Pure cotton linen-like yarn and production process thereof
By mixing combed cotton with broken trousers and using bamboo yarn process to make pure cotton imitation linen yarn, the problem of roughness and shortness of the linen fiber is solved, reducing costs and improving the quality and yarn quality and consuming properties. It achieves a similar appearance to the yarn and the administrative nature of the cotton yarn.
Patent Information
- Application Number
- CN202411056303.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-12
AI Technical Summary
In the traditional cotton-linen blended yarn process, there are problems such as roughness, shortness and easy breakage, resulting in poor yarn quality and high price of hemp raw materials, which limits the popularization of the prices of hemp-containing raw materials. The traditional imitation hemp yarn is uncontrollable and Higher cost.
After the combed cotton dropping and the broken trouser sliver is mixed, pure cotton imitation linen yarn is made through the roving and fine yarn process, combining the bamboo joint yarn yarn process, and the content of combed cotton dropping and bamboo joint yarn joint yarn to achieve style and quality. promote.
It reduces production costs, improves the quality and consuming properties of yarn, achieves a similar appearance to yarn, and has good consuming properties of cotton yarn, meeting mass production and consumption needs.
Smart Images

Figure BDA0004976531430000061 
Figure BDA0004976531430000071 
Figure BDA0004976531430000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of textiles, and in particular to a pure cotton imitation linen yarn and a production process thereof. Background Art
[0002] The traditional cotton and linen blended spinning process adopts the package blending process, and the production process is as follows: linen fiber + cotton fiber → package blending, secondary packaging → roll → combing → head and end → coarse yarn → fine yarn → winding; then dyeing, weaving, and finishing are carried out to achieve the required style. In the production of cotton and linen blends, linen fibers are generally blended with cotton fibers to achieve the style and effect of cotton and linen. However, linen fibers have problems such as being rough, short, and easy to break, resulting in many deficiencies in spinning, and the high price of linen raw materials has always restricted the popularization of the price of linen raw materials. In addition, cotton noil is the cotton strips combed off when passing through the combing machine. It cannot be used to spin combed yarn, but is used to make air-spinning or paid brand yarn. The yarn count is coarse and the general utilization rate is not high.
[0003] Traditional imitation linen yarn is a form of spinning that is made by mixing cotton waste with cotton fibers for the second time, and then using short fiber aggregation and cotton knots to simulate the linen yarn effect. The yarn shape is uncontrollable and the linen effect is not obvious.
[0004] Chinese invention patent CN108660573A discloses a vortex-spun linen-like yarn, which includes a main core yarn fiber and short fibers, wherein the short fibers are wrapped around the main core yarn fibers in an irregular state; 80-90% of the short fibers are scattered on the main core yarn fibers, thereby forming scattered point-like short fibers or scattered fiber-like short fibers; 10-20% of the short fibers are glued to the main core yarn fibers in a clustered state, thereby forming clustered short fibers. The effect of linen yarn can be well simulated, but vortex spinning equipment needs to be purchased, which increases the cost of the enterprise, and the reproducibility of the yarn effect is unstable. More than 80% of the fibers in this invention are chemical fibers, which are not comfortable to wear.
[0005] Chinese invention patent CN110965163A discloses a cotton-linen blended yarn imitating linen yarn and its spinning method, which is made of 40%-70% of raw fine cotton carding noil, 30%-50% of fine cotton, and 0%-10% of flax fiber. The raw materials are mixed, and the carding → drawing → roving process is carried out, and then fine yarn and cone yarn are spun compactly; the yarn strength is improved, the fine yarn breakage is reduced, and the blended yarn feels hard and is closer to the feel of pure linen yarn; when the flax fiber is 0%, it is carding noil and normal cotton, which are mixed and then spun to produce normal pure cotton yarn, which weakens the effect of linen yarn.
[0006] Chinese invention patent CN101892538A discloses a blended spinning of flax fiber and cotton fiber and its manufacturing process. The raw materials are 20%-60% flax fiber and 40%-80% cotton fiber. The manufacturing process is to soak them separately, and then spin them into yarn through the steps of mixing with hemp, cleaning, combing, drawing, roving, and spinning to obtain a pure natural and comfortable textile product. This invention is to spin the roving blended with hemp fiber and cotton fiber into spun yarn in the form of embedded spinning with polyester filament. The process is relatively complicated and the cost is increased. Summary of the invention
[0007] The technical problem to be solved by the present invention is: to overcome the shortcomings of the prior art and provide a pure cotton imitation linen yarn and a production process thereof, which is beneficial to reducing costs and protecting the environment. The spun pure cotton imitation linen yarn has a prominent style, and has both the appearance style of linen yarn and the good wearability of cotton yarn.
