Resist composition and pattern forming method
By using tin cluster compounds of specific structures and resist compositions of organic solvents, combined with high-energy ray exposure and development technology, the problems of sensitivity, resolution and LWR in EUV lithography are solved, and efficient fine pattern formation is achieved.
Patent Information
- Application Number
- CN202410567595.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
In high-energy ray lithography technology, especially in EUV lithography, existing resist materials are difficult to take into account the excellent high sensitivity, resolution and linewidth roughness (LWR), and chemical amplification resists exist in fine pattern formation. Problems of acid diffusion and insufficient sensitivity.
A resist composition with a main component of a tin cluster compound having a specific structure is used, and combined with an organic solvent and a surfactant, a resist film is formed through high-energy radiation exposure and development to achieve non-chemically amplified pattern formation.
This resist composition significantly improves sensitivity and resolution in EUV lithography, and optimizes linewidth roughness, which is suitable for precision machining of fine patterns and enhances device performance.
Smart Images

Figure CN118938599A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a resist composition and a pattern forming method. Background Art
[0002] As the IoT market expands, the pursuit of higher integration, higher speed, and lower power consumption of LSIs is further pursued, and the miniaturization of pattern rules is progressing rapidly. In particular, logic devices are leading the miniaturization. As for the most advanced miniaturization technology, mass production of 10nm node devices using double patterning, triple patterning, and quadruple patterning of ArF immersion lithography is in progress, and the review of 7nm node devices using the next-generation extreme ultraviolet (EUV) lithography with a wavelength of 13.5nm is underway.
[0003] As the miniaturization progresses, image blurring due to acid diffusion has become a problem (Non-Patent Document 1). In order to ensure the resolution of fine patterns after the processing size of 45nm, it has been proposed that it is not only important to improve the dissolution contrast as proposed in the past, but also to control the acid diffusion (Non-Patent Document 2). However, since chemically amplified resist compositions improve sensitivity and contrast by acid diffusion, if attempts are made to reduce the post-exposure baking (PEB) temperature or shorten the time to extremely suppress acid diffusion, the sensitivity and contrast will be significantly reduced.
[0004] It is effective to add an acid generator that generates an acid with a large barrier to inhibit acid diffusion. Therefore, it has been proposed to copolymerize an acid generator having an onium salt of a polymerizable olefin with a polymer. However, it is believed that in the pattern formation of a resist film with a processing size of 16nm or more, chemically amplified resist materials cannot form patterns from the perspective of acid diffusion, and it is necessary to develop non-chemically amplified resist compositions.
[0005] As for the materials used in non-chemically amplified resist compositions, polymethyl methacrylate (PMMA) can be cited. PMMA is a positive resist material whose main chain is cut by electron beam (EB) or EUV irradiation, and its molecular weight is reduced, thereby increasing its solubility in organic solvent developers. However, it has the disadvantages of low etching resistance and high outgassing during exposure due to the lack of a ring structure.
[0006] Hydrogen silsesquioxane (HSQ) is a negative resist material that becomes insoluble in alkaline developer by crosslinking due to the condensation reaction of silanols produced by EB or EUV irradiation. In addition, chlorine-substituted calixarene also acts as a negative resist material. These negative resist materials have small edge roughness and very high resolution because of the small molecular size before crosslinking and no blurring caused by acid diffusion, and are used as pattern transfer materials for displaying the resolution limit of exposure equipment. However, the sensitivity of these materials is insufficient and needs to be further improved.
[0007] The reason why the development of materials for EUV lithography is difficult is that the number of photons in EUV exposure is scarce. The energy of EUV is much higher than that of ArF excimer laser, and the number of photons in EUV exposure is 1 / 14 of that in ArF exposure. Moreover, the size of the pattern formed by EUV exposure is less than half of that of ArF exposure. Therefore, EUV exposure is easily affected by the variation of the number of photons. The variation of the number of photons in the region of extremely short wavelength radiation light is the shot noise of physical phenomena, and this influence cannot be eliminated. Therefore, the so-called probability theory (Stochastics) has attracted attention. Although the influence of shot noise cannot be eliminated, some people discuss how to reduce its influence. Due to the influence of shot noise, not only the size uniformity (CDU) and line width roughness (LWR) increase, but also the phenomenon of hole clogging is observed with a probability of one in millions. If the hole is blocked, it will cause poor conduction and the transistor will not work, so it will have an adverse effect on the overall performance of the device.
