Mixed silver particles and preparation method and application thereof

By using mixed silver particles and sulfate modifiers in the preparation of photovoltaic silver powder, the problem of high energy consumption and difficult to meet industrial needs in the prior art is solved, and the combination of efficient conductivity and printing performance is achieved. Preparation of conductive layer in photovoltaic cell.

CN118942762APending Publication Date: 2024-11-12SHENZHEN HASHEN TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411101465.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the existing preparation methods of photovoltaic silver powder, the physical method has high energy consumption and high cost, while the silver powder prepared by chemical method is difficult to meet industrial needs in large-scale production, and the particle size, shape and surface morphology of the silver powder are responsible for conductivity and printing. The performance has a great impact and it is difficult to meet the requirements of conductivity and printing performance at the same time.

Method used

A mixed silver granules are used, composed of sheet-like silver granules and spherical silver granules. By adding sulfate as a modifier to the oxide liquid and reducing liquid, the shape and size of the silver granules are controlled, and the dependence of later airflow grinding is reduced, and the dependence of later airflow grinding is improved. Conductive and printing properties.

Benefits of technology

The uniform distribution and dense layer formation of conductive silver paste are achieved, which improves the conductivity and fluidity, reduces resistance, enhances the physical and mechanical properties of the sintered film, adapts to changes in substrate shape, reduces cracking and fracture, and increases low temperature Conductive properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942762A_ABST
    Figure CN118942762A_ABST
Patent Text Reader

Abstract

The invention discloses mixed silver particles and a preparation method and application thereof. The mixed silver particles comprise flaky silver particles and spherical-like silver particles, the flaky silver particles comprise polygonal or elliptical flaky silver particles, the particle size of the flaky silver particles is 0.5-8 [mu] m, the particle size of the spherical-like silver particles is 0.2-5 [mu] m, and the average particle size of the flaky silver particles is larger than that of the spherical-like silver particles. The silver particles comprise flaky silver particles and spherical-like silver particles with proper particle sizes; the spherical-like silver particles are favorable for reducing contact resistance among the particles and improving conductivity and reliability, and meanwhile, the flowability and coating property of the conductive silver paste can be improved, so that the silver paste can be more uniformly distributed on the substrate in the printing process to form a uniform and compact conductive layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field related to metal powder and conductive paste, and in particular to mixed silver particles and a preparation method and application thereof. Background Art

[0002] In the photovoltaic field, photovoltaic silver powder is an indispensable industrial material, and its performance has a decisive influence on the energy conversion efficiency and stability of photovoltaic cells and photovoltaic devices. Silver powder, with its excellent conductivity and chemical stability, has become a key factor in maintaining the stable performance of photovoltaic devices. The preparation methods of photovoltaic silver powder mainly involve two categories: physical method and chemical method. Among them, the physical method vaporizes the silver element and condenses it into particles by heating and evaporating. Although the silver powder prepared by it has high purity, it has high energy consumption and high cost, so it is limited in large-scale production. In contrast, the room temperature and atmospheric pressure liquid phase reduction method in the chemical method has been widely used in the photovoltaic industry because of its simple operation, low cost and good sintering performance of the silver powder produced.

[0003] The particle size, shape and surface morphology of silver powder will significantly affect its performance. Smaller particle size and larger specific surface area can enhance the sintering activity of the powder, reduce the sintering temperature, and thus improve the conductivity. In terms of shape, silver powder can be roughly divided into spherical, flaky and dendritic. Among them, spherical silver powder occupies a dominant position in photovoltaic conductive paste due to its high solid content and superior conductivity. However, the surface morphology of silver powder not only affects its specific surface area and surface activity, but is also closely related to the compatibility of the paste, which in turn affects the printing performance of the paste.

[0004] Specifically, in the slurry preparation process, its printing performance and conductive performance need to be considered at the same time. The conductive performance of the slurry is closely related to the solid content and sintering performance of the conductive powder, while the printing performance is affected by factors such as slurry viscosity and particle uniformity. In order to obtain good conductive and printing performance, the conductive powder in the slurry must have a suitable particle size and slurry fineness, while avoiding agglomeration. This requires the silver powder to have a specific surface morphology to achieve effective control of viscosity.

