Method for improving oxidation resistance of TiAl alloy by depositing Dy and Hf modified AlCoCrFeNi high-entropy alloy film
Dy and Hf modified AlCoCrFeNi high-entropy alloy films were prepared through vacuum non-consumable arc smelting and magnetron sputtering technology, which solved the problem of insufficient high-temperature oxidation resistance of TiAl alloy, formed protective Al2O3 oxides, significantly improved TiAl alloy antioxidant properties.
Patent Information
- Application Number
- CN202410998885.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-24
AI Technical Summary
TiAl alloy has poor oxidation resistance at high temperatures, and the existing MCrAlY coating is insufficient in compatibility with the TiAl alloy matrix, resulting in low adhesion of the coating and unable to effectively improve the high-temperature oxidation resistance of TiAl alloy.
Dy and Hf modified AlCoCrFeNi high-entropy alloy targets were prepared by vacuum non-consumable arc smelting technology, and modified AlCoCrFeNi high-entropy alloy film was deposited through magnetron sputtering technology to form a film with a single-phase BCC structure to improve the TiAl alloy Antioxidant properties.
At 900°C, Dy and Hf modified AlCoCrFeNi high-entropy alloy films formed protective Al2O3 oxides, which significantly improved the oxidation resistance of TiAl alloy and extended the stability of the oxide layer.
Smart Images

Figure CN118932307A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of high entropy alloy film preparation, and more particularly to a method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy films to improve the oxidation resistance of TiAl alloys. Background Art
[0002] TiAl alloys have the advantages of low density, high specific strength at high temperature, and good creep performance, so they are expected to be used in aeroengines. With the continuous improvement of the thrust-to-weight ratio of aeroengines, the operating temperature of turbine blade materials is also getting higher and higher. It is well known that TiAl alloys form a non-protective mixture of TiO2 and Al2O3 at high temperatures, rather than a single continuous Al2O3. Therefore, the poor high-temperature oxidation resistance limits the application of TiAl alloys. The addition of elements such as niobium, tungsten and silicon seems to enhance the high-temperature oxidation resistance of alloy TiAl, but often reduces its mechanical properties. Therefore, a protective coating is needed to improve the high-temperature oxidation resistance of TiAl alloys. MCrAlY (M = Ni, Co or both) cladding type coatings can protect TiAl alloys from oxidation at high temperatures. However, MCrAlY coatings have defects in compatibility with TiAl alloys. Severe interdiffusion between the TiAl alloy substrate and the MCrAlY coating leads to the formation of brittle phases and internal oxidation, which reduces the adhesion of the coating and ultimately leads to premature failure of the coating. Therefore, it is necessary to develop an anti-oxidation coating with good compatibility with the TiAl alloy substrate.
[0003] The concept of high entropy alloys (HEAs) was proposed by Ye and Cantor in 2004. HEAs are usually composed of at least five elements with equal or nearly equal atomic percentages. The special structure and excellent performance of HEAs are due to their four major effects, including high entropy effect, severe lattice distortion effect, hysteresis diffusion effect and cocktail effect. High mixing entropy makes HEAs have simple solid solution structures, such as face-centered cubic (FCC), body-centered cubic (BCC) or hexagonal close packing (HCP), rather than complex alloys. Therefore, HEAs have excellent high-temperature strength, oxidation resistance and corrosion resistance, and are expected to be used as high-temperature protective coating materials. Dong et al. prepared AlCoCrFeNi2.1Tix coating on Ti-6Al-4V alloy by spark plasma sintering. The study found that a dense oxide film composed of aluminum oxide and a small amount of chromium oxide was formed on the surface of Ti-6Al-4V alloy, which hindered the inward diffusion of oxygen and improved the oxidation resistance of Ti-6Al-4V alloy at 800℃. Zhang et al. prepared AlCoCrFeNiSix high entropy alloy coating on 316L stainless steel substrate by gas phase plasma spraying. The oxidation test results at 800℃ showed that the proper addition of Si element can improve the oxidation resistance of high entropy alloy coating, and it is expected to be used as a bonding layer for thermal barrier coating. Chang et al. prepared FeCrxCoNiB coating on AISI1045 steel substrate by laser cladding technology and studied the oxidation resistance of the coating at 900℃. The results showed that when x≥2, the coating had good oxidation resistance due to the formation of a continuous and dense Cr2O3 oxide film. Among all high entropy alloys, AlCoCrFeNi system has a unique microstructure and good mechanical properties, so it is an ideal candidate material for high temperature protective coating. However, AlCoCrFeNi has poor oxidation resistance at high temperature because the oxide contains spinel or mixed oxides, which accelerates the large-scale peeling of the oxide layer.
