Double-network gel electrolyte for large-area electrochromic device and preparation method
Through the design of dual-network gel electrolyte, the movement of purple essence is limited, and the contrast reduction and uneven coloring problems caused by dimerization in large-area electrochromic devices are solved, and the efficient and stable electrochromic effect is achieved. It is suitable for Large-size application scenarios.
Patent Information
- Application Number
- CN202411019116.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
Purple essence is prone to dimerization when large-area electrochromic devices are powered on for a long time, resulting in reduced contrast and uneven coloring. It is difficult for the prior art to effectively solve these problems.
Using dual network gel electrolytes, the movement of cathode electrochromic materials is restricted through the copolymerization reaction of the first network polymer and the second network polymer, reducing the risk of dimerization, and improving the contrast and stability of the device. .
Significantly improve the performance and reliability of electrochromic devices, achieve long life, large-area applications, uniform fading, rapid color change response, low drive voltage and good cycle stability, suitable for large-size application scenarios such as aircraft portholes and buildings Glass curtain wall.
Smart Images

Figure BDA0004966664190000021 
Figure BDA0004966664190000031 
Figure BDA0004966664190000032
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of electrochromism, and in particular to a double network gel electrolyte for large-area electrochromism devices and a preparation method thereof. Background Art
[0002] Electrochromic devices refer to materials that undergo reversible redox reactions under electrical stimulation, accompanied by changes in optical properties and color. Viologen (or bipyridyl salt compounds) is a class of compounds with stable redox properties and high optical contrast. By regulating its substituents, cathode electrochromic materials of various colors can be synthesized. Based on its good properties, it has been successfully applied in small-area smart glass scenes such as automotive anti-glare rearview mirrors, AR / VR glasses, snow goggles, and 3C camera lenses. However, viologen will dimerize when powered on for a long time and over a large area, which will reduce the contrast and device stability, affecting its actual use. This is because after the electric field is applied, the divalent cations of viologen will migrate from the solution to the cathode and obtain electrons at the electrode to become colored free radical cations. The free radical cations are prone to dimerization, consuming the free radical cations, so the color becomes lighter, the colored state transmittance becomes larger, and the device contrast decreases. Especially in the case of large-area and long-term power-on, this phenomenon will be more obvious due to the increase in resistance away from the electrode side and the increase in the migration time of viologen.
[0003] At present, there are methods such as adding ionic liquid to the electrolyte, anchoring viologen at the electrode end, and designing viologen polymers to stabilize the viologen free radical cations, but these methods still have problems such as being unable to be widely used over a large area, low coloring and fading efficiency, and high cost. Patent CN116410396A limits the migration of viologen compounds and electrode materials through a cross-linked network in a gel electrolyte. Since the viologen molecules are still free in the electrolyte solution, as the voltage is applied for a long time, the viologen small molecules can still pass through the holes of the cross-linked network and reach the electrode surface. Summary of the invention
[0004] In view of the above shortcomings of the prior art, the present invention provides a double-network gel electrolyte for large-area electrochromic devices to solve the problems of existing viologen easily dimerizing when large-area electrochromic devices are powered on for a long time, resulting in reduced device transmittance and uneven coloring.
[0005] In order to achieve the above purpose, the technical solution adopted by the present invention is:
[0006] A double network gel electrolyte for a large-area electrochromic device, the double network gel electrolyte comprising:
[0007] A first network polymer, wherein the first network polymer is obtained by copolymerization of a cathode electrochromic material with an unsaturated bond, an anode electrochromic material with an unsaturated bond, and a methacrylate monomer; and
[0008] A second network polymer, wherein the second network polymer is obtained by copolymerizing an olefin unsaturated bond-containing monomer and a polyacrylate crosslinking agent;
[0009] Among them, the first network polymer is first reacted completely and then dissolved in a solvent; then the olefin unsaturated bond-containing monomer and the polyacrylate crosslinking agent are added to the solution of the first network polymer to perform a copolymerization and crosslinking reaction to obtain the second network polymer. The double network gel electrolyte of the present invention not only enhances the overall structure of the electrolyte through a two-step construction method, but also significantly reduces the risk of reduced contrast of the electrochromic device due to dimerization by limiting the movement of the cathode electrochromic material. This design effectively improves the problem of uneven coloring and improves the performance and reliability of the electrochromic device.
[0010] As a preferred technical solution, the chemical structural formula of the cathode electrochromic material with unsaturated bonds is shown in general formula I:
[0011]
[0012] In the formula, R1 and R6 are alkyl groups with 1 to 8 carbon atoms respectively;
[0013] R2 to R5 and R7 to R 10 Independently selected from H, CH3, C2H5 or CN;
[0014] X - It is at least one of a halogen anion, an acetate anion, a tetrafluoroborate anion, a trifluoromethanesulfonate anion, a perchlorate anion, a bis(trifluoromethanesulfonyl)imide anion, and a tris(trifluoromethanesulfonyl)methyl anion.
