the surface layer to the maximum extent.

[0010] In order to achieve the above object, the present invention adopts the following technical solutions:

[0011] A method for high-concentration carbon doping on the surface and inner surface layer of a refractory metal comprises the following steps:

[0012] The refractory noble metal material is placed in a sealed cavity, a carbon source is placed or introduced, and the carbon source and the refractory noble metal material (4) in the sealed cavity are heated to 800-1200° C. and maintained for 3-20 hours or longer to complete carbon doping of various requirements.

[0013] Preferably, before heating, an inert gas is used to expel air from the sealed cavity.

[0014] Preferably, the carbon source is a solid carbon source or a gaseous carbon source.

[0015] Further, solid carbon sources include carbon black, graphite fine powder, pitch and carbonized resin powder.

[0016] Furthermore, the solid carbon source is brought into contact with the refractory precious metal material, and the heating process is performed at a rate of 20-30° C. per minute, and the temperature remains constant after reaching 800° C.-1200° C.

[0017] Preferably, the carbon source is an organic gas with a high carbon content.

[0018] Furthermore, the high carbon content organic gas includes any one or more of CH4, C2H4, C3H6, heptane and gasoline vapor.

[0019] Furthermore, the temperature is heated to 800-1200°C at 20-30°C per minute, and a high-carbon organic gas is introduced into the sealed cavity. The pressure in the sealed cavity is maintained at 0.1-0.2Mpa, and the high-carbon organic gas is subjected to hot wire high-temperature cracking at 800-900°C.

[0020] A device for high-concentration carbon doping on the surface and inner surface layer of a refractory metal, comprising a heater, a solid carbon source, a compact, a carbon seal and a vacuum chamber;

[0021] The carbon seal and the heater are both located inside the vacuum chamber. Refractory precious metal materials are placed inside the carbon seal. The refractory precious metal materials are covered with a solid carbon source. A briquette is placed on top of the solid carbon source. The carbon seal seals and wraps the refractory precious metal materials, the solid carbon source and the briquette.

[0022] A device for high-concentration carbon doping on the surface and inner surface layer of a refractory metal, comprising an intake regulating valve, an exhaust regulating valve, a heater, a sealed chamber and a hot wire;

[0023] The hot wire and the heater are both located inside the sealed chamber, and the sealed chamber is connected to the outside world via an air inlet pipe and an air outlet pipe, on which an air inlet regulating valve and an air exhaust regulating valve are respectively arranged, and the air inlet pipe is connected to an organic gas carbon source.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] The present invention utilizes the high energy of carbon atoms cracked at high temperature to diffuse highly active carbon atoms from the surface of refractory precious metal materials into a body of a certain thickness below the surface with high energy. Since the energy obtained by carbon atoms at high temperature is large, they can diffuse at a faster speed in the refractory precious metal. The number of carbon atoms entering the metal per unit time is huge, which can reach 10 19 Pieces / cm 2As mentioned above, the content of carbon atoms diffused into the refractory metal can reach or approach its theoretical proportion, thereby achieving maximum uniform carbon atom doping, which enables a large number of carbon atoms to enter the crystal cell gaps, grain boundaries and voids inside the material stably and for a long time until they are full.

[0026] Furthermore, carbon atoms are excited in the solid carbon to diffuse from the surface of the refractory precious metal layer in contact with it into the interior. At a reasonable temperature, high-concentration carbon atoms diffuse from the surface to a certain thickness of the refractory precious metal below the surface layer with a faster diffusion coefficient. At high temperatures, the solid solubility of carbon atoms in the refractory precious metal is high, and an atomic percentage close to the theoretical value can be obtained.

[0027] Furthermore, in the process of hot wire cracking organic gas, as the pressure and temperature in the chamber increase, the temperature of the refractory precious metal material rises, and the organic gas encounters high temperature and automatically cracks into carbon and hydrogen. The formed carbon atoms are adsorbed on the surface of the refractory precious metal material and diffuse from the surface into the body of the material with a certain thickness below the surface layer. When the pressure in the chamber reaches the set value, the carbon atoms obtain higher energy and diffuse from the surface to the body with a larger diffusion coefficient. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is the metallographic image of the longitudinal section of the refractory precious metal plate under the traditional rolling process;

[0029] Figure 2 This is a schematic structural diagram of a solid-solid high-temperature diffusion device according to Example 1 of the present invention;

[0030] Figure 3 This is a schematic structural diagram of a gas-solid high-temperature diffusion device according to Example 2 of the present invention;

[0031] Figure 4 This is a schematic diagram of carbon atoms diffusing into the surface layer of a refractory metal according to the present invention;

[0032] Figure 5 Schematic diagram of the distribution of carbon impurity atoms in the surface layer of refractory metal according to the present invention;

[0033] Figure 6 This is a metallographic diagram of a longitudinal section of a refractory precious metal plate after high-concentration and uniform carbon doping using the process of the present invention.