[0008] As for the method of reducing the influence of shot noise from the resist aspect, an inorganic resist composition using an element with large EUV absorption as a core has been proposed (Patent Document 1). However, although the inorganic resist composition has a high sensitivity, it is still insufficient, and has a large number of problems such as insufficient solubility in resist solvents, storage stability, and defects.
[0009] Non-patent document 3 proposes a negative resist composition using a tin compound. This is a non-chemically amplified resist whose main component is tin, which has high EUV light absorption. It can improve stochastics and achieve a certain improvement in sensitivity and resolution, but it is still insufficient and there is a strong need to develop further improved products.
[0010] Prior art literature
[0011] Patent Literature
[0012] [Patent Document 1] Japanese Patent Application Publication No. 2015-108781
[0013] Non-patent literature
[0014] [Non-patent document 1] SPIE Vol.5039, p1 (2003)
[0015] [Non-patent document 2] SPIE Vol.6520, p65203L-1 (2007)
[0016] [Non-patent document 3] SPIE Vol.9051, p90511B-1 (2014) Summary of the invention
[0017] [Problems to be solved by the invention]
[0018] The present invention is made in view of the above situation, and an object of the present invention is to provide a resist composition having excellent sensitivity, resolution and LWR in optical lithography using high-energy rays, especially EUV lithography, and a pattern forming method using the resist composition.
[0019] [Methods to solve the problem]
[0020] The inventors of the present application have repeatedly and diligently studied to achieve the aforementioned purpose and have found that a resist composition whose main component is a tin cluster compound with a specific structure has high sensitivity and provides a resist film exhibiting excellent resolution and LWR, which is very effective in precise micro-machining, thereby completing the present invention.
[0021] That is, the present invention provides the following resist composition and pattern forming method.
[0022] 1. A resist composition comprising a tin compound represented by the following formula (1) and an organic solvent,
[0023] [Chemistry 1]
[0024]
[0025] In the formula, R 1A ~R 10A and R 1B ~R 10B are each independently a hydrocarbon group having 1 to 20 carbon atoms,
[0026] R 11 ~R 14 are each independently a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms,
[0027] L a1 and L a2 Each is independently a linking group.
[0028] 2. The resist composition of 1, wherein L a1 and L a2 Each is independently a group represented by any one of the following formulae (2a) to (2d),
[0029] [Chemistry 2]
[0030]
[0031] Wherein, the dotted line represents the atomic bond with Sn.
[0032] 3. The resist composition according to 1 or 2, wherein R 1A ~R 10A and R 1B ~R 10B is isopropyl, n-butyl, tert-butyl or benzyl.
[0033] 4. The resist composition according to any one of 1 to 3, further comprising a surfactant.
[0034] 5. A pattern forming method comprising the following steps:
[0035] A resist film is formed on a substrate using the resist composition of any one of items 1 to 4, the resist film is exposed to high-energy rays, and the exposed resist film is developed using a developer.
[0036] 6. The pattern forming method of 5, wherein the high-energy ray is EB or EUV.
[0037] [Effects of the Invention]
[0038] The resist composition of the present invention can achieve both high sensitivity and high resolution in optical lithography using high-energy rays, especially EUV lithography, and has excellent LWR, so it is very useful for forming fine patterns. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] [ Figure 1 ] The tin compound M-1 obtained in Synthesis Example 1 1 H-NMR spectrum.
[0040] [ Figure 2 ] The tin compound M-1 obtained in Synthesis Example 1 119 Sn-NMR spectrum.
[0041] [ Figure 3 ] shows an SEM image of a line-and-space (LS) pattern with a spacing width of 20 nm and a pitch of 40 nm in Eop of Example 2-1.
[0042] [ Figure 4 ] For the resist film produced in Example 3, the relationship between film thickness and exposure amount was plotted (contrast curve and PEB shrinkage) to obtain the results. DETAILED DESCRIPTION
[0043] [Resist composition]
[0044] The resist composition of the present invention comprises a predetermined tin compound and an organic solvent.
