Ordered membrane electrode based on ultrathin alkaline membrane and preparation method thereof
By combining ultrathin alkaline membranes with composite catalysts, the stability and conductivity issues of ordered membrane electrodes were resolved, thereby improving the efficiency and stability of the water electrolysis hydrogen production process.
Patent Information
- Application Number
- CN202411145930.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-12
AI Technical Summary
The stability, conductivity, and ionic conductivity of ordered membrane electrodes in existing technologies are poor, which limits the efficiency and stability of the water electrolysis hydrogen production process.
An ultrathin alkaline membrane was prepared from 1,2-diphenylethylenedione, 3,5-dimethylbenzaldehyde, n-butylamine, 1,6-dibromohexane and polyvinyl alcohol. A composite catalyst was prepared by combining thioacetamide, sodium molybdate, sodium vanadate and carbon cloth. An ordered membrane electrode based on the ultrathin alkaline membrane was formed by hot pressing.
It improves the stability, conductivity, and ionic conductivity of the membrane electrode, enhances catalytic activity and chemical stability, shortens the ion transport distance, and promotes the electrode reaction.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of ordered membrane electrode preparation, and in particular relates to an ordered membrane electrode based on an ultra-thin alkaline film and a preparation method thereof. Background Art
[0002] Under the background of global energy structure transformation and environmental protection, the development of clean and renewable energy technologies has become the key to achieving sustainable development. Hydrogen energy, as an efficient and clean secondary energy source, is regarded as an important component of the future energy system because its combustion product is only water. As one of the main ways to produce hydrogen energy, water electrolysis has the advantages of mature technology, wide range of raw materials, and environmental friendliness, and is attracting widespread attention from the global scientific research community. However, although the traditional alkaline water electrolysis hydrogen production technology has the advantages of low cost and mild operating conditions, its low electrolysis current density, high energy consumption, and poor stability limit its large-scale application. As the core component of the water electrolysis hydrogen production system, the membrane electrode directly affects the efficiency and stability of the electrolysis process. Therefore, how to design and prepare high-performance and low-cost membrane electrodes has become a research hotspot in the field of water electrolysis hydrogen production. The ordered membrane electrode based on ultra-thin alkaline membrane and its preparation method came into being in this context. By optimizing the internal structure of the membrane electrode, the material transfer efficiency and electrochemical reaction rate in the electrolysis process can be improved, thereby reducing the energy consumption of hydrogen production and improving the stability and life of the system.
[0003] Patent CN 111740122 B discloses an ordered membrane electrode and a preparation method thereof, which utilizes the external field driving force of electrochemical deposition to cause an oxidation-reduction reaction of the active components on the surface of the gas diffusion layer, so that the catalyst grows in situ on the surface of the gas diffusion layer to obtain a catalyst layer with a three-dimensional multi-level structure; the in-situ growth of the catalyst on the surface of the gas diffusion layer increases the binding force between the catalyst and the gas diffusion layer and the binding force between the multi-layer catalysts, making it difficult for the catalyst to detach, thereby improving the battery life, while reducing the contact resistance between the catalyst and the gas diffusion layer, thereby promoting ion diffusion and charge transfer, which is beneficial to improving battery performance and improving the utilization rate of the catalyst. At the same time, the structure also enables the membrane electrode to have an excellent multiphase mass transfer channel, which is beneficial to improving battery performance. However, the stability, conductivity and ion conductivity of the ordered membrane electrode prepared by this method still have room for improvement. Summary of the invention
[0004] The object of the present invention is to provide an ordered membrane electrode based on an ultra-thin alkaline membrane and a preparation method thereof, so as to solve the technical problems of poor stability, electrical conductivity and ion conductivity of the ordered membrane electrode in the prior art.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions: The invention provides an ordered membrane electrode based on an ultrathin alkaline membrane, which is composed of an anion exchange membrane, a gas diffusion layer and a composite catalyst, wherein the anion exchange membrane is prepared by ion exchange of the ultrathin alkaline membrane, and the ultrathin alkaline membrane solution is prepared by 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine, 1,6-dibromohexane and polyvinyl alcohol, and the composite catalyst is prepared by thioacetamide, sodium molybdate, sodium vanadate and carbon cloth.
