80-year-life K3 type power cable and manufacturing method thereof

By using a combination of multi-core insulated cable core and low-smoke, halogen-free flame retardant materials in cables for nuclear power plants, the problems of radiation resistance and long life of cables for nuclear power plants are solved, and the service life and high resistance of cables of more than 80 years have been achieved. Fueling performance simplifies cable structure and reduces costs.

CN118942788APending Publication Date: 2024-11-12CHINA NUCLEAR POWER ENGINEERING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411273734.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

It is difficult to design K3 low-voltage power cables for nuclear power plants that meet their 80-year lifespan, especially in terms of radiation resistance, service life and flame retardant properties.

Method used

Using multi-core insulated cable core structure, including non-hygroscopic lithomb material filler rope and low-smoke halogen-free flame retardant material, combined with crosslinked polyethylene and crosslinked polyolefin insulation, plus flame retardant winding cladding and outer sheath , verify the long-life performance of the cable by accelerating thermal aging and radiation tests.

Benefits of technology

It achieves more than 80 years of service life of the cable, improves flame retardant performance and radiation uniformity, simplifies the cable structure, reduces cost and volume, and ensures the safety and reliability of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942788A_ABST
    Figure CN118942788A_ABST
Patent Text Reader

Abstract

The invention discloses a K3 type power cable with the service life of 80 years and a manufacturing method thereof, the power cable is formed by sequentially wrapping a flame-retardant wrapping layer and an outer sheath on the outer side of a cable core, the cable core is a single-core type insulating cable core, the single-core type insulating cable core is formed by wrapping a first flame-retardant belt on the outer side of an insulating wire core, or the cable core is a multi-core type insulating cable core, and the outer side of the multi-core type insulating cable core is wrapped by a second flame-retardant belt. The multi-core insulated cable core is formed by twisting more than two insulated wire cores and a plurality of filling ropes, the filling ropes comprise non-hygroscopic rock wool materials, and the plurality of filling ropes are located between the adjacent insulated wire cores; each insulating wire core is formed by wrapping an insulating layer on the outer side of a conductor, and the insulating layer comprises an inner insulating layer and an outer insulating layer; and the flame-retardant wrapping layer is formed by wrapping more than two layers of second flame-retardant tapes. The K3 type low-voltage power cable has the advantages that the service life is 80 years at the cable core temperature of 90 DEG C, nuclear radiation is resisted, the flame retardant property is good, and the electrical property is good.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of cable technology, and in particular to a K3 type power cable with a service life of 80 years and a manufacturing method thereof. Background Art

[0002] At present, the design life of the third-generation nuclear power plant is 60 years. Many countries are carrying out the life extension of nuclear power plants. Subsequent domestic nuclear power technology is planned to adopt an 80-year life span, which is higher than the life span of ordinary residential buildings. In order to meet the life extension needs of nuclear power plants, it is necessary to design a K3 low-voltage power cable with an 80-year life span.

[0003] The nuclear safety level 1E environment of nuclear power plants requires cables to meet the requirements of operating under nuclear radiation conditions. Their radiation resistance, service life, flame retardancy and other properties are higher than those of ordinary cables. Compared with cables with a service life of 60 years, the performance requirements for an 80-year service life increase by 25%. This first directly poses a challenge to the service life of the insulation and sheath materials themselves. Then, it is required that the overall service life of the cable, after being combined with the main copper material for power transmission, the filling material for cable roundness, and the tightening material, must still meet 80 years, which is a test of the cable manufacturing process.

[0004] While increasing the service life, raw materials will sacrifice certain electrical properties, processing properties and other properties. Therefore, we have developed a new extrusion process based on previous experience in the production of insulation layers and sheaths. For cables with unequal cores in power cables, a special filling process is implemented to make the cable cores stable and round. For the irradiation of the outer sheath of power cables, a special irradiation process is implemented to improve the irradiation uniformity of cables with large cross-sections. In order to ensure that the overall flame retardant performance of the cable is not affected, improvements have been made in the filling structure and sheath extrusion method.

[0005] Prior art CN205810460U discloses a low-voltage power cable for nuclear power plants with a lifespan of 60 years and simple process, and its structure is as follows: a sheath and a sheath are arranged in sequence from the inside to the outside of the cable core; the cable core is composed of a filling rope and at least two wire cores twisted together, and the pitch-diameter ratio of the twisted wire is not greater than 40; the wire core is composed of a single conductor with an insulating layer; each conductor is composed of tinned copper monofilaments twisted together.

[0006] Prior art CN212434311U discloses a low-voltage power cable for nuclear power plants that has passed severe fire resistance test conditions, and its structure is as follows: a cable core is wrapped with a sheath and a sheath in sequence from the inside to the outside; the cable core is composed of a ceramic fire-proof and fire-resistant filling rope and at least two cores twisted together; each core is twisted around the same axis l; adjacent cores are separated by a bundle of ceramic fire-proof and fire-resistant filling ropes; the ceramic fire-proof and fire-resistant filling ropes and the cores are twisted in the same direction; the core is composed of a single conductor wrapped with a fire-resistant layer and an insulating layer in sequence.

[0007] The above-mentioned low-voltage power cables are difficult to achieve the requirement of a service life of more than 80 years in nuclear power plants in terms of material selection, structural design and production and manufacturing processes.

[0008] In view of the above technical problems, the present invention is specially introduced. Summary of the invention

[0009] The main purpose of the present invention is to provide a K3 type low-voltage power cable with an 80-year service life for a nuclear power plant and a manufacturing method thereof.

[0010] In order to achieve the above-mentioned purpose, according to one aspect of the present invention, a K3 type power cable with a service life of 80 years is proposed, comprising a cable core, wherein the power cable is composed of a flame retardant sheath and an outer sheath wrapped in sequence on the outer side of the cable core, the cable core is a single-core insulated cable core, the single-core insulated cable core is composed of a first flame retardant tape wrapped around the outer side of an insulating core, or the cable core is a multi-core insulated cable core, the multi-core insulated cable core is composed of more than two insulating cores twisted with a plurality of filling ropes, the filling ropes include non-hygroscopic rock wool material, and the plurality of filling ropes are located between adjacent insulating cores; the insulating core is composed of an insulating layer wrapped around the outer side of the conductor, the insulating layer includes an inner insulating layer and an outer insulating layer, the inner insulating layer is composed of a cross-linked polyethylene insulating material, and the outer insulating layer is composed of a cross-linked polyolefin insulating material; the flame retardant sheath is formed by wrapping more than two layers of the second flame retardant tape, and the outer sheath is composed of a polyolefin material.

