Bonding method for 3D wafer level packaging

By using nano-scale metal particle interface adhesive and heat treatment process in 3D packaging technology, the electrical connection, mechanical strength and thermal matching problems between material layers are solved, and the accuracy and reliability of 3D packaging is improved, suitable for complex electronics Equipment manufacturing.

CN118943026APending Publication Date: 2024-11-12THING ELEMENT SEMICON TECH (QINGDAO) CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410995190.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

3D packaging technology has accuracy and reliability challenges in alignment, bonding and thermal, mechanical connections, especially the electrical connection, mechanical strength and thermal matching between different material layers, resulting in unstable packaging performance and life.

Method used

Interface adhesive containing nano-scale metal particles is used for spin coating and fixed point coating. Combined with the heat treatment process, the thermal expansion matching and mechanical strength between materials are optimized, and structural stability and long-term reliability are improved.

Benefits of technology

Through precise bonding and heat treatment, the accuracy, reliability and performance of 3D packaging is improved, and the mechanical strength and electrical conductivity of electronic devices are enhanced. It is suitable for the manufacturing of complex electronic devices and micro devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943026A_ABST
    Figure CN118943026A_ABST
Patent Text Reader

Abstract

The invention designs a bonding method for 3D wafer level packaging. The bonding method comprises the following steps: providing a first substrate and a second substrate which are provided with bonding interfaces; uniformly spin-coating an interface adhesive containing nano-scale metal particles on a bonding interface of the two substrates; scanning the three-dimensional images of the first substrate and the second substrate to obtain height distribution of a bonding interface; dispensing an interface adhesive at a fixed point on the bonding interface based on the height distribution, so that the bonding interfaces of the two substrates are highly complementary; aligning and pressing the first bonding interface and the second bonding interface; and performing hot reflux treatment on the first substrate and the second substrate which are laminated at a preset hot reflux temperature. According to the method, highly complementary accurate bonding between the substrates is realized by dispensing the interface adhesive, the bonding precision and the interface bonding strength are improved, thermal expansion matching between the two bonding interfaces is optimized through the heat treatment process, and the stability and long-term reliability of the whole structure of the two bonded substrates are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of semiconductor production, and in particular relates to a bonding method for 3D wafer-level packaging. Background Art

[0002] 3D packaging, also known as three-dimensional packaging, is an advanced electronic packaging technology that stacks multiple chips or wafers in the vertical direction and achieves electrical, thermal and mechanical connections between chips or wafers through a specific bonding process. It can greatly improve packaging density, shorten internal connection length, reduce power loss and signal delay, and achieve mutual integration of chips of different materials, devices and structures. It is an important development direction of electronic packaging technology.

[0003] However, although 3D packaging technology has many advantages, it also faces some challenges and disadvantages in practical applications. On the one hand, 3D packaging involves alignment, bonding and post-processing steps in multiple dimensions. These steps have extremely high requirements for equipment and processes. A small alignment error or poor bonding may cause the entire package to fail. On the other hand, in 3D packaging, the stacking between different material layers needs to ensure the reliability of electrical connection, mechanical strength and thermal matching. The failure of any layer may affect the performance and life of the entire package. In addition, there may be problems such as corrosion and stress concentration at the interface between layers, further increasing the reliability risk. Summary of the invention

[0004] The purpose of the present invention is to solve one of the above-mentioned technical problems and provide a bonding method for 3D wafer-level packaging, which uses an interface adhesive containing metal nanoparticles to enhance the mechanical strength and electrical conductivity of the connection. In addition, the thermal expansion matching between materials is optimized by combining the spot coating of the interface adhesive with the heat treatment process, thereby improving the overall structural stability and long-term reliability.

