Preparation method of crystalline silicon-broadband gap compound heterojunction solar cell
Through in-situ plasma processing and interface passivation process, the work function of V2OX film is regulated, the work function modulation problem of TMOs material is solved, the efficiency of crystalline silicon/compound heterojunction solar cells is improved, and more efficient carriers are achieved Transmission and passivation contact characteristics.
Patent Information
- Application Number
- CN202410987631.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-23
AI Technical Summary
The prior art is difficult to accurately modulate the work function of transition metal oxide (TMOs) materials, resulting in difficulty in improving its carrier selectivity and transmission capacity, limiting the efficiency improvement of crystalline silicon/compound heterojunction solar cells.
In situ plasma treatment method is adopted, by introducing hydrogen/oxygen/fluorine plasma during the atomic layer deposition process, the work function of the V2OX film is regulated, and the passivation characteristics of the c-Si/TMOs interface are optimized, Improve the passivation contact characteristics of the hole transport layer.
The conversion efficiency of crystalline silicon/compound heterojunction solar cells is improved, and the carrier transmission performance and interface passivation effect are enhanced by precisely regulating the work function and conductivity of TMOs materials.
Smart Images

Figure CN118932314A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of solar cells, and in particular to a method for preparing a crystalline silicon-wide bandgap compound heterojunction solar cell. Background Art
[0002] Silicon-based solar cells dominate the photovoltaic market, and the current cell is PERC (Passivated Emitter and Rear Solar Cell). Since the metal electrode in the rear contact area of the structure is in direct contact with the silicon substrate, and the carrier recombination is serious in this area, its theoretical efficiency limit is limited to about 24.5%. The industry continuously reduces the contact area to make the power conversion efficiency (PCE) close to this limit, and further efficiency development requires the search for new solar cell technology. Therefore, TOPCon (Tunnel Oxide Passivated Contact) and SHJ (Silicon Hereto-junction) based on passivation contact technology came into being and gradually replaced PERC solar cells to further improve PCE. However, due to the use of amorphous silicon and transparent conductive oxide (usually indium tin oxide) in SHJ and the use of doped polycrystalline silicon in TOPCon, these two cells have serious parasitic absorption, that is, the problem of low short-circuit current density. In order to increase JSC and thus efficiency at a lower cost, people are committed to studying wide bandgap, high work function, undoped materials, especially transition metal oxides (TMOs) to replace P-type doped amorphous silicon (a-Si:H(p)) or P-type doped polysilicon layers as new hole transport layers. TMOs with high work function and wide bandgap can induce upward bending of the energy band on the c-Si surface, thereby achieving the effect of hole transport. Among them, the high work function characteristics and energy band matching of TMOs (the conduction band of TMOs is similar to the valence band energy of c-Si) are the key to achieving excellent hole transport characteristics, and the work function is closely related to the oxygen vacancy defects of the TMOs themselves. If there are more oxygen vacancies, the work function is low, and if there are fewer oxygen vacancy defects, the work function increases. Transition metal oxides used as hole transport layers mainly include molybdenum oxide (MoO X ), vanadium oxide (V2O X ), tungsten oxide (WO X )wait.
[0003] MoO X It is considered to be the most successful hole transport layer to date, with a high work function (>5eV) and a wide band gap (~3.0eV). The conversion efficiency has been increased from the initial 16.7% to the current highest 23.83%. Its interface passivation layer is plasma-treated intrinsic hydrogenated amorphous silicon. XCompared with V2O X With a higher work function, it can produce a larger upward bending of the energy band on the c-Si surface to produce better hole transport characteristics. The efficiency of the device grown directly on the surface of the silicon wafer is 19.77%. After the interface is inserted with intrinsic hydrogenated amorphous silicon, the efficiency is increased to 21.6%. Similarly, by using the c-Si / tungsten oxide (WO X ) introduces an intrinsic hydrogenated amorphous silicon interface layer between the two layers, increasing the efficiency to 17.9%. In addition, the hole transport layer of cuprous oxide (Cu2O) and nickel oxide (NiO X ) were grown on alumina (Al2O X ) and silicon oxide (SiO X )A hole-passivated contact stack is formed on the interface passivation layer, with efficiencies reaching 20.35% and 19.2%, respectively.