[0011] Furthermore, the power cable adopts the accelerated thermal aging test method based on the Arrhenius model to verify that the thermal life of the power cable is not less than 80 years at an insulation core temperature of 90°C.

[0012] Furthermore, the multi-core insulated cable core includes 3 to 5 insulating cores, the insulating cores include a first core and a second core, the cross-sectional area of ​​the first core is larger than that of the second core, or; the multi-core insulated cable core includes 2 to 5 insulating cores with equal cross-sectional areas.

[0013] Further, the multi-core insulated cable core includes 2 first cores and 1 second core, or includes 3 first cores and 1 second core, or includes 3 first cores and 2 second cores, or includes 4 first cores and 1 second core.

[0014] Furthermore, the outer diameter of the filling rope is 2 to 3 mm, and the rock wool rope is twisted with non-hygroscopic rock wool material. Two or more insulating cores and multiple rock wool ropes are a common right-hand twisted structure, and the twisted pitch diameter ratio ranges from 30 to 40.

[0015] Furthermore, the second flame retardant tape adopts low-smoke halogen-free flame retardant fabric tape, and the flame retardant wrapping layer is formed by wrapping two layers of halogen-free flame retardant fabric tape, the wrapping direction is inner left and outer right, the thickness of the halogen-free flame retardant fabric tape ranges from 0.19 to 0.22 mm, and the wrapping overlap rate ranges from 30% to 45%.

[0016] Furthermore, the wrapped first flame retardant tape has a left-handed overlapping structure, and the overlapping rate is between 35% and 50%.

[0017] Furthermore, the nominal thickness range of the insulating layer is 0.7-2.4 mm, the thickness of the thinnest part of the insulating layer is not less than 90% of the nominal value minus 0.1 mm, the thickness of the inner insulating layer is 0.15-0.45 mm, and the thickness of the outer insulating layer is 0.55-2.0 mm.

[0018] Furthermore, the outer diameter of the power cable ranges from 11.0 to 70.8 mm, the nominal thickness of the outer sheath ranges from 1.8 to 3.7 mm, and the thickness of the thinnest part of the outer sheath is not less than 80% of the nominal value minus 0.2 mm.

[0019] Furthermore, the diameter of the conductor ranges from 1.6 mm to 30.3 mm; the conductor is composed of annealed soft round tinned copper monofilaments twisted together, the pitch diameter ratio of the twisted copper monofilaments ranges from 16 to 30, the twisting direction of the copper monofilaments is left-handed, and the diameter of the copper monofilaments ranges from 0.52 to 3.33 mm.

[0020] The application of the power cable technical solution of the present invention achieves at least the following beneficial effects:

[0021] 1. The power cable of the present invention has a wide range of application scenarios by designing the structure of single-core and multi-core cables, and the cable structure design is relatively simple and reasonable. The inner sheath required for the previous cross-linked sheath cable is eliminated, and the complex wrapping structure in the previous cable structure is reduced, making the cable lighter.

[0022] 2. The power cable of the present invention designs a variety of unequal-core cable structures and reasonably reduces the cross-section design of the neutral line and the grounding core, which can effectively simplify the cable structure, reduce the cable outer diameter, and reduce the volume and cost of the cable from the design end.

[0023] 3. The power cable of the present invention is designed to be filled with multiple non-hygroscopic rock wool ropes with small outer diameters. The cable gaps of equal-core cables and unequal-core cables are effectively filled with flame retardants, and are wrapped with highly flame-retardant, low-smoke, halogen-free flame-retardant cloth tapes, so that the gaps in the cable core are reduced, and the wrapping coverage range is increased by 10% to 15% compared with ordinary cables. The number of layers is 2, which ensures the tightening performance of the cable core and improves the flame retardant performance.

[0024] 4. The power cable of the present invention adopts low-smoke, halogen-free and flame-retardant insulation, filling, wrapping and sheathing materials, so that the cable as a whole meets the low-smoke, halogen-free and flame-retardant performance, thereby preventing the fire from spreading through the cable.

[0025] In order to achieve the above-mentioned purpose, according to another aspect of the present invention, a method for manufacturing a power cable is proposed. Further, for manufacturing the power cable with a multi-core insulated cable core according to the above-mentioned method, the manufacturing method comprises the following steps: a conductor manufacturing step; an insulating core manufacturing step, wrapping the insulating material on the outside of the conductor by double-layer co-extrusion to form an inner insulating layer and an outer insulating layer; an irradiation cross-linking step, controlling the cross-linking degree of the insulating layer by insulation irradiation cross-linking; a cable core manufacturing step, including a filling step, filling a plurality of filling ropes between two or more insulating cores; also including a twisting step, twisting the insulating core and the filling ropes together to form a multi-core insulated cable core; a cable core outer wrapping step, wrapping a second flame retardant tape on the outer side of the multi-core insulated cable core to form a flame retardant wrapping layer; an outer sheath extrusion step S6 and an outer sheath irradiation step S7.

[0026] Furthermore, the manufacturing method also includes a test and inspection step. After the outer sheath irradiation step, the test and inspection step includes conducting an accelerated thermal aging test equivalent to 80 years of operation, winding the power cable sample into multiple test coils, and placing the multiple test coils in a circulating air aging oven for accelerated thermal aging. Based on the Arrhenius model, the accelerated thermal aging temperature is selected to be above 155°C, and the accelerated aging time is selected to be above 1313h. After the accelerated thermal aging, the test coil is subjected to an appearance inspection, a withstand voltage test, an insulation resistance measurement, and a flame retardant test.

[0027] Furthermore, the test and inspection steps also include radiation aging test. After the accelerated thermal aging test, the cable samples after accelerated thermal aging are placed in the air for cobalt 60 source gamma irradiation, with a cumulative dose of not less than 36.9 Mrad and a dose rate of ≤1 Mrad / h. After the irradiation, appearance inspection and voltage withstand test are carried out.

[0028] Furthermore, in the filling step, when the cross-sectional areas of the insulating cores of the cable core are all equal, one filling rope is used at the axial position of the cable core for filling, and two equal-section cores are filled on the cabling sides with two groups of 4 to 8 filling ropes; three equal-section cores are filled on the cabling sides with three groups of 4 to 6 filling ropes; four equal-section cores are filled on the cabling sides with four groups of 2 to 5 filling ropes; and five equal-section cores are filled on the cabling sides with five groups of 1 to 4 filling ropes.