[0004] It is well known that small amounts of reactive elements (REs, such as Dy and Hf) can improve the high-temperature oxidation resistance of alloys and coatings by improving the adhesion of the oxide layer. Feng et al. reported that Dy doping can improve the oxidation resistance of Al-Si coatings because the stronger Dy-O bonds increase the adhesion energy of the oxide layer. In addition, several studies have shown that Hf doping can inhibit the inward diffusion of oxygen and form Hf-rich "pinning" oxides at the interface between the oxide layer and the substrate, thereby improving the adhesion of the oxide layer. At present, high-entropy alloy coatings are usually prepared by processes such as laser cladding, thermal spraying, magnetron sputtering, and electrochemical deposition. Among these technologies, magnetron sputtering has attracted increasing attention due to its advantages such as high deposition rate, dense film structure, and controllable film thickness.
[0005] Therefore, it is an urgent technical problem to modify the AlCoCrFeNi high entropy alloy using active elements Dy and Hf and further improve the oxidation resistance of TiAl alloy by improving the adhesion performance of the oxide layer. Summary of the invention
[0006] The purpose of the present application is to provide a method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy films to improve the oxidation resistance of TiAl alloys, thereby improving the oxidation resistance of TiAl alloys.
[0007] The present application provides a method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy films to improve the oxidation resistance of TiAl alloys, comprising the following steps:
[0008] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb matrix was prepared by vacuum non-consumable arc melting technology;
[0009] S2. Weigh pure metal raw materials Al, Co, Cr, Fe, Ni and pure active raw materials Dy and Hf, and prepare modified AlCoCrFeNi high entropy alloy target by vacuum non-consumable arc melting technology;
[0010] S3. Mount the Ti-45Al-8Nb substrate in step S1 on a fixture of a magnetron sputtering device, place the modified AlCoCrFeNi high entropy alloy target in step S2 on a radio frequency target, and use magnetron sputtering technology to obtain a TiAl alloy covered with a modified AlCoCrFeNi high entropy alloy film.
[0011] Preferably, in step S3, the magnetron sputtering parameters are: the temperature of the Ti-45Al-8Nb substrate is 80-100°C, the power of the AlCoCrFeNi high entropy alloy target is 300W, the sputtering time is 7-8h, the gas pressure is 0.4Pa, and the vacuum degree is 1x10 -4 ~6x10 - 4 Pa.
[0012] Preferably, step S1 further comprises the following steps:
[0013] 1) The prepared Ti-45Al-8Nb matrix is cut by wire cutting to obtain a sample, and the sample is polished by water-abrasive sandpaper and then polished to a mirror surface by a polishing machine;
[0014] 2) The Ti-45Al-8Nb substrate polished in step 1) is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the ultrasonic cleaning time is 10-20min, and after ultrasonic cleaning, it is placed in an oven at 80°C for drying.
[0015] Preferably, step S2 further includes the following steps:
[0016] (1) cutting the modified AlCoCrFeNi high entropy alloy target by wire cutting and grinding the surface oil by sandpaper;
[0017] (2) The modified AlCoCrFeNi high entropy alloy target treated in step (1) is placed in an alcohol solution for ultrasonic cleaning at an ultrasonic frequency of 50 to 60 kHz for a cleaning time of 10 to 20 min, and then placed in an oven at 80° C. for drying.
[0018] Preferably, in the modified AlCoCrFeNi high entropy alloy target, the doping amount of Dy and Hf is 0.01-0.03% at.
[0019] Preferably, in the modified AlCoCrFeNi high entropy alloy target, the atomic ratio of Al, Co, Cr, Fe and Ni is 1:1:1:1:1.
[0020] Preferably, in step 1), the sample is polished with 200#, 400#, 800#, 1000#, and 1200# water-abrasive sandpaper in sequence.
[0021] Preferably, the mass fraction of the alcohol solution is 85-99.9%.
[0022] Preferably, before weighing the pure metal raw materials Al, Co, Cr, Fe, Ni and the pure active raw materials Dy and Hf, the block, granular and flaky pure metal raw materials Al, Co, Cr, Fe, Ni and the pure active raw materials Dy and Hf are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and sediment impurities, and then placed in Nb foil in order from low to high melting points, wrapped together and placed at the bottom of a copper crucible for smelting.
[0023] Preferably, the vacuum is drawn to 4-5×10 -3 Pa, and filled with high-purity argon gas to 1.0×10 5 Pa is used for protection, and the raw materials are repeatedly melted 5-6 times under argon protection.