[0034] Among them: 1- platform; 2- vacuum chamber; 3- heater; 4- refractory precious metal material; 5- solid carbon source; 6- pressing block; 7- carbon seal; 8- sealed chamber; 9- air inlet regulating valve; 10- exhaust regulating valve; 11- hot wire. DETAILED DESCRIPTION

[0035] The embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0036] In the description of the present invention, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise" and the like indicate positions or positional relationships based on the positions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.

[0037] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which the present invention belongs. The terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal connection of two elements or the interaction relationship between two elements. The term "and / or" used in this article includes any and all combinations of one or more related listed items. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to the specific circumstances. The terms used in the specification of the present invention herein are only for the purpose of describing specific embodiments and are not intended to limit the present invention.

[0038] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may include that the first and second features are in direct contact, or may include that the first and second features are not in direct contact but are in contact through another feature between them. Moreover, a first feature being "above", "above" and "above" a second feature includes that the first feature is directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being "below", "below" and "below" a second feature includes that the first feature is directly below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0039] The disclosure below provides many different embodiments or examples to realize different structures of the present invention. In order to simplify the disclosure of the present invention, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present invention. In addition, the present invention can repeat reference numbers and / or reference letters in different examples, and this repetition is for the purpose of simplification and clarity, which itself does not indicate the relationship between the various embodiments and / or settings discussed. In addition, the examples of various specific processes and materials provided by the present invention, but those of ordinary skill in the art can be aware of the application of other processes and / or the use of other materials.

[0040] The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal described in the present invention includes the following process.

[0041] Place the refractory precious metal material 4 in a closed cavity and add a carbon source. First, use an inert gas to purge the closed cavity to remove the air in the cavity, and then start heating slowly until the set temperature is reached. Under high temperature, carbon atoms diffuse from the surface of the refractory precious metal material 4 to the inside of the surface.

[0042] At high temperatures, the solid solubility of carbon atoms in refractory precious metals is high, and an atomic ratio close to the theoretical value can be obtained.

[0043] The present invention uses constant and continuous high temperature to incorporate highly active carbon atoms into the material surface and the inner surface of a certain thickness with a high mobility. Since the energy obtained by carbon atoms at high temperature is large and the diffusion coefficient in refractory precious metals is large, the number of carbon atoms entering the metal per unit time is huge, which can reach 10 19 Pieces / cm 2 The carbon content in the refractory metal can reach or approach its theoretical proportion, thereby achieving maximum carbon doping. Based on the reasonable constant high temperature obtained by the present invention, a large number of carbon atoms can stably enter the unit cell gaps of the material, the grain boundaries of the material, and the cavities inside the material for a long time and fill them up.

[0044] Use carbon atoms with smaller radius to fill the atomic unit cells of refractory precious metals with larger radius, and at the same time, realize carbon accumulation and filling of the voids formed by refractory precious metals during processing, eliminate the voids formed by metal materials during processing, and make the grain boundaries of various shapes in the material seamlessly connected through carbon atoms, forming chemically stable M with refractory precious metals on the surface and the inner surface of a certain thickness. x C y Ceramic phase, thereby better improving and enhancing the anti-sputtering ability of workpieces made of refractory precious metal materials under high ambient temperature or strong field conditions and in medium energy particle radiation environment, so that the life or reliability of the entire system can be greatly improved.

[0045] Embodiment 1:

[0046] This embodiment adopts a solid-solid high-temperature carbon doping method to activate the solid carbon source 5 at high temperature. According to the diffusion principle, the activated carbon atoms obtain greater energy and diffuse from the surface of the refractory precious metal to the inner layer.

[0047] This embodiment uses a device such as Figure 2 As shown, it includes a heater 3, a solid carbon source 5, a pressing block 6, a carbon seal 7, a vacuum chamber 2 and a stage 1.

[0048] The solid carbon source 5 includes carbon black, graphite fine powder, pitch and carbonized resin powder.