[0029] Furthermore, in the filling step, when the cross-sectional areas of the insulating cores of the cable core are not equal, 1 to 3 filling ropes are used for filling at the center position of the cable core; 3 groups of 1 to 9 filling ropes are used for filling the cabling sides of 2 first cores and 1 second core; 4 groups of 2 to 8 filling ropes are used for filling the cabling sides of 3 first cores and 1 second core; 5 groups of 2 to 6 filling ropes are used for filling the cabling sides of 3 first cores and 2 second cores; 5 groups of 2 to 5 filling ropes are used for filling the cabling sides of 4 first cores and 1 second core.

[0030] Furthermore, in the conductor manufacturing step, when the cross-sectional area of ​​the conductor is 300 mm 2 When the conductor cross-sectional area is 35mm, the inner diameter ratio of the conductor stranding shall not exceed 22 times, and the outermost diameter ratio shall not exceed 20 times; 2 ~300mm 2 When the conductor is twisted, the inner layer pitch diameter ratio is not more than 40 times, and the outer layer pitch diameter ratio is not more than 16 times; when the cross-sectional area of ​​the conductor is 35mm 2 For conductors with diameters of 200 mm or less, the conductor twisting pitch ratio shall not be greater than 16 times; the conductor twisting pitch tolerance shall be ±10 mm. During the conductor twisting process, anhydrous alcohol shall be continuously dripped in front of the wire feed die.

[0031] Furthermore, in the insulating core manufacturing step, the extrusion form is extrusion, the control range of the inner insulating layer is 0.12-0.18 mm, the eccentricity is controlled to be no more than 10%, and the color ratio of the outer insulating layer is a 1% setting of masterbatch and base material.

[0032] Furthermore, in the outer sheath irradiation step, the elongation under load is controlled at 60% to 120%, the permanent deformation rate after cooling is not more than 15%, the number of wire passes under the titanium window is 2 to 14, the irradiation energy is 2.1 to 5.0 MeV, the beam current is 10 to 40 mA, the wire speed is 4 to 35 m / min, the deviation range of the irradiation energy is ±0.5 MeV, the deviation range of the beam current is ±3 mA, and the deviation range of the wire speed is ±2 m / min.

[0033] Furthermore, in the twisting step, when the insulated wire core with the largest cross-sectional area is 25mm 2 For the following specifications, the cable pitch ratio control range is 16 to 20 times; when the largest cross-sectional area of ​​the insulated wire core is 35mm 2 ~95mm 2 The cable pitch ratio is controlled within a range of 25 to 30 times. When the insulated wire core with the largest cross-sectional area is 120 mm 2 ~300mm 2 When the specification is met, the control range of the cable pitch diameter ratio is 30 to 40 times.

[0034] Furthermore, in the radiation cross-linking step, the elongation of the insulated wire core under load is controlled at 60% to 80%, the permanent deformation rate after cooling is not greater than 15%, and the conductor of the insulated wire core is grounded and fully discharged for 24 hours after irradiation.

[0035] Furthermore, in the outer sheath extrusion step, an extrusion die is used, the core diameter is the measured value of the cable core outer diameter plus 0.3-0.6 mm, the sleeve diameter is the core diameter plus 2 times the nominal thickness of the sheath, the sleeve wire length is 3-7 mm, and the distance between the dies is 1.5-2 times the nominal thickness of the sheath. During extrusion, the cooling is carried out in sections, the water temperature of the first section of the water tank is controlled between 35°C and 60°C according to the climate, the second section of the water tank is cooled at normal temperature, and the temperature of the extruder is controlled as follows: 100-120°C for zone 1, 110-130°C for zone 2, 120-140°C for zone 3, 130-150°C for zone 4, 140-160°C for zone 5, and 140-160°C for zone 6.

[0036] The application of the cable manufacturing method technical solution of the present invention achieves at least the following beneficial effects:

[0037] 1. The cable manufacturing method of the present invention improves the process of radiation cross-linking of the outer sheath and increases the radiation density, so that the radiation uniformity of the large-section cable is effectively guaranteed, so that the performance of the cable outer sheath meets the requirements.

[0038] 2. The cable manufacturing method of the present invention improves the service life and radiation resistance of the cable by designing the production process of the insulation layer and the outer sheath and using insulation layer and outer sheath materials with long heat aging resistance and radiation resistance. By further designing test and inspection steps, it is ensured that the cable can be stably used in nuclear power plants and has a design service life of more than 80 years.

[0039] 3. The cable manufacturing method of the present invention designs filling rope filling methods for different types of multi-core cables, so that the cable core structure is more stable and round, and the flame retardant effect is better; by adopting an outer sheath extrusion production process, the extrusion force of the machine head is used to remove the air between the cable core and the outer sheath, thereby further improving the flame retardant performance.

[0040] 4. The cable manufacturing method of the present invention can ensure the conductor purity of the power cable and improve the electrical performance by continuously dripping anhydrous alcohol in front of the wire feed die during the conductor twisting process of the conductor manufacturing step.

[0041] 5. The cable manufacturing method of the present invention ensures that the electrical properties and flame retardant properties of the insulation layer are qualified by designing the color ratio of the outer insulation layer and controlling the ratio of the inner insulation layer to the outer insulation layer during the insulation core manufacturing step. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] The accompanying drawings constituting a part of the present invention are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the accompanying drawings:

[0043] Figure 1 A schematic cross-sectional view of a uniform core low-voltage power cable is shown;

[0044] Figure 2 A schematic cross-sectional view of an unequal core low-voltage power cable is shown;

[0045] Figure 3 A schematic cross-sectional view of the low-voltage power cable in Example 1 is shown.

[0046] The above drawings include the following reference numerals:

[0047] 1. Conductor; 2. Inner insulation layer; 3. Outer insulation layer; 4. Filling rope; 5. Flame retardant wrapping layer; 6. Outer sheath; 7. Ground wire conductor; 8. Inner insulation layer of ground wire; 9. Outer insulation layer of ground wire; 10. Insulated wire core; 11. First wire core; 12. Second wire core. DETAILED DESCRIPTION

[0048] It should be noted that, in the absence of conflict, the embodiments of the present invention and the features in the embodiments can be combined with each other. The present invention will be described in detail below with reference to the accompanying drawings and in combination with the embodiments.

[0049] The present invention is further described in detail below in conjunction with specific embodiments, and these embodiments cannot be understood as limiting the scope of protection claimed by the present invention. The term "including" when used indicates the existence of a feature, but does not exclude the existence or addition of one or more other features; the orientation or position relationship indicated by the terms "lateral", "upper", "lower", "front", "rear", "left", "right", "top", "bottom", "inside", "outside", etc. is based on the orientation or position relationship shown in the drawings, which is only for the convenience of description, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention; in addition, the terms "first" and "second" are only used for descriptive purposes, and cannot be understood as indicating or implying relative importance.