[0004] Through the above development of transition metal oxides for hole transport layers, the way to improve the efficiency of devices is mainly focused on adding an interface passivation layer and pre-treating the passivation layer to improve the passivation contact properties. The key to improving the PCE of TMO-based hole transport layer devices is to improve the carrier selectivity or transport capacity of TMOs, which depends on the work function and band structure of the TMOs material itself. The work function and band structure are closely related to external excitation and stoichiometry / defects, such as the deposition process, oxygen vacancies (V O In previous studies, oxygen vacancies and ion doping usually improve the conductivity or electron selectivity of TMOs, but reduce the high work function and hole selectivity of TMOs. This is because it is impossible to adjust the V O This is caused by the lack of effective modification of the TMOs material itself, which is caused by the precise modulation of the work function by adjusting the content of doping atoms.
[0005] At present, the methods to improve the PCE of hole transport layer devices based on TMOs are mainly focused on interface research, that is, adding an interface passivation layer between c-Si and TMOs and pre-treating the interface passivation layer to improve the passivation contact properties. The purpose of interface research is to reduce the redox reaction between TMOs and the silicon surface, reduce the oxygen vacancies in the TMOs themselves, and prevent the reduction of the work function of TMOs. However, improving the PCE of hole transport layers based on TMOs is mainly to improve the carrier selectivity or transport capacity of the TMOs material itself. This ability is highly dependent on the work function and band structure of the material itself, which are closely related to external excitation and stoichiometry / defects, such as deposition process, oxygen vacancies (V O ) and ion doping. Previous studies have been unable to precisely modulate the work function, making it difficult to improve carrier selectivity and transport capabilities. Summary of the invention
[0006] In order to overcome the problems existing in the prior art, the present invention provides a method for regulating the work function of a hole transport layer by in-situ plasma treatment and a method for preparing a solar cell. The method is universal for TMOs used as hole transport layers, for example, for MoO X , WO X and V2O X Specifically, V2O is grown by atomic layer deposition. X Taking in-situ HPT / OPT / FPT as an example, the number of cycles of VTIP and deionized water precursor (i.e., atomic layer deposition of a certain thickness of V2O X ) and then perform a HPT / OPT / FPT treatment to adjust V2O by changing the value of n. X Work function of thin films, and simultaneous regulation of c-Si / V2O X Passivation characteristics between interfaces. Final ALD-V2O X In-situ HPT / OPT / FPT treatment improves c-Si / V2O X Passivation contact properties of hole transport stacks improve V2O-based X The device conversion efficiency of thin-film solar cells. In addition, this method can be combined with the interface passivation process to further improve the device efficiency. The introduction of hydrogen / oxygen / fluorine can optimize the passivation contact characteristics of the c-Si / TMOs interface, that is, improve chemical passivation and field effect passivation; the introduction of hydrogen / oxygen / fluorine can achieve the balanced regulation of the work function and conductivity of the TMOs material itself, and optimize the carrier transmission performance.
[0007] The present invention prepares a high-efficiency crystalline silicon / compound heterojunction solar cell based on the hydrogen / oxygen / fluorinated TMOs process: the back surface hole transport stack of the crystalline silicon / compound heterojunction solar cell is c-Si(p) / TMOs, and the present invention specifically is c-Si(p) / HPT / OPT / FPT-V2O X (Hydrogen / Oxygen / Fluoride Vanadium Oxide), compared to c-Si(p) / i-V2O X (intrinsic vanadium oxide), the photoelectric parameters are comprehensively improved, and the device conversion efficiency is greatly improved.
[0008] In order to achieve the above object, the technical solution adopted by the present invention is:
[0009] The first aspect of the present invention provides a method for in-situ modification of a transition metal oxide, comprising the following steps:
[0010] Place a P-type silicon wafer in a plasma enhanced atomic layer deposition chamber and use an atomic layer deposition method to prepare pure transition metal oxides; after n cycles of pure transition metal oxides, add a modified gas plasma treatment once, which is a large cycle, and then repeat N large cycles to achieve in-situ modification of transition metal oxides;
[0011] The modified gas is one of hydrogen-containing gas, oxygen, or fluorine-containing gas.
[0012] Preferably, the P-type silicon wafer has a thickness of 160 μm and a resistivity of 0.6-1.0 ohm·cm.