[0015] As a preferred technical solution, the chemical structural formula of the anode electrochromic material with unsaturated bonds is shown in general formula II:
[0016]
[0017] In the formula, R 11 is CHCH3, CHC2H5 or CHC3H7;
[0018] R 12 To R 18 Independently selected from H, CH3 or CN.
[0019] As a preferred technical solution, the chemical structural formula of the methacrylate monomer is as shown in general formula III:
[0020]
[0021] In the formula, R 19 It is an alkyl group having 1 to 8 carbon atoms.
[0022] As a preferred technical solution, the olefin unsaturated bond-containing monomer is at least one of methyl acrylate, methyl methacrylate, acrylamide, methacrylamide, acrylic acid, methacrylic acid, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, n-butyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, and n-octyl methacrylate.
[0023] As a preferred technical solution, the polyacrylate crosslinking agent is at least one of 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol dimethacrylate, ditrimethylolpropane tetraacrylate, ethoxypentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.
[0024] As a preferred technical solution, the mass ratio of the olefin unsaturated bond-containing monomer and the polyacrylate crosslinking agent to the first network high molecular polymer is 10-30:0.1-5:2-5.
[0025] As a preferred technical solution, the solvent includes but is not limited to one or more of propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, N-methylpyrrolidone, cyclopentane, dimethyl sulfoxide, dimethylformamide, dimethylacetamide, acetonitrile, and diethylene glycol butyl ether.
[0026] Another aspect of the present invention is to provide a method for preparing the double network gel electrolyte for large-area electrochromic devices as described above, the preparation method comprising the following steps:
[0027] S1: Under certain reaction conditions, methacryloyl chloride is first reacted with bromoalkyl alcohol shown in structural formula a to obtain bromoalkyl methacrylate; then the bromoalkyl methacrylate is reacted with a bipyridine compound shown in structural formula b to obtain a monosubstituted bipyridine compound; then the monosubstituted bipyridine compound is reacted with bromoalkyl to obtain a disubstituted bipyridine compound, and after anion exchange reaction, a cathode electrochromic material with an unsaturated bond shown in general formula I is obtained;
[0028]
[0029] In the formula, R1 and R6 are alkyl groups with 1 to 8 carbon atoms;
[0030] R2 to R5 and R7 to R 10 Independently selected from H, CH3, C2H5 or CN;
[0031] X - is at least one of a halogen anion, an acetate anion, a tetrafluoroborate anion, a trifluoromethanesulfonate anion, a perchlorate anion, a bis(trifluoromethanesulfonyl)imide anion, and a tris(trifluoromethanesulfonyl)methyl anion;
[0032] S2: Under certain reaction conditions, an alkyl acyl chloride is reacted with a ferrocene compound shown in the structural formula C under the action of anhydrous aluminum chloride to obtain orange needle-shaped acylated ferrocene after separation; the acylated ferrocene is reacted with lithium aluminum tetrahydride and ammonium chloride to obtain 1-ferrocenyl alkanol; and the acylated ferrocene is reacted with methacryloyl chloride to obtain an unsaturated bond-bearing anode electrochromic material shown in the general formula II;
[0033]
[0034] In the formula, R 11 is CHCH3, CHC2H5 or CHC3H7;
[0035] R 12 To R 18 Independently selected from H, CH3 or CN;
[0036] S3: copolymerizing the cathode electrochromic material with unsaturated bonds obtained in step S1, the anode electrochromic material with unsaturated bonds obtained in step S2, and a methacrylate monomer to obtain a first network polymer;
[0037] S4: dissolving the first network polymer obtained in step S3 in a solvent, adding an olefin unsaturated bond-containing monomer and a polyacrylate crosslinking agent, and adding an initiator, and stirring sufficiently to obtain a double network gel electrolyte prepolymer solution; the double network gel electrolyte prepolymer solution undergoes a polymerization reaction under ultraviolet light, that is, a copolymerization and crosslinking reaction is carried out in the solution of the first network polymer to obtain a double network gel electrolyte comprising the first network polymer and the second network polymer.
[0038] As a preferred technical solution, in step S1, the molar ratio of the methacryloyl chloride to the bromoalkyl alcohol is 1-1.5:1, and the molar ratio of the bromoalkyl methacrylate to the bipyridine compound shown in structural formula b is 1:1-1.2; in step S2, the molar ratio of the alkyl chloride to the ferrocene compound shown in structural formula c is 1-1.3:1, and the molar ratio of the 1-ferrocenylalkanol to methacryloyl chloride is 1:1.1-1.5.
[0039] As a preferred technical solution, in step S3, the mass ratio of the cathode electrochromic material with unsaturated bonds, the anode electrochromic material with unsaturated bonds and the methacrylate monomer is 1:0.2 to 2:0.4 to 2.5.