[0024] Therefore, the present application adopts the above-mentioned method of depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film to improve the oxidation resistance of TiAl alloy, which has the following beneficial effects:
[0025] (1) The AlCoCrFeNi high entropy alloy film containing 0.02 at.% active elements Dy and Hf has a single-phase BCC columnar crystal structure with an average grain size of 21.1 nm;
[0026] (2) The oxide of the AlCoCrFeNi high entropy alloy film containing 0.02 at.% active elements Dy and Hf oxidized at 900℃ for 100h is protective Al2O3, and the oxidation weight gain is 0.81 mg·cm -2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is the principle diagram of magnetron sputtering of this application;
[0028] Figure 2 is a BSE cross-sectional view of a high entropy alloy film prepared in Example 1 of the present application and the content of each element at a point taken in the view; wherein a is a BSE cross-sectional view of a high entropy alloy film prepared in Example 1, and b is the content of each element at a point taken in the view;
[0029] Figure 3 is the GiXRD pattern of the high entropy alloy film prepared in Example 1;
[0030] Figure 4 The graph is an oxidation weight gain curve of the high entropy alloy film prepared in the present application compared with the TiAl alloy oxidized at 900°C for 100h, wherein HEF1 is a Dy and Hf modified AlCoCrFeNi high entropy alloy film, HEF2 is an unmodified AlCoCrFeNi high entropy alloy film, HEF3 is a Dy modified AlCoCrFeNi high entropy alloy film, and HEF4 is a Hf modified AlCoCrFeNi high entropy alloy film. (a) is a relationship diagram between the oxidation weight gain per unit area and the oxidation time, and (b) is a fitting curve of the relationship between the oxidation weight gain per unit area and the square root of the oxidation time, which further indicates that the oxidation kinetics curve of the sample follows the parabolic law and conforms to the classical oxidation theory. DETAILED DESCRIPTION
[0031] The present application provides a method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy films to improve the oxidation resistance of TiAl alloys, comprising the following steps:
[0032] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb matrix was prepared by vacuum non-consumable arc melting technology; the prepared Ti-45Al-8Nb matrix was cut into a sample by wire cutting, and the sample was polished with 200#, 400#, 800#, 1000# and 1200# water-abrasive sandpaper in succession, and then polished to a mirror surface by a polishing machine; then the polished Ti-45Al-8Nb matrix was placed in an alcohol solution with a mass fraction of 85-99..9% for ultrasonic cleaning, the ultrasonic frequency was 50-60KHz, the ultrasonic cleaning time was 10-20min, and the matrix was dried in an oven at 80°C after ultrasonic cleaning.
[0033] S2. Weigh pure metal raw materials Al, Co, Cr, Fe, Ni and pure active raw materials Dy and Hf, and prepare modified AlCoCrFeNi high entropy alloy target by vacuum non-consumable arc melting technology; before weighing the raw materials, mechanically grind the block, granular and flaky raw materials and put them into acetone or anhydrous ethanol for ultrasonic cleaning to remove oxide film and sediment impurities, and put them into Nb foil in the order of melting point from low to high, cover them together and place them at the bottom of copper crucible for melting, and evacuate to 4-5×10 -3 Pa, and filled with high-purity argon gas to 1.0×10 5 Pa is used for protection, and the raw materials are repeatedly melted 5-6 times under argon protection to prepare a modified AlCoCrFeNi high entropy alloy target; the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is polished off with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target after degreasing is placed in an alcohol solution with a mass fraction of 85-99..9% for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the cleaning time is about 10-20min, and then it is placed in an oven at 80°C for drying; the doping amounts of Dy and Hf in the modified AlCoCrFeNi high entropy alloy target are 0.02%at; the atomic ratios of Al, Co, Cr, Fe and Ni in the modified AlCoCrFeNi high entropy alloy target are 1:1:1:1:1.
[0034] S3, the Ti-45Al-8Nb substrate in step S1 is mounted on the fixture of the magnetron sputtering equipment, the modified AlCoCrFeNi high entropy alloy target in step S2 is placed on the radio frequency target, and the TiAl alloy covered with the modified AlCoCrFeNi high entropy alloy film is obtained by magnetron sputtering technology; the magnetron sputtering parameters are: the temperature of the Ti-45Al-8Nb substrate is 80-100°C, the power of the AlCoCrFeNi high entropy alloy target is 300W, the sputtering time is 7-8h, the gas pressure is 0.4Pa, and the vacuum degree is 1x10 -4 ~6x10 -4 Pa.
[0035] Example 1
[0036] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix with a size of 10×10×2 mm was obtained by vacuum non-consumable arc melting technology.
[0037] S2. The Ti-45Al-8Nb (at.%) substrate prepared in step S1 is polished with 200#, 400#, 800#, 1000#, and 1200# water-abrasive sandpaper in sequence, and then polished to a mirror surface with a polishing machine.
[0038] S3. The polished Ti-45Al-8Nb (at.%) substrate obtained in step S2 is placed in an alcohol solution with a mass fraction of 99.9% for ultrasonic cleaning to remove dirt. The ultrasonic frequency is 53 KHz. After cleaning for 10 minutes, the substrate is placed in an oven at 80° C. for drying and then set aside.