[0045] [Tin compounds]
[0046] The tin compound is a main component of the resist composition of the present invention, and is represented by the following formula (1): In the present invention, the main component means a component with the largest content other than the solvent.
[0047] [Chemistry 3]
[0048]
[0049] In formula (1), R 1A ~R 10A and R 1B ~R 10B Each R is independently a hydrocarbon group having 1 to 20 carbon atoms. 11 ~R 14 Each independently represents a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms. a1 and L a2 Each is independently a linking group.
[0050] R 1A ~R 10A , R 1B ~R 10B and R 11 ~R 14 The hydrocarbon group having 1 to 20 carbon atoms represented by may be saturated or unsaturated, and may be straight-chain, branched, or cyclic. Specific examples thereof include alkyl groups having 1 to 20 carbon atoms, such as methyl, ethyl, propyl, isopropyl, n-butyl, sec-butyl, tert-butyl, tert-pentyl, n-pentyl, n-hexyl, n-octyl, 2-ethylhexyl, n-nonyl, and n-decyl; cyclopentyl, cyclohexyl, cyclopentylmethyl, cyclopentylethyl, cyclopentylbutyl, cyclohexylmethyl, cyclohexylethyl, cyclohexylbutyl, norbornyl, tricyclo[5.2.1.0 2,6 ] cyclic saturated hydrocarbon groups having 3 to 20 carbon atoms, such as decyl, adamantyl, and adamantylmethyl; alkenyl groups having 2 to 20 carbon atoms, such as vinyl and allyl; aryl groups having 6 to 20 carbon atoms, such as phenyl and naphthyl; aralkyl groups having 7 to 20 carbon atoms, such as benzyl and phenethyl; groups obtained by combining these groups, etc.
[0051] Furthermore, part or all of the hydrogen atoms of the aforementioned hydrocarbon group may be substituted with groups containing heteroatoms such as oxygen atoms, sulfur atoms, nitrogen atoms, halogen atoms, etc. 2 - may also be substituted with a group containing a heteroatom such as an oxygen atom, a sulfur atom, or a nitrogen atom, and as a result, may also include a hydroxyl group, a cyano group, a halogen atom, a carbonyl group, an ether bond, a thioether bond, an ester bond, a sulfonate bond, a carbonate bond, a carbamate bond, a lactone ring, a sultone ring, a carboxylic anhydride (-C(=O)-OC(=O)-), and the like.
[0052] Considering the easy acquisition of raw materials and the ease of manufacturing, R 1A ~R 10A For the same group, R 1B ~R 10B Preferably, R 1A ~R 10A and R 1B ~R 10B Preferably, all of them are the same group.
[0053] Just R1A ~R 10A and R 1B ~R 10B For R, isopropyl, n-butyl, tert-butyl, benzyl, etc. are preferred, and n-butyl, tert-butyl, benzyl, etc. are more preferred. 11 ~R 14 For , it is preferably a hydrogen atom or a methyl group.
[0054] Just L a1 and L a2 As for the connecting group represented by, for example, a group represented by any one of the following formulae (2a) to (2d) can be mentioned,
[0055] [Chemistry 4]
[0056]
[0057] Wherein, the dotted line represents the atomic bond with Sn.
[0058] Specific examples of the tin compound represented by formula (1) include the following, but are not limited thereto: In the following formula, Bn is a benzyl group, nBu is an n-butyl group, tBu is a tert-butyl group, iPr is an isopropyl group, and Me is a methyl group.
[0059] [Chemistry 5]
[0060]
[0061] [Chemistry 6]
[0062]
[0063] [Chemistry 7]
[0064]
[0065] [Chemistry 8]
[0066]
[0067] [Chemistry 9]
[0068]
[0069] [Chemistry 10]
[0070]
[0071] [Chemistry 11]
[0072]
[0073] [Chemistry 12]
[0074]
[0075] The tin compound represented by formula (1) may be used alone or in combination of two or more. From the viewpoint of improving the uniformity of the components, it is preferred to use one alone or in combination of two.