[0040] As a preferred technical solution, the bromoalkyl alcohol is at least one of 2-bromo-1-ethanol, 3-bromo-1-propanol, 4-bromo-1-butanol, 5-bromo-1-pentanol, 6-bromo-1-hexanol, 7-bromo-1-heptanol and 8-bromo-1-octanol.
[0041] As a preferred technical solution, the bipyridine compound is at least one of 4,4'-bipyridine, 2,2'-dimethyl-4,4'-bipyridine, 2,2',6,6'-tetramethyl-4,4'-bipyridine, [4,4-bipyridine]-2,2'-dicarbonitrile, and [4,4-bipyridine]-3,3'-dicarbonitrile.
[0042] As a preferred technical solution, the bromoalkane is at least one of methyl bromide, ethyl bromide, propyl bromide, butyl bromide, pentane bromide, hexyl bromide, heptane bromide and octane bromide.
[0043] As a preferred technical solution, the alkyl acyl chloride is at least one of acetyl chloride, propionyl chloride and butyryl chloride.
[0044] As a preferred technical solution, the ferrocene compound is at least one of ferrocene, cyanoferrocene and methylferrocene.
[0045] The third aspect of the present invention is to provide an electrochromic device based on a double network gel electrolyte, the electrochromic device comprising a first conductive substrate, a second conductive substrate and a double network gel electrolyte electrochromic layer arranged between the first conductive substrate and the second conductive substrate; wherein the double network gel electrolyte electrochromic layer comprises a solvent, a first network polymer formed by copolymerization of at least one cathode electrochromic material and an anode electrochromic material, and a second network polymer formed by copolymerization of an olefin unsaturated bond-containing monomer and a polyacrylate crosslinking agent.
[0046] As a preferred technical solution, the substrates of the first conductive substrate and the second conductive substrate can be selected from a hard transparent substrate or a flexible substrate; for example, the hard transparent substrate is glass or plastic polymer, and the flexible substrate is PET film, PDMS film, PE film, PU film, etc. The transparent conductive layer on the substrates of the first conductive substrate and the second conductive substrate can be selected from at least one of tin oxide, zinc oxide, indium tin oxide, indium gallium zinc oxide composite, fluorine-doped tin oxide, aluminum-doped zinc oxide, and fluorine-doped zinc oxide.
[0047] Compared with the prior art, the present invention has the following beneficial effects:
[0048] The dual network gel electrolyte of the present invention significantly improves the application potential of electrochromic technology through innovative structural design. Its main advantages are that it realizes the long life and large-area application of the device, while maintaining uniform fading, fast color change response, low driving voltage, high contrast and good cycle stability. These characteristics make the device of the present invention not only suitable for small-sized application scenarios such as automotive anti-glare rearview mirrors, but also meet large-sized application scenarios such as aircraft windows and building glass curtain walls.
[0049] In addition, the present invention also effectively reduces the risk of leakage through the dual network structure, enhancing the safety and reliability of the device. In the continuous power-on test, the device exhibits high stability, proving its durability and long-term performance retention in practical applications. DETAILED DESCRIPTION
[0050] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.
[0051] Example 1
[0052] The present embodiment is a double network gel electrolyte for a large-area electrochromic device, which includes a first network polymer and a second network polymer; the first network polymer is obtained by copolymerization of a cathode electrochromic material with an unsaturated bond, an anode electrochromic material with an unsaturated bond and a methacrylate monomer; the second network polymer is obtained by copolymerization of a monomer containing an olefin unsaturated bond and a multi-acrylate crosslinking agent; wherein the first network polymer is first reacted completely and then dissolved in a solvent; then the monomer containing an olefin unsaturated bond and the multi-acrylate crosslinking agent are added, and a copolymerization and crosslinking reaction is carried out in a solution of the first network polymer to obtain the second network polymer.
[0053] Specifically, the method for preparing a double network gel electrolyte for a large-area electrochromic device described in this embodiment comprises the following steps:
[0054] S1: In an ice-water bath, 1.4 mol of methacryloyl chloride was slowly dripped into a mixture consisting of 1 mol of 2-bromo-1-ethanol, 1.15 mol of triethylamine and 800 mL of dichloromethane. After the dripping was completed, the mixture was stirred at room temperature overnight. After filtration, the filtrate was acid-washed, water-washed and alkaline-washed, and the solvent was removed. Finally, methyl bromide was obtained by vacuum distillation (1000 Pa, 80°C); then methyl bromide was reacted with 2,2'-dimethyl-4,4'-bipyridine in a molar ratio of 1:1.1 in acetonitrile to obtain a monosubstituted bipyridine compound. The monosubstituted bipyridine compound is reacted with bromoheptane (molar ratio of 1:1.2) in acetonitrile to obtain a disubstituted bipyridine compound (i.e., 1-heptyl-1'-(2-(methacryloyloxy)ethyl)-2,2'-dimethyl-4,4'-bipyridine dibromide); the disubstituted bipyridine compound is reacted with lithium bis(trifluoromethanesulfonyl)imide in an aqueous solution to obtain a cathode electrochromic material with an unsaturated bond.