[0039] S4, weigh Al, Co, Cr, Fe, Ni pure metal raw materials and Dy, Hf pure active raw materials according to the ratio; the atomic percentage content of Dy and Hf is 0.02at%; the atomic percentage content ratio of Al, Co, Cr, Fe, Ni is 1:1:1:1, before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni, and Al, Dy, Ni, Co, Fe, Cr, Hf are placed in Nb foil in the order of melting point from low to high, and are wrapped together and placed at the bottom of a copper crucible, and the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 4-5×10 -3 Pa, and high-purity argon gas is filled to 1.0×105Pa for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make the various elements in the material more evenly distributed and reduce the internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is ground with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the cleaning time is 10min, and then it is placed in an 80℃ oven for drying.
[0040] S5. Use 60# water-abrasive sandpaper to remove the oil stains on the surface of the high entropy alloy target prepared in step S4, and then place it in a 99.9% alcohol solution for ultrasonic cleaning to remove dirt. Under the condition of an ultrasonic frequency of 53KHz, after cleaning for 10 minutes, place it in an oven for drying and set aside.
[0041] S6. Preparation of high entropy alloy thin films with uniform composition by magnetron sputtering
[0042] The Ti-45Al-8Nb (at.%) substrate dried in S3 was mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S5 was placed on the RF target for sputtering. The magnetron sputtering process parameters were adjusted as follows: the temperature of the Ti-45Al-8Nb substrate was 80 °C, the power of the high entropy alloy target was 300 W, the sputtering time was 8 h, the gas pressure was 0.4 Pa, and the vacuum degree was 1x10 -4 Pa.
[0043] The magnetron sputtering equipment used in this example is from Shenyang Scientific Instrument Co., Ltd., Chinese Academy of Sciences.
[0044] The magnetron sputtering equipment produced by Figure 1 Schematic diagram of magnetron sputtering. Figure 2 is a BSE cross-sectional view of a high entropy alloy film prepared in Example 1 of the present application and the content of each element at a point taken in the view; Figure 3 is the GiXRD pattern of the high entropy alloy film prepared in Example 1 of the present application; Figure 4 This is the oxidation weight gain curve of the high entropy alloy film prepared in Example 1 of the present application compared with the TiAl alloy oxidized at 900°C for 100 hours, wherein HEF1 is a Dy and Hf modified AlCoCrFeNi high entropy alloy film, HEF2 is an unmodified AlCoCrFeNi high entropy alloy film, HEF3 is a Dy modified AlCoCrFeNi high entropy alloy film, and HEF4 is a Hf modified AlCoCrFeNi high entropy alloy film. It can be seen from the figure that compared with the TiAl alloy, the oxidation weight gain of the unmodified AlCoCrFeNi high entropy alloy film oxidized at 900°C for 100 hours has been significantly reduced, while the oxidation weight gain of the Dy and Hf modified AlCoCrFeNi high entropy alloy film is further reduced.
[0045] Example 2
[0046] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix is obtained by vacuum non-consumable arc melting technology. Then the obtained Ti-45Al-8Nb (at.%) matrix is polished with 200#, 400#, 800#, 1000# and 1200# water-abrasive sandpaper in succession, and then polished to a mirror surface with a polishing machine, and then the polished Ti-45Al-8Nb (at.%) matrix is placed in an alcohol solution with a mass fraction of 85% for ultrasonic cleaning to remove dirt, and the ultrasonic frequency is 50KHz. After cleaning for 10 minutes, it is placed in an oven at 80°C for drying and then used for standby.
[0047] S2. Weigh pure metal raw materials of Al, Co, Cr, Fe, Ni and pure active raw materials of Dy and Hf according to the ratio; the atomic percentage content of Dy and Hf is 0.01 at%; the atomic percentage content ratio of Al, Co, Cr, Fe, and Ni is 1:1:1:1. Before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni are placed in the order of melting point from low to high, Al, Dy, Ni, Co, Fe, Cr, Hf, and are coated together in Nb foil and placed at the bottom of a copper crucible; the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 5×10 -3 Pa, and high-purity argon is filled to 1.0×105Pa for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make the various elements in the material more evenly distributed and reduce the internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is removed by grinding with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 60KHz, the cleaning time is 20min, and then it is placed in an 80℃ oven for drying, and then the obtained high entropy alloy target is ground with 60# water abrasive paper to remove the surface oil, and then placed in an alcohol solution with a mass fraction of 99.9% for ultrasonic cleaning to remove dirt, under the condition of an ultrasonic frequency of 60KHz, after cleaning for 20min, it is placed in an oven for drying and standby.
[0048] S3, the Ti-45Al-8Nb (at.%) substrate dried in S1 is mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S2 is placed on the RF target for sputtering. The magnetron sputtering process parameters are adjusted as follows: the temperature of the Ti-45Al-8Nb substrate is 80°C, the power of the high entropy alloy target is 300 watts, the sputtering time is 7 hours, the gas pressure is 0.4 Pa, and the vacuum degree is 1x10 - 4 Pa.