[0050] In the description, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense. For example, it can be a fixed connection, a detachable connection, or an integral connection; it can be directly connected, or indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances. In addition, in the description of the present invention, unless otherwise specified, "plurality" means two or more.

[0051] Embodiment 1:

[0052] This embodiment discloses a K3 type low-voltage power cable with a service life of 80 years for a nuclear power plant, including a cable core, such as Figure 3As shown, the power cable is composed of a flame retardant wrapping layer 5 and an outer sheath 6 wrapped around the outer side of the cable core in sequence. The cable core is a single-core insulated cable core, which is composed of a first flame retardant tape wrapped around the outer side of an insulating core 10. The power cable uses an accelerated thermal aging test method based on the Arrhenius model to verify that the thermal life of the insulating core 10 at a temperature of 90°C is not less than 80 years.

[0053] Preferably, the first flame retardant tape is a low-smoke halogen-free flame retardant tape, and the wrapped low-smoke halogen-free flame retardant tape has a left-handed overlapping structure, and the overlapping rate is between 35% and 50%.

[0054] The insulated wire core 10 is composed of an insulating layer wrapped around the outer side of a conductor 1. The insulating layer includes an inner insulating layer 2 and an outer insulating layer 3. The inner insulating layer 2 is composed of a cross-linked polyethylene insulating material, and the outer insulating layer 3 is composed of a cross-linked polyolefin insulating material.

[0055] Preferably, the material of the inner insulating layer 2 is composed of a radiation-resistant low-smoke halogen-free cross-linked polyethylene insulation material with a lifespan of 80 years at 90 degrees Celsius, and the material of the outer insulating layer 3 is composed of a radiation-resistant low-smoke halogen-free flame-retardant cross-linked polyolefin insulation material with a lifespan of 80 years at 90 degrees Celsius.

[0056] Preferably, the outer diameter of the power cable is in the range of 11.0 to 70.8 mm, the nominal thickness of the insulation is in accordance with the requirements of GB / T12706.1-2020, and the average thickness of the insulation layer should not be less than the specified nominal value. The nominal thickness of the insulation layer is in the range of 0.7 to 2.4 mm, the thickness of the thinnest part of the insulation layer is not less than 90% of the nominal value minus 0.1 mm, the thickness of the inner insulation layer 2 is 0.15 to 0.45 mm, and the thickness of the outer insulation layer 3 is 0.55 to 2.0 mm.

[0057] The flame retardant wrapping layer 5 is formed by wrapping more than two layers of the second flame retardant tape, and the outer sheath 6 is made of polyolefin material. Preferably, the second flame retardant tape adopts a highly flame retardant low-smoke halogen-free flame retardant cloth tape, and the flame retardant wrapping layer 5 is formed by wrapping two layers of halogen-free flame retardant cloth tape, the wrapping direction is inner left and outer right, the thickness of the halogen-free flame retardant cloth tape ranges from 0.19 to 0.22 mm, and the wrapping overlap ranges from 30% to 45%. The outer sheath 6 is made of thermosetting low-smoke halogen-free flame retardant polyolefin material.

[0058] The nominal thickness of the outer sheath 6 ranges from 1.8 to 3.7 mm, and the thickness of the thinnest part of the outer sheath 6 is not less than 80% of the nominal value minus 0.2 mm.

[0059] The diameter of conductor 1 ranges from 1.6mm to 30.3mm; conductor 1 is composed of annealed soft round tinned copper monofilaments, and the conductor shall be the second type of tinned single-wire stranded annealed copper conductor specified in GB / T 3956-2008. The pitch diameter ratio of the copper monofilament stranding ranges from 16 to 30, the stranding direction of the copper monofilament is left-handed, and the diameter of the copper monofilament ranges from 0.52 to 3.33mm.

[0060] Embodiment 2:

[0061] This embodiment discloses a K3 type low voltage power cable with a service life of 80 years for a nuclear power station. Figure 1-Figure 2 As shown, the power cable comprises a cable core, and the outer side of the cable core is wrapped with a flame retardant sheath 5 and an outer sheath 6 in sequence. The cable core is a multi-core insulated cable core, and the multi-core insulated cable core is composed of more than two insulated wire cores 10 and a plurality of filling ropes 4 twisted together. The power cable adopts an accelerated thermal aging test method based on the Arrhenius model to verify that the thermal life of the insulated wire core 10 at a temperature of 90°C is not less than 80 years.

[0062] Specifically, the filling rope 4 includes a non-hygroscopic rock wool material, and a plurality of filling ropes 4 are located between adjacent insulating cores 10. Preferably, the outer diameter of the filling rope 4 is 2 to 3 mm, and the filling rope 4 is a rock wool rope twisted with a non-hygroscopic rock wool material, and the two or more insulating cores 10 and the plurality of rock wool ropes are in a common right-hand twisted structure, and the twisted pitch ratio ranges from 30 to 40.

[0063] The insulated wire core 10 is composed of an insulating layer wrapped around the outer side of a conductor 1. The insulating layer includes an inner insulating layer 2 and an outer insulating layer 3. The inner insulating layer 2 is composed of a cross-linked polyethylene insulating material, and the outer insulating layer 3 is composed of a cross-linked polyolefin insulating material.

[0064] Preferably, the material of the inner insulating layer 2 is composed of a radiation-resistant low-smoke halogen-free cross-linked polyethylene insulation material with a lifespan of 80 years at 90 degrees Celsius, and the material of the outer insulating layer 3 is composed of a radiation-resistant low-smoke halogen-free flame-retardant cross-linked polyolefin insulation material with a lifespan of 80 years at 90 degrees Celsius.

[0065] Preferably, the outer diameter of the power cable is in the range of 11.0 to 70.8 mm, the nominal thickness of the insulation is in accordance with the requirements of GB / T12706.1-2020, and the average thickness of the insulation layer should not be less than the specified nominal value. The nominal thickness of the insulation layer is in the range of 0.7 to 2.4 mm, the thickness of the thinnest part of the insulation layer is not less than 90% of the nominal value minus 0.1 mm, the thickness of the inner insulation layer 2 is 0.15 to 0.45 mm, and the thickness of the outer insulation layer 3 is 0.55 to 2.0 mm.

[0066] The flame retardant wrapping layer 5 is formed by wrapping more than two layers of the second flame retardant tape, and the outer sheath 6 is made of polyolefin material. Preferably, the second flame retardant tape adopts a highly flame retardant low-smoke halogen-free flame retardant cloth tape, and the flame retardant wrapping layer 5 is formed by wrapping two layers of halogen-free flame retardant cloth tape, the wrapping direction is inner left and outer right, the thickness of the halogen-free flame retardant cloth tape ranges from 0.19 to 0.22 mm, and the wrapping coverage ranges from 30% to 45%. The wrapping coverage range is increased by 10% to 15% compared with ordinary cables, and the number of layers is 2, which ensures the tightening performance of the cable core and improves the flame retardant performance.