[0013] Preferably, the P-type silicon wafer needs to be cleaned first, and the cleaning steps include tetramethylammonium hydroxide solution (TMAH) cleaning and standard RCA cleaning; more preferably, the TMAH cleaning specifically includes: putting TMAH with a concentration of 25% into a water bath at a temperature of 90°C, and immersing the basket containing the P-type silicon wafer in TMAH for cleaning for 10 minutes after the TMAH solution rises to 70°C; the standard RCA cleaning specifically includes: taking out the P-type silicon wafer after TMAH cleaning, washing it with deionized water, and then immersing it in a 70-80°C RCA1 solution for cleaning for 10 minutes, taking it out, immersing it in a 2% hydrofluoric acid (HF) solution for 1 minute, taking it out, immersing it in a 70-80°C RCA2 solution for cleaning, taking it out, immersing it in a 2% HF solution, and taking it out for use. The P-type silicon wafer needs to be cleaned with deionized water three times each time before proceeding to the next step.
[0014] Preferably, the preparation process of the pure transition metal oxide is: placing a P-type silicon wafer into a plasma enhanced atomic layer deposition chamber, the chamber temperature is 100-350°C, turning on the mechanical pump switch to evacuate the chamber, and growing a pure transition metal oxide film through n cycles of transition metal precursors and oxygen precursors; the transition metal precursor is one of molybdenum hexacarbonyl, tungsten hexacarbonyl, triisopropoxy vanadium oxide, dimethylamino molybdenum, tricarbonyl cycloheptatrienyl molybdenum, ethyl vanadium butyrate amide, vanadium acetate, and dimethylethylenediamine vanadium; the oxygen precursor is deionized water or ozone; further preferably, the chamber is evacuated to a vacuum degree lower than 5E-2torr.
[0015] Preferably, the value of n is 5-100, and the value of N is 1-40.
[0016] Further preferably, when the modified gas is a hydrogen-containing gas, the value of n is 5-10, and the value of N is 10-20; when the modified gas is oxygen, the value of n is 40-60, and the value of N is 1-3.
[0017] Preferably, the hydrogen-containing gas is selected from argon-hydrogen mixed gas, nitrogen-hydrogen mixed gas, and hydrogen; when the hydrogen-containing gas is argon-hydrogen mixed gas or nitrogen-hydrogen mixed gas, the content of hydrogen is 10%.
[0018] Preferably, the fluorine-containing gas is selected from carbon tetrafluoride, nitrogen trifluoride and sulfur hexafluoride.
[0019] Preferably, the gas flow rate of the modified gas plasma treatment is 100-140 sccm, the power is 20-250 W, and the time of one modified gas plasma treatment is 0.5-1200 s.
[0020] Further preferably, when the modifying gas is a hydrogen-containing gas, the time for one modifying gas plasma treatment is 2-4 s; when the modifying gas is oxygen, the time for one modifying gas plasma treatment is 1-3 s.
[0021] A second aspect of the present invention provides a heterojunction solar cell, wherein the structure of the heterojunction solar cell includes a hole transport layer, and the hole transport layer is prepared by the in-situ modification method of the transition metal oxide.
[0022] Preferably, the structure of the heterojunction solar cell includes, from bottom to top, a back full-area electrode, a hole transport layer, a silicon substrate, an N+ / N++ doped layer, a passivation layer, an anti-reflection layer, and a gate electrode;
[0023] The area of the N+ / N++ doped layer corresponding to the gate line electrode is an N++ doped layer, and the rest of the area is an N+ doped layer.
[0024] The third aspect of the present invention provides a method for preparing the heterojunction solar cell, comprising the following steps:
[0025] (1) Texturing the front surface and polishing the back surface of the P-type silicon substrate;
[0026] (2) diffusing phosphorus on the front surface of the substrate to form an N+ doped layer to form a pn junction; performing laser N-type heavy doping on the metal gate line area on the front surface of the silicon substrate to form an N++ doped layer;
[0027] (3) removing the PSG layer at the edge and back of the substrate and polishing the back of the substrate;
[0028] (4) oxidizing the front and back surfaces of the substrate to generate silicon dioxide, and removing the silicon dioxide on the front surface;
[0029] (5) depositing a passivation layer and an anti-reflection layer in sequence on the front surface of the substrate; performing screen printing on the corresponding N++ doped region on the anti-reflection layer to obtain the gate line electrode;
[0030] (6) removing silicon dioxide from the back surface of the substrate;
[0031] (7) preparing a hole transport layer on the back surface of the substrate, wherein the hole transport layer is prepared by the in-situ modification method of the transition metal oxide;
[0032] (8) Ag is thermally evaporated on the hole transport layer to form the back full-area electrode.