[0005] Therefore, preparing silver particles with suitable particle size and morphology is of great significance for preparing photovoltaic conductive silver paste with excellent performance. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a mixed silver particle, the mixed silver particle has a suitable particle size and morphology, and the conductive silver paste prepared using the silver particle has good printing performance.

[0007] According to one aspect of the present invention, a mixed silver particle is proposed, comprising flaky silver particles and quasi-spherical silver particles, wherein the flaky silver particles comprise polygonal or elliptical flaky silver particles, the particle size of the flaky silver particles is 0.5-8 μm, the particle size of the quasi-spherical silver particles is 0.2-5 μm, and the average particle size of the flaky silver particles is greater than the average particle size of the quasi-spherical silver particles.

[0008] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the silver particles of the present invention include flaky silver particles and spherical silver particles of suitable particle size; the spherical silver particles are conducive to reducing the contact resistance between particles, improving the conductivity and reliability, and at the same time, they can improve the fluidity and coating of the conductive silver paste, so that during the printing process, the silver paste can be more evenly distributed on the substrate to form a uniform and dense conductive layer; the flaky silver particles have a large specific surface area, can provide a larger contact area, and lower resistance, and the presence of the flaky silver particles enhances the conductivity and activity, and at the same time, a dense sintered film can be formed during the sintering process, which helps to improve the physical and mechanical properties of the conductive silver paste. In addition, during the printing process, the flaky silver powder can better adapt to the shape and size changes of the substrate, and reduce the cracking and fracture caused by stress concentration. If the flaky silver particles reach a more appropriate ratio, it is possible to improve the adaptability of the powder and paste to the low-temperature conductive paste.

[0009] In some embodiments of the present invention, the particle size of the flaky silver particles is 1-5 μm.

[0010] In some embodiments of the present invention, the particle size of the mixed silver particles is 0.7-3 μm.

[0011] In some embodiments of the present invention, the particle size of the mixed silver particles is 1 to 2 μm.

[0012] In some embodiments of the present invention, the particle size of the flaky silver particles is not less than the particle size of the quasi-spherical silver particles.

[0013] In some embodiments of the present invention, the surface of the mixed silver particles has no obvious crystal face structure and crystal edge. The crystal face structure and crystal edge are basically gone, and the existing ratio is less than 1%.

[0014] In some embodiments of the present invention, the mixed silver particles are composed of flaky silver particles and spherical silver particles; preferably, the number of flaky silver particles accounts for 5%-10%.

[0015] In some embodiments of the present invention, the polygon is a convex polygon that conforms to crystal symmetry and exposes certain flat crystal faces.

[0016] According to another aspect of the present invention, a method for preparing the above-mentioned mixed silver particles is provided, comprising the following steps:

[0017] At the same time, an oxidizing solution containing silver salt and a reducing solution containing a reducing agent are added to a reaction base solution containing a dispersant and a modifier, and the mixed silver particles are obtained after the reaction, wherein the modifier is sulfate, and the mass of the sulfate is 0.5% to 5% of the mass of the silver salt.

[0018] According to a preferred embodiment of the present invention, the preparation method has at least the following beneficial effects: the present invention adds sulfate in the process of preparing silver particles, and the sulfate can affect the crystal growth direction and speed during the growth of silver particles, thereby controlling the shape and size of the silver particles, and then obtaining silver particles with specific morphology and performance; at the same time, the addition of sulfate can also reduce its dependence on the later airflow milling. In the traditional silver particle preparation process, it is usually necessary to control the morphology and distribution of the particles by physical means such as airflow milling. However, this method is not only complicated to operate, but also costly. The present invention achieves chemical shaping by adding sulfate, and the original powder crystal face structure and crystal edges of the obtained silver particles basically disappear, and the dependence on the later airflow milling is reduced, and the generation and aggregation of silver particles can be directly controlled during the reaction, thereby reducing the need for later physical treatment. In addition, sulfate also has good solubility and stability, which can ensure that a continuous and stable chemical environment is provided during the reaction, which is crucial to maintaining the uniformity and consistency of the reaction and helps to prepare high-quality silver particles.