[0005] To achieve the above object, the technical solution adopted by the present invention is:

[0006] A bonding method for 3D wafer-level packaging, characterized in that it comprises the following steps:

[0007] Providing a first substrate and a second substrate, wherein the first substrate has a first bonding interface, and the second substrate has a second bonding interface;

[0008] Uniformly spin-coating an interface adhesive comprising nano-scale metal particles on the first bonding interface and the second bonding interface;

[0009] Scanning a three-dimensional stereoscopic image of the first substrate and the second substrate to obtain height distributions of surfaces of the first bonding interface and the second bonding interface;

[0010] Applying the interface adhesive at fixed points on the first bonding interface and / or the second bonding interface based on the height distribution, so that the heights of the first bonding interface and the second bonding interface surfaces are complementary;

[0011] The first bonding interface and the second bonding interface are aligned and pressed.

[0012] In some embodiments of the present invention, the following steps are further included:

[0013] The first substrate and the second substrate after being pressed together are subjected to a heat reflow treatment at a predetermined heat reflow temperature.

[0014] In some embodiments of the present invention, the heat reflow temperature ranges from 200°C to 400°C.

[0015] In some embodiments of the present invention, the following steps are further included:

[0016] After the heat reflow treatment, the interface adhesive is cooled at a predetermined ambient temperature until the interface adhesive is completely cured.

[0017] In some embodiments of the present invention, the following steps are further included:

[0018] The invention discloses preparing an interface adhesive containing nano-sized metal particles. The graphene is mixed with a thermoplastic polymer, and the nano-sized metal particles are added thereto to obtain the interface adhesive containing nano-sized metal particles.

[0019] In some embodiments of the present invention, the adhesion of the interface adhesive is 0-100 cp.

[0020] In some embodiments of the present invention, the metal is one or more of aluminum, copper, and gold.

[0021] In some embodiments of the present invention, the following steps are further included:

[0022] After the interface adhesive is applied at fixed points, the interface adhesive is allowed to dry naturally at a predetermined temperature, or the interface adhesive is baked at a predetermined temperature to make the interface adhesive reach a semi-cured state.

[0023] In some embodiments of the present invention, the following steps are further included:

[0024] Before spin coating the interface adhesive, the first bonding interface and the second bonding interface are cleaned using a chemical solvent or deionized water.

[0025] In some embodiments of the present invention, the method for uniformly spin coating the interface adhesive containing nano-sized metal particles is spraying, brushing or printing.

[0026] The beneficial effects of the present invention are:

[0027] 1. The present invention obtains the height distribution information of the two interfaces to be bonded by scanning the three-dimensional images of the two substrates to be bonded, and further applies the interface adhesive at fixed points on the concave parts of one or two interfaces based on the height distribution information, thereby achieving highly complementary and precise bonding between the substrates, and improving the bonding accuracy and interface bonding strength;

[0028] 2. The present invention uses an interface adhesive containing nano-scale metal particles, which enhances the mechanical strength and electrical conductivity of the connection between the two substrates after bonding, which is beneficial to improving the overall performance of the electronic device;

[0029] 3. The present invention introduces a heat treatment process after bonding, optimizes the thermal expansion matching between the two bonding interfaces, and improves the stability and long-term reliability of the overall structure of the two substrates after bonding;

[0030] 4. The bonding method provided by the present invention can be applied to 3D packaging technology, improves the accuracy, reliability and performance of 3D packaging, and can be used to manufacture complex electronic devices and micro devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the specific embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0032] Figure 1 A flow chart of a bonding method for 3D wafer-level packaging provided by the present invention;

[0033] Figure 2 Schematic diagram of height distribution of bonding interface;

[0034] Wherein, (a) is a schematic diagram of the height distribution of the first bonding interface, and (b) is a schematic diagram of the height distribution of the second bonding interface;

[0035] Figure 3 It is a schematic diagram of the effect of thermal reflow treatment;

[0036] Among them, (a) is a schematic diagram of the gap distribution between the two substrates before thermal reflow treatment, and (b) is a schematic diagram of the gap distribution between the two substrates after thermal reflow treatment. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical solutions and advantages of the present application clearer, the present application is described and illustrated below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not intended to limit the present application. Based on the embodiments provided in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application.

[0038] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.

[0039] In the absence of conflict, the embodiments of the present invention and the features of the embodiments may be combined with each other.

[0040] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and the accompanying drawings.