[0006] Preferably, the method for preparing the ultra-thin alkaline film comprises the following steps: Q1: Add 1,2-diphenylethanedione to a container containing acetic acid, then add 3,5-dimethylbenzaldehyde, n-butylamine and ammonium acetate, stir until completely dissolved, heat to reflux, cool after reflux, transfer to deionized water, add concentrated ammonia water to adjust the pH, extract, dry by rotary evaporation, and purify to obtain compound 1; Q2: Compound 1 is added to a container containing acetonitrile, 1,6-dibromohexane is added, and the mixture is heated to reflux. After the reflux is completed, the mixture is decompressed, washed, and filtered to obtain Compound 2; Q3: Dissolve polyvinyl alcohol with dimethyl sulfoxide, add compound 2 under nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate to reflux, remove potassium carbonate after reflux, heat treat, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
[0007] In the above process, the synthesis reaction formula of the ultra-thin alkaline membrane is as follows:
[0008] Preferably, in Q1, the molar ratio of 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine and ammonium acetate is (1-2): (0.9-1.95): (1.1-2): (1.1-2.1), the heating reflux temperature is 110-120°C, the reflux time is 3-5h, concentrated ammonia water is added to adjust the pH to 7-7.2, extraction is carried out with dichloromethane and deionized water, and purification is carried out using a flash chromatography column method, and the volume ratio of petroleum ether: ethyl acetate in the chromatographic column is 50:1.
[0009] Preferably, in Q2, the molar ratio of compound 1 and 1,6-dibromohexane is (1-2): (1.1-2.2), the heating reflux temperature is 80-90°C, the reflux time is 20-24h, and washing is performed with methyl n-butyl ether; in Q3, the amount ratio of polyvinyl alcohol, dimethyl sulfoxide and compound 2 is (0.5-1) g: (30-60) mL: (0.175-0.225) g, the reflux time is 48-52h, and the heating treatment temperature is 90-110°C.
[0010] Preferably, the method for preparing the composite catalyst comprises the following steps: S1: adding thioacetamide, sodium molybdate and sodium vanadate to ultrapure water, stirring and mixing to obtain a mixed solution, then transferring the mixed solution to an autoclave reaction vessel, sealing, heating, cooling after heating, centrifuging, washing, and vacuum drying to obtain compound A; S2: placing the carbon cloth in a mixed solution of ethanol and ultrapure water for ultrasonic treatment, drying, and then immersing the dried carbon cloth in a mixed solution of nitric acid and sulfuric acid, heating, washing, and drying to obtain a pretreated carbon cloth; S3: Compound A and ultrapure water are mixed and stirred to obtain a mixed solution of Compound A, and then the pretreated carbon cloth is added to the mixed solution of Compound A, stirred, and then placed in a hydrothermal reactor to heat the reaction. After the reaction is completed, a composite catalyst is obtained.
[0011] In the above process, firstly, thioacetamide, sodium molybdate and sodium vanadate are used as raw materials to synthesize compound A by a one-step hydrothermal method, then the carbon cloth is acidified, and the acidified carbon cloth is compounded with compound A to prepare a composite catalyst through a hydrothermal reaction.
[0012] Preferably, in S1, the molar ratio of thioacetamide, sodium molybdate and sodium vanadate is (8-10): (1.4-1.75): (0.6-0.75), the stirring mixing speed is 600-800 rpm, the mixing time is 40-60 min, the heating treatment temperature is 180-200 ° C, the time is 20-24 h, the centrifugal separation speed is 10000-12000 rpm, the separation time is 5-8 min, and the product is washed with ultrapure water and anhydrous ethanol for 3-5 times respectively. The vacuum drying temperature is 60-80 ° C, and the time is 6-8 h.
[0013] Preferably, in S2, the volume ratio of ethanol to ultrapure water is 1:11, the ultrasonic treatment time is 20-30 min, the drying temperature is 60-70°C, the volume ratio of nitric acid to sulfuric acid is 1:3, the heating treatment temperature is 60-80°C, and the time is 3-5h.
[0014] Preferably, in S3, the dosage ratio of compound A to ultrapure water is (0.25-0.5) g: (60-120) mL, the stirring time is 30-45 min, the heating reaction temperature is 200-220° C., and the time is 20-24 h.
[0015] Preferably, the method for preparing the ordered membrane electrode based on the ultra-thin alkaline film comprises the following steps: Step (1): immersing the ultra-thin alkaline membrane in a sodium hydroxide solution for ion exchange, and after the ion exchange is completed, washing and freeze-drying to obtain an anion exchange membrane; Step (2): adding carbon black and polytetrafluoroethylene to a mixed solvent of ethanol, isopropanol and ultrapure water, dispersing by ultrasonication, and then coating the mixture on the surface of carbon paper, and then adhering the carbon paper to graphene, heating and calcining the mixture to obtain a gas diffusion layer; Step (3): The composite catalyst, the anion exchange membrane and the ultra-thin alkaline membrane are composited by hot pressing to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane.