[0019] In some embodiments of the present invention, the concentration of silver ions in the oxidizing solution is 0.3-3 mol / L.

[0020] In some embodiments of the present invention, the silver salt is silver nitrate, silver oxalate or silver sulfate.

[0021] In some embodiments of the present invention, the reducing agent is at least one of formalin, hydrazine hydrate or vitamin C.

[0022] In some embodiments of the present invention, the molar amount of the reducing agent in the reducing solution is 0.5-1 times the molar amount of silver ions.

[0023] In some embodiments of the present invention, the reducing liquid and the oxidizing liquid have the same volume, which is convenient for operation.

[0024] In some embodiments of the present invention, the concentration of the reducing agent in the reducing solution is 0.15-3 mol / L.

[0025] In some embodiments of the present invention, the dispersant is a water-soluble polymer.

[0026] In some embodiments of the present invention, the dispersant is at least one of polyvinyl pyrrolidone, gelatin, and gum arabic.

[0027] In some embodiments of the present invention, the added amount of the dispersant is 10-30% of the mass of the silver salt.

[0028] In some embodiments of the present invention, the mass fraction of the dispersant in the reaction base liquid is 2%-10%.

[0029] In some embodiments of the present invention, the molar amount of sulfate in the reaction base solution is 0.2-5% of the molar amount of silver in the oxidation solution.

[0030] In some embodiments of the present invention, the sulfate is at least one of potassium sulfate, sodium sulfate or zinc sulfate.

[0031] In some embodiments of the present invention, the mass of the sulfate is 0.5% to 5% of the mass of the silver salt.

[0032] By controlling the type and concentration of sulfate, the morphology and size of silver particles can be precisely controlled, thereby better controlling the properties of the conductive silver paste.

[0033] In some embodiments of the present invention, the oxidizing solution and the reducing solution are added for less than 30 minutes.

[0034] In some embodiments of the present invention, the oxidizing solution and the reducing solution are added for 5-20 minutes.

[0035] In some embodiments of the present invention, the oxidizing solution and the reducing solution are added for 10-15 minutes.

[0036] In some embodiments of the present invention, the reaction is carried out under stirring at a stirring speed of 100-500 rpm.

[0037] In some embodiments of the present invention, the stirring is performed by mechanical blade stirring, and the blade is made of polytetrafluoroethylene or stainless steel. The use of a corrosion-resistant blade stirring makes the reaction more uniform.

[0038] In some embodiments of the present invention, the reaction stirring time is 5-30 min.

[0039] In some embodiments of the present invention, the reaction temperature is 20-30°C.

[0040] In some embodiments of the present invention, the preparation method further comprises a post-processing step, specifically comprising collecting the solid phase part in the system after the reaction, washing and drying.

[0041] In some embodiments of the present invention, the washing refers to washing until the conductivity of the cleaning solution is less than 50 μS / cm.

[0042] In some embodiments of the present invention, the drying temperature is 35-80°C.

[0043] According to another aspect of the present invention, a conductive silver paste is provided, comprising a conductive phase, a binder phase and a solvent, wherein the conductive phase is the above-mentioned mixed silver particles.

[0044] According to a preferred embodiment of the present invention, at least the following beneficial effects are achieved: the viscosity of the conductive silver paste of the present invention at 1.0rpm (2.0min) is between 150,000 and 270,000 mPa·s. If the viscosity is too high, the paste will be too thick. If the viscosity is too low, it will be difficult to form a stable printed film, affecting the printing quality. At the same time, if the viscosity is too low, the film-forming property may be poor, and it will be difficult to form a continuous and uniform conductive layer, resulting in unstable or decreased conductive performance. The conductive silver paste exhibits good printing performance due to its unique viscosity characteristics, and can ensure the formation of a uniform and fine conductive layer on the conductive circuit of the solar photovoltaic cell, thereby effectively improving its performance and extending its service life.