[0049] The vacuum chamber 2 is located above the table 1, and the carbon seal 7 and the heater 3 are both located inside the vacuum chamber 2. A refractory precious metal material 4 is placed in the carbon seal 7, and the refractory precious metal material 4 is covered with a solid carbon source 5. A compact 6 is placed on top of the solid carbon source 5. The carbon seal 7 seals and wraps the refractory precious metal material 4, the solid carbon source 5 and the compact 6. The heater 3 is used to heat the carbon seal 7 and its interior.

[0050] The carbon seal 7 is an amorphous shell made of high-purity graphite powder.

[0051] During operation, the refractory precious metal material 4 is placed in the carbon seal 7, the refractory precious metal material 4 is covered with the solid carbon source 5, and the compact 6 is placed on the top of the solid carbon source 5. The carbon seal 7 seals and wraps the refractory precious metal material 4, the solid carbon source 5 and the compact 6. The inert gas is used to drive out the gas until the air in the vacuum chamber is purged. The heater 3 is turned on and the inert gas is used to drive out the gas while heating. The solid carbon source 5 is heated at a low temperature of 300-550°C for 1-3h. The air remaining due to adsorption is further removed. Some of the residual gas in the carbon seal 7 is absorbed by the carbon seal 7 during the low-temperature heating process. Then, the temperature is slowly heated at 20-30°C per minute. After the temperature reaches 800°C-1200°C and remains constant, the carbon atoms excited in the solid carbon source 5 at high temperature diffuse from the surface of the refractory precious metal material in contact with it to the inside. The diffusion time is determined by the diffusion depth of carbon atoms in the refractory metal, which is generally 3-30 hours. When there are specific requirements, the time can be extended, depending on the requirements.

[0052] Embodiment 2:

[0053] This embodiment uses high-carbon content organic gas as the carbon source and utilizes high temperature to crack the organic gas to produce high-concentration carbon atoms, which are deposited on the surface of the refractory metal and diffuse from the surface into the interior of the refractory precious metal material 4, forming a high-concentration carbon-doped layer of a certain thickness on the surface of the refractory precious metal material 4.

[0054] The high carbon content organic gas includes any one or more of CH4, C2H4, C3H6, heptane and gasoline vapor.

[0055] This embodiment uses a device such as Figure 3 As shown, it includes an intake regulating valve 9, an exhaust regulating valve 10, a heater 3, a sealed chamber 8, a hot wire 11 and a platform 1.

[0056] The sealed chamber 8 is located above the platform 1, the hot wire 11 and the heater 3 are both located inside the sealed chamber 8, the sealed chamber 8 is connected to the outside world via an air inlet pipe and an air outlet pipe, an air inlet regulating valve 9 and an air exhaust regulating valve 10 are respectively provided on the air inlet pipe and the air outlet pipe, and the air inlet pipe is connected to an organic gas carbon source.

[0057] During operation, the refractory precious metal material 4 is placed in a sealed chamber 8. Similarly, an inert gas is first used to drive out the gas to remove the atmosphere in the sealed chamber 8. After degassing, the heater 3 is turned on to further remove the air and other impurity gases remaining due to adsorption, and then heating is started to reach 800-1200°C at 20-30°C per minute. At the same time, the air inlet valve and the exhaust valve are adjusted to introduce organic gas into the sealed chamber 8 to maintain the pressure in the sealed chamber 8 at 0.1-0.2Mpa. The power supply of the hot wire 11 is turned on to perform high-temperature cracking of the organic gas at 800-900°C by the hot wire 11 to produce a large amount of carbon atoms. At high temperature, the carbon atoms diffuse from the surface of the refractory metal material to the inside of the surface. During the process of the hot wire 11 cracking the organic gas, as the air pressure in the sealed chamber 8 increases, the temperature of the refractory precious metal material 4 rises, and the organic gas encounters high temperature and automatically cracks into carbon and hydrogen. The formed carbon atoms are adsorbed on the surface of the refractory precious metal material 4 and diffuse into the inner surface of the material. After 3 to 20 hours, the carbon atoms reach a depth of 10 μm to 100 μm or even deeper in the refractory metal material. When the pressure in the sealed chamber 8 reaches the set value, the carbon atoms obtain higher energy and diffuse from the surface of the refractory metal material into the body with a larger diffusion coefficient.