[0076] The tin compound represented by formula (1) can be synthesized with reference to Z. Naturforsch. 2010, 65b, 1293-1300, Inorg. Chim. Acta 357, (9), 2791-2797, 2004, and the like.
[0077] [Organic solvents]
[0078] The resist composition of the present invention includes an organic solvent. As for the aforementioned solvent, there is no particular limitation as long as it can dissolve the tin compound represented by formula (1) and form a film. As for such an organic solvent, for example, ketones such as cyclohexanone and methyl-2-n-pentanone; alcohols such as 3-methoxybutanol, 3-methyl-3-methoxybutanol, 1-methoxy-2-propanol, 1-ethoxy-2-propanol, diacetone alcohol (DAA); ethers such as propylene glycol monomethyl ether, ethylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol monoethyl ether, propylene glycol dimethyl ether, diethylene glycol dimethyl ether; propylene glycol monomethyl ether acetate (P Esters such as propylene glycol monoethyl ether acetate, propylene glycol monoethyl ether acetate, ethyl lactate, ethyl pyruvate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, methyl 2-hydroxyisobutyrate, tert-butyl acetate, cyclohexyl acetate, tert-butyl propionate, propylene glycol monotert-butyl ether acetate; lactones such as γ-butyrolactone; carboxylic acids such as acetic acid and propionic acid, aromatics such as toluene, xylene, cresol, anisole, trifluorotoluene, etc.; mixed solvents thereof, etc.
[0079] The content of the organic solvent is preferably 200 to 20,000 parts by mass, more preferably 500 to 10,000 parts by mass, based on 100 parts by mass of the tin compound represented by formula (1).
[0080] The resist composition of the present invention is a so-called molecular resist composition, whose main component is a low molecular compound, and is a resist composition that does not contain a base polymer used in a polymer resist composition. It is speculated that the resist composition of the present invention is insoluble in the developer by photodecomposition of the tin compound as the main component and the subsequent cross-linking reaction, which causes a change in solvent solubility. This reaction is not a catalytic reaction, so the resist composition of the present invention will function as a non-chemically amplified resist composition. Therefore, compared with the known chemically amplified resist composition whose main component is a multi-polymer, the limiting resolution is improved. In particular, in EUV lithography, tin atoms have high EUV absorption energy, so they can provide a resist material with improved Stochastics, sensitivity, and LWR.
[0081] The aforementioned tin compound is a 10-nuclear complex of tin, i.e., a cluster compound. By using a thermodynamically stable cluster structure, the storage stability is also excellent. In addition, the aforementioned non-patent document 3 illustrates a 12-nuclear complex of tin cluster compounds, which also have the same advantage of thermodynamic stability, but have low solubility in organic solvents. In this case, if the resist composition is stored for a long time, there are concerns about precipitation and deterioration of film-forming properties over time. On the other hand, the aforementioned tin compound has excellent solvent solubility. Although the reason for this is unclear, it is speculated that the factor L in formula (1) a1 and L a2 The presence of (i.e., the connecting part) causes the rigidity of the cluster structure to be relaxed, which contributes to the solvent solubility. In addition, the aforementioned tin compound has the characteristic of large film shrinkage during exposure. It is believed that the pattern obtained by exposure can be miniaturized and dense by shrinkage, and defects such as pattern collapse and line breakage are not seen even in fine lines, and the ultimate resolution will be improved. Moreover, the film shrinkage is preferably 20% or more, more preferably 30% or more, and more preferably 50% or more.
[0082] The resist composition of the present invention may also contain a surfactant as another component. As for the surfactant, it is preferably a fluorine-based and / or silicone-based surfactant. As for such surfactants, the surfactants described in paragraph
[0276] of the specification of U.S. Patent Application Publication No. 2008 / 0248425 can be used. They can be used alone or in combination of two or more. Furthermore, the present invention can also use other surfactants other than the fluorine-based and / or silicone-based surfactants described in paragraph
[0280] of the specification of U.S. Patent Application Publication No. 2008 / 0248425. When the resist composition of the present invention contains a surfactant, its content is preferably 0.001 to 20 parts by mass, and more preferably 0.1 to 10 parts by mass, relative to 100 parts by mass of the aforementioned tin compound. The aforementioned surfactants can be used alone or in combination of two or more.