[0045] In some embodiments of the present invention, when the conductive silver paste is tested by the rotational viscosity test method in GB / T 17473.5-2008 "Testing methods for precious metal pastes for microelectronics", the viscosity is 150,000 to 250,000 mPa·s when tested at 1 rpm for 2 minutes.

[0046] When the conductive silver paste viscosity is within this range and the average particle size is 1 to 2 μm, it has better printing performance.

[0047] In some embodiments of the present invention, the adhesive phase is at least one of tributyl citrate and diethylene glycol butyl ether acetate. Any adhesive phase commonly used in the art can be selected.

[0048] In some embodiments of the present invention, the solvent is selected from at least one of DBE and dimethyl silicone oil, and any solvent commonly used in the art can be selected.

[0049] According to another aspect of the present invention, the use of the above-mentioned silver particles or conductive silver paste in the preparation of solar cells or electronic components is proposed.

[0050] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be apparent from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0051] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0052] Figure 1 3 is a SEM image of the mixed silver particles prepared in Example 1 of the present invention.

[0053] Figure 2 3 is a SEM image of the mixed silver particles prepared in Example 2 of the present invention.

[0054] Figure 3 3 is a SEM image of the mixed silver particles prepared in Example 3 of the present invention.

[0055] Figure 4 3 is a SEM image of the mixed silver particles prepared in Comparative Example 1 of the present invention.

[0056] Figure 5 3 is a SEM image of the mixed silver particles prepared in Comparative Example 2 of the present invention.

[0057] Figure 6 3 is a SEM image of the mixed silver particles prepared in Comparative Example 3 of the present invention.

[0058] Figure 7 3 is a SEM image of the mixed silver particles prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0059] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of them. Based on the embodiments of the present invention, other embodiments obtained by technicians in this field without creative work are all within the scope of protection of the present invention. The test methods used in the embodiments are conventional methods unless otherwise specified; the materials, reagents, etc. used, unless otherwise specified, can be reagents and materials obtained from commercial channels. Unless otherwise specified, the same parameter in each embodiment has the same value. The embodiments described below are exemplary and are only used to explain the present invention, and cannot be understood as limitations on the present invention.

[0060] Example 1

[0061] In this example, a mixed silver particle is prepared, which is composed of flaky silver particles and spherical silver particles. The specific process is as follows:

[0062] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0063] (2) Weigh 0.75 g of potassium sulfate solid and 5 g of polyvinyl pyrrolidone and dissolve them in 500 g of water for later use as the reaction base liquid, which is system B;

[0064] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0065] (4) System A and System C were slowly injected into System B via a peristaltic pump for 10 min. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0066] (5) After the reaction is completed, stirring is maintained for 5 minutes, and then the powder is washed with deionized water by suction filtration. The powder is stopped after the conductivity of the washing liquid is reduced to 50 μS / cm. The powder is dried in an oven at 70°C for 4 hours, and the sample is taken out for testing.

[0067] Example 2

[0068] In this example, a mixed silver particle is prepared, which is composed of flaky silver particles and spherical silver particles. The specific process is as follows:

[0069] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0070] (2) Weigh 2.5 g of potassium sulfate solid and 5 g of polyvinyl pyrrolidone and dissolve them in 500 g of water for later use as the reaction base liquid, which is system B;

[0071] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0072] (4) System A and System C were slowly injected into System B via a peristaltic pump for 10 min. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0073] (5) After the reaction is completed, stirring is maintained for 5 minutes, and then the powder is washed with deionized water by suction filtration. The powder is stopped after the conductivity of the washing liquid is reduced to 50 μS / cm. The powder is dried in an oven at 70°C for 4 hours, and the sample is taken out for testing.