[0058] Gas-solid high-temperature and high-pressure carbon atom doping is also a constant source doping. Carbon atoms enter the refractory precious metal material 4 from the surface. Within a certain thickness range below the surface of the refractory metal, the carbon atoms are roughly distributed in a residual error. From the surface to the inside, the carbon impurity concentration decreases with increasing depth.

[0059] In the present invention, the carbon atoms activated at high temperature diffuse inward from the surface of the refractory metal with higher energy, such as Figure 4 As shown. Both methods belong to constant source diffusion, carbon atoms diffuse into the refractory metal at high temperature to form doping, such as Figure 5 shown.

[0060] Taking a certain refractory precious metal as an example, the carbon atoms in it account for approximately 33% to 43%, and the thickness of the carbon-doped layer can reach 70-80μm. Microscopic examination of metallographic sample preparation shows that no voids are observed in the carbon-doped layer of the refractory precious metal after high-concentration carbon doping, indicating that carbon impurities have effectively filled the voids, and the grain interfaces of the material are dense and uniform. Figure 6 shown.

[0061] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0062] It should be understood that the above description is for illustration and not for limitation. Many embodiments and many applications beyond the examples provided will be apparent to those skilled in the art upon reading the above description. Therefore, the scope of the present application should not be determined with reference to the above description, but rather with reference to the foregoing claims and the full scope of equivalents to which such claims are entitled. For the purpose of comprehensiveness, all articles and references, including disclosures of patent applications and publications, are incorporated herein by reference. The omission of any aspect of the subject matter disclosed herein in the foregoing claims is not intended to be a waiver of such subject matter, nor should it be considered that the applicant has not considered such subject matter to be part of the disclosed inventive subject matter.

Claims

1. A method for high-concentration carbon doping on the surface and inner surface layer of a refractory metal, characterized in that: The process includes: The refractory noble metal material (4) is placed in a sealed cavity, a carbon source is placed or introduced, and the carbon source and the refractory noble metal material (4) in the sealed cavity are heated to 800-1200° C. and maintained for 3-20 hours to complete carbon doping.

2. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 1, characterized in that: Before heating, an inert gas is used to purge the inside of the sealed cavity.

3. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 1, characterized in that: The carbon source is a solid carbon source (5).

4. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 3, characterized in that: The solid carbon source (5) includes carbon black, graphite fine powder, pitch and carbonized resin powder.

5. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 3, characterized in that: The solid carbon source (5) is brought into contact with the refractory noble metal material (4), and the heating process is performed at a rate of 20-30°C per minute, and the temperature remains constant after reaching 800°C-1200°C.

6. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 1, characterized in that: The carbon source also uses organic gas with high carbon content.

7. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 6, characterized in that: The high carbon content organic gas includes any one or more of CH4, C2H4, C3H6, heptane and gasoline vapor.

8. The method for high-concentration carbon doping on the surface and inner surface layer of refractory metal according to claim 6, characterized in that: The temperature is heated to 800-1200°C at 20-30°C per minute, and a high-carbon organic gas is introduced into the sealed cavity to keep the pressure in the sealed cavity between 0.1-0.2Mpa. The high-carbon organic gas is subjected to high-temperature cracking by a hot wire (11) at 800-900°C.

9. A device for high-concentration carbon doping on the surface and inner surface layer of refractory metal based on the method according to any one of claims 3 to 5, characterized in that: It comprises a heater (3), a solid carbon source (5), a pressing block (6), a carbon seal (7) and a vacuum chamber (2); The carbon seal (7) and the heater (3) are both located inside the vacuum chamber (2). A refractory precious metal material (4) is placed inside the carbon seal (7). The refractory precious metal material (4) is covered with a solid carbon source (5). A compact (6) is placed on top of the solid carbon source (5). The carbon seal (7) completely seals and wraps the refractory precious metal material (4), the solid carbon source (5) and the compact (6).

10. A device for high-concentration carbon doping on the surface and inner surface layer of refractory metal based on the method according to any one of claims 6 to 8, characterized in that: It comprises an air intake regulating valve (9), an exhaust regulating valve (10), a heater (3), a sealed chamber (8) and a hot wire (11); The hot wire (11) and the heater (3) are both located inside the sealed chamber (8). The sealed chamber (8) is connected to the outside world via an air inlet pipe and an air outlet pipe. An air inlet regulating valve (9) and an air outlet regulating valve (10) are provided on the air inlet pipe and the air outlet pipe, respectively. The air inlet pipe is connected to an organic gas carbon source.