[0067] The outer sheath 6 is made of thermosetting low-smoke halogen-free flame-retardant polyolefin material. The nominal thickness of the outer sheath 6 ranges from 1.8 to 3.7 mm, and the thickness of the thinnest part of the outer sheath 6 is not less than 80% of the nominal value minus 0.2 mm.

[0068] Preferably, the multi-core insulated cable core includes 3 to 5 insulated wire cores 10, such as Figure 2 As shown, the insulating core 10 comprises a first core 11 and a second core 12, and the cross-sectional area of ​​the first core 11 is larger than that of the second core 12. A filling rope 4 is arranged at the center of the power cable.

[0069] The multi-core insulated cable core can be set in various forms such as 2 large and 1 small, 3 large and 1 small, 3 large and 2 small, 4 large and 1 small, etc. Specifically, the multi-core insulated cable core includes 2 first cores 11 and 1 second core 12, or includes 3 first cores 11 and 1 second core 12, or includes 3 first cores 11 and 2 second cores 12, or includes 4 first cores 11 and 1 second core 12.

[0070] like Figure 2 The multi-core insulated cable core includes two first cores 11 and one second core 12. The second core 12 is a ground wire, including a ground wire conductor 7 and a ground wire inner insulation layer 8 and a ground wire outer insulation layer 9 wrapped outside the ground wire conductor 7. The materials and parameters of the ground wire conductor 7, the ground wire inner insulation layer 8 and the ground wire outer insulation layer 9 refer to the conductor 1, the inner insulation layer 2 and the outer insulation layer 3.

[0071] In addition, the multi-core insulated cable core can also be set as follows Figure 1 As shown, the multi-core insulated cable core includes 2 to 5 insulating wire cores 10 with equal cross-sectional areas. For a cable having more than three insulating wire cores with equal cross-sectional areas, a filling rope 4 is arranged at the axial position of the power cable.

[0072] The diameter of conductor 1 ranges from 1.6mm to 30.3mm; conductor 1 is composed of annealed soft round tinned copper monofilaments, and the conductor shall be the second type of tinned single-wire stranded annealed copper conductor specified in GB / T 3956-2008. The pitch diameter ratio of the copper monofilament stranding ranges from 16 to 30, the stranding direction of the copper monofilament is left-handed, and the diameter of the copper monofilament ranges from 0.52 to 3.33mm.

[0073] The following takes the parameters of a 3×70 power cable as an example. After the cable of this specification adopts this structure, the cable surface quality is excellent, and the electrical performance and structural dimensions are qualified.

[0074] The measured outer diameter of the cable is 33.1mm, and the twisted pitch ratio of the cable core is 37; the diameter of the tinned copper monofilament of conductor 1 is 2.21mm, the twisted diameter of the conductor is 9.7mm, and the twisted pitch ratio is 16. The overall average thickness of the insulation layer is 1.16mm, of which the thickness of the inner insulation layer 2 is 0.42mm, and the thickness of the outer insulation layer 3 is 0.74mm. The thickness of the high flame retardant, low smoke, halogen-free flame retardant fabric tape used in the second flame retardant tape is 0.2mm, and the thickness after 2 layers of wrapping is 1.2mm, and the wrapping overlap rate ranges from 40% to 45%. The measured thickness of the outer sheath is 2.9mm.

[0075] In summary, from the above description, it can be seen that the above-mentioned Embodiment 1 and Embodiment 2 of the present invention achieve the following technical effects:

[0076] 1. The power cable of the present invention has a wide range of application scenarios by designing the structure of single-core and multi-core cables, and the cable structure design is relatively simple and reasonable. The inner sheath required for the previous cross-linked sheath cable is eliminated, and the complex wrapping structure in the previous cable structure is reduced, making the cable lighter.

[0077] 2. The power cable of the present invention designs a variety of unequal-core cable structures and reasonably reduces the cross-section design of the neutral line and the grounding core, which can effectively simplify the cable structure, reduce the cable outer diameter, and reduce the volume and cost of the cable from the design end.

[0078] 3. The power cable of the present invention is designed to be filled with multiple non-hygroscopic rock wool ropes with small outer diameters. The cable gaps of equal-core cables and unequal-core cables are effectively filled with flame retardants, and are wrapped with highly flame-retardant, low-smoke, halogen-free flame-retardant cloth tapes, so that the gaps in the cable core are reduced, and the wrapping coverage range is increased by 10% to 15% compared with ordinary cables. The number of layers is 2, which ensures the tightening performance of the cable core and improves the flame retardant performance.

[0079] 4. The power cable of the present invention adopts low-smoke, halogen-free and flame-retardant insulation, filling, wrapping and sheathing materials, so that the cable as a whole meets the low-smoke, halogen-free and flame-retardant performance, thereby preventing the fire from spreading through the cable.

[0080] Embodiment 3:

[0081] This embodiment proposes a method for manufacturing a low-voltage power cable, which is used to manufacture a power cable with a multi-core insulated cable core according to the above-mentioned embodiment 2. The cable performance requirements are as follows: the maximum operating temperature of the cable conductor is 90°C, and the design service life of the cable is not less than 80 years. When the cable is short-circuited (the maximum duration does not exceed 5s), the maximum temperature of the conductor does not exceed 250°C. The use environment requirements are as follows: Ambient temperature: (-35~60)°C; Gamma ray normal operating condition irradiation cumulative dose: 335kGy (33.5Mrad). The minimum bending radius during cable installation should not be less than 8 times the actual outer diameter of the cable. The cable should be fixedly laid in cable brackets, cable ducts, cable trenches and cable tunnels. Combined with Figure 1-Figure 2 As shown, the manufacturing method thereof comprises the following steps:

[0082] In the conductor manufacturing step S1, a conductor 1 is manufactured by twisting.

[0083] Specifically, in the conductor manufacturing step S1, when the cross-sectional area of ​​the conductor 1 is 300 mm 2 When the cross-sectional area of ​​conductor 1 is 35mm 2 ~300mm 2 When the conductor is twisted, the inner layer pitch ratio is not greater than 40 times, and the outer layer pitch ratio is not greater than 16 times; when the cross-sectional area of ​​conductor 1 is 35mm 2 When the conductor stranding pitch ratio is less than 16 times, the conductor stranding pitch ratio is not more than 16 times; the conductor stranding pitch tolerance is ±10mm. During the conductor stranding process, continuous dripping of anhydrous alcohol in front of the wire feed die can ensure the conductor purity of the power cable and improve the electrical performance.