[0083] [Pattern Formation Method]
[0084] When the resist composition of the present invention is used in the manufacture of various integrated circuits, known photolithography techniques can be used. For example, as for the pattern forming method, a method comprising the following steps can be cited: using the resist composition to form a resist film on a substrate, exposing the resist film to high-energy rays, and developing the exposed resist film using a developer.
[0085] First, the resist composition of the present invention is applied to a substrate (Si, SiO 2, SiN, SiON, TiN, WSi, BPSG, SOG, organic anti-reflection film, etc.) or substrates for mask circuit manufacturing (Cr, CrO, CrON, MoSi 2 、SiO 2 The film is coated with a suitable coating method such as spin coating, roller coating, flow coating, dip coating, spray coating, scraping coating, etc., so that the coating thickness becomes 0.01 to 2 μm. The film is placed on a hot plate and pre-baked at preferably 60 to 150° C. for 10 seconds to 30 minutes, more preferably at 80 to 120° C. for 30 seconds to 20 minutes to form a resist film.
[0086] Then, the resist film is exposed using high-energy radiation. Examples of the high-energy radiation include ultraviolet rays, far ultraviolet rays, EB, EUV, X-rays, soft X-rays, excimer lasers, gamma rays, synchrotron radiation, and the like. When ultraviolet rays, far ultraviolet rays, EUV, X-rays, soft X-rays, excimer lasers, gamma rays, synchrotron radiation, and the like are used as the high-energy radiation, the exposure is preferably about 1 to 200 mJ / cm2 directly or using a mask for forming a target pattern. 2 , more preferably about 10 to 100 mJ / cm 2 When EB is used as high-energy radiation, the exposure amount is preferably about 0.1 to 5000 μC / cm2, either directly or using a mask for forming a target pattern. 2 , preferably about 0.5 to 4000 μC / cm 2 Furthermore, the resist composition of the present invention is particularly suitable for fine patterning by KrF excimer laser, ArF excimer laser, EB, EUV, X-ray, soft X-ray, gamma ray, synchrotron radiation among high energy rays, and is particularly suitable for fine patterning by EB or EUV.
[0087] The resist composition of the present invention may also be subjected to post-exposure baking (PEB) in order to promote or terminate the reaction after photolysis. When performing PEB, after exposure, it is preferably carried out on a hot plate or in an oven at 30 to 200° C. for 10 seconds to 30 minutes, more preferably at 60 to 180° C. for 30 seconds to 20 minutes.
[0088] After exposure or PEB, development is performed using an organic solvent. The development is performed by a conventional method such as dipping, puddle, or spraying on the exposed resist film for 3 seconds to 3 minutes, preferably 5 seconds to 2 minutes, to form a target pattern. The resist composition of the present invention is a negative type, so the portion irradiated with light will not dissolve in the developer, and the portion not exposed will dissolve.
[0089] Examples of the organic solvent used as the developer include 2-octanone, 2-nonanone, 2-heptanone, 3-heptanone, 4-heptanone, 2-hexanone, 3-hexanone, diisobutyl ketone, methylcyclohexanone, acetophenone, methylacetophenone, propyl acetate, butyl acetate, isobutyl acetate, amyl acetate, butyl acetate, isoamyl acetate, propyl formate, cyclohexyl acetate, butyl formate, isobutyl formate, amyl formate, isoamyl formate, methyl valerate, methyl pentenoate, and methyl crotonate. Ester, ethyl crotonate, methyl propionate, ethyl propionate, ethyl 3-ethoxypropionate, methyl lactate, ethyl lactate, propyl lactate, butyl lactate, isobutyl lactate, amyl lactate, isoamyl lactate, methyl 2-hydroxyisobutyrate, ethyl 2-hydroxyisobutyrate, methyl benzoate, ethyl benzoate, phenyl acetate, benzyl acetate, methyl phenylacetate, ethyl phenylacetate, benzyl formate, phenylethyl formate, methyl 3-phenylpropionate, benzyl propionate, 2-phenylethyl acetate, etc. These organic solvents may be used alone or in combination of two or more.