[0008] The technical solution of the present invention is:
[0009] On the one hand, the present invention provides a production process of pure cotton imitation linen yarn, which comprises mixing combed cotton waste with broken combed cotton strips, spinning coarse yarn, and then spinning fine yarn. The fine yarn process adopts bamboo yarn technology, and the pure cotton imitation linen yarn is made after winding.
[0010] Preferably, the combed cotton noil is pure cotton combed cotton noil, and the broken combed cotton slivers are formed by breaking fine-neck cotton combed cotton slivers.
[0011] Preferably, the combing noil is noil from the combing process of fine-staple cotton or long-staple cotton.
[0012] Preferably, the length of the broken card sliver is 10-15 cm.
[0013] Preferably, after the comber noil is mixed with the broken card sliver, the comber noil accounts for 30-40%.
[0014] Preferably, the roving weight is 6.5-7.5g / 10m, the machine speed is 800r / min, and the twist coefficient is 100-110; the machine speed in the spun yarn is 9000-11000r / min, the spinning is 21S, the twist coefficient is 450-480, the bamboo node length is 8-20mm, the bamboo node ratio is 1.5-2.5 times, and the bamboo node spacing is 400-2000mm.
[0015] Preferably, the method specifically comprises the following steps:
[0016] S1 Collection of comber noil: collect and pack the noil from the comber noil baler;
[0017] S2: Production of the broken carded sliver: Place the carded sliver behind the drawing frame, remove the second rubber roller of the drawing frame, break the carded sliver, and pack it for later use;
[0018] S3 Blowing disc: mixes combing noil and broken combing slivers;
[0019] S4 coiling machine: coiling;
[0020] S5 carding machine: Spinning combed cotton noil and broken carding sliver mixed with carding sliver;
[0021] S6 pre-drawing: further mixing the mixed carded slivers;
[0022] S7 drawing: adopts two-pass drawing method to further deepen the mixing degree between fibers;
[0023] S8 roving: spun roving;
[0024] S9 spun yarn: spun yarn is produced by using the spinning form of precision slub yarn;
[0025] S10 winding: produce package yarn, made into pure cotton imitation linen yarn.
[0026] Preferably, the carding weight of the carding machine is 24-25g / 5m, the cylinder-movable cover gauge is 12-14 inches, and the machine speed is ≥12kg / h.
[0027] Preferably, the pre-drawing weight is 24.5g / 5m, the post-drawing multiple is 1.7 times, and the pre-drawing speed is 350m / min; the drawing weight is 24g / 5m, the post-drawing multiple is 1.3 times, and the drawing speed is 300m / min.
[0028] The style of the pure cotton imitation linen yarn of the invention is achieved by controlling the content of combed noil and the bamboo yarn knot process.
[0029] On the other hand, the present invention provides pure cotton imitation linen yarn prepared by the production process of the pure cotton imitation linen yarn.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The production process of the pure cotton imitation linen yarn of the present invention adopts the method of adding combed cotton waste and combed cotton strips to mix, and after the different slub yarn processes in the spinning process, a special style of yarn is spun, and the compact spinning slub yarn is adopted, the yarn quality is good, green and environmentally friendly, and meets the indicators of mass production. And the production process of the present invention uses the normal slub yarn spinning process, does not need to install equipment separately, and does not increase the cost; in the process, combed cotton waste is added to reduce the cost of cotton, the investment cost is low, the spinning efficiency is high, and the pure cotton imitation linen yarn has a prominent style, which has both the style of linen yarn and the good wearability of cotton yarn, and is very popular with the public.
[0032] 2. The production process of the pure cotton imitation linen yarn of the present invention, pure cotton replaces linen fiber, adds a large amount of cotton waste, saves raw material costs, has a high rate of repeated recycling of combed cotton waste, and reduces enterprise costs; increases the variety structure, enriches the enterprise's yarn types, and improves the enterprise's competitiveness; the pure cotton imitation linen yarn produced by the present invention does not contain linen fiber, adds cotton waste, has obvious linen yarn style and the indicators meet the standard strength requirements of the yarn, replaces linen fiber to improve the feel of the yarn, the fabric has no itching, is soft and comfortable, is cheaper than linen fabrics, and is more likely to be loved by consumers. DETAILED DESCRIPTION
[0033] In order to enable persons skilled in the art to better understand the technical solution of the present invention, the technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention.