[0074] Example 3

[0075] In this example, a mixed silver particle is prepared, which is composed of flaky silver particles and spherical silver particles. The specific process is as follows:

[0076] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0077] (2) Weigh 0.75 g of potassium sulfate solid and 5 g of polyvinyl pyrrolidone and dissolve them in 500 g of water for later use as the reaction base liquid, which is system B;

[0078] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0079] (4) System A and System C were rapidly injected into System B for 5 seconds. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0080] (5) After the reaction, the powder was stirred for 5 min, and then the powder was washed with deionized water by filtration until the conductivity of the washing solution dropped to 50 μS / cm. The powder was dried in an oven at 70°C for 4 hours, and the sample was taken out for testing. The SEM test results are shown in the following table. Figure 3 shown.

[0081] Comparative Example 1

[0082] In this example, a mixed silver particle is prepared, which is composed of flaky silver particles and spherical silver particles. The specific process is as follows:

[0083] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0084] (2) Weigh 0.1 g of potassium sulfate solid and 5 g of polyvinyl pyrrolidone and dissolve them in 500 g of water for later use as the reaction base liquid, which is system B;

[0085] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0086] (4) System A and System C were slowly injected into System B via a peristaltic pump for 10 min. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0087] (5) After the reaction is completed, stirring is maintained for 5 minutes, and then the powder is washed with deionized water by suction filtration. The powder is stopped after the conductivity of the washing liquid is reduced to 50 μS / cm. The powder is dried in an oven at 70°C for 4 hours, and the sample is taken out for testing.

[0088] Comparative Example 2

[0089] In this example, a type of silver particle is prepared, which is composed of bulk silver particles. The specific process is as follows:

[0090] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0091] (2) Weigh 3 g of potassium sulfate solid and 5 g of polyvinyl pyrrolidone and dissolve them in 500 g of water for later use as the reaction base liquid, which is system B;

[0092] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0093] (4) System A and System C were slowly injected into System B via a peristaltic pump for 10 min. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0094] (5) After the reaction is completed, stirring is maintained for 5 minutes, and then the powder is washed with deionized water by suction filtration. The powder is stopped after the conductivity of the washing liquid is reduced to 50 μS / cm. The powder is dried in an oven at 70°C for 4 hours, and the sample is taken out for testing.

[0095] Comparative Example 3

[0096] In this example, a type of silver particle is prepared, and the silver particle is composed of spherical silver particles. The specific process is as follows:

[0097] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0098] (2) 5 g of polyvinyl pyrrolidone was dissolved in 500 g of water and used as the reaction base liquid, which is system B;

[0099] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0100] (4) System A and System C were slowly injected into System B via a peristaltic pump for 10 min. During the process, the system was kept in a water bath at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle.

[0101] (5) After the reaction is completed, keep stirring for 5 minutes, then wash the powder with deionized water by suction filtration, and stop washing after the conductivity of the washing liquid is reduced to 50μS / cm. Dry in an oven at 70°C for 4 hours, and take out the sample for testing.

[0102] Comparative Example 4

[0103] In this example, a type of silver particles is prepared, and the silver particles are composed of block-shaped and spherical silver particles. The specific process is as follows:

[0104] (1) Weigh 50 g of solid silver nitrate and dissolve it in 500 g of water for later use as a silver source and oxidant, which is system A;

[0105] (2) Weigh 5 g of polyvinyl pyrrolidone and dissolve it in 500 g of water and inject 2 ml of sulfuric acid (mass fraction 19.6%) as the reaction base liquid, which is system B;

[0106] (3) Weigh 32.5 g of vitamin C and dissolve it in 500 g of water for later use as a reducing agent, which is system C;

[0107] (4) System A and System C were slowly injected into System B through a peristaltic pump for 10 min. During the process, the water bath was kept at room temperature of 25°C and stirred at 300 rpm using a mechanical stirring paddle. After the reaction was completed, stirring was maintained for 5 min. The powder was then washed with deionized water by filtration until the conductivity of the washing solution was reduced to 50 μS / cm. The powder was then dried in an oven at 70°C for 4 hours and the sample was taken out for testing.

[0108] Comparative Example 5

[0109] This example prepares a silver particle, which is different from Example 1 in that sodium chloride is used instead of potassium sulfate.

[0110] Comparative Example 6

[0111] This example prepares a silver particle, which is different from Example 1 in that potassium nitrate is used instead of potassium sulfate.