[0016] Preferably, in the step (1), the concentration of the sodium hydroxide solution is 1 mol / L, and the ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours, washed with deionized water, and the freeze-drying pressure is 0.05 mbar, the temperature is -50~-70°C, and the time is 24-28 hours; in the step (2), the amount ratio of carbon black, polytetrafluoroethylene, ethanol, isopropanol and ultrapure water is (1-2) g: (0.06-0.12) g: (20-40) mL: (10-20) mL: (10-20) mL, the ultrasonic dispersion time is 8-10 hours, the heating calcination temperature is 350-400°C, and the time is 0.5-1 hour; in the step (3), the hot pressing composite pressure is 3.44-4.13 MPa, the temperature is 130-150°C, and the time is 2-4 minutes.
[0017] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are: 1. The present invention first uses 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine, 1,6-dibromohexane and polyvinyl alcohol as raw materials to prepare an ultra-thin alkaline film, and then uses thioacetamide, sodium molybdate, sodium vanadate and carbon cloth as raw materials to prepare a composite catalyst, which is added to the ordered membrane electrode at the same time, which can effectively improve its stability, conductivity and ion conductivity.
[0018] 2. The present invention uses 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine, 1,6-dibromohexane and polyvinyl alcohol as raw materials to prepare an ultra-thin alkaline membrane, which is applied to an ordered membrane electrode, which can effectively improve the ion conductivity, enhance the chemical stability and promote the formation of an ordered membrane electrode. The ultra-thin alkaline membrane has an extremely thin thickness, which shortens the transmission distance of ions in the membrane and improves the ion conduction efficiency. In the process of preparing the alkaline membrane, the cross-linking effect of glutaraldehyde and hydrochloric acid forms a more compact and stable membrane structure. The presence of the cross-linked structure not only improves the mechanical strength of the membrane, but also enhances its chemical stability. The interface compatibility between the ultra-thin alkaline membrane and the electrode material helps it to form a more uniform and dense film layer on the electrode surface, and the uniform film layer helps the transmission of ions and the electrode reaction.
[0019] 3. The present invention uses thioacetamide, sodium molybdate, sodium vanadate and carbon cloth as raw materials to prepare a composite catalyst, which is applied to an ordered membrane electrode, which can effectively improve catalytic activity, enhance stability and improve conductivity. The prepared compound A is combined with the carbon cloth through a hydrothermal reaction, which not only helps the catalyst to exist stably on the electrode surface, but also promotes the rapid transmission of electrons and ions between the catalyst and the electrode, thereby improving the catalytic activity and stability; and the carbon cloth itself has excellent conductivity, and as a carrier of the catalyst, it can ensure the rapid transmission of electrons in the electrode. When the catalyst is combined with the carbon cloth, the electrons can be quickly transmitted to the electrode surface through the close contact between the carbon cloth and the catalyst, thereby improving the conductivity of the electrode. DETAILED DESCRIPTION
[0020] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. Example
[0021] This embodiment discloses a method for preparing an ultra-thin alkaline film, comprising the following steps: Q1: Add 2.61 g of 1,2-diphenylethanedione to a container containing 15 mL of acetic acid, then add 1.59 g of 3,5-dimethylbenzaldehyde, 1.27 mL of n-butylamine and 1.02 g of ammonium acetate, stir until completely dissolved, heat and reflux at 110°C for 5 h, cool after reflux, transfer to deionized water, add concentrated ammonia water to adjust pH=7, extract with dichloromethane and deionized water, dry by rotary evaporation, and purify by flash chromatography. The volume ratio of petroleum ether: ethyl acetate in the chromatographic column is 50:1 to obtain compound 1; Q2: Add 1.5 g of compound 1 to a container containing 30 mL of acetonitrile, add 1.07 g of 1,6-dibromohexane, heat and reflux at 80°C for 24 h, and after reflux, decompress the mixture, wash with methyl n-butyl ether, and filter to obtain compound 2; Q3: Dissolve 0.75g of polyvinyl alcohol in 45mL of dimethyl sulfoxide, add 0.2g of compound 2 under nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate and reflux for 48h. After reflux, remove potassium carbonate, heat at 100°C, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
[0022] This embodiment discloses a method for preparing a composite catalyst, comprising the following steps: S1: 2.34 g of thioacetamide, 1.3 g of sodium molybdate and 0.29 g of sodium vanadate were added to 60 mL of ultrapure water, and the mixture was stirred at 800 rpm for 60 min to obtain a mixed solution, and then the mixed solution was transferred to an autoclave reaction vessel, sealed, and heated at 180° C. for 24 h. After the heating was completed, the mixture was cooled, centrifuged at 10000 rpm for 8 min, washed with ultrapure water and anhydrous ethanol for 3 times respectively, and vacuum dried at 80° C. for 8 h to obtain compound A; S2: The carbon cloth was placed in a mixed solution of ethanol and ultrapure water (the volume ratio of ethanol to ultrapure water was 1:11) for ultrasonic treatment for 30 minutes, and then dried at 70°C. The dried carbon cloth was then immersed in a mixed solution of nitric acid and sulfuric acid (the volume ratio of nitric acid to sulfuric acid was 1:3), heated at 60°C for 5 hours, washed, and dried to obtain the pretreated carbon cloth; S3: Mix 0.38 g of compound A and 90 mL of ultrapure water and stir for 45 minutes to obtain a mixed solution of compound A. Then add the pretreated carbon cloth to the mixed solution of compound A, stir, and then put it into a hydrothermal reactor and heat it at 220°C for 24 hours. After the reaction is completed, a composite catalyst is obtained.