[0041] As attached Figure 1 - Attachment Figure 3 As shown, in an exemplary embodiment of a bonding method for 3D wafer-level packaging of the present invention, the method can be applied to advanced packaging, i.e., 3D packaging technology, for manufacturing a three-dimensional structure, and the method comprises the following steps:

[0042] S1: Material preparation, selecting the material layer to be connected, providing a first substrate and a second substrate, both of which are semiconductor substrates. In this embodiment, both of which are wafers. The first substrate has a first bonding interface, and the second substrate has a second bonding interface. The first bonding interface and the second bonding interface can be the same material layer or different material layers.

[0043] In some embodiments of the present invention, in order to prevent interface defects during the bonding process and improve the bonding quality and reliability, the first bonding interface and the second bonding interface are cleaned before spin coating the interface adhesive to ensure that the material surfaces of the first bonding interface and the second bonding interface are clean and free of dust, oil or other contaminants.

[0044] The specific method of cleaning the substrate is to soak or spray the cleaning solution. The specific steps of cleaning the substrate include:

[0045] Pre-cleaning is performed before formal cleaning to remove large particles and dust on the surface of the wafer substrate and reduce the risk of damage to the wafer in subsequent steps.

[0046] Chemical cleaning involves immersing the wafer substrate in a specific chemical solution, which can be an acidic, alkaline or oxidizing solution, respectively used to remove different types of contaminants. For example, the chemical solution can use APM (NH4OH / H2O2 / H2O) and HPM (HCl / H2O2 / H2O) solutions in RCA cleaning. If necessary, megahertz-level ultrasound can be added during the cleaning process to further improve the cleaning effect.

[0047] Deionized water rinse,After chemical cleaning, the wafer substrate is rinsed multiple times with deionized water to remove chemical solution residues and prevent cross contamination in subsequent processes.

[0048] Spin drying: The cleaned wafer substrate is spin dried to remove moisture from the surface. It should be noted that this step needs to be performed under controlled conditions to prevent water stains or other defects.

[0049] Inspection and monitoring, after the cleaning process is completed, the surface of the wafer substrate is inspected to ensure the cleaning effect, and the cleaning quality is evaluated through various monitoring technologies, such as optical microscopy, scanning electron microscopy, etc.

[0050] S2: Applying the interface adhesive, uniformly spin-coating the interface adhesive containing nano-scale metal particles on the first bonding interface and the second bonding interface, and ensuring uniform coverage of the interface adhesive during the spin-coating process. The coating technology of the interface adhesive is one of spraying, brushing or printing.

[0051] During the coating process of the interface adhesive, high-precision spin coating equipment is used. By controlling the spin coating parameters of the spin coating equipment, such as speed, acceleration and deceleration, the rotation speed of the substrate and the coating duration during spin coating are accurately controlled to achieve a uniform coating effect.

[0052] When the first bonding interface and the second bonding interface have thicker adhesive layers or higher uniformity, multiple spin coatings may be performed with appropriate drying between the multiple spin coatings.

[0053] In some embodiments of the present invention, step S2 further includes the following steps.

[0054] The invention discloses a method for preparing an interface adhesive containing nano-scale metal particles. The specific method comprises mixing graphene with a thermoplastic polymer and adding the nano-scale metal particles therein to obtain the interface adhesive containing nano-scale metal particles.

[0055] Since nanoparticles can fill tiny gaps on the surface of materials, thereby providing a stronger mechanical anchoring effect, the use of an interface adhesive containing nanoscale metal particles in the present invention can significantly improve the bonding strength between two bonding interfaces, that is, between two material layers. At the same time, it also helps to improve the electrical conductivity of the connection interface, thereby improving the overall performance of subsequently manufactured electronic devices.

[0056] During the preparation process, ensure that the viscosity, fluidity of the adhesive and the dispersion of the nano-metal particles meet the specific process requirements. It should be noted that the larger the defect or the wider the defect area, the lower the viscosity and fluidity of the adhesive need to be, the better. Conversely, the smaller the defect or the smaller the defect area, the higher the viscosity and fluidity of the adhesive need to be, the better.