[0090] After development, rinsing is performed as needed. As the rinsing liquid, a solvent that is miscible with the developer and does not dissolve the resist film is preferred. As such a solvent, alcohols having 3 to 10 carbon atoms, ether compounds having 8 to 12 carbon atoms, alkanes, alkenes, alkynes, and aromatic solvents having 6 to 12 carbon atoms are preferably used.
[0091] Examples of the alcohol having 3 to 10 carbon atoms include n-propanol, isopropanol, 1-butanol, 2-butanol, isobutanol, tert-butanol, 1-pentanol, 2-pentanol, 3-pentanol, tert-pentanol, neopentyl alcohol, 2-methyl-1-butanol, 3-methyl-1-butanol, 3-methyl-3-pentanol, cyclopentanol, 1-hexanol, 2-hexanol, 3-hexanol, 2,3-dimethyl-2-butanol, 3,3-dimethyl-1-butanol, 3,3-dimethyl-2-butanol, 2-ethyl-1-butanol, 2-methyl-1-pentanol, 2-methyl-2-pentanol, 2-methyl-3-pentanol, 3-methyl-1-pentanol, 3-methyl-2-pentanol, 3-methyl-3-pentanol, 4-methyl-1-pentanol, 4-methyl-2-pentanol, 4-methyl-3-pentanol, cyclohexanol, and 1-octanol.
[0092] Examples of the ester compound having 8 to 12 carbon atoms include di-n-butyl ether, diisobutyl ether, di-sec-butyl ether, di-n-pentyl ether, diisopentyl ether, di-sec-pentyl ether, di-tert-pentyl ether, and di-n-hexyl ether.
[0093] Examples of the aforementioned alkanes having 6 to 12 carbon atoms include hexane, heptane, octane, nonane, decane, undecane, dodecane, methylcyclopentane, dimethylcyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, cycloheptane, cyclooctane, and cyclononane. Examples of the aforementioned alkenes having 6 to 12 carbon atoms include hexene, heptene, octene, cyclohexene, methylcyclohexene, dimethylcyclohexene, cycloheptene, and cyclooctene. Examples of the aforementioned alkynes having 6 to 12 carbon atoms include hexyne, heptyne, and octyne.
[0094] Examples of the aromatic solvent include toluene, xylene, ethylbenzene, cumene, tert-butylbenzene, and mesitylene.
[0095] By performing rinsing, the collapse of the resist pattern and the generation of defects can be reduced. In addition, rinsing is not necessary, and the amount of solvent used can be reduced by not performing rinsing.
[0096] Example
[0097] Hereinafter, the present invention will be specifically described by showing examples and comparative examples, but the present invention is not limited to the following examples. The following apparatus was used.
[0098] IR: NICOLET 6700 manufactured by Thermo Fisher Scientific
[0099] · 1 H-NMR: ECA-500 manufactured by JEOL Ltd.
[0100] [1] Synthesis of tin compounds
[0101] [Synthesis Example 1] Synthesis of Tin Compound M-1
[0102] [Chemistry 13]
[0103]
[0104] In the formula, Bn is benzyl and Me is methyl.
[0105] A mixture of 1.6 g of dibenzyl dichloride, 1.5 g of dimethyl carbonate, 1.1 g of methanol and 60 g of toluene was stirred at 110°C for 3 hours, returned to room temperature and filtered, and the insoluble portion was removed and concentrated under reduced pressure. Toluene was added to the concentrated residue and heated to dissolve it, and then returned to room temperature and recrystallized and purified to obtain 0.9 g of the target tin compound M-1 (yield 55%).
[0106] The IR spectrum data of the tin compound M-1 are shown below. Figure 1 and 2 Display NMR spectrum ( 1 H-NMR / CDCl 3 and119 Sn-NMR / CDCl 3 ) results. And, it is observed that 1 Residual solvent (toluene) in H-NMR.
[0107] IR(D-ATR):3635,3079,3057,3023,2929,1599,1538,1492,1451,1405,1366,1210,1115,1052,1029,756,731,709,698,618,518,464,455cm -1 .
[0108] [Synthesis Example 2] Synthesis of Tin Compound M-2
[0109] [Chemistry 14]
[0110]
[0111] In the formula, nBu is n-butyl and Et is ethyl.