[0049] Example 3
[0050] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix is obtained by vacuum non-consumable arc melting technology. Then the obtained Ti-45Al-8Nb (at.%) matrix is polished with 200#, 400#, 800#, 1000# and 1200# water-abrasive sandpaper in succession, and then polished to a mirror surface with a polishing machine, and then the polished Ti-45Al-8Nb (at.%) matrix is placed in an alcohol solution with a mass fraction of 85% for ultrasonic cleaning to remove dirt, and the ultrasonic frequency is 60KHz. After cleaning for 20 minutes, it is placed in an oven at 80°C for drying and then used.
[0051] S2. Weigh pure metal raw materials of Al, Co, Cr, Fe, Ni and pure active raw materials of Dy and Hf according to the ratio; the atomic percentage content of Dy and Hf is 0.03at%; the atomic percentage content ratio of Al, Co, Cr, Fe, and Ni is 1:1:1:1. Before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni are placed in the order of melting point from low to high, Al, Dy, Ni, Co, Fe, Cr, Hf, and are coated together in Nb foil and placed at the bottom of a copper crucible; the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 5×10 -3 Pa, and filled with high-purity argon gas to 1.0×10 5 Pa is used for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make various elements in the material more evenly distributed and reduce internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is removed by grinding with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50KHz, the cleaning time is 15min, and then it is placed in an 80℃ oven for drying, and then the obtained high entropy alloy target is ground with 60# water abrasive paper to remove the surface oil, and then it is placed in an alcohol solution with a mass fraction of 90% for ultrasonic cleaning to remove dirt, under the condition of an ultrasonic frequency of 50KHz, after cleaning for 15min, it is placed in an oven for drying and standby.
[0052] S3, the Ti-45Al-8Nb (at.%) substrate dried in S1 is mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S2 is placed on the RF target for sputtering. The magnetron sputtering process parameters are adjusted as follows: the temperature of the Ti-45Al-8Nb substrate is 90°C, the power of the high entropy alloy target is 300 watts, the sputtering time is 7.5h, the air pressure is 0.4Pa, and the vacuum degree is 5x10 -4 Pa.
[0053] Example 4
[0054] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix is obtained by vacuum non-consumable arc melting technology. Then the obtained Ti-45Al-8Nb (at.%) matrix is polished with 200#, 400#, 800#, 1000# and 1200# water-abrasive sandpaper in succession, and then polished to a mirror surface with a polishing machine, and then the polished Ti-45Al-8Nb (at.%) matrix is placed in an alcohol solution with a mass fraction of 85% for ultrasonic cleaning to remove dirt, and the ultrasonic frequency is 60KHz. After cleaning for 20 minutes, it is placed in an oven at 80°C for drying and then used.
[0055] S2. Weigh pure metal raw materials of Al, Co, Cr, Fe, Ni and pure active raw materials of Dy and Hf according to the proportion; the atomic percentage content of Dy is 0.03at%; the atomic percentage content of Hf is 0.02at%, and the atomic percentage content ratio of Al, Co, Cr, Fe, and Ni is 1:1:1:1. Before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni are placed in the order of melting point from low to high, Al, Dy, Ni, Co, Fe, Cr, Hf, in Nb foil, wrapped together and placed at the bottom of a copper crucible, and the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 5×10 -3 Pa, and filled with high-purity argon gas to 1.0×10 5Pa is used for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make various elements in the material more evenly distributed and reduce internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is removed by grinding with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50KHz, the cleaning time is 15min, and then it is placed in an 80℃ oven for drying, and then the obtained high entropy alloy target is ground with 60# water abrasive paper to remove the surface oil, and then it is placed in an alcohol solution with a mass fraction of 90% for ultrasonic cleaning to remove dirt, under the condition of an ultrasonic frequency of 50KHz, after cleaning for 15min, it is placed in an oven for drying and standby.
[0056] S3, the Ti-45Al-8Nb (at.%) substrate dried in S1 is mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S2 is placed on the RF target for sputtering. The magnetron sputtering process parameters are adjusted as follows: the temperature of the Ti-45Al-8Nb substrate is 90°C, the power of the high entropy alloy target is 300 watts, the sputtering time is 7.5h, the air pressure is 0.4Pa, and the vacuum degree is 5x10 -4 Pa.
[0057] Comparative Example 1
[0058] In this comparative example, the content of pure Dy active material in terms of atomic percentage is 0.02 at%, and the content of pure Hf active material in terms of atomic percentage is 0 at%. The remaining steps and parameters are the same as those in Example 1.
[0059] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix with a size of 10×10×2 mm was obtained by vacuum non-consumable arc melting technology.
[0060] S2. The Ti-45Al-8Nb (at.%) substrate prepared in step S1 is polished with 200#, 400#, 800#, 1000#, and 1200# water-abrasive sandpaper in sequence, and then polished to a mirror surface with a polishing machine.
[0061] S3. The polished Ti-45Al-8Nb (at.%) substrate obtained in step S2 is placed in an alcohol solution with a mass fraction of 99.9% for ultrasonic cleaning to remove dirt. The ultrasonic frequency is 53 KHz. After cleaning for 10 minutes, the substrate is placed in an oven at 80° C. for drying and then set aside.