[0112] Test example

[0113] This test example tests the morphology of the silver particles prepared in the examples and comparative examples and the performance of the silver particles after being prepared into conductive silver paste.

[0114] 1) Morphological characterization

[0115] The morphology of the mixed silver particles obtained in Examples 1 to 3 and Comparative Examples 1 to 6 was characterized by scanning electron microscopy. Some of the results are as follows: Figures 1 to 7 At the same time, the particle size distribution is tested by a laser particle size analyzer.

[0116] from Figure 1 It can be seen that most of the mixed silver particles prepared in Example 1 are irregularly spherical, and some are polygonal lamellar. There is no obvious crystal face structure and crystal edge. The overall particle size distribution is about 0.7-5μm, among which the particle size of the flaky silver particles is 1-5μm, and the particle size of the spherical silver particles is 0.7-2.5μm, and the average particle size of the flaky silver particles is larger than the average particle size of the spherical silver particles.

[0117] from Figure 2It can be seen that most of the mixed silver particles prepared in Example 2 are irregularly spherical, and the rest are polygonal or elliptical lamellar. The particle size of the spherical silver particles is about 1-2.5 μm, while the lamellar silver particles are larger in area, with a diameter of about 3-5 μm. The sample particles have obvious surface shaping effect, the original crystal face structure and crystal edges of the powder grains basically disappear, and part of the powder eventually grows into larger lamellar powder due to agglomeration and deformation.

[0118] from Figure 3 It can be seen that when the injection speed of the raw material liquid is increased, most of the mixed silver particles obtained are irregular spherical, and the rest are polygonal lamellar. The particles are smaller than those of the double-flow method. The particle size of the spherical silver particles is about 0.5-1μm, and the particle size of the flaky silver particles is 0.5-2μm.

[0119] from Figure 4 It can be seen that when the amount of modifier added is too low, the silver particles mainly present irregular spherical shapes, some of which have a slight lamellar tendency, and the proportion of flaky silver particles is less than 2%. The surface of the powder partially retains the crystal structure and the corresponding crystal edges. The overall particle size distribution of the powder is about 0.5-2.5μm.

[0120] from Figure 5 It can be seen that when the amount of modifier added is too much, the particle size in the field of view is uneven, and generally appears to be a state of large particles covered with a layered shell. The particles are severely agglomerated and no longer form an obvious spherical state. In addition, the powder appears to be compacted macroscopically and cannot be used for slurry preparation.

[0121] from Figure 6 It can be seen that when no modifier is added and other operations are the same, no lamellar silver particles are produced in the prepared silver particles, and only spherical powders with obvious crystal face structure and crystal edges exist.

[0122] from Figure 7 It can be seen that when sulfuric acid, which also contains sulfate ions, is used as a modifier, the silver particles obtained are a mixture of large blocks and irregular spherical particles, among which large blocks of silver particles account for more than 20%.

[0123] Since a large amount of white silver chloride precipitate impurities were generated during the reaction in Comparative Example 5, it could not be used for silver paste preparation and no further analysis was performed.

[0124] The effect of Comparative Example 6 is similar to that of Comparative Example 3, and is not shown one by one to avoid redundancy. When nitrate is added, the effect is equivalent to that when no shaping agent is added. Since the original silver nitrate also contains nitrate ions, the addition of nitrate does not affect the formation process of silver particles.

[0125] From the above results, it can be seen that the addition and dosage of the shaping agent have a significant effect on the morphology of silver particles. However, when potassium sulfate is added in large quantities or sulfuric acid is used instead, it may cause the silver particles to aggregate at the microscopic level, generating irregular large-particle powders that are blocky.

[0126] 2) Performance testing

[0127] The silver particles prepared in the above examples and comparative examples were used as conductive phases for the preparation of conductive silver paste. The amount of silver particles was 4.45 g, 0.15 g of tributyl citrate and 0.175 g of diethylene glycol butyl ether acetate were used as the binding phase, 0.15 g of DBE solvent and 0.075 g of dimethyl silicone oil were mixed and stirred evenly, and ground 4 times (3 to 5 times) using a three-roll grinder to obtain a conductive silver paste.