[0033] Preferably, in step (2), the phosphorus diffusion is liquid POCl3, and the phosphorus doping concentration is 1E20-1E22 atoms / cm 3 , the doping depth (pn junction) is 150-300nm.
[0034] Preferably, in step (2), the laser N-type heavy doping is laser doping of phosphorus, and the doping concentration is 1E22-1E23atoms / cm 3 .
[0035] Preferably, in step (3), HF is used to remove the PSG layer.
[0036] Preferably, in step (4), the growth mode of the silicon dioxide is thermal oxidation growth, and the specific steps are: the substrate is placed in an oxidation furnace at 740-760° C., nitrogen and oxygen gas are introduced, and the oxidation time is 28-32 minutes.
[0037] Preferably, in step (6), HF is used to remove silicon dioxide, and the HF concentration is 2-5 wt%.
[0038] Preferably, the thickness of the passivation layer is 10-20 nm, the thickness of the anti-reflection layer is 60-80 nm, the thickness of the hole transport layer is 2-13 nm, and the thickness of the back full-area electrode is 100-1000 nm.
[0039] Preferably, the material of the passivation layer includes aluminum oxide; and the material of the anti-reflection layer includes silicon nitride.
[0040] Compared with the prior art, the present invention has the following beneficial effects:
[0041] Compared to passivating the silicon surface and inhibiting the redox reaction between the silicon surface and transition metal oxides by growing an interface layer, such as growing silicon oxide, aluminum oxide, and intrinsic hydrogenated amorphous silicon, the present invention performs in-situ hydrogen-oxygen plasma treatment during the atomic layer deposition of transition metal oxides, accurately controls the work function of the TMOs material itself, achieves effective material modification, and optimizes the c-Si / TMOs interface passivation contact characteristics. On the one hand, the HPT / FPT treatment effectively introduces hydrogen / fluorine atoms, and the hydrogen / fluorine atoms bond to silicon at the interface of c-Si / TMOs, passivating additional silicon surface dangling bonds, achieving good chemical passivation. At the same time, after the interface hydrogen / fluorine atoms bond to the dangling bonds, they promote the electrons on the interface to move to the silicon side, forming an electric field pointing from the outside to the inside relative to silicon, eliminating the interface dipole while bending the energy band on one side of the silicon surface upward, enhancing the hole transmission effect. On the other hand, the OPT treatment effectively reduces V OThe content increases the work function of TMOs, making the energy band on one side of the silicon surface bend upward more, enhancing the field passivation effect and improving the passivation contact characteristics.
[0042] In summary, the present invention realizes in-situ hydrogen / oxygen / fluorine plasma treatment of atomic layer deposition transition metal oxides, the introduction of hydrogen / fluorine atoms, and enhanced chemical passivation and field effect passivation of the interface. At the same time, it realizes in-situ oxygen plasma treatment of atomic layer deposition transition metal oxides, improves the work function of TMOs materials, and enhances interface field effect passivation. Further, the conversion efficiency of crystalline silicon / compound heterojunction solar cell devices is improved based on HPT treatment. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 The passivation contact performance at different HPT ratios and different HPT times;
[0044] Figure 2 The passivation contact performance with different OPT treatment times;
[0045] Figure 3 A structural diagram of a heterojunction solar cell according to the present invention;
[0046] Figure 4 The JV curves of solar cells with intrinsic vanadium oxide and hydrogenated vanadium oxide as hole transport layers;
[0047] Attached Figure 3 Marking in the middle: 1-gate line electrode, 2-N++ heavily doped layer, 3-anti-reflection layer, 4-passivation layer, 5-N+ doped layer, 6-substrate, 7-hole transport layer, 8-full area electrode. DETAILED DESCRIPTION
[0048] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0049] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0050] Example 1
[0051] V2O X For example, this embodiment provides a method for in-situ hydrogen plasma treatment of atomic layer deposition TMOs, including the following steps:
[0052] (1) TMAH cleaning: double-sided polished crystalline silicon substrate (P-type silicon wafer, resistivity 0.6-1.0 ohm·cm, thickness 160 um) was cut into 4 cm*4 cm squares, placed in a flower basket, and the silicon wafer was immersed in a 90°C water bath heated TMAH solution (25% aqueous solution) for cleaning for 10 min. The silicon wafer was taken out and washed three times with deionized water for later use;
[0053] (2) RCA cleaning: The P-type silicon wafer cleaned in step (1) is immersed in an RCA1 solution (50 ml ammonia water + 50 ml hydrogen peroxide + 300 ml deionized water) heated in a water bath at 80°C for 10 min, taken out, and washed three times with deionized water, immersed in a 2% HF solution for 1 min, taken out, and washed three times with deionized water, immersed in an RCA2 solution (60 ml ammonia water + 60 ml hydrochloric acid + 300 ml deionized water) heated in a water bath at 80°C for 10 min, taken out, and washed three times with deionized water, immersed in a 2% HF solution for 1 min, taken out, and washed three times with deionized water for later use;
[0054] (3) Atomic layer deposition of V2O X Thin film: Place the P-type silicon wafer after the above cleaning into the PEALD chamber, evacuate to 5E-2torr, and grow pure V2O through n cycles of precursors of triisopropoxy vanadium oxide and deionized water. X Thin films, depositing intrinsic vanadium oxide thin films for fixed n (5 / 10 / 25 / 50 / 100) cycles;
[0055] (4) In-situ hydrogen plasma treatment with a fixed total number of cycles: after depositing the intrinsic vanadium oxide film for a fixed number of cycles of n, an in-situ hydrogen plasma treatment is performed, wherein the gas is an argon-hydrogen mixed gas of Ar:H2=90%:10%, the gas flow rate is 120sccm, the plasma power is 70W, the plasma treatment time is 3s, and the intrinsic vanadium oxide is deposited for a fixed number of times n (5 / 10 / 25 / 50 / 100) and treated with hydrogen plasma once as a small cycle, and the small cycle is subjected to a large cycle of N (1 / 2 / 4 / 10 / 20) times, with a total number of cycles of 100 cycles (in terms of n), and the film thickness is about 6nm; a hydrogenated vanadium oxide film is grown on both sides of a P-type silicon wafer substrate to prepare a passivation test sample; a hydrogenated vanadium oxide film is grown on one side of a P-type silicon wafer substrate, and then 300nm to 500nm of silver (Ag) is grown on the hydrogenated vanadium oxide film using a transmission line model (TLM) metal mask to prepare a contact test sample;
[0056] (5) In-situ hydrogen plasma treatment with a fixed doping ratio: that is, the doping ratio is n:1=5:1, the plasma treatment time is (1 / 3 / 4.5 / 6 / 10s), and a large cycle of N=20 is performed, the total number of cycles is 100 cycles, and the film thickness is about 6nm; a hydrogenated vanadium oxide film is grown on both sides of a P-type silicon wafer substrate to prepare a passivation test sample; a hydrogenated vanadium oxide film is grown on one side of a P-type silicon wafer substrate, and then 300nm~500nm of Ag is grown on the hydrogenated vanadium oxide film using a TLM metal mask to prepare a contact test sample.
[0057] Passivation contact test: Minority carrier lifetime test equipment (WCT-120) tests hidden open circuit voltage (iV OC ), four-probe test and TLM method to extract contact resistance (ρ c );like Figure 1 As shown, for different HPT ratio variables, the iV of 6nm native vanadium oxide without HPT treatment OC is 609.1mV, c 47mΩ·cm 2 ; After HPT treatment, as the HPT ratio increases, the passivation increases first and then decreases, and the contact decreases first and then increases, especially when the HPT ratio is 5:1, iV OC is 654.9mV, C 43mΩ·cm 2 For different HPT treatment time variables, after HPT treatment, as the HPT time increases, the passivation gradually increases, and the contact generally decreases first and then increases, especially when the HPT time is 3s, iV OC is 654.6mV, C 43mΩ·cm 2 Compared with the samples without HPT treatment, the passivation contact performance of the samples treated with different HPT ratios was improved, and the passivation of the samples treated with different HPT times was improved. The contact resistance first decreased and then increased, which may be related to the decrease in the work function of hydrogenated vanadium oxide itself. But in general, the passivation contact performance of c-Si / TMOs stack can be improved by adjusting the HPT ratio and time.
