CZTSSe solar cell and preparation method of buffer layer of CZTSSe solar cell

By introducing alkali metal salt and ammonia-ammonium salt buffering system in the chemical water bath deposition method, the growth mode of CdS film is regulated, and the problem of high defect density of CZTSSe/CdS interface is solved and the efficiency of solar cells is improved.

CN118943234APending Publication Date: 2024-11-12INSTITUTE OF PHYSICS CHINESE ACADEMY OF SCIENCES
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310522754.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are a large number of deep energy level defects and leakage channels in the CZTSSe/CdS heterojunction interface, resulting in low solar cell efficiency. It is difficult to prepare high crystallinity and high uniformity CdS films in the existing chemical water bath deposition method.

Method used

Introducing alkali metal salt and ammonia-ammonium salt buffering system during chemical water bath deposition, the ionic environment in the solution is regulated, the 'ion-ion' growth mode is promoted, the interface defect density is reduced and the S element loss is suppressed, and high-quality CdS is prepared Buffer layer.

Benefits of technology

The defect density at the CZTSSe/CdS interface is significantly reduced, the crystallinity and uniformity of the CdS film is improved, the open circuit voltage and filling factor of the solar cell are improved, and the photoelectric conversion efficiency is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943234A_ABST
    Figure CN118943234A_ABST
Patent Text Reader

Abstract

The invention provides a CZTSSe solar cell and a preparation method of a buffer layer of the CZTSSe solar cell. The preparation method comprises the following steps: immersing a CZTSSe film into a solution containing a first concentration of cadmium salt under the condition of keeping stirring, wherein the solution also contains an ammonia water-ammonium salt buffer system and alkali metal salt; adding thiourea into the solution, and completely dissolving thiourea; and placing the solution in a water bath environment at a specified temperature for chemical water bath deposition for a preset time so as to deposit a CdS film on the surface of the CZTSSe film as a buffer layer. According to the preparation method, the alkali metal salt is introduced into the chemical bath deposition solution, so that the deep energy level defect on the surface of CZTSSe can be eliminated, and the defect density at the CZTSSe / CdS interface is reduced, thereby preparing the CdS film with high crystallinity and high uniformity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of thin-film solar cells, and in particular to a method for preparing a buffer layer of a CZTSSe solar cell, and a CZTSSe solar cell having a buffer layer prepared according to the preparation method. Background Art

[0002] Copper zinc tin sulfur selenium (Cu2ZnSn(S x Se 1-x )4, referred to as CZTSSe) solar cells have the advantages of abundant raw material reserves, low cost, environmental friendliness, and good stability. It is one of the thin-film solar cells that has developed rapidly in recent years. As a pn junction semiconductor device, the structure of CZTSSe solar cells usually includes Mo / CZTSSe / cadmium sulfide (CdS) / zinc oxide / ITO / Al. At present, the device efficiency of CZTSSe solar cells has reached 13.8%, which is still far from the theoretical limit. This is mainly because it faces serious bulk and interface non-radiative recombination problems. The heterojunction interface of CZTSSe / CdS is an important place for the separation and transport of photogenerated carriers. Therefore, how to reduce the defect density at this interface is the key to further improving the performance of photovoltaic devices.

[0003] At present, the commonly used methods for preparing CZTSSe / CdS heterojunctions include chemical water bath deposition and magnetron sputtering. Compared with magnetron sputtering, the advantage of chemical water bath deposition is that it can conformally grow CdS thin films on the CZTSSe surface while avoiding sputtering damage. However, the CZTSSe / CdS heterojunction prepared by this method still has obvious interface lattice mismatch, excessive S loss of CdS, and insufficient coverage of CdS thin film, which leads to a large number of deep energy level defects and leakage channels at the interface, and reduces the open circuit voltage and fill factor of solar cells. Therefore, it is urgent to optimize the chemical water bath deposition process of the CdS buffer layer. Summary of the invention

[0004] In view of the above problems, the present invention is proposed to provide a method for preparing a buffer layer of a CZTSSe solar cell, which overcomes the above problems or at least partially solves the above problems, and a CZTSSe solar cell having a buffer layer prepared according to the preparation method.

[0005] An object of the present invention is to provide a method for preparing a buffer layer of a CZTSSe solar cell, which can eliminate deep energy level defects on the CZTSSe surface and reduce the defect density at the CZTSSe / CdS interface, thereby preparing a CdS film with high crystallinity and high uniformity.

[0006] A further object of the present invention is to improve the deposition rate and deposition uniformity of CdS and avoid the introduction of undesirable impurities.

[0007] Another object of the present invention is to further suppress the loss of S element in the CdS film during the chemical water bath deposition process.

[0008] According to one aspect of the present invention, a method for preparing a buffer layer of a CZTSSe solar cell is provided, comprising:

[0009] Immersing the CZTSSe film in a solution containing a cadmium salt of a first concentration while stirring, wherein the solution further contains an ammonia-ammonium salt buffer system and an alkali metal salt;

[0010] adding thiourea to the solution and allowing the thiourea to completely dissolve;

[0011] The solution is placed in a water bath environment at a specified temperature for chemical water bath deposition for a predetermined time to deposit a CdS film as a buffer layer on the surface of the CZTSSe film.

[0012] Optionally, the cation of the alkali metal salt comprises Li + 、Na + , K + , Rb + and Cs + One or more of .

[0013] Optionally, the anion of the alkali metal salt comprises CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of .

[0014] Optionally, the molar concentration of the alkali metal salt in the solution is 0.001-0.01 mol / L.

[0015] Optionally, the first concentration of the cadmium salt is 0.001-0.01 mol / L; and

[0016] The anion of the cadmium salt includes CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of .

[0017] Optionally, thiourea and Cd in the solution2+ The molar ratio is 5-50.

[0018] Optionally, the molar concentration of