[0084] In the insulating core manufacturing step S2, an insulating material is wrapped around the outside of the conductor 1 by a double-layer co-extrusion method to form an inner insulating layer 2 and an outer insulating layer 3.

[0085] Specifically, in the insulating core manufacturing step S2, the extrusion form is extrusion, the control range of the inner insulating layer 2 is 0.12-0.18 mm, the eccentricity is controlled to be no more than 10%, and the color ratio of the outer insulating layer 3 is 1% of the masterbatch and the base material. By designing the color ratio of the outer insulating layer in the insulating core manufacturing step and controlling the ratio of the inner insulating layer to the outer insulating layer, the electrical properties and flame retardant properties of the insulating layer are guaranteed to be qualified.

[0086] The radiation cross-linking step S3 controls the cross-linking degree of the insulation layer by insulation radiation cross-linking.

[0087] Specifically, in the radiation cross-linking step S3, the elongation of the insulated wire core 10 under load is controlled at 60% to 80%, and the permanent deformation rate after cooling is not greater than 15%. After the insulated wire core 10 is irradiated, the conductor 1 needs to be grounded and fully discharged for 24 hours.

[0088] For example: for a cross-sectional area of ​​50mm 2 The insulation core has an insulation layer thickness of 1.2mm, 28 threading passes, irradiation energy of 2.0MeV, irradiation dose of 20Mrad, beam current of 10mA, wire speed of 25m / min, and dose setting of 2.5m / min / mA. The irradiation method adopts the "racetrack shape", and the deviation range of irradiation energy is ±0.5MeV; the deviation range of beam current is ±3mA; the deviation range of wire speed is ±5m / min.

[0089] The cable core manufacturing step S4 includes a filling step S4-1, in which a plurality of filling ropes 4 are filled between two or more insulating cores 10. Specifically, in the filling step S4-1, when the cross-sectional areas of the insulating cores 10 of the cable core are all equal, one filling rope 4 is used for filling at the axial position of the cable core, and two equal-section cores are filled with two groups of 4 to 8 filling ropes 4 for the cabling side; three equal-section cores are filled with three groups of 4 to 6 filling ropes 4 for the cabling side; four equal-section cores are filled with four groups of 2 to 5 filling ropes 4 for the cabling side; and five equal-section cores are filled with five groups of 1 to 4 filling ropes 4 for the cabling side.

[0090] In addition, when the cross-sectional areas of the insulating cores 10 of the cable core are not equal, 1 to 3 filling ropes 4 are used for filling at the center position of the cable core; the cabling sides of the two first cores 11 and the one second core 12 are filled with three groups of 1 to 9 filling ropes 4; the cabling sides of the three first cores 11 and the one second core 12 are filled with four groups of 2 to 8 filling ropes 4; the cabling sides of the three first cores 11 and the two second cores 12 are filled with five groups of 2 to 6 filling ropes 4; and the cabling sides of the four first cores 11 and the one second core 12 are filled with five groups of 2 to 5 filling ropes 4.

[0091] The cable core manufacturing step S4 also includes a twisting step S4-2, in which the insulating core 10 and the filling rope 4 are twisted together to form a multi-core insulating cable core.

[0092] Specifically, in the twisting step S4-2, when the insulated wire core 10 with the largest cross-sectional area, i.e., the main wire core, is 25 mm 2 For the following specifications, the cable pitch ratio control range is 16 to 20 times; when the main line core is 35mm 2 ~95mm 2 The cable pitch ratio is controlled within a range of 25 to 30 times. When the main line core is 120 mm 2 ~300mm 2 When the specification is met, the control range of the cable pitch diameter ratio is 30 to 40 times.

[0093] In the cable core outer wrapping step S5, a second flame retardant tape is wrapped around the outer side of the multi-core insulating cable core to form a flame retardant wrapping layer 5. The second flame retardant tape is wrapped in an overlapping wrapping manner, the overlapping rate is controlled to be 30% to 45%, and the wrapping direction is inner left and outer right. The cable core manufacturing step S4 increases the simplicity of the cable structure on the one hand, and the filling and wrapping process improves the low-smoke halogen-free flame retardant performance of the cable to prevent the spread of fire on the other hand.

[0094] In the outer sheath extrusion step S6, the sheath material is extruded on the outer side of the flame retardant wrapping layer 5 by a sheath extrusion extrusion method, and then cooled to form an outer sheath 6. By adopting the outer sheath extrusion production process, the extrusion force of the machine head is used to remove the air between the cable core and the outer sheath, thereby further improving the flame retardant performance.

[0095] Specifically, in the outer sheath extrusion step S6, an extrusion die is used, the core diameter is the measured value of the cable core outer diameter plus 0.3-0.6 mm, the sleeve diameter is the core diameter plus 2 times the nominal thickness of the sheath, the sleeve wire length is 3-7 mm, and the distance between the dies is 1.5-2 times the nominal thickness of the sheath. During extrusion, the cooling is carried out in sections, the water temperature of the first section of the water tank is controlled between 35°C and 60°C according to the climate, the second section of the water tank is cooled at room temperature, and the temperature of the extruder is controlled as follows: 100-120°C for zone 1, 110-130°C for zone 2, 120-140°C for zone 3, 130-150°C for zone 4, 140-160°C for zone 5, and 140-160°C for zone 6.

[0096] In the outer sheath irradiation step S7, the outer sheath 6 is irradiated by using a multi-pass irradiation method and adding a reflective magnet. By improving the outer sheath irradiation cross-linking process and increasing the irradiation density, the irradiation uniformity of the large-section cable is effectively guaranteed, so that the performance of the cable outer sheath meets the requirements.

[0097] Specifically, in the outer sheath irradiation step S7, the elongation under load is controlled at 60% to 120%, the permanent deformation rate after cooling is not more than 15%, the irradiation method adopts a "runway" shape, the number of wire passes under the titanium window is 2 to 14, the irradiation energy is 2.1 to 5.0 MeV, the beam current is 10 to 40 mA, the wire speed is 4 to 35 m / min, the deviation range of the irradiation energy is ±0.5 MeV, the deviation range of the beam current is ±3 mA, and the deviation range of the wire speed is ±2 m / min.