[0062] S4, weigh Al, Co, Cr, Fe, Ni pure metal raw materials and Dy pure active raw materials according to the ratio; the atomic percentage content of Dy is 0.02at%; the atomic percentage content ratio of Al, Co, Cr, Fe, Ni is 1:1:1:1, before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni are placed in the order of melting point from low to high, Al, Dy, Ni, Co, Fe, Cr are placed in Nb foil in turn, wrapped together and placed at the bottom of the copper crucible, the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 4-5×10 -3 Pa, and high-purity argon gas is filled to 1.0×105Pa for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make the various elements in the material more evenly distributed and reduce the internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is ground with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the cleaning time is 10min, and then it is placed in an 80℃ oven for drying.
[0063] S5. Use 60# water-abrasive sandpaper to remove the oil stains on the surface of the high entropy alloy target prepared in step S4, and then place it in a 99.9% alcohol solution for ultrasonic cleaning to remove dirt. Under the condition of an ultrasonic frequency of 53KHz, after cleaning for 10 minutes, place it in an oven for drying and set aside.
[0064] S6. Preparation of high entropy alloy thin films with uniform composition by magnetron sputtering
[0065] The Ti-45Al-8Nb (at.%) substrate dried in S3 was mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S5 was placed on the RF target for sputtering. The magnetron sputtering process parameters were adjusted as follows: the temperature of the Ti-45Al-8Nb substrate was 80 °C, the power of the high entropy alloy target was 300 W, the sputtering time was 8 h, the gas pressure was 0.4 Pa, and the vacuum degree was 1x10 -4 Pa.
[0066] Depend on Figure 4 It can be seen that the anti-oxidation performance of the modified example doped with Dy only is slightly worse than that of the modified example co-doped with Dy and Hf.
[0067] Comparative Example 2
[0068] In this comparative example, the atomic percentage content of pure Dy active material is 0 at %, the atomic percentage content of pure Hf active material is 0.02 at %, and the remaining steps and parameters are the same as those in Example 1.
[0069] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix with a size of 10×10×2 mm was obtained by vacuum non-consumable arc melting technology.
[0070] S2. The Ti-45Al-8Nb (at.%) substrate prepared in step S1 is polished with 200#, 400#, 800#, 1000#, and 1200# water-abrasive sandpaper in sequence, and then polished to a mirror surface with a polishing machine.
[0071] S3. The polished Ti-45Al-8Nb (at.%) substrate obtained in step S2 is placed in an alcohol solution with a mass fraction of 99.9% for ultrasonic cleaning to remove dirt. The ultrasonic frequency is 53 KHz. After cleaning for 10 minutes, the substrate is placed in an oven at 80° C. for drying and then set aside.
[0072] S4, weigh Al, Co, Cr, Fe, Ni pure metal raw materials and Dy pure active raw materials according to the ratio; the atomic percentage content of Dy is 0.02at%; the atomic percentage content ratio of Al, Co, Cr, Fe, Ni is 1:1:1:1, before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni, in the order of melting point from low to high, Al, Ni, Co, Fe, Cr, Hf are sequentially placed in Nb foil, wrapped together and placed at the bottom of the copper crucible, the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 4-5×10 -3 Pa, and high-purity argon gas is filled to 1.0×105Pa for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make the various elements in the material more evenly distributed and reduce the internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is ground with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the cleaning time is 10min, and then it is placed in an 80℃ oven for drying.
[0073] S5. Use 60# water-abrasive sandpaper to remove the oil stains on the surface of the high entropy alloy target prepared in step S4, and then place it in a 99.9% alcohol solution for ultrasonic cleaning to remove dirt. Under the condition of an ultrasonic frequency of 53KHz, after cleaning for 10 minutes, place it in an oven for drying and set aside.
[0074] S6. Preparation of high entropy alloy thin films with uniform composition by magnetron sputtering
[0075] The Ti-45Al-8Nb (at.%) substrate dried in S3 was mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S5 was placed on the RF target for sputtering. The magnetron sputtering process parameters were adjusted as follows: the temperature of the Ti-45Al-8Nb substrate was 80 °C, the power of the high entropy alloy target was 300 W, the sputtering time was 8 h, the gas pressure was 0.4 Pa, and the vacuum degree was 1x10 -4 Pa. By Figure 4 It can be seen that the anti-oxidation performance of the modified example doped with Hf only is slightly worse than that of the modified example co-doped with Dy and Hf.
[0076] Comparative Example 3
[0077] In this comparative example, the atomic percentage content of pure Dy active material is 0 at %, the atomic percentage content of pure Hf active material is 0 at %, and the remaining steps and parameters are the same as those in Example 1.
[0078] S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb (at.%) matrix with a size of 10×10×2 mm was obtained by vacuum non-consumable arc melting technology.