[0112] A mixture of 1.0 g of di-n-butyltin dichloride, 0.3 g of sodium carbonate and 100 g of a 95% by mass ethanol aqueous solution was stirred at 60°C overnight, returned to room temperature and filtered to obtain an insoluble portion. The insoluble portion was washed with a 30% by mass ethanol aqueous solution, and the washed powder was dried under reduced pressure to obtain 0.6 g (yield 67%) of the target tin compound M-2.
[0113] The IR spectrum data of the tin compound M-2 are shown below.
[0114] IR(D-ATR):2958,2925,2871,2858,1510,1464,1378,1287,1157,1079,1020,965,870,826,678,640,487cm -1 .
[0115] [Synthesis Example 3] Synthesis of Tin Compound M-3
[0116] [Chemistry 15]
[0117]
[0118] In the formula, nBu is n-butyl, and Me is methyl.
[0119] A mixture of 2.5 g of di-n-butyltin oxide, 0.9 g of dimethyl carbonate, 20 g of toluene and 0.2 g of methanol was stirred at 110°C for 1 hour. After the reaction solution returned to room temperature, it was concentrated under reduced pressure, and the concentrated residue was washed with methanol. The obtained powder was heated and dried under reduced pressure to obtain 2.2 g (yield 83%) of the target tin compound M-3.
[0120] The IR spectrum data of the tin compound M-3 are shown below.
[0121] IR(D-ATR):2956,2922,2871,2855,2801,1541,1463,1419,1376,1068,669,605,577,534cm -1 .
[0122] [2] Preparation of resist composition
[0123] [Example 1-1, Comparative Examples 1-1 to 1-2]
[0124] Resist materials were mixed and dissolved in the composition shown in Table 1 below, and the obtained solution was filtered through a 0.2 μm Teflon (registered trademark) filter membrane to prepare the resist composition R-1 of the present invention and comparative resist compositions CR-1 and CR-2.
[0125] [Table 1]
[0126]
[0127] In Table 1, the materials of the chemically amplified resist composition CR-1 as a comparative example, namely P-1 (base polymer), PAG-1 (photoacid generator), Q-1 (sensitivity adjuster) and surfactant (SF-1) are as follows.
[0128] ·P-1: p-Hydroxystyrene / 1-Methylcyclopentyl Methacrylate Copolymer
[0129] [Chemistry 16]
[0130]
[0131] ·PAG-1: 2-(adamantane-1-carbonyloxy)-1,1,3,3,3-pentafluoropropane-1-sulfonic acid triphenylsulfonium
[0132] [Chemistry 17]
[0133]
[0134] Q-1: 2-Morpholinylethyl Laurate
[0135] [Chemistry 18]
[0136]
[0137] SF-1: PF-636 (manufactured by OMNOVA)
[0138] In Table 1, the tin compound CM-1, which is a material of the non-chemically amplified resist composition CR-2 of the comparative example, was synthesized according to the non-patent document: Angewandte Chemie, International Edition (2017), 56 (34), 10140-10144. Its structure is as follows.
[0139] [Chemistry 19]
[0140]
[0141] In Table 1, PGMEA is propylene glycol monomethyl ether acetate, and DAA is diacetone alcohol.
[0142] [3]EB Lithography Evaluation
[0143] (1) Evaluation of sensitivity, LWR and limiting resolution
[0144] [Example 2-1, Comparative Examples 2-1 to 2-2]
[0145] Each resist composition (R-1, CR-1 and CR-2) was spin-coated on a Si substrate formed with an anti-reflective film DUV-42 manufactured by Nissan Chemical Co., Ltd. with a film thickness of 60 nm, and pre-baked at 100°C for 60 seconds using a hot plate to prepare a resist film with a film thickness of 40 nm. The resist film was exposed using an EB drawing device (ELS-F125, accelerating voltage 125 kV) manufactured by ELIONIX, and PEB was performed for 60 seconds on a hot plate at the temperature described in Table 2, and developed for 30 seconds using the developer described in Table 2 to form a pattern. In Example 2-1 and Comparative Example 2-2, the resist film of the exposed portion remained, showing a negative tone characteristic. In Comparative Example 2-1, the resist film of the unexposed portion remained, showing a positive tone characteristic. As a result, a negative or positive line-and-space (LS) pattern with a spacing width of 20 nm and a pitch of 40 nm was obtained. The sensitivity, LWR and limiting resolution of the obtained LS pattern were evaluated according to the following method. The results are shown in Table 2. Figure 3 : is a SEM image showing a line and space (LS) pattern with a space width of 20 nm and a pitch of 40 nm in Eop of Example 2-1.