[0098] The manufacturing method also includes a test and inspection step S8. After the outer sheath irradiation step S7, the test and inspection step S8 includes conducting an accelerated thermal aging test equivalent to 80 years of operation, winding the power cable sample into a plurality of test coils, placing the plurality of test coils in a circulating air aging oven for accelerated thermal aging, and after the accelerated thermal aging, performing an appearance inspection, a withstand voltage test, an insulation resistance measurement on the test coils and passing a flame retardant test.

[0099] Specifically, the effective test length of each test coil is not less than 3.05m, and the test temperature and time of the circulating air aging oven are derived from the insulation thermal life assessment test results. Based on the Arrhenius model, the accelerated thermal aging temperature is selected and the accelerated thermal aging time is calculated. The steps are as follows:

[0100] Based on the Arrhenius equation, we can get:

[0101] In the formula, τ is the time required for a certain change of the material, in h,

[0102] Ea——Material activation energy, unit eV,

[0103] R——Boltzmann constant, 0.00008617,

[0104] H——insulation temperature, unit K,

[0105] A—Constants related to materials and diagnostic tests.

[0106] Transforming the equation yields:

[0107] Activation energy data of internal insulation: Ea = 126.8 kJ / mol = 1.314 eV,

[0108] Activation energy data of external insulation: Ea = 129.2 kJ / mol = 1.339 eV,

[0109] Activation energy data of outer sheath: Ea = 127.4 kJ / mol = 1.320 eV,

[0110] Working temperature of the material: H2 = 273.15 + 90 = 363.15K,

[0111] Accelerated aging temperature: H1 = 273.15 + 155 = 428.15K,

[0112] The life of the material to be identified: τ2 = 80 × 365 × 24 = 700800h,

[0113] Substituting the above parameters, we can get the accelerated thermal aging time τ1 = 1194h,

[0114] Add 10% margin, 1313h.

[0115] Based on the Arrhenius model, the accelerated thermal aging temperature is selected to be above 155°C, and a 10% margin is added, and the accelerated thermal aging time is calculated to be above 1313h.

[0116] During the appearance inspection, the cable structure is required to remain intact, without obvious deformation, cracking and other abnormal phenomena. The cable sample is bent into a coil with an inner diameter not exceeding 20 times the outer diameter of the cable and immersed in water for 1 hour, and then subjected to a withstand voltage test. An AC voltage of 3150V / mm is applied between conductors and conductors, and between conductors and water and shielding for 5 minutes, and the insulation should not be broken down. Insulation resistance measurement is performed, and the insulation resistance value must be greater than 1MΩ·km (at an ambient temperature of 20±5℃). Pass the bundled B-type flame retardant test.

[0117] The test inspection step S8 also includes performing a radiation aging test. After the accelerated thermal aging test, the cable sample after accelerated thermal aging is placed in the air for cobalt 60 source γ irradiation, with a cumulative dose of not less than 36.9 Mrad (33.5 Mrad + 10% margin), and a dose rate of ≤1 Mrad / h. After the irradiation, an appearance inspection and a withstand voltage test are performed.

[0118] During the appearance inspection, the cable structure is required to remain intact, without obvious deformation, cracking and other abnormal phenomena. The cable sample is bent into a coil with an inner diameter not exceeding 20 times the outer diameter of the cable and immersed in water for 1 hour, and then subjected to a withstand voltage test. An AC voltage of 3150V / mm is applied between conductors and conductors, and between conductors and water and shielding for 5 minutes, and the insulation should not be broken down.

[0119] Preferably, the power cable manufactured by the manufacturing method of this embodiment can also withstand the following tests: voltage test, conductor resistance measurement, insulation resistance test, 4h voltage test, conductor inspection and dimension inspection, insulation mechanical properties test before and after aging, insulation thermal extension test, insulation water absorption test, insulation shrinkage test, insulation toxicity index, sheath mechanical properties test before and after aging, sheath thermal extension test, sheath water absorption test, sheath low temperature performance test, sheath anti-cracking test, sheath oil immersion test, wear resistance test, finished cable additional aging test, single vertical burning test, bundled burning Class B test, smoke density test, pH and conductivity test, acid gas content test, finished cable bending test, printed mark abrasion resistance test, and the test results are passed.

[0120] In summary, from the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0121] 1. The cable manufacturing method of the present invention improves the process of radiation cross-linking of the outer sheath and increases the radiation density, so that the radiation uniformity of the large-section cable is effectively guaranteed, so that the performance of the cable outer sheath meets the requirements.

[0122] 2. The cable manufacturing method of the present invention improves the service life and radiation resistance of the cable by designing the production process of the insulation layer and the outer sheath and using insulation layer and outer sheath materials with long heat aging resistance and radiation resistance. By further designing test and inspection steps, it is ensured that the cable can be stably used in nuclear power plants and has a design service life of more than 80 years.

[0123] 3. The cable manufacturing method of the present invention designs filling rope filling methods for different types of multi-core cables, so that the cable core structure is more stable and round, and the flame retardant effect is better; by adopting an outer sheath extrusion production process, the extrusion force of the machine head is used to remove the air between the cable core and the outer sheath, thereby further improving the flame retardant performance.

[0124] 4. The cable manufacturing method of the present invention can ensure the conductor purity of the power cable and improve the electrical performance by continuously dripping anhydrous alcohol in front of the wire feed die during the conductor twisting process of the conductor manufacturing step.

[0125] 5. The cable manufacturing method of the present invention ensures that the electrical properties and flame retardant properties of the insulation layer are qualified by designing the color ratio of the outer insulation layer and controlling the ratio of the inner insulation layer to the outer insulation layer during the insulation core manufacturing step.

[0126] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A K3 power cable with a service life of 80 years, comprising a cable core, wherein the power cable is composed of a flame retardant wrapping layer (5) and an outer sheath (6) wrapped in sequence on the outer side of the cable core, characterized in that: The cable core is a single-core insulated cable core, which is composed of an insulating wire core (10) with a first flame retardant tape wrapped around the outer side. Alternatively, the cable core is a multi-core insulating cable core, the multi-core insulating cable core is composed of two or more insulating wire cores (10) twisted together with a plurality of filling ropes (4), the filling ropes (4) include non-hygroscopic rock wool material, and the plurality of filling ropes (4) are located between adjacent insulating wire cores (10); The insulated wire core (10) is composed of an insulating layer wrapped around the outer side of a conductor (1), the insulating layer comprising an inner insulating layer (2) and an outer insulating layer (3), the inner insulating layer (2) being composed of a cross-linked polyethylene insulating material, and the outer insulating layer (3) being composed of a cross-linked polyolefin insulating material; The flame retardant wrapping layer (5) is formed by wrapping more than two layers of the second flame retardant tape, and the outer sheath (6) is made of polyolefin material.