[0023] This embodiment discloses a method for preparing an ordered membrane electrode based on an ultra-thin alkaline film, comprising the following steps: Step (1): immersing the ultra-thin alkaline membrane in a 1 mol / L sodium hydroxide solution for ion exchange. The ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours. After the ion exchange is completed, it is washed with deionized water, and freeze-dried at 0.05 mbar and -50°C for 24 hours to obtain an anion exchange membrane; Step (2): 1.5 g of carbon black and 0.09 g of polytetrafluoroethylene were added to a mixed solvent of 30 mL of ethanol, 15 mL of isopropanol and 15 mL of ultrapure water, and after ultrasonic dispersion for 8 h, the mixture was scraped onto the surface of carbon paper, and then the carbon paper and graphene were adhered, and heated and calcined at 400 ° C for 0.5 h to obtain a gas diffusion layer; Step (3): The composite catalyst, anion exchange membrane and ultra-thin alkaline membrane are composited by hot pressing at 4.13 MPa and 150° C. for 4 min to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane. Example
[0024] This embodiment discloses a method for preparing an ultra-thin alkaline film, comprising the following steps: Q1: 1.74 g of 1,2-diphenylethanedione was added to a container containing 15 mL of acetic acid, followed by 1 g of 3,5-dimethylbenzaldehyde, 0.91 mL of n-butylamine and 0.7 g of ammonium acetate. After stirring until completely dissolved, the mixture was heated to reflux at 110°C for 5 h. After the reflux, the mixture was cooled and transferred to deionized water. Concentrated ammonia was added to adjust the pH to 7. The mixture was extracted with dichloromethane and deionized water, dried by rotary evaporation, and purified by flash chromatography. The volume ratio of petroleum ether to ethyl acetate in the chromatographic column was 50:1 to obtain compound 1. Q2: Add 1 g of compound 1 to a container containing 30 mL of acetonitrile, add 0.71 g of 1,6-dibromohexane, heat and reflux at 80°C for 24 h, and after reflux, decompress the mixture, wash with methyl n-butyl ether, and filter to obtain compound 2; Q3: Dissolve 0.5 g of polyvinyl alcohol in 30 mL of dimethyl sulfoxide, add 0.175 g of compound 2 under a nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate and reflux for 48 hours. After reflux, remove the potassium carbonate, heat at 100°C, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
[0025] This embodiment discloses a method for preparing a composite catalyst, comprising the following steps: S1: 2.08 g of thioacetamide, 1 g of sodium molybdate and 0.25 g of sodium vanadate were added to 60 mL of ultrapure water, and the mixture was stirred at 800 rpm for 60 min to obtain a mixed solution, and then the mixed solution was transferred to an autoclave reaction vessel, sealed, and heated at 180° C. for 24 h. After the heating was completed, the mixture was cooled, centrifuged at 10000 rpm for 8 min, washed with ultrapure water and anhydrous ethanol for 3 times respectively, and vacuum dried at 80° C. for 8 h to obtain compound A; S2: The carbon cloth was placed in a mixed solution of ethanol and ultrapure water (the volume ratio of ethanol to ultrapure water was 1:11) for ultrasonic treatment for 30 minutes, and then dried at 70°C. The dried carbon cloth was then immersed in a mixed solution of nitric acid and sulfuric acid (the volume ratio of nitric acid to sulfuric acid was 1:3), heated at 60°C for 5 hours, washed, and dried to obtain the pretreated carbon cloth; S3: Mix 0.25 g of compound A and 60 mL of ultrapure water and stir for 45 minutes to obtain a mixed solution of compound A. Then add the pretreated carbon cloth to the mixed solution of compound A, stir, and then put it into a hydrothermal reactor and heat it at 220°C for 24 hours. After the reaction is completed, a composite catalyst is obtained.