[0079] S2. The Ti-45Al-8Nb (at.%) substrate prepared in step S1 is polished with 200#, 400#, 800#, 1000#, and 1200# water-abrasive sandpaper in sequence, and then polished to a mirror surface with a polishing machine.
[0080] S3. The polished Ti-45Al-8Nb (at.%) substrate obtained in step S2 is placed in an alcohol solution with a mass fraction of 99.9% for ultrasonic cleaning to remove dirt. The ultrasonic frequency is 53 KHz. After cleaning for 10 minutes, the substrate is placed in an oven at 80° C. for drying and then set aside.
[0081] S4, weigh Al, Co, Cr, Fe, Ni pure metal raw materials and Dy pure active raw materials according to the ratio; the atomic percentage content of Dy is 0.02at%; the atomic percentage content ratio of Al, Co, Cr, Fe, Ni is 1:1:1:1, before weighing the raw materials, the block, granular and flaky raw materials are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove the oxide film and other sediment impurities; then the weighed raw materials Al, Co, Cr, Fe, Ni are placed in the order of melting point from low to high, Al, Ni, Co, Fe, Cr, in Nb foil, wrapped together and placed at the bottom of the copper crucible, and the copper crucible is placed in a vacuum non-consumable arc melting furnace for melting, and the vacuum is evacuated to 4-5×10 -3 Pa, and high-purity argon gas is filled to 1.0×105Pa for protection, the raw material is repeatedly smelted 5-6 times under argon protection to make the various elements in the material more evenly distributed and reduce the internal stress, and magnetic stirring is turned on during the smelting process, and a modified AlCoCrFeNi high entropy alloy target is obtained after smelting, and then the modified AlCoCrFeNi high entropy alloy target is cut by a wire cutting process, and the surface oil is ground with water abrasive paper; the modified AlCoCrFeNi high entropy alloy target with oil removed is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the cleaning time is 10min, and then it is placed in an 80℃ oven for drying.
[0082] S5. Use 60# water-abrasive sandpaper to remove the oil stains on the surface of the high entropy alloy target prepared in step S4, and then place it in a 99.9% alcohol solution for ultrasonic cleaning to remove dirt. Under the condition of an ultrasonic frequency of 53KHz, after cleaning for 10 minutes, place it in an oven for drying and set aside.
[0083] S6. Preparation of high entropy alloy thin films with uniform composition by magnetron sputtering
[0084] The Ti-45Al-8Nb (at.%) substrate dried in S3 was mounted on the fixture of the magnetron sputtering equipment, and the high entropy alloy target dried in S5 was placed on the RF target for sputtering. The magnetron sputtering process parameters were adjusted as follows: the temperature of the Ti-45Al-8Nb substrate was 80 °C, the power of the high entropy alloy target was 300 W, the sputtering time was 8 h, the gas pressure was 0.4 Pa, and the vacuum degree was 1x10 -4 Pa.
[0085] Example 4
[0086] Oxidation performance is one of the important properties of TiAl alloy. This application characterizes the oxidation performance of TiAl alloy of Dy and Hf modified AlCoCrFeNi high entropy alloy film and TiAl alloy of unmodified AlCoCrFeNi high entropy alloy film through high temperature oxidation experiment. The specific steps are as follows:
[0087] Step 1: Place the sample in anhydrous ethanol, ultrasonically clean for 10 minutes, blow dry with cold air, measure the sample size and weigh the original weight.
[0088] Step 2: Place the 95% porcelain alumina crucible and porcelain boat into anhydrous ethanol, ultrasonically treat for 10 minutes, and blow dry for later use.
[0089] Step 3: The high-temperature oxidation tube furnace is heated to 900°C. An S-type platinum-rhodium thermocouple is used to calibrate the temperature of the tube furnace. One end of the thermocouple is placed in the constant temperature zone of the tube furnace. The other end of the thermocouple is connected to a digital potentiometer to measure the actual temperature inside the furnace tube and adjust the equipment to the accurate operating temperature.
[0090] Step 4: Place the cleaned 95% porcelain alumina crucible and porcelain boat in a tube furnace and dry for 30 minutes to remove ethanol and other impurities.
[0091] Step 5: Place the sample in an alumina crucible, and use nickel-chromium wire to mark the number on the surface of the crucible and the crucible cover, put them into a porcelain boat, and push the porcelain boat to the constant temperature zone of the tube furnace.
[0092] Step 6: After oxidation for 1, 5, 10, 24, 48, 72, and 100 hours, take out the sample, cool it to room temperature with a fan, weigh it, and store it in a sample box.
[0093] Therefore, the present application provides a method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film to improve the oxidation resistance of TiAl alloy, and the obtained modified AlCoCrFeNi high entropy alloy film improves the oxidation resistance of TiAl alloy.
[0094] In the description of this specification, the description with reference to the terms "an experimental example", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the experimental example or example are included in at least one experimental example or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same experimental example or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more experimental examples or examples in a suitable manner.