[0058] Example 2
[0059] V2O X For example, the present invention provides a method for in-situ oxygen plasma treatment of atomic layer deposition TMOs, comprising the following steps:
[0060] (1) TMAH cleaning: double-sided polished crystalline silicon substrate (P-type silicon wafer, resistivity 0.6-1.0 ohm·cm, thickness 160 um) was cut into 4 cm*4 cm squares, placed in a flower basket, and the silicon wafer was immersed in a 90°C water bath heated TMAH solution (25% aqueous solution) for cleaning for 10 min. The silicon wafer was taken out and washed three times with deionized water for later use;
[0061] (2) RCA cleaning: The P-type silicon wafer cleaned in step 1 is immersed in an RCA1 solution (50 ml ammonia water + 50 ml hydrogen peroxide + 300 ml deionized water) heated in a water bath at 80°C for 10 min, taken out, and washed three times with deionized water, immersed in a 2% HF solution for 1 min, taken out, and washed three times with deionized water, immersed in an RCA2 solution (60 ml ammonia water + 60 ml hydrochloric acid + 300 ml deionized water) heated in a water bath at 80°C for 10 min, taken out, and washed three times with deionized water, immersed in a 2% HF solution for 1 min, taken out, and washed three times with deionized water for later use;
[0062] (3) Atomic layer deposition of V2O X Thin film: Place the P-type silicon wafer after the above cleaning into the PEALD chamber, evacuate to 5E-2torr, and grow pure V2O through n cycles of precursors of triisopropoxy vanadium oxide and deionized water. X Thin films, depositing intrinsic vanadium oxide thin films for fixed n (50) cycles;
[0063] (4) In-situ oxygen plasma treatment at different times: After depositing the fixed n cycles of intrinsic vanadium oxide thin film, an in-situ oxygen plasma treatment is performed, in which the gas is ultrapure oxygen, the gas flow rate is 120 sccm, the plasma power is 50 W, and the plasma treatment time is X (2 / 5 / 8) s. The intrinsic vanadium oxide is deposited for a fixed number of n (50) times and then treated with oxygen plasma once as a small cycle, and the small cycle is subjected to N (2) large cycles, with a total number of cycles of 100 cycles (in terms of n), and the film thickness is about 6 nm; a vanadium oxide thin film is grown on both sides of a P-type silicon wafer substrate to prepare a passivation test sample; a vanadium oxide thin film is grown on one side of a P-type silicon wafer substrate, and then 300 nm to 500 nm of silver (Ag) is grown on the hydrogenated vanadium oxide thin film using a transmission line model (TLM) metal mask to prepare a contact test sample.
[0064] Passivation contact test: Minority carrier lifetime test equipment (WCT-120) tests hidden open circuit voltage (iV OC ), four-probe test and TLM method to extract contact resistance (ρ C );like Figure 2As shown in the figure, for different OPT treatment time variables, after OPT treatment, as the OPT time increases, the passivation first increases and then decreases, and the contact generally decreases first and then increases. Especially when the OPT time is 2s, iV OC is 622.4mV, C 23mΩ·cm 2 Compared with the samples without OPT treatment, the passivation contact of the samples treated with 2s OPT was improved, which means that the passivation contact performance of c-Si / TMOs stack can be improved by adjusting the OPT time.
[0065] Example 3
[0066] This example is based on the hydrogenation of V2O described in Example 1 above. X As a hole transport layer, a hybrid crystalline silicon / compound heterojunction solar cell is provided.
[0067] like Figure 3 As shown, the hydrogenated V2O X The structure of the crystalline silicon / compound heterojunction solar cell as a hole transport layer is: a P-type silicon wafer 6 is used as a substrate, the P-type silicon has a pyramid front surface and a polished back surface, the front surface of the P-type silicon 6 has an N+ doped layer 5, an N++ heavily doped layer 2, a passivation layer 4, an anti-reflection layer 3 and a gate line electrode 1, and the back surface of the P-type silicon 6 has a hole transport layer (hydrogenated vanadium oxide) 7 and a full-area electrode 8.