[0128] The viscosity of the conductive silver paste was tested by the rotational viscosity test method in the national standard GB / T 17473.5-2008. The viscosity of the conductive silver paste was measured and the results are shown in Table 1 below.

[0129] Table 1

[0130] 0.5RPM(2min) 1.0RPM(2min) 5.0RPM(2min) Measurement average value (mPa﹒s) Measurement average value (mPa﹒s) Measurement average value (mPa﹒s) Example 1 200027.52 151608.16 92076.16 Example 2 337978.88 246703.36 141449.40 Example 3 369909.4 261615.04 132564.8 Comparative Example 1 425317.76 331791.68 149703.13 Comparative Example 2 Powder compaction makes it impossible to prepare samples none none Comparative Example 3 431805.44 302422.56 130652.89 Comparative Example 4 598495.04 444505.6 157852 Comparative Example 5 Too many impurities, no slurry preparation none none Comparative Example 6 Powder compaction makes it impossible to prepare samples none none

[0131] It can be seen from the above test results that the use of sulfate-containing substances in the system of preparing silver powder by wet reduction can play a role in changing the surface morphology and particle size of silver powder. Under the condition of relatively suitable sulfate dosage, the surface of the powder is shaped to a certain extent, and the crystal planes and edges on its surface disappear, forming relatively rounded spherical powder particles. At the same time, the viscosity of the slurry prepared by this type of powder is low, and the printing fluidity is improved. By compounding spherical and flaky silver particles of specific sizes, the viscosity of the slurry can be adjusted to a larger extent to meet the requirements of printing performance. However, when too much sulfate substance is added or sulfuric acid is directly used to provide sulfate, the morphological change of the powder will be more obvious, and large-diameter block silver powder will appear. The uniformity of the particle size distribution of the powder will be greatly affected, and it will also have a negative effect on the application of the slurry. Therefore, this scheme prefers sulfate, and the concentration of sulfates must be within a specific range to obtain silver particles with better performance.

[0132] At present, the liquid phase reduction method is more commonly used in the preparation of silver powder. Low concentrations of oxidants and reductants are used to react in a liquid environment, and with the help of seed crystals that have been formed in the liquid or added exogenously, the seeds are nucleated and eventually grow into silver powder particles of the desired particle size. The silver powder prepared by this method usually has a more complex morphology structure on the surface, including the adhesion of small particles, the edges and corners of the crystals, etc. Subsequently, physical methods are more commonly used for surface modification and shaping of the powder, that is, using ball mills, crushing and shaping machines, air flow mills and other equipment to treat the powder surface, and during the physical treatment process, the powder surface can also be modified by adding a variety of surface coating agents of different properties. At present, most of the preparation methods of silver powder describe the preparation of spherical silver powder, but rarely involve the subsequent treatment of the powder and related effects. There is no relevant preparation method reported yet, which can obtain relatively controllable surface morphology and spherical silver powder with controllable roughness in a liquid phase system. The present invention adopts a liquid phase reduction system, adds sulfate and dispersant as a base liquid system, reacts with a silver source solution as an oxidant, and directly obtains a spherical silver powder with a surface shaping effect through a redox reaction. In traditional literature and patents, the application of sulfate is mostly concentrated on stabilizers to obtain spherical silver powder with a narrow particle size distribution. A small number of literature uses it as a morphology control agent to obtain products that are all flaky silver powder. The quasi-spherical silver powder obtained in this scheme is surface shaped and modified by a sulfate solution, and silver particles with different morphological characteristics and different degrees of roughness can be obtained. Therefore, this method can prepare a variety of powders with different viscosity characteristics and corresponding slurries, which are suitable for different printing scenarios. These silver powders that have been surface modified and treated can eliminate or reduce the surface shaping process involved in the later treatment of the powder, which saves energy, reduces costs and adapts to more application scenarios compared to traditional powder preparation methods, and has great advantages.