[0034] Example 1
[0035] The production process of the pure cotton imitation linen yarn of this embodiment comprises the following steps:
[0036] S1 Collection of comber noil: collect and pack the comber noil from the comber noil baler, where the comber noil is the noil from the combing process of fine cotton;
[0037] S2 Preparation of broken carded cotton strips: Place the fine cotton carded cotton strips behind the drawing frame, remove the second rubber roller of the drawing frame, break the carded cotton strips, and pack them for standby use. The length of the broken carded cotton strips is 10-15cm;
[0038] S3 Blowing disc: Mix combing noil and broken carding slivers in the ratio of 30% combing noil and 70% carding slivers;
[0039] S4 coiling machine: coiling;
[0040] S5 carding machine: the basis weight is controlled at 25g / 5m, the cylinder-movable flat plate distance is controlled at 14-12-12-12-14 inches, and the carding speed is not less than 12kg / h;
[0041] S6 pre-drawing: the basis weight is controlled at 24.5g / 5m, the post-drafting multiple is 1.7 times, the roller center distance is 46×58mm, the post-machine is 8-drawing, and the pre-drawing speed is 350m / min;
[0042] S7 drawing frame: the basis weight is controlled at 24g / 5m, the rear drafting ratio is 1.3 times, the roller center distance is 44×56mm, the rear drawing is 8 times, and the drawing speed is 300m / min;
[0043] S8 roving: the weight is controlled at 7.5g / 10m, the speed is 800r / min, the twist coefficient is controlled at 100, and the center distance of the roving roller is 42×51×53mm;
[0044] S9 spun yarn: the speed is controlled at 9000r / min, the wire ring is 4.5mm, the spinning form of compact spinning slub yarn is adopted, the yarn count is 21S, the twist coefficient is 480, and the slub yarn process (slub length is 10-20mm, the slub ratio is 2-2.5, and the slub spacing is 400-800mm);
[0045] S10 winding: produce package yarn, made into pure cotton imitation linen yarn.
[0046] Example 2
[0047] The difference from Example 1 is that the combing noil accounts for 40% in the raw material.
[0048] Example 3
[0049] The difference from Example 2 is that in step S9, in the slub yarn process, the slub length is 10-20 mm, the slub ratio is 1.5-2, and the slub spacing is 800-1000 mm.
[0050] Example 4
[0051] The difference from Example 1 is that in step S9, in the slub yarn process, the slub length is 10-20 mm, the slub ratio is 1.5-2, and the slub spacing is 800-1000 mm.
[0052] Example 5
[0053] The difference from Example 2 is that in step S9, in the slub yarn process, the slub length is 10-20 mm, the slub ratio is 2-2.5, and the slub spacing is 1000-2000 mm.
[0054] Example 6
[0055] The difference from Example 2 is that in step S9, in the slub yarn process, the slub length is 10-15 mm, the slub ratio is 2-2.5, and the slub spacing is 1000-2000 mm.
[0056] Example 7
[0057] The difference from Example 2 is that in step S9, in the slub yarn process, the slub length is 10-20 mm, the slub ratio is 1.8-2.3, and the slub spacing is 1000-2000 mm.
[0058] Example 8
[0059] The difference from Example 2 is that in step S9, in the slub yarn process, the slub length is 10-20 mm, the slub ratio is 1.8-2.3, and the slub spacing is 800-1200.
[0060] Comparative Example 1
[0061] Comparative Example 1 uses purchased 21s-100% linen yarn with a twist coefficient of 229.
[0062] Comparative Example 2
[0063] The difference from Example 1 is that S9 spun yarn: the spun yarn is spun in the form of compact spinning, the speed is controlled at 9000r / min, the gauge block is 4.5mm, the yarn count is 21S, the twist coefficient is 480, there is no bamboo knot, and from the yarn style, there is no obvious cotton and linen concave and convex style, and the cotton knots are more prominent.
[0064] Comparative Example 3
[0065] The difference from Example 1 is that S9 spun yarn is spun in the form of ring spinning, the speed is controlled at 9000r / min, the gauge block is 4.5mm, the yarn count is 21S, the twist coefficient is 480, there is no bamboo knot, and from the yarn style, there is no obvious cotton and linen concave and convex style, and the cotton knots are more prominent than in Comparative Example 2.
[0066] Comparative Example 4
[0067] The difference from Example 1 is that the carded slivers are not broken and are directly mixed with the combed cotton waste. The length of the carded slivers is 300 m. During the mixing process, the slivers are entangled with the beaters of the cotton cleaning discs. The friction causes the beaters to heat up severely, posing a fire hazard.