2. The power cable according to claim 1, characterized in that: The power cable uses an accelerated thermal aging test method based on the Arrhenius model to verify that the thermal life of the insulating core (10) is not less than 80 years at a temperature of 90°C.

3. The power cable according to claim 1, characterized in that: The multi-core insulated cable core comprises 3 to 5 insulated cores (10), the insulated cores (10) comprise a first core (11) and a second core (12), the cross-sectional area of ​​the first core (11) is larger than that of the second core (12), or; The multi-core insulating cable core comprises 2 to 5 insulating wire cores (10) with equal cross-sectional areas.

4. The power cable according to claim 2, characterized in that: The multi-core insulated cable core comprises two first cores (11) and one second core (12), or comprises three first cores (11) and one second core (12), or comprises three first cores (11) and two second cores (12), or comprises four first cores (11) and one second core (12).

5. The power cable according to any one of claims 1 to 3, characterized in that: The filling rope (4) has an outer diameter of 2 to 3 mm and is a rock wool rope twisted with non-hygroscopic rock wool material. The two or more insulating cores (10) and the plurality of rock wool ropes are in a common right-hand twisted structure, and the twisted pitch-diameter ratio ranges from 30 to 40.

6. The power cable according to claim 4, characterized in that: The second flame retardant tape is made of low-smoke halogen-free flame retardant fabric tape, and the flame retardant wrapping layer (5) is formed by wrapping two layers of the halogen-free flame retardant fabric tape, with the wrapping direction being inner left and outer right. The thickness of the halogen-free flame retardant fabric tape ranges from 0.19 to 0.22 mm, and the wrapping overlap ranges from 30% to 45%.

7. A method for manufacturing a power cable, characterized in that: For manufacturing a power cable having a multi-core insulated cable core according to any one of claims 1 to 6, the manufacturing method comprises the following steps: Conductor manufacturing step S1; Insulated wire core manufacturing step S2, using a double-layer co-extrusion method to wrap the insulating material on the outside of the conductor (1) to form an inner insulating layer (2) and an outer insulating layer (3); Radiation cross-linking step S3, controlling the cross-linking degree of the insulation layer by insulation radiation cross-linking; The cable core manufacturing step S4 comprises a filling step S4-1, filling a plurality of filling ropes (4) between two or more insulating cores (10); and a twisting step S4-2, twisting the insulating cores (10) and the filling ropes (4) together to form a multi-core insulating cable core; Cable core outer wrapping step S5, wrapping a second flame retardant tape on the outer side of the multi-core insulating cable core to form a flame retardant wrapping layer (5); The outer sheath is extruded in step S6 and irradiated in step S7.

8. The manufacturing method according to claim 7, characterized in that: The manufacturing method also includes a test and inspection step S8. After the outer sheath irradiation step S7, the test and inspection step S8 includes performing an accelerated thermal aging test equivalent to 80 years of operation, winding the sample of the power cable into a plurality of test coils, placing the plurality of test coils in a circulating air aging oven for accelerated thermal aging, selecting an accelerated thermal aging temperature of more than 155°C and an accelerated aging time of more than 1313h based on the Arrhenius model, and performing an appearance inspection, a withstand voltage test, an insulation resistance measurement, and passing a flame retardant test on the test coil after the accelerated thermal aging.

9. The manufacturing method according to claim 8, characterized in that: The test and inspection step S8 also includes performing a radiation aging test. After the accelerated thermal aging test, the cable sample after accelerated thermal aging is placed in the air for cobalt 60 source gamma irradiation, with a cumulative dose of not less than 36.9 Mrad and a dose rate of ≤1 Mrad / h. After the irradiation, an appearance inspection and a withstand voltage test are performed.

10. The manufacturing method according to claim 7, characterized in that: In the filling step S4-1, when the cross-sectional areas of the insulating cores (10) of the cable core are all equal, one filling rope (4) is used for filling at the axial position of the cable core; two equal-section cores are filled with two groups of 4 to 8 filling ropes (4) on the cabling side; three equal-section cores are filled with three groups of 4 to 6 filling ropes (4) on the cabling side; four equal-section cores are filled with four groups of 2 to 5 filling ropes (4) on the cabling side; and five equal-section cores are filled with five groups of 1 to 4 filling ropes (4) on the cabling side.

11. The manufacturing method according to claim 10, characterized in that: In the filling step S4-1, when the cross-sectional areas of the insulating cores (10) of the cable core are not equal, 1 to 3 filling ropes (4) are used for filling at the center of the cable core; 3 groups of 1 to 9 filling ropes (4) are used for filling at the cabling sides of 2 first cores (11) and 1 second core (12); 4 groups of 2 to 8 filling ropes (4) are used for filling at the cabling sides of 3 first cores (11) and 1 second core (12); 5 groups of 2 to 6 filling ropes (4) are used for filling at the cabling sides of 3 first cores (11) and 2 second cores (12); and 5 groups of 2 to 5 filling ropes (4) are used for filling at the cabling sides of 4 first cores (11) and 1 second core (12).

12. The manufacturing method according to claim 7, characterized in that: In the conductor manufacturing step S1, when the cross-sectional area of ​​the conductor (1) is 300 mm 2 When the cross-sectional area of ​​the conductor (1) is 35 mm 2 ~300mm 2 When the conductor is twisted, the inner layer pitch diameter ratio is not greater than 40 times, and the outer layer pitch diameter ratio is not greater than 16 times; when the cross-sectional area of ​​the conductor (1) is 35mm 2 For conductors with diameters of 200 mm or less, the conductor twisting pitch ratio shall not be greater than 16 times; the conductor twisting pitch tolerance shall be ±10 mm. During the conductor twisting process, anhydrous alcohol shall be continuously dripped in front of the wire feed die.

13. The manufacturing method according to claim 7, characterized in that: In the insulating wire core manufacturing step S2, the extrusion form is extrusion, the control range of the inner insulating layer (2) is 0.12-0.18 mm, the eccentricity is controlled to be no more than 10%, and the color ratio of the outer insulating layer (3) is a masterbatch and a base material ratio set to be added at 1%.

14. The manufacturing method according to claim 7, characterized in that: In the twisting step S4-2, when the insulated wire core (10) with the largest cross-sectional area is 25 mm 2 When the specifications are as follows, the cable pitch ratio control range is 16 to 20 times; when the insulating wire core (10) with the largest cross-sectional area is 35mm 2 ~95mm 2 When the cable pitch ratio is controlled within a range of 25 to 30 times, the insulated wire core (10) with the largest cross-sectional area is 120 mm 2 ~300mm 2 When the specification is met, the control range of the cable pitch diameter ratio is 30 to 40 times.