[0055] S2: Under ice-water bath conditions, 1.2 mol of acetyl chloride in dichloromethane solution (300 mL) was slowly dripped into 1.4 mol of anhydrous aluminum chloride in dichloromethane solution (400 mL), stirred until the anhydrous aluminum chloride was basically dissolved, and then the solution was dripped into 1 mol of methyl ferrocene in dichloromethane solution (600 mL) at 0 ° C, and stirred at room temperature until no HCl gas emerged. The reaction solution was poured into a large amount of ice water, the organic phase was separated, washed three times with saturated sodium carbonate solution and water, and the solvent was spin-dried to obtain a purple solid, and orange needle-shaped 1-methyl-1'-acetyl ferrocene was obtained after recrystallization. The 1-methyl-1'-acetyl ferrocene was vacuum dried and dissolved in anhydrous tetrahydrofuran, and dripped into a tetrahydrofuran solution containing lithium tetrahydrogen aluminum at -10 ° C, heated to reflux for 2h, cooled and quenched, and a saturated ammonium chloride solution was added, washed with water, and the solvent was spin-dried to obtain 1-methyl-1'-(1-hydroxyethyl)-ferrocene. The 1-methyl-1'-(1-hydroxyethyl)-ferrocene and methacryloyl chloride in a molar ratio of 1:1.1 are reacted to obtain an anode electrochromic material with an unsaturated bond (i.e., 1-methyl-1'-(1-(methacryloyloxy)ethyl)-ferrocene).
[0056] S3: 10 g of the cathode electrochromic material with an unsaturated bond obtained in step S1, 5 g of the anode electrochromic material with an unsaturated bond obtained in step S2 and 4 g of ethyl methacrylate are added to a tetrahydrofuran solution (60 mL), and a catalytic amount of AIBN (azobisisobutyronitrile) is added to carry out copolymerization in a nitrogen atmosphere for 8 hours. After cooling, the mixture is poured into petroleum ether for precipitation and dried, and then dissolved in tetrahydrofuran, poured into petroleum ether for precipitation and dried. The mixture is repeated three times to wash away unreacted monomers to obtain a first network polymer, recorded as P10F5M4, and dried for use.
[0057] S4: dissolving 2 g of the first network polymer obtained in step S3 in 83 g of propylene carbonate by heating, adding 10 g of n-butyl methacrylate and 5 g of hexanediol dimethacrylate after cooling, and adding an initiator amount of AIBN, and stirring sufficiently to obtain a double network gel electrolyte prepolymer solution; the double network gel electrolyte prepolymer solution undergoes a polymerization reaction under ultraviolet light, i.e., a copolymerization and cross-linking reaction is carried out in the solution of the first network polymer to obtain a double network gel electrolyte comprising the first network polymer and the second network polymer.
[0058] Furthermore, when the dual network gel electrolyte prepolymer prepared in this embodiment is encapsulated in a large-area electrochromic device, the specific operation is as follows: first, a piece of ITO glass substrate is attached to the outer periphery of another piece of ITO glass substrate with a sealant along its periphery, and a cavity is formed between the two pieces of ITO glass substrates, and a small hole is left. The dual network gel electrolyte prepolymer is poured into the cavity between the two pieces of ITO glass substrates (25cm*40cm) under vacuum conditions, and after sealing, the dual cross-linked network gel electrolyte electrochromic device DN-EC is obtained by polymerization reaction for 8 hours under ultraviolet light.
[0059] The performance of the electrochromic device prepared in this embodiment was tested using a DC regulated power supply and a transmittance detector. The test results showed that the color change voltage was 1.2V, the transmittance was 78% before the color change, the transmittance was 20% after the color change, the contrast was 58%, the coloring time was 5.3s, and the fading time was 15.8s. After continuous power supply for 72h, the contrast became 56%.
[0060] Comparative Example 1
[0061] The preparation method of the electrolyte in this comparative example is basically the same as that in Example 1, except that this comparative example uses a small molecule monomer cathode material (1-1'-diheptyl-2,2'-dimethyl-4,4'-bipyridyl dibis(trifluoromethanesulfonyl)imide salt) and an anode material (1-methyl-1'-(1-hydroxyethyl)-ferrocene) without double bonds to replace the cathode electrochromic material with unsaturated bonds in step S1 of Example 1 and the anode electrochromic material with unsaturated bonds in step S2, respectively.