[0026] This embodiment discloses a method for preparing an ordered membrane electrode based on an ultra-thin alkaline film, comprising the following steps: Step (1): immersing the ultra-thin alkaline membrane in a 1 mol / L sodium hydroxide solution for ion exchange. The ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours. After the ion exchange is completed, it is washed with deionized water, and freeze-dried at 0.05 mbar and -50°C for 24 hours to obtain an anion exchange membrane; Step (2): 1 g of carbon black and 0.06 g of polytetrafluoroethylene are added to a mixed solvent of 20 mL of ethanol, 10 mL of isopropanol and 10 mL of ultrapure water, and after ultrasonic dispersion for 8 h, the mixture is scraped onto the surface of carbon paper, and then the carbon paper and graphene are adhered, and heated and calcined at 400 ° C for 0.5 h to obtain a gas diffusion layer; Step (3): The composite catalyst, anion exchange membrane and ultra-thin alkaline membrane are composited by hot pressing at 4.13 MPa and 150° C. for 4 min to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane. Example
[0027] This embodiment discloses a method for preparing an ultra-thin alkaline film, comprising the following steps: Q1: 3.48 g of 1,2-diphenylethanedione was added to a container containing 15 mL of acetic acid, followed by 2.17 g of 3,5-dimethylbenzaldehyde, 1.64 mL of n-butylamine and 1.34 g of ammonium acetate. After stirring until completely dissolved, the mixture was heated to reflux at 110°C for 5 h. After the reflux, the mixture was cooled and transferred to deionized water. Concentrated ammonia was added to adjust the pH to 7. The mixture was extracted with dichloromethane and deionized water, dried by rotary evaporation, and purified by flash chromatography. The volume ratio of petroleum ether to ethyl acetate in the chromatographic column was 50:1 to obtain compound 1. Q2: Add 2 g of compound 1 to a container containing 30 mL of acetonitrile, add 1.42 g of 1,6-dibromohexane, heat and reflux at 80°C for 24 h, and after reflux, decompress the mixture, wash with methyl n-butyl ether, and filter to obtain compound 2; Q3: Dissolve 1g of polyvinyl alcohol in 60mL of dimethyl sulfoxide, add 0.225g of compound 2 under nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate and reflux for 48h. After reflux, remove potassium carbonate, heat at 100°C, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
[0028] This embodiment discloses a method for preparing a composite catalyst, comprising the following steps: S1: 2.6 g of thioacetamide, 1.25 g of sodium molybdate and 0.32 g of sodium vanadate were added to 60 mL of ultrapure water, and the mixture was stirred at 800 rpm for 60 min to obtain a mixed solution, and then the mixed solution was transferred to an autoclave reaction vessel, sealed, and heated at 180° C. for 24 h. After the heating was completed, the mixture was cooled, centrifuged at 10000 rpm for 8 min, washed with ultrapure water and anhydrous ethanol for 3 times respectively, and vacuum dried at 80° C. for 8 h to obtain compound A; S2: The carbon cloth was placed in a mixed solution of ethanol and ultrapure water (the volume ratio of ethanol to ultrapure water was 1:11) for ultrasonic treatment for 30 minutes, and then dried at 70°C. The dried carbon cloth was then immersed in a mixed solution of nitric acid and sulfuric acid (the volume ratio of nitric acid to sulfuric acid was 1:3), heated at 60°C for 5 hours, washed, and dried to obtain the pretreated carbon cloth; S3: Mix 0.5 g of compound A and 120 mL of ultrapure water and stir for 45 min to obtain a mixed solution of compound A. Then add the pretreated carbon cloth to the mixed solution of compound A, stir, and then put it into a hydrothermal reactor and heat it at 220°C for 24 h. After the reaction is completed, a composite catalyst is obtained.