[0095] Finally, it should be noted that the above experimental examples are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred experimental examples, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.
Claims
1. A method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloys, characterized in that: The following steps are involved: S1. Using Ti, Al and Nb as synthetic raw materials, a Ti-45Al-8Nb matrix was prepared by vacuum non-consumable arc melting technology; S2. Weigh pure metal raw materials Al, Co, Cr, Fe, Ni and pure active raw materials Dy and Hf, and prepare modified AlCoCrFeNi high entropy alloy target by vacuum non-consumable arc melting technology; S3. Mount the Ti-45Al-8Nb substrate in step S1 on a fixture of a magnetron sputtering device, place the modified AlCoCrFeNi high entropy alloy target in step S2 on a radio frequency target, and use magnetron sputtering technology to obtain a TiAl alloy covered with a modified AlCoCrFeNi high entropy alloy film.
2. The method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloy according to claim 1, characterized in that: In step S3, the magnetron sputtering parameters are: the temperature of the Ti-45Al-8Nb substrate is 80-100°C, the power of the AlCoCrFeNi high entropy alloy target is 300W, the sputtering time is 7-8h, the gas pressure is 0.4Pa, and the vacuum degree is 1x10 -4 ~6x10 -4 Pa.
3. The method for improving the oxidation resistance of TiAl alloy by depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film according to claim 1, characterized in that: Step S1 also includes the following steps: 1) The prepared Ti-45Al-8Nb matrix is cut into a sample by a wire cutting process, and the sample is polished with water-abrasive sandpaper and then polished to a mirror surface by a polishing machine; 2) The Ti-45Al-8Nb substrate polished in step 1) is placed in an alcohol solution for ultrasonic cleaning, the ultrasonic frequency is 50-60KHz, the ultrasonic cleaning time is 10-20min, and after ultrasonic cleaning, it is placed in an oven at 80°C for drying.
4. The method for improving the oxidation resistance of TiAl alloy by depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film according to claim 1, characterized in that: Step S2 also includes the following steps: (1) cutting the modified AlCoCrFeNi high entropy alloy target by wire cutting and grinding the surface oil by sandpaper; (2) The modified AlCoCrFeNi high entropy alloy target treated in step (1) is placed in an alcohol solution for ultrasonic cleaning at an ultrasonic frequency of 50 to 60 kHz for a cleaning time of 10 to 20 min, and then placed in an oven at 80° C. for drying.
5. The method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloy according to claim 1, characterized in that: In the modified AlCoCrFeNi high entropy alloy target, the doping amount of Dy and Hf is 0.01-0.03%at.
6. The method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloy according to claim 4, characterized in that: In the modified AlCoCrFeNi high entropy alloy target, the atomic ratio of Al, Co, Cr, Fe and Ni is 1:1:1:1:
1.
7. The method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloy according to claim 3, characterized in that: In the step 1), the sample is polished with 200#, 400#, 800#, 1000# and 1200# water-abrasive sandpaper in sequence.
8. A method for improving the oxidation resistance of TiAl alloy by depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film according to claim 3 or 4, characterized in that: The mass fraction of the alcohol solution is 85-99.9%.
9. The method for depositing Dy and Hf modified AlCoCrFeNi high entropy alloy thin films to improve the oxidation resistance of TiAl alloy according to claim 1, characterized in that: Before weighing pure metal raw materials Al, Co, Cr, Fe, Ni and pure active raw materials Dy and Hf, the block, granular and flaky pure metal raw materials Al, Co, Cr, Fe, Ni and pure active raw materials Dy and Hf are mechanically polished and ultrasonically cleaned in acetone or anhydrous ethanol to remove oxide film and sediment impurities, and then placed in Nb foil in order from low to high melting point, wrapped together and placed at the bottom of a copper crucible for smelting.
10. The method for improving the oxidation resistance of TiAl alloy by depositing Dy and Hf modified AlCoCrFeNi high entropy alloy film according to claim 9, characterized in that: During melting, vacuum is drawn to 4~5×10 -3 Pa, and filled with high-purity argon gas to 1.0×10 5 Pa is used for protection, and the raw materials are repeatedly melted 5-6 times under argon protection.
Citation Information
Patent Citations
Material for dual active element co-doping thermal barrier coating bonding layer and preparation method
CN103966602A
Long-life anti-oxidation high-entropy bonding layer material and preparation method thereof
CN113881884A
Novel rare earth tantalate / platinum-iridium-based alloy thermal barrier coating, preparation method and application
CN114959542A
Composite magnetic conductive layer for cookware, preparation method of composite magnetic conductive layer and cookware
CN115161638A
Refractory high-entropy alloy with high-temperature ablation resistance and high-temperature oxidation resistance and preparation method of refractory high-entropy alloy
CN117403117A
Cited By
Preparation method of high-temperature wear-resistant multilayer material on surface of precision part