[0068] Hydrogenated V2O X The method for preparing a crystalline silicon / compound heterojunction solar cell as a hole transport layer comprises the following steps:
[0069] (1) Select a P-type silicon wafer 6 with a resistivity of 0.7 to 1 ohm·cm, and texture the front surface of the P-type silicon substrate 6 to a texture thickness of 5 μm and a reflectivity of 7.5%. Polish the back surface of the P-type silicon substrate 6 using a 70° C. 50% sodium hydroxide solution as the polishing solution;
[0070] (2) Phosphorus is diffused on the front side of the silicon substrate 6 to form an N+ doped layer 5 to form a pn junction. The temperature is maintained at 1100° C. Phosphorus is diffused on the front side of the silicon substrate. The phosphorus source is POCl3 and the phosphorus doping concentration is 4E21 atoms / cm 3 , the junction depth is 250nm;
[0071] (3) Laser scanning doping is performed on the metal gate line area on the front side of the silicon substrate 6 to form the N++ heavily doped layer 2 with a doping concentration of 5E22 atoms / cm 3 ;
[0072] (4) Using 40% HF to remove the PSG layer on the edge and back, using NaOH solution to neutralize HF and complete etching and polishing on the back of the silicon wafer;
[0073] (5) Using thermal oxidation to prepare silicon dioxide on the front and back surfaces, the silicon substrate 6 is placed in an oxidation furnace at 750° C., nitrogen and oxygen gas are introduced, and the oxidation time is 30 minutes; 2% HF is used to remove the silicon dioxide on the front surface;
[0074] (6) depositing the aluminum oxide passivation layer 4 on the front surface of the silicon substrate 6 by using the ALD process, with a thickness of 10 nm;
[0075] (7) depositing the silicon nitride passivation anti-reflection layer 3 on the front side of the silicon substrate 6 by using a PECVD process, with a thickness of 70 nm;
[0076] (8) Screen printing is performed on the N++ heavily doped region 2 on the front side of the silicon substrate 6 to obtain the gate line Ag electrode 1;
[0077] (9) Using 2% HF to remove silicon dioxide from the back surface;
[0078] (10) ALD is used to grow intrinsic vanadium oxide and hydrogenated vanadium oxide on the back surface of the silicon substrate 6 to prepare the hole transport layer 7. The preparation process is based on Example 1. The thickness is 6 nm. During the growth of hydrogenated vanadium oxide, n is 5, N is 20, the hydrogenation power is 70 W, the flow rate of 90% / 10% argon-hydrogen mixed gas is 120 sccm, and the hydrogenation treatment time is 3 s.
[0079] (11) Ag is grown on the back side of the silicon substrate 6 by thermal evaporation to form the back side full-area electrode 8 with a thickness of 300 nm. Finally, a V2O-based back surface X / Ag crystalline silicon / compound heterojunction solar cells.
[0080] Comparative Example 1
[0081] On the basis of Example 3, intrinsic vanadium oxide was prepared as a comparison. The difference between this comparative example and Example 3 is that in step (10), no in-situ hydrogen plasma treatment is performed.
[0082] Experimental results:
[0083] Figure 4 This is the JV curve of solar cells with intrinsic vanadium oxide and hydrogenated vanadium oxide as hole transport layers. Figure 4 As shown in Figure 2, when intrinsic vanadium oxide is used as a hole transport layer, the open circuit voltage is 644.9 mV and the short circuit current density is 40.39 mA / cm 2, the fill factor is 78.55%, and the battery conversion efficiency is 20.46%. When vanadium hydroxide is used as the hole transport layer, the open circuit voltage is 663.0mV and the short circuit current density is 41.07mA / cm 2 , the filling factor is 80.64%, and the cell conversion efficiency is 21.96%. It is proved that the method of in-situ hydrogenation growth of transition metal oxide as a hole transport layer proposed by the present invention can comprehensively improve the photoelectric performance parameters of the cell and greatly improve the conversion efficiency.
[0084] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for in-situ modification of transition metal oxides, It is characterized in that The following steps are involved: Place a P-type silicon wafer in a plasma enhanced atomic layer deposition chamber and use an atomic layer deposition method to prepare pure transition metal oxides; after n cycles of pure transition metal oxides, add a modified gas plasma treatment once, which is a large cycle, and then repeat N large cycles to achieve in-situ modification of transition metal oxides; The modified gas is one of hydrogen-containing gas, oxygen, or fluorine-containing gas.