[0029] This embodiment discloses a method for preparing an ordered membrane electrode based on an ultra-thin alkaline film, comprising the following steps: Step (1): immersing the ultra-thin alkaline membrane in a 1 mol / L sodium hydroxide solution for ion exchange. The ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours. After the ion exchange is completed, it is washed with deionized water, and freeze-dried at 0.05 mbar and -50°C for 24 hours to obtain an anion exchange membrane; Step (2): 2 g of carbon black and 0.12 g of polytetrafluoroethylene are added to a mixed solvent of 40 mL of ethanol, 20 mL of isopropanol and 20 mL of ultrapure water, and after ultrasonic dispersion for 8 h, the mixture is scraped onto the surface of carbon paper, and then the carbon paper and graphene are adhered, and heated and calcined at 400 ° C for 0.5 h to obtain a gas diffusion layer; Step (3): The composite catalyst, anion exchange membrane and ultra-thin alkaline membrane are composited by hot pressing at 4.13 MPa and 150° C. for 4 min to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane. Example
[0030] This embodiment discloses a method for preparing an ultra-thin alkaline film, comprising the following steps: Q1: Add 2.18 g of 1,2-diphenylethanedione to a container containing 15 mL of acetic acid, then add 1.3 g of 3,5-dimethylbenzaldehyde, 1.46 mL of n-butylamine and 0.86 g of ammonium acetate, stir until completely dissolved, heat and reflux at 110°C for 5 h, cool after reflux, transfer to deionized water, add concentrated ammonia water to adjust pH=7, extract with dichloromethane and deionized water, dry by rotary evaporation, and purify by flash chromatography. The volume ratio of petroleum ether: ethyl acetate in the chromatographic column is 50:1 to obtain compound 1; Q2: Add 1.2 g of compound 1 to a container containing 30 mL of acetonitrile, add 0.84 g of 1,6-dibromohexane, heat and reflux at 80°C for 24 h, and after reflux, decompress the mixture, wash with methyl n-butyl ether, and filter to obtain compound 2; Q3: Dissolve 0.63 g of polyvinyl alcohol in 35 mL of dimethyl sulfoxide, add 0.188 g of compound 2 under a nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate and reflux for 48 hours. After reflux, remove the potassium carbonate, heat at 100°C, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
[0031] This embodiment discloses a method for preparing a composite catalyst, comprising the following steps: S1: 2.21 g of thioacetamide, 1.06 g of sodium molybdate and 0.27 g of sodium vanadate were added to 60 mL of ultrapure water, and the mixture was stirred at 800 rpm for 60 min to obtain a mixed solution, and then the mixed solution was transferred to an autoclave reaction vessel, sealed, and heated at 180° C. for 24 h. After the heating was completed, the mixture was cooled, centrifuged at 10000 rpm for 8 min, washed with ultrapure water and anhydrous ethanol for 3 times respectively, and vacuum dried at 80° C. for 8 h to obtain compound A; S2: The carbon cloth was placed in a mixed solution of ethanol and ultrapure water (the volume ratio of ethanol to ultrapure water was 1:11) for ultrasonic treatment for 30 minutes, and then dried at 70°C. The dried carbon cloth was then immersed in a mixed solution of nitric acid and sulfuric acid (the volume ratio of nitric acid to sulfuric acid was 1:3), heated at 60°C for 5 hours, washed, and dried to obtain the pretreated carbon cloth; S3: 0.32 g of compound A and 75 mL of ultrapure water were mixed and stirred for 45 min to obtain a mixed solution of compound A. The pretreated carbon cloth was then added to the mixed solution of compound A, stirred, and then placed in a hydrothermal reactor and heated at 220° C. for 24 h. After the reaction was completed, a composite catalyst was obtained.
[0032] This embodiment discloses a method for preparing an ordered membrane electrode based on an ultra-thin alkaline film, comprising the following steps: Step (1): immersing the ultra-thin alkaline membrane in a 1 mol / L sodium hydroxide solution for ion exchange. The ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours. After the ion exchange is completed, it is washed with deionized water, and freeze-dried at 0.05 mbar and -50°C for 24 hours to obtain an anion exchange membrane; Step (2): 1.2 g of carbon black and 0.08 g of polytetrafluoroethylene were added to a mixed solvent of 25 mL of ethanol, 12 mL of isopropanol and 18 mL of ultrapure water, and after ultrasonic dispersion for 8 h, the mixture was scraped onto the surface of carbon paper, and then the carbon paper and graphene were adhered, and heated and calcined at 400 ° C for 0.5 h to obtain a gas diffusion layer; Step (3): The composite catalyst, anion exchange membrane and ultra-thin alkaline membrane are composited by hot pressing at 4.13 MPa and 150° C. for 4 min to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane.
[0033] Comparative Example 1 Comparative Example 1 Compared with Example 1, in the preparation process of the ultra-thin alkaline film in Comparative Example 1, 1,2-diphenylethanedione is not added, and other conditions remain unchanged.
[0034] Comparative Example 2 Comparative Example 2 Compared with Example 1, in the preparation process of the ultra-thin alkaline film in Comparative Example 2, 1,6-dibromohexane is not added, and other conditions remain unchanged.