[0146] [Sensitivity evaluation]
[0147] The above LS pattern was observed by electron microscope to obtain the optimal exposure Eop (μC / cm2) for the LS pattern with a pitch width of 20 nm and a pitch of 40 nm. 2 ) and define it as sensitivity.
[0148] [LWR evaluation]
[0149] For the LS pattern obtained by irradiation with the optimal exposure Eop, the dimensions of 10 locations along the long side direction of the pitch width were measured using CD-SEM (CG-5000) manufactured by Hitachi Advanced Technology Co., Ltd., and the value (3σ) tripled by the standard deviation (σ) was obtained from the results to be used as LWR. The smaller this value is, the smaller the roughness and the more uniform the pitch width pattern can be obtained.
[0150] [Limiting resolution evaluation]
[0151] The minimum line width (nm) of the separable LS pattern at the optimum exposure Eop is defined as the limiting resolution.
[0152] [Table 2]
[0153]
[0154] From the results shown in Table 2, it can be seen that the resist composition of the present invention is excellent in LWR and limiting resolution in negative-tone pattern formation by organic solvent development using EB.
[0155] (2) Contrast curve and PEB shrinkage evaluation
[0156] [Example 3]
[0157] The resist composition R-1 was spin-coated on a Si substrate on which an antireflection film DUV-42 manufactured by Nissan Chemical Co., Ltd. was formed with a film thickness of 60 nm, and pre-baked at 100° C. for 60 seconds using a hot plate to prepare a resist film with a film thickness of 40 nm. The resist film was subjected to an EB drawing apparatus (ELS-F125) manufactured by ELIONIX Corporation at an acceleration voltage of 50 kV and an exposure amount of 3 to 3800 μC / cm 2 The film was then exposed to light in a range of . Afterwards, PEB was performed on a hot plate at 150°C for 60 seconds, and the film thickness was measured to calculate PEB shrinkage. Furthermore, development was performed using 2-heptanone for 30 seconds, and the film thickness after development was measured. The results of plotting the relationship between film thickness and exposure amount (contrast curve and PEB shrinkage) are shown in Figure 4 .
[0158] Depend on Figure 4 From the results shown, it can be seen that the more the exposure dose increases, the more the PEB shrinks and the more insoluble the film becomes.
[0159] Furthermore, although the sensitivity of the resist composition of the present invention is relatively low in EB lithography, it is expected to have a fairly high sensitivity in EUV lithography because it contains tin atoms having high EUV light absorption energy at a high density.
Claims
1. A resist composition comprising a tin compound represented by the following formula (1) and an organic solvent, In the formula, R 1A ~R 10A and R 1B ~R 10B are each independently a hydrocarbon group having 1 to 20 carbon atoms, R 11 ~R 14 are each independently a hydrogen atom or a hydrocarbon group having 1 to 20 carbon atoms, L a1 and L a2 Each is independently a linking group.
2. The resist composition according to claim 1, wherein L a1 and L a2 Each is independently a group represented by any one of the following formulae (2a) to (2d), Wherein, the dotted line represents the atomic bond with Sn.
3. The resist composition according to claim 1, wherein R 1A ~R 10A and R 1B ~R 10B is isopropyl, n-butyl, tert-butyl or benzyl. The resist composition according to claim 1 , further comprising a surfactant.
5. A pattern forming method comprising the following steps: A resist film is formed on a substrate using the resist composition according to any one of claims 1 to 4, the resist film is exposed to high-energy rays, and the exposed resist film is developed using a developer.
6. The pattern forming method according to claim 5, wherein: The high-energy rays are electron beams or extreme ultraviolet rays.