2. The method for in-situ modification of transition metal oxides according to claim 1, It is characterized in that The preparation process of the pure transition metal oxide is as follows: a P-type silicon wafer is placed in a plasma enhanced atomic layer deposition chamber, the chamber temperature is 100-350° C., a mechanical pump switch is turned on to evacuate the chamber, and a pure transition metal oxide film is grown through n cycles of transition metal precursors and oxygen precursors; the transition metal precursor is one of molybdenum hexacarbonyl, tungsten hexacarbonyl, triisopropoxy vanadium oxide, dimethylamino molybdenum, tricarbonyl cycloheptatrienyl molybdenum, ethyl vanadium butyrate amide, vanadium acetate, and dimethylethylenediamine vanadium; the oxygen precursor is deionized water or ozone.
3. The method for in-situ modification of transition metal oxide according to claim 1, It is characterized in that The value of n is 5-100, and the value of N is 1-40.
4. The method for in-situ modification of transition metal oxides according to claim 1, It is characterized in that The gas flow rate of the modified gas plasma treatment is 100-140 sccm, the power is 20-250 W, and the time of one modified gas plasma treatment is 0.5-1200 s.
5. The method for in-situ modification of transition metal oxides according to claim 3, It is characterized in that When the modified gas is a hydrogen-containing gas, the value of n is 5-10, and the value of N is 10-20; when the modified gas is oxygen, the value of n is 40-60, and the value of N is 1-3.
6. The method for in-situ modification of transition metal oxides according to claim 4, It is characterized in that When the modifying gas is a hydrogen-containing gas, the time for one modifying gas plasma treatment is 2-4 s; when the modifying gas is oxygen, the time for one modifying gas plasma treatment is 1-3 s.
7. A heterojunction solar cell, It is characterized in that The structure of the heterojunction solar cell includes a hole transport layer, and the hole transport layer is prepared by the method for in-situ modification of a transition metal oxide according to any one of claims 1 to 6.
8. The heterojunction solar cell according to claim 7, It is characterized in that The structure of the heterojunction solar cell includes, from bottom to top, a back full-area electrode, a hole transport layer, a silicon substrate, an N+ / N++ doping layer, a passivation layer, an anti-reflection layer, and a gate electrode; The area of the N+ / N++ doped layer corresponding to the gate line electrode is an N++ doped layer, and the rest of the area is an N+ doped layer.
9. A method for preparing the heterojunction solar cell according to claim 7 or 8, It is characterized in that The following steps are involved: (1) Texturing the front surface and polishing the back surface of the P-type silicon substrate; (2) diffusing phosphorus on the front surface of the substrate to form an N+ doped layer to form a pn junction; performing laser N-type heavy doping on the metal gate line area on the front surface of the silicon substrate to form an N++ doped layer; (3) removing the PSG layer at the edge and back of the substrate and polishing the back of the substrate; (4) oxidizing the front and back surfaces of the substrate to generate silicon dioxide, and removing the silicon dioxide on the front surface; (5) depositing a passivation layer and an anti-reflection layer in sequence on the front surface of the substrate; performing screen printing on the corresponding N++ doped region on the anti-reflection layer to obtain the gate line electrode; (6) removing silicon dioxide from the back surface of the substrate; (7) preparing a hole transport layer on the back surface of the substrate, wherein the hole transport layer is prepared by the method for in-situ modification of a transition metal oxide according to any one of claims 1 to 6; (8) Ag is thermally evaporated on the hole transport layer to form the back full-area electrode.
10. The method for preparing a heterojunction solar cell according to claim 9, It is characterized in that The depth of the pn junction is 150-300 nm, the thickness of the passivation layer is 10-20 nm, the thickness of the anti-reflection layer is 60-80 nm, and the thickness of the hole transport layer is 2-13 nm.
Citation Information
Patent Citations
Method for preparing transparent copper thin film conductive electrode through replacement reaction via atomic layer deposition technology
CN106868470A
A back-passivated crystalline silicon solar cell and a preparation method thereof
CN109087965A
Modified metal oxide and preparation method thereof, and quantum dot light-emitting diode
CN112390298A
Method for treating surface of metal oxide, method for manufacturing perovskite solar cell, and metal oxide surface treatment device
WO2023132259A1