[0062] Add 1g of 1-1'-diheptyl-2,2'-dimethyl-4,4'-bipyridyl dibis(trifluoromethanesulfonyl)imide salt, 1g of 1-methyl-1'-(1-hydroxyethyl)-ferrocene, 83g of propylene carbonate, 10g of n-butyl methacrylate, and 5g of hexanediol dimethacrylate, and add an initiator dose of AIBN, and stir thoroughly. Use the same method to pour the solution into the cavity between two ITO glass substrates (25cm*40cm), seal them, and polymerize them under ultraviolet light for about 8h to obtain an electrochromic device D-EC in which small molecule cathode materials and anode materials are free in the gel electrolyte.
[0063] The performance test results show that the color change voltage is 1.0V, the transmittance before color change is 82%, the transmittance after color change is 17%, the contrast is 65%, the color change time is 4.1s, and the fading time is 13.7s. After continuous power-on for 72 hours, the electrochromic device shows obvious uneven color change. The contrast in the middle area away from the two sides of the electrode drops to 20%, and the contrast on the electrode side becomes 67%. The device is slightly transparent in the middle, and the coloring at both ends of the electrode is slightly darker; it failed the long-term power-on test.
[0064] Comparative Example 2
[0065] The preparation method of the electrolyte in this comparative example is basically the same as that in Example 1, except that in step S4 of this comparative example, 10 g of n-butyl methacrylate and 5 g of hexanediol dimethacrylate are not added, and an initiator dose of AIBN is not added; instead, the first network polymer (P10F5M4) obtained in step S3 is directly heated and dissolved in 98 g of propylene carbonate, and after cooling, the solution is poured into the cavity between two ITO glass substrates (25 cm*40 cm), and the cavity is sealed to obtain a single network electrochromic device S-EC.
[0066] The performance test results show that the color change voltage is 1.0V, the transmittance before color change is 83%, the transmittance after color change is 34%, the contrast is 49%, the color change time is 3.6s, and the fading time is 12.7s. After continuous power-on for 72 hours, the electrochromic device shows obvious color unevenness. The contrast in the middle area away from the two sides of the electrode drops to 10%, and the contrast on the electrode side becomes 52%. The device is transparent in the middle, and the coloring at both ends of the electrode deepens; it failed the long-term power-on test.
[0067] Example 2
[0068] The present embodiment is a double network gel electrolyte for a large-area electrochromic device, which includes a first network polymer and a second network polymer; the first network polymer is obtained by copolymerization of a cathode electrochromic material with an unsaturated bond, an anode electrochromic material with an unsaturated bond and a methacrylate monomer; the second network polymer is obtained by copolymerization of a monomer containing an olefin unsaturated bond and a multi-acrylate crosslinking agent; wherein the first network polymer is first reacted completely and then dissolved in a solvent; then the monomer containing an olefin unsaturated bond and the multi-acrylate crosslinking agent are added, and a copolymerization and crosslinking reaction is carried out in a solution of the first network polymer to obtain the second network polymer.
[0069] Specifically, the method for preparing a double network gel electrolyte for a large-area electrochromic device described in this embodiment comprises the following steps:
[0070] S1: In an ice-water bath, 9.57 mol of methacryloyl chloride was slowly dripped into a mixture consisting of 9.5 mol of 5-bromo-1-pentanol, 11.3 mol of triethylamine and 5 L of dichloromethane. After the dripping was completed, the mixture was stirred at room temperature overnight. After filtration, the filtrate was acid-washed, water-washed and alkaline-washed, and the solvent was removed. Finally, bromopentyl methacrylate was obtained by vacuum distillation (1000 Pa, 110°C); then bromopentyl methacrylate with a molar ratio of 1:1.1 was refluxed with [4,4'-bipyridine]-2,2'-dicarbonitrile in acetonitrile to obtain monosubstituted A bipyridine compound (i.e., 1-(2-(methacryloyloxy)pentyl)-2,2'-dinitrile-4,4'-bipyridine bromide), and then the monosubstituted bipyridine compound is refluxed with bromopropane (molar ratio of 1:1.2) in acetonitrile to obtain a disubstituted bipyridine compound (i.e., 1-propyl-1'-(2-(methacryloyloxy)pentyl)-2,2'-dinitrile-4,4'-bipyridine dibromide); the disubstituted bipyridine compound is subjected to anion exchange reaction with sodium fluoroborate in an aqueous solution to obtain a cathode electrochromic material with an unsaturated bond.