[0057] In this embodiment, the adhesion of the interface adhesive is controlled below 100 cp during the preparation process.

[0058] In some embodiments of the present invention, the metal particles in the interface adhesive are one or more of aluminum, copper, and gold.

[0059] S3: Use a measuring machine to scan the three-dimensional image of the first substrate and the second substrate to obtain the height distribution of the first bonding interface and the second bonding interface surface for fixed point selection. In this embodiment, the measuring machine used is Onto's IRISS machine. The height distribution of the first bonding interface and the second bonding interface surface is shown in the attached figure. Figure 2 As shown, (a) is a schematic diagram of the height distribution of the first bonding interface, and (b) is a schematic diagram of the height distribution of the second bonding interface.

[0060] S4: Apply the interface adhesive at fixed points on the depressions of the first bonding interface and the second bonding interface based on the height distribution, so that the heights of the surfaces of the first bonding interface and the second bonding interface are complementary. In this embodiment, the interface adhesive is applied only on one of the bonding interfaces, and during the application process, the depression of the bonding interface and the point opposite to the depression of the other bonding interface on the bonding interface are selected as fixed points. The present invention achieves precise bonding with complementary heights between two bonding interfaces by combining three-dimensional image scanning with fixed-point adhesive application, effectively improving the bonding accuracy and interface bonding strength.

[0061] In some embodiments of the present invention, step S4 further includes the following steps.

[0062] After the interface adhesive is applied at fixed points, the interface adhesive is dried naturally at a predetermined temperature, or the interface adhesive is baked at a predetermined temperature to make the interface adhesive reach a semi-cured state. In this embodiment, the predetermined temperature is room temperature or 23°C.

[0063] S5: The first bonding interface coated with the interface adhesive is precisely aligned with the second bonding interface to ensure the alignment accuracy between the bonding interfaces. A pressure of 1.8N is applied to the center of the first substrate and the center of the second substrate simultaneously for 10 seconds. The first substrate and the second substrate are pressed together to make the bonding interfaces of the two substrates in close contact and squeeze out the excess interface adhesive. The pressure applied to the two substrates is precisely controlled during the alignment and bonding process to ensure uniform contact and prevent misalignment.

[0064] The method for achieving precise alignment of the first bonding interface and the second bonding interface includes:

[0065] A high-precision optical imaging system is used to observe and align the two substrates.

[0066] Specific alignment marks are pre-made on the substrate to serve as reference points during the alignment process.

[0067] Machine vision algorithms and cameras are used to identify marks or features on the substrate and perform automatic alignment.

[0068] Electrostatic adsorption technology is used to fix the substrate to prevent displacement during alignment and bonding.

[0069] Use alignment equipment with multi-axis adjustment capabilities to make fine adjustments in X, Y, Z, and rotational axes.

[0070] Perform alignment and bonding in a clean room or controlled environment to reduce the impact of external factors such as dust, vibration and humidity on alignment accuracy.

[0071] In the specific implementation process, one or more combinations of the above alignment methods can be selected to ensure accurate alignment during the substrate bonding process, thereby improving the bonding quality and the reliability of the electronic device.

[0072] In some embodiments of the present invention, the following steps are further included.

[0073] S6: Determine the heat reflow temperature based on the material and internal structure of the first substrate and the second substrate, and perform heat reflow treatment on the pressed first substrate and the second substrate at the predetermined heat reflow temperature. In this embodiment, the predetermined heat reflow temperature is selected to be 350°C. Through the heat treatment process, the thermal expansion coefficient matching between different wafer substrates, that is, different material layers can be optimized to reduce the stress accumulation caused by temperature changes, thereby improving the overall stability and long-term reliability of the structure. During the heat treatment process, the temperature and duration are precisely controlled to further optimize the thermal expansion matching between materials. The distribution of gaps at the connection interface of the two substrates before and after the heat reflow treatment is shown in the attached figure. Figure 3 As shown, (a) is a schematic diagram of the gap distribution between the two substrates before thermal reflow treatment, and (b) is a schematic diagram of the gap distribution between the two substrates after thermal reflow treatment.