[0035] Comparative Example 3 Comparative Example 3 Compared with Example 1, in the preparation process of the composite catalyst in Comparative Example 3, no sodium molybdate was added, and other conditions remained unchanged.
[0036] Comparative Example 4 Comparative Example 4 Compared with Example 1, in the preparation process of the composite catalyst in Comparative Example 4, no carbon cloth was added, and other conditions remained unchanged.
[0037] Experimental example The samples prepared according to Examples 1-4 and Comparative Examples 1-4 were activated at an activation temperature of 80°C. Ultrapure water was introduced into the anode side, and high-purity nitrogen was introduced into the cathode side. After 4 hours of activation, the internal resistance test was performed. The activation was considered to be completed when the internal resistance decreased to about 150 mΩ. If it reached the specified range, the activation was continued. After the activation was completed, a 3 mol / L formic acid solution was introduced into the cathode at a flow rate of 3 mL / min, and dry high-purity oxygen was introduced into the cathode at a flow rate of 100 mL / min. A single cell test was performed after 1 hour. The stability test was performed using a constant potential method, and the voltage was maintained at 0.5 V. The resistivity of the sample was tested according to GB / T 39978-2021. The test results are shown in Table 1:
[0038] From the test results in Table 1, it can be seen that the ordered membrane electrode based on the ultra-thin alkaline film prepared by Examples 1-4 of the present invention has excellent stability and conductivity. From the comparison between Comparative Example 1 and Examples 1-4, it can be seen that the addition of 1,2-diphenylethanedione can make the obtained ordered membrane electrode have excellent stability and conductivity; from the comparison between Comparative Example 2 and Examples 1-4, it can be seen that the addition of 1,6-dibromohexane can make the obtained ordered membrane electrode have excellent stability and conductivity; from the comparison between Comparative Example 3 and Examples 1-4, it can be seen that the addition of sodium molybdate can make the obtained ordered membrane electrode have excellent stability; from the comparison between Comparative Example 4 and Examples 1-4, it can be seen that the addition of carbon cloth can make the obtained ordered membrane electrode have excellent stability.
[0039] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
[0040] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to only specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. An ordered membrane electrode based on an ultra-thin alkaline film, characterized in that: It consists of an anion exchange membrane, a gas diffusion layer and a composite catalyst, wherein the anion exchange membrane is prepared by ion exchange of an ultra-thin alkaline membrane, and the ultra-thin alkaline membrane is prepared by 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine, 1,6-dibromohexane and polyvinyl alcohol, and the composite catalyst is prepared by thioacetamide, sodium molybdate, sodium vanadate and carbon cloth.
2. The ordered membrane electrode based on ultra-thin alkaline film according to claim 1, characterized in that: The method for preparing the ultra-thin alkaline film comprises the following steps: Q1: Add 1,2-diphenylethanedione to a container containing acetic acid, then add 3,5-dimethylbenzaldehyde, n-butylamine and ammonium acetate, stir until completely dissolved, heat to reflux, cool after reflux, transfer to deionized water, add concentrated ammonia water to adjust the pH, extract, dry by rotary evaporation, and purify to obtain compound 1; Q2: Compound 1 is added to a container containing acetonitrile, 1,6-dibromohexane is added, and the mixture is heated to reflux. After the reflux is completed, the mixture is decompressed, washed, and filtered to obtain Compound 2; Q3: Dissolve polyvinyl alcohol with dimethyl sulfoxide, add compound 2 under nitrogen atmosphere, stir and mix, add anhydrous potassium carbonate to reflux, remove potassium carbonate after reflux, heat treat, then add anhydrous acetone solvent and glutaraldehyde aqueous solution, and then add hydrochloric acid dropwise for cross-linking to obtain an ultra-thin alkaline film.
3. The ordered membrane electrode based on ultra-thin alkaline film according to claim 2, characterized in that: In the Q1, the molar ratio of 1,2-diphenylethanedione, 3,5-dimethylbenzaldehyde, n-butylamine and ammonium acetate is (1-2): (0.9-1.95): (1.1-2): (1.1-2.1), the heating reflux temperature is 110-120°C, the reflux time is 3-5h, concentrated ammonia water is added to adjust the pH to 7-7.2, extraction is carried out with dichloromethane and deionized water, and purification is carried out using a flash chromatography column method, and the volume ratio of petroleum ether: ethyl acetate in the chromatographic column is 50:
1.
4. The ordered membrane electrode based on ultra-thin alkaline film according to claim 2, characterized in that: In Q2, the molar ratio of compound 1 and 1,6-dibromohexane is (1-2): (1.1-2.2), the heating reflux temperature is 80-90°C, the reflux time is 20-24h, and the washing is carried out with methyl n-butyl ether; in Q3, the amount ratio of polyvinyl alcohol, dimethyl sulfoxide and compound 2 is (0.5-1) g: (30-60) mL: (0.175-0.225) g, the reflux time is 48-52h, and the heating treatment temperature is 90-110°C.
5. The ordered membrane electrode based on ultra-thin alkaline film according to claim 1, characterized in that: The preparation method of the composite catalyst comprises the following steps: S1: adding thioacetamide, sodium molybdate and sodium vanadate to ultrapure water, stirring and mixing to obtain a mixed solution, then transferring the mixed solution to an autoclave reaction vessel, sealing, heating, cooling after heating, centrifuging, washing, and vacuum drying to obtain compound A; S2: placing the carbon cloth in a mixed solution of ethanol and ultrapure water for ultrasonic treatment, drying, and then immersing the dried carbon cloth in a mixed solution of nitric acid and sulfuric acid, heating, washing, and drying to obtain a pretreated carbon cloth; S3: Compound A and ultrapure water are mixed and stirred to obtain a mixed solution of Compound A, and then the pretreated carbon cloth is added to the mixed solution of Compound A, stirred, and then placed in a hydrothermal reactor to heat the reaction. After the reaction is completed, a composite catalyst is obtained.
6. The ordered membrane electrode based on ultra-thin alkaline film according to claim 5, characterized in that: In the S1, the molar ratio of thioacetamide, sodium molybdate and sodium vanadate is (8-10): (1.4-1.75): (0.6-0.75), the stirring mixing speed is 600-800 rpm, the mixing time is 40-60 min, the heating treatment temperature is 180-200° C., the time is 20-24 h, the centrifugal separation speed is 10000-12000 rpm, the separation time is 5-8 min, and the product is washed with ultrapure water and anhydrous ethanol for 3-5 times respectively. The vacuum drying temperature is 60-80° C., and the time is 6-8 h.
7. The ordered membrane electrode based on ultra-thin alkaline film according to claim 5, characterized in that: In the S2, the volume ratio of ethanol to ultrapure water is 1:11, the ultrasonic treatment time is 20-30 min, the drying temperature is 60-70°C, the volume ratio of nitric acid to sulfuric acid is 1:3, the heating treatment temperature is 60-80°C, and the time is 3-5h.
8. The ordered membrane electrode based on ultra-thin alkaline film according to claim 5, characterized in that: In the S3, the dosage ratio of compound A to ultrapure water is (0.25-0.5) g: (60-120) mL, the stirring time is 30-45 min, the heating reaction temperature is 200-220° C., and the time is 20-24 h.
9. A method for preparing an ordered membrane electrode based on an ultra-thin alkaline film according to any one of claims 1 to 8, characterized in that: The following steps are involved: Step (1): immersing the ultra-thin alkaline membrane in a sodium hydroxide solution for ion exchange, and after the ion exchange is completed, washing and freeze-drying to obtain an anion exchange membrane; Step (2): adding carbon black and polytetrafluoroethylene to a mixed solvent of ethanol, isopropanol and ultrapure water, dispersing by ultrasonication, and then coating the mixture on the surface of carbon paper, and then adhering the carbon paper to graphene, heating and calcining the mixture to obtain a gas diffusion layer; Step (3): The composite catalyst, the anion exchange membrane and the ultra-thin alkaline membrane are composited by hot pressing to obtain an ordered membrane electrode based on the ultra-thin alkaline membrane.
10. The method for preparing an ordered membrane electrode based on an ultra-thin alkaline film according to claim 9, characterized in that: In the step (1), the concentration of the sodium hydroxide solution is 1 mol / L, and the ion exchange process is as follows: the sodium hydroxide solution is replaced every 20 minutes in the first hour, and after 1 hour, it is kept in the sodium hydroxide solution for 48 hours, washed with deionized water, and the freeze-drying pressure is 0.05 mbar, the temperature is -50~-70°C, and the time is 24-28 hours. In the step (2), the amount ratio of carbon black, polytetrafluoroethylene, ethanol, isopropanol and ultrapure water is (1-2) g: (0.06-0.12) g: (20-40) mL: (10-20) mL: (10-20) mL, the ultrasonic dispersion time is 8-10 hours, and the heating calcination temperature is 350-400°C and the time is 0.5-1 hour. In the step (3), the hot pressing composite pressure is 3.44-4.13 MPa, the temperature is 130-150°C, and the time is 2-4 minutes.