[0071] S2: In an ice-water bath, 5.7 mol of dichloromethane solution (2.5 L) of butyryl chloride is slowly dripped into 5.8 mol of anhydrous aluminum chloride solution (4 L), stirred until the anhydrous aluminum chloride is basically dissolved, and then the solution is dripped into 5.4 mol of dichloromethane solution (5 L) of ferrocene at 0 ° C, and stirred at room temperature until no HCl gas emerges. The reaction solution is poured into a large amount of ice water, the organic phase is separated, washed three times with saturated sodium carbonate solution and water, and the solvent is spin-dried to obtain a purple solid, and orange needle-shaped 1-butyryl ferrocene is obtained after recrystallization. The 1-butyryl ferrocene is vacuum dried and dissolved in anhydrous tetrahydrofuran, and dripped into a tetrahydrofuran solution containing lithium tetrahydrogen aluminum at -10 ° C, heated to reflux for 3h, cooled and quenched, a saturated ammonium chloride solution is added, washed with water, and the solvent is spin-dried to obtain 1-ferrocenyl-1-butanol. The 1-ferrocenyl-1-butanol and methacryloyl chloride in a molar ratio of 1:1.15 were reacted to obtain an anode electrochromic material with an unsaturated bond (i.e., 1-(1-(methacryloyloxy)butyl)-ferrocene).
[0072] S3: 10 g of the cathode electrochromic material with unsaturated bonds obtained in step S1, 20 g of the anode electrochromic material with unsaturated bonds obtained in step S2 and 25 g of methyl methacrylate are added to a tetrahydrofuran solution (200 mL), and a catalytic amount of AIBN is added to carry out copolymerization in a nitrogen atmosphere for 8 hours. After cooling, the mixture is poured into petroleum ether for precipitation and dried, and then dissolved in tetrahydrofuran, poured into petroleum ether for precipitation and dried. The mixture is repeated three times to wash away unreacted monomers to obtain a first network polymer, recorded as P10F20M25, and dried for use.
[0073] S4: 5 g of the first network polymer obtained in step S3 is heated and dissolved in 75 g of N-methylpyrrolidone, and after cooling, 20 g of methyl methacrylate and 0.6 g of ethoxypentaerythritol tetraacrylate are added, and an initiator amount of AIBN is added, and after sufficient stirring, a double network gel electrolyte prepolymer solution is obtained; the double network gel electrolyte prepolymer solution is subjected to a polymerization reaction under ultraviolet light, that is, a copolymerization and cross-linking reaction is carried out in the solution of the above-mentioned first network polymer to obtain a double network gel electrolyte including the first network polymer and the second network polymer.
[0074] Furthermore, when the dual network gel electrolyte prepolymer prepared in this embodiment is encapsulated in a large-area electrochromic device, the specific operation is as follows: first, a piece of ITO glass substrate is attached to the outer periphery of another piece of ITO glass substrate with a sealant along its periphery, and a cavity is formed between the two pieces of ITO glass substrates, and a small hole is left. The dual network gel electrolyte prepolymer is poured into the cavity between the two pieces of ITO glass substrates (25cm*40cm) under vacuum conditions, and after sealing, the dual cross-linked network gel electrolyte electrochromic device DN-EC is obtained by polymerization reaction for 8 hours under ultraviolet light.
[0075] The performance of the electrochromic device prepared in this embodiment was tested using a DC regulated power supply and a transmittance detector. The test results showed that the color change voltage was 1.2V, the transmittance before the color change was 82%, the transmittance after the color change was 24%, the contrast ratio was 58%, the coloring time was 5.6s, and the fading time was 16.7s. After continuous power-on for 72h, the contrast ratio became 53%.
[0076] Example 3
[0077] The present embodiment is a double network gel electrolyte for a large-area electrochromic device, which includes a first network polymer and a second network polymer; the first network polymer is obtained by copolymerization of a cathode electrochromic material with an unsaturated bond, an anode electrochromic material with an unsaturated bond and a methacrylate monomer; the second network polymer is obtained by copolymerization of a monomer containing an olefin unsaturated bond and a multi-acrylate crosslinking agent; wherein the first network polymer is first reacted completely and then dissolved in a solvent; then the monomer containing an olefin unsaturated bond and the multi-acrylate crosslinking agent are added, and a copolymerization and crosslinking reaction is carried out in a solution of the first network polymer to obtain the second network polymer.
[0078] Specifically, the method for preparing a double network gel electrolyte for a large-area electrochromic device described in this embodiment comprises the following steps:
[0079] S1: In an ice-water bath, 30 mmol of methacryloyl chloride was slowly dripped into a mixture of 20 mmol of 8-bromo-1-octanol, 32 mmol of triethylamine and 20 mL of dichloromethane. After the dripping was completed, the mixture was stirred at room temperature overnight. After filtration, the filtrate was acid-washed, water-washed and alkaline-washed to remove the solvent. Finally, methacrylate bromoctyl ester was obtained by vacuum distillation (1000 Pa, 130°C). Then, methacrylate bromoctyl ester and 4,4'-bipyridine in a molar ratio of 1:1.15 were refluxed in acetonitrile to obtain a single extract. The monosubstituted bipyridine compound (i.e., 1-(2-(methacryloyloxy)octyl)-4,4'-bipyridine bromide) is reacted with bromooctane (molar ratio of 1:1.2) in acetonitrile for reflux reaction to obtain a disubstituted bipyridine compound (i.e., 1-octyl-1'-(2-(methacryloyloxy)octyl)-4,4'-bipyridine dibromide); the disubstituted bipyridine compound is reacted with lithium bis(trifluoromethanesulfonyl)imide in an aqueous solution for anion exchange reaction to obtain a cathode electrochromic material with an unsaturated bond.