[0074] In some embodiments of the present invention, the heat reflow temperature ranges from 200°C to 400°C.

[0075] In some embodiments of the present invention, the following steps are further included.

[0076] S7: Cooling and curing. After the heat reflow treatment, the interface adhesive is slowly cooled at a predetermined ambient temperature to avoid internal stress caused by rapid temperature changes until the interface adhesive is completely cured and a stable mechanical and electrical connection is formed between the two bonding interfaces. The predetermined ambient temperature is room temperature or 23°C.

[0077] In some embodiments of the present invention, the following steps are further included.

[0078] S7: Quality inspection: quality inspection of the two substrates after connection, including mechanical strength test, conductivity test and long-term reliability test, etc., to ensure that all indicators of the two substrates after bonding meet the design requirements and application standards.

[0079] Finally, it should be noted that: the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0080] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A bonding method for 3D wafer-level packaging, characterized in that: The following steps are involved: Providing a first substrate and a second substrate, wherein the first substrate has a first bonding interface, and the second substrate has a second bonding interface; Uniformly spin-coating an interface adhesive containing nano-scale metal particles on the first bonding interface and the second bonding interface; Scanning three-dimensional stereo images of the first substrate and the second substrate to obtain height distributions of the first bonding interface and the second bonding interface; Based on the height distribution, applying the interface adhesive at fixed points on the first bonding interface and / or the second bonding interface, so that the heights of the surfaces of the first bonding interface and the second bonding interface are complementary; The first bonding interface and the second bonding interface are aligned and pressed.

2. The bonding method for 3D wafer level packaging according to claim 1, characterized in that: Further comprising the steps of: The first substrate and the second substrate after being pressed together are subjected to a heat reflow treatment at a predetermined heat reflow temperature.

3. The bonding method for 3D wafer level packaging according to claim 2, characterized in that: The heat reflux temperature ranges from 200°C to 400°C.

4. The bonding method for 3D wafer level packaging according to claim 2 or 3, characterized in that: Further comprising the steps of: After the heat reflow treatment, the interface adhesive is cooled at a predetermined ambient temperature until the interface adhesive is completely cured.

5. The bonding method for 3D wafer level packaging according to claim 1, characterized in that: Further comprising the steps of: The invention discloses preparing an interface adhesive containing nano-sized metal particles. The graphene is mixed with a thermoplastic polymer, and the nano-sized metal particles are added thereto to obtain the interface adhesive containing nano-sized metal particles.

6. The bonding method for 3D wafer level packaging according to claim 5, characterized in that: The interface adhesive has an adhesion of 0-100 cp.

7. The bonding method for 3D wafer level packaging according to claim 1, 5 or 6, characterized in that: The metal is one or more of aluminum, copper and gold.

8. The bonding method for 3D wafer level packaging according to claim 1, characterized in that: Further comprising the steps of: After the interface adhesive is applied at fixed points, the interface adhesive is allowed to dry naturally at a predetermined temperature, or the interface adhesive is baked at a predetermined temperature to make the interface adhesive reach a semi-cured state.

9. The bonding method for 3D wafer level packaging according to claim 1, characterized in that: Further comprising the steps of: Before spin coating the interface adhesive, the first bonding interface and the second bonding interface are cleaned.

10. The bonding method for 3D wafer level packaging according to claim 1, characterized in that: The method of uniformly coating the interface adhesive containing nano-sized metal particles is spraying, brushing or printing.

Citation Information

Patent Citations

  • Wafer bonding interface defect detection method and storage medium

    CN111599709A

  • Wafer bonding defect position positioning method and manufacturing method of semiconductor device sample

    CN111816582A

  • Copper-copper low-temperature bonding method based on graphene / tin modified copper nanoparticles

    CN111916344A

  • Interface-enhanced multilayer composite conductive gel and preparation method thereof

    CN114835931A

  • Substrate inspection device, substrate processing device, substrate inspection method, and substrate processing method

    JP2020153854A