[0068] Comparative Example 5
[0069] The difference from Example 1 is that, in step S3, the cotton cleaning disc: the combed cotton noil and the broken carded cotton slivers are mixed in a ratio of 50% of the combed cotton noil and 50% of the carded cotton slivers.
[0070] Comparative Example 6
[0071] The difference from Example 1 is that, in step S3, the cotton cleaning disc: the combed cotton noil and the broken carded cotton slivers are mixed in a ratio of 20% of the combed cotton noil and 80% of the carded cotton slivers.
[0072] The evenness of the textiles of Examples 1-8 and Comparative Examples 1-6 was tested using the Uster UT4 fully automatic evenness tester at a test speed of 400 m / min. The breaking strength and strength variation coefficient of the textiles of Examples 1-8 and Comparative Examples 1-6 were tested using the Uster fast strength tester at a test speed of 400 m / min. The performance test results are shown in Table 1-2:
[0073] Table 1 Performance test results of textiles of Examples 1-8
[0074]
[0075] Table 2 Performance test results of textiles of comparative examples 1-6
[0076]
[0077]
[0078] Yarn enterprise standard BZ-101 of Lu Thai Textile Co., Ltd. is shown in Table 3:
[0079] Table 3 Standard indicators of yarn enterprises
[0080]
[0081]
[0082] It can be seen from Tables 1 and 3 that the pure cotton imitation linen yarn prepared in the embodiments of the present invention has passed the actual implementation and confirmed the indicators. At the same time, it can be seen from Tables 1-2 that compared with Example 1, in the actual production of Comparative Example 5, the number of broken ends in the spinning process increased, the cotton drop content was high, and the post-process control was more difficult; while the cotton drop content of Comparative Example 6 was relatively small, and from the yarn style, it was more like cotton yarn, without obvious cotton and linen knot style.
Claims
1. The production process of pure cotton imitation linen yarn is characterized in that: The combed cotton noil is mixed with the broken carded cotton strips to spin coarse yarn, and then spun into fine yarn. The spun yarn process adopts the bamboo yarn process, and after winding, it is made into pure cotton imitation linen yarn.
2. The production process of pure cotton imitation linen yarn according to claim 1, characterized in that: The combed cotton noil is the combed cotton noil of pure cotton, and the broken combed cotton sliver is made by breaking the fine cotton combed cotton sliver.
3. The production process of pure cotton imitation linen yarn according to claim 2, characterized in that: Combing noil is the noil from the combing process of fine-staple cotton or long-staple cotton.
4. The production process of pure cotton imitation linen yarn according to claim 2, characterized in that: The length of the broken carded cotton strip is 10-15 cm.
5. The production process of pure cotton imitation linen yarn according to claim 1, characterized in that: After the comber noil is mixed with the broken card sliver, the comber noil accounts for 30-40%.
6. The production process of pure cotton imitation linen yarn according to claim 1, characterized in that: The roving weight is 6.5-7.5g / 10m, and the twist coefficient is 100-110; the spinning speed is 9000-11000r / min, the spinning is 21S, the twist coefficient is 450-480, the bamboo node length is 8-20mm, the bamboo node ratio is 1.5-2.5 times, and the bamboo node spacing is 400-2000mm.
7. The production process of pure cotton imitation linen yarn according to claim 1, characterized in that: The specific processes include: combed cotton noil and broken carded slivers are put into the cotton cleaning disc for mixing, and then enter the rolling machine for rolling, the carding machine for slivering, pre-sliver drawing, roving machine for spinning roving, spinning machine for spinning sliver, and then the warp bobbin to produce cheese yarn, and finally make pure cotton imitation linen yarn.
8. The production process of pure cotton imitation linen yarn according to claim 7, characterized in that: The carding weight of the carding machine is 24-25g / 5m, the cylinder-movable cover gauge is 12-14 inches, and the machine speed is ≥12kg / h.
9. The production process of pure cotton imitation linen yarn according to claim 7, characterized in that: The pre-drawing weight is 24.5g / 5m, the post-drawing ratio is 1.7 times, and the pre-drawing speed is 350m / min; the drawing weight is 24g / 5m, the post-drawing ratio is 1.3 times, and the drawing speed is 300m / min.
10. The pure cotton imitation linen yarn prepared by the production process of the pure cotton imitation linen yarn according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method of producing linen-like segment-colored slub yarn fabric
CN102493088A
Cotton and hemp blended yarn based imitation pure hemp yarn and spinning method thereof
CN110965163A
Novel linen-like colored spun yarn process method
CN113529229A