[0080] S2: In an ice-water bath, slowly drip a dichloromethane solution (15 mL) of 20 mmol propionyl chloride into a dichloromethane solution (15 mL) of 24 mmol anhydrous aluminum chloride, stir until the anhydrous aluminum chloride is basically dissolved, then drip the solution into a dichloromethane solution (15 mL) of 16 mmol cyanoferrocene at 0°C, and stir at room temperature until no HCl gas emerges. Pour the reaction solution into a large amount of ice water, separate the organic phase, wash it three times with a saturated sodium carbonate solution and water, spin dry the solvent to obtain a purple solid, and recrystallize to obtain an orange needle-shaped 1-cyano-1'-propionyl ferrocene. The 1-cyano-1'-propionyl ferrocene is vacuum dried and dissolved in anhydrous tetrahydrofuran, and dripped into a tetrahydrofuran solution containing lithium tetrahydrogen aluminum at -10°C, heated to reflux for 1h, cooled and quenched, and a saturated ammonium chloride solution is added, washed with water, and the solvent is spin dried to obtain 1'-(1-cyano)ferrocenyl-1-propanol. The 1'-(1-cyano)ferrocenyl-1-propanol and methacryloyl chloride in a molar ratio of 1:1.3 are reacted to obtain an anode electrochromic material with an unsaturated bond (i.e., 1-cyano-1'-(1-(methacryloyloxy)propyl)-ferrocene).
[0081] S3: Add 1 g of the cathode electrochromic material with unsaturated bonds obtained in step S1, 1 g of the anode electrochromic material with unsaturated bonds obtained in step S2, and 0.8 g of propyl methacrylate to a tetrahydrofuran solution (10 mL), add a catalytic amount of AIBN, and carry out copolymerization in a nitrogen atmosphere for 8 hours. After cooling, pour into petroleum ether to precipitate and dry, then dissolve in tetrahydrofuran, pour into petroleum ether to precipitate and dry, repeat three times to wash away unreacted monomers, and obtain a first network high molecular polymer, recorded as P1F1M0.8, and dry for use.
[0082] S4: 3 g of the first network polymer obtained in step S3 is heated and dissolved in 67 g of diethyl carbonate, and after cooling, 30 g of methacrylamide and 0.1 g of dipentaerythritol hexaacrylate are added, and an initiator amount of AIBN is added, and after sufficient stirring, a double network gel electrolyte prepolymer solution is obtained; the double network gel electrolyte prepolymer solution is subjected to a polymerization reaction under ultraviolet light, that is, a copolymerization and cross-linking reaction is carried out in the solution of the above-mentioned first network polymer to obtain a double network gel electrolyte including the first network polymer and the second network polymer.
[0083] Furthermore, when the dual network gel electrolyte prepolymer prepared in this embodiment is encapsulated in a large-area electrochromic device, the specific operation is as follows: first, a piece of ITO glass substrate is attached to the outer periphery of another piece of ITO glass substrate with a sealant along its periphery, and a cavity is formed between the two pieces of ITO glass substrates, and a small hole is left. The dual network gel electrolyte prepolymer is poured into the cavity between the two pieces of ITO glass substrates (25cm*40cm) under vacuum conditions, and after sealing, the dual cross-linked network gel electrolyte electrochromic device DN-EC is obtained by polymerization reaction for 8 hours under ultraviolet light.
[0084] The performance of the electrochromic device prepared in this embodiment was tested using a DC regulated power supply and a transmittance detector. The test results showed that the color change voltage was 1.2V, the transmittance before the color change was 85%, the transmittance after the color change was 28%, the contrast ratio was 57%, the coloring time was 4.8s, and the fading time was 13.7s. After continuous power-on for 72h, the contrast ratio became 53%.
[0085] It can be seen that the patent of the present invention has considerable advantages over the currently used technology. The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. The present invention may have various changes and improvements without departing from the spirit and scope of the present invention, and these changes and improvements fall within the scope of the present invention to be protected.
Claims
1. A double network gel electrolyte for large-area electrochromic devices, It is characterized in that The double network gel electrolyte comprises: A first network polymer, wherein the first network polymer is obtained by copolymerization of a cathode electrochromic material with an unsaturated bond, an anode electrochromic material with an unsaturated bond, and a methacrylate monomer; and A second network polymer, wherein the second network polymer is obtained by copolymerizing an olefin unsaturated bond-containing monomer and a polyacrylate crosslinking agent; The first network polymer is first reacted completely and then dissolved in a solvent; then the olefin unsaturated bond-containing monomer and the polyacrylate crosslinking agent are added to carry out copolymerization and crosslinking reaction in the solution of the first network polymer to obtain the second network polymer.
2. The double network gel electrolyte for large-area electrochromic devices according to claim 1, It is characterized in that The chemical structural formula of the cathode electrochromic material with unsaturated bonds is shown in general formula I. In the formula, R 1 , R 6 are alkyl groups having 1 to 8 carbon atoms; R 2 To R 5 and R 7 To R 10 Independently selected from H, CH 3 , C 2 H 5 or CN; X - It is at least one of a halogen anion, an acetate anion, a tetrafluoroborate anion, a trifluoromethanesulfonate anion, a perchlorate anion, a bis(trifluoromethanesulfonyl)imide anion, and a tris(trifluoromethanesulfonyl)methyl anion.
3. The double network gel electrolyte for large-area electrochromic devices according to claim 1, It is characterized in that The chemical structural formula of the anode electrochromic material with unsaturated bonds is shown in general formula II: In the formula, R 11 CHCH 3 , CHC 2 H 5 or CHC 3 H 7 ; R 12 To R 18 Independently selected from H, CH 3 or CN.
4. The double network gel electrolyte for large-area electrochromic devices according to claim 1, It is characterized in that The chemical structural formula of the methacrylate monomer is shown in Formula III, In the formula, R 19 It is an alkyl group having 1 to 8 carbon atoms.
5. The double network gel electrolyte for large-area electrochromic devices according to claim 1, It is characterized in that The olefin unsaturated bond-containing monomer is at least one of methyl acrylate, methyl methacrylate, acrylamide, methacrylamide, acrylic acid, methacrylic acid, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, n-butyl methacrylate, hydroxyethyl acrylate, hydroxyethyl methacrylate, 2-ethylhexyl acrylate, 2-ethylhexyl methacrylate, lauryl methacrylate, and n-octyl methacrylate.
6. The double network gel electrolyte for large-area electrochromic devices according to claim 1, It is characterized in that The polyacrylate crosslinking agent is at least one of 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, diethylene glycol dimethacrylate, ditrimethylolpropane tetraacrylate, ethoxypentaerythritol tetraacrylate and dipentaerythritol hexaacrylate.
7. A method for preparing a double network gel electrolyte for a large-area electrochromic device as claimed in any one of claims 1 to 6, It is characterized in that The preparation method comprises the following steps: S1: Under certain reaction conditions, methacryloyl chloride is first reacted with bromoalkyl alcohol shown in structural formula a to obtain bromoalkyl methacrylate; then the bromoalkyl methacrylate is reacted with a bipyridine compound shown in structural formula b to obtain a monosubstituted bipyridine compound; then the monosubstituted bipyridine compound is reacted with bromoalkyl to obtain a disubstituted bipyridine compound, and after anion exchange reaction, a cathode electrochromic material with an unsaturated bond shown in general formula I is obtained; In the formula, R 1 , R 6 are alkyl groups having 1 to 8 carbon atoms; R 2 To R 5 and R 7 To R 10 Independently selected from H, CH 3 , C 2 H 5 or CN; X - is at least one of a halogen anion, an acetate anion, a tetrafluoroborate anion, a trifluoromethanesulfonate anion, a perchlorate anion, a bis(trifluoromethanesulfonyl)imide anion, and a tris(trifluoromethanesulfonyl)methyl anion; S2: Under certain reaction conditions, an alkyl acyl chloride is reacted with a ferrocene compound shown in the structural formula C under the action of anhydrous aluminum chloride to obtain acylated ferrocene after separation; the acylated ferrocene is reduced to obtain 1-ferrocenyl alkanol; and the 1-ferrocenyl alkanol is reacted with methacryloyl chloride to obtain an anodic electrochromic material with an unsaturated bond shown in the general formula II; In the formula, R 11 CHCH 3 , CHC 2 H 5 or CHC 3 H 7 ; R 12 To R 18 Independently selected from H, CH 3 or CN; S3: copolymerizing the cathode electrochromic material with unsaturated bonds obtained in step S1, the anode electrochromic material with unsaturated bonds obtained in step S2, and a methacrylate monomer to obtain a first network polymer; S4: dissolving the first network polymer obtained in step S3 in a solvent, adding an olefin unsaturated bond-containing monomer and a polyacrylate crosslinking agent, and performing a copolymerization and crosslinking reaction in the solution of the first network polymer to obtain a double network gel electrolyte including the first network polymer and the second network polymer.