[0133] The embodiments of the present invention are described in detail above, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge scope of ordinary technicians in the relevant technical field without departing from the purpose of the present invention.

Claims

1. A mixed silver particle, characterized in that: It includes flaky silver particles and spherical silver particles, the flaky silver particles include polygonal or elliptical flaky silver particles, the particle size of the flaky silver particles is 0.5-8μm, the particle size of the spherical silver particles is 0.2-5μm, and the average particle size of the flaky silver particles is greater than the average particle size of the spherical silver particles.

2. The mixed silver particles according to claim 1, characterized in that: The particle size of the flaky silver particles is 1-5 μm; and / or, the particle size of the mixed silver particles is 0.7-3 μm; and / or, the particle size of the flaky silver particles is not less than the particle size of the quasi-spherical silver particles; and / or, the mixed silver particles are composed of flaky silver particles and quasi-spherical silver particles, and the number of flaky silver particles accounts for less than 10%; preferably, the particle size of the mixed silver particles is 1-2 μm; preferably, the number of flaky silver particles accounts for more than 2%.

3. A method for preparing mixed silver particles, characterized in that: The steps include: At the same time, an oxidizing solution containing silver salt and a reducing solution containing a reducing agent are added to a reaction base solution containing a dispersant and a modifier, and the mixed silver particles are obtained after the reaction, wherein the modifier is sulfate, and the mass of the sulfate is 0.5% to 5% of the mass of the silver salt.

4. The method for preparing mixed silver particles according to claim 3, characterized in that: The concentration of silver ions in the oxidizing solution is 0.3-3 mol / L; and / or, the silver salt is silver nitrate, silver oxalate or silver sulfate; and / or, the reducing agent is at least one of formalin, hydrazine hydrate or vitamin C; and / or, the molar amount of the reducing agent in the reducing solution is 0.5-1 times the molar amount of silver ions; and / or, the concentration of the reducing agent in the reducing solution is 0.15-3 mol / L.

5. The method for preparing mixed silver particles according to claim 3, characterized in that: The dispersant is a water-soluble polymer; and / or, the dispersant is at least one of polyvinyl pyrrolidone, gelatin, and gum arabic; and / or, the amount of the dispersant added is 10-30% of the mass of the silver salt; and / or, the mass fraction of the dispersant in the reaction base liquid is 2%-10%; and / or, the molar amount of sulfate in the reaction base liquid is 0.2-5% of the molar amount of silver in the oxidizing solution; and / or, the sulfate is at least one of potassium sulfate, sodium sulfate or zinc sulfate; and / or, the mass of the sulfate is 0.5% to 5% of the mass of the silver salt.

6. The method for preparing mixed silver particles according to claim 3, characterized in that: The addition time of the oxidizing liquid and the reducing liquid is less than 30 minutes; preferably, the addition time of the oxidizing liquid and the reducing liquid is 5-20 minutes; preferably, the addition time of the oxidizing liquid and the reducing liquid is 10-15 minutes.

7. The method for preparing mixed silver particles according to claim 3, characterized in that: The reaction is carried out under stirring at a stirring speed of 100-500 rpm; and / or, the reaction stirring time is 5-30 min; and / or, the reaction temperature is 20-30°C.

8. A conductive silver paste, characterized in that: The invention comprises a conductive phase, a bonding phase and a solvent, wherein the conductive phase is the mixed silver particles as claimed in claim 1 or 2 or the mixed silver particles prepared by the preparation method as claimed in any one of claims 3 to 7.

9. The conductive silver paste according to claim 8, characterized in that: When the conductive silver paste is tested by the rotational viscosity test method in GB / T 17473.5-2008 GB / T 17473.5-2008 "Testing methods for precious metal pastes for microelectronics", the viscosity is 150000-250000 mPa·s when tested at 1 rpm for 2 minutes.

10. Use of the mixed silver particles according to claim 1 or 2, the mixed silver particles prepared by the preparation method according to any one of claims 3 to 7, or the conductive silver paste according to claim 8 or 9 in the preparation of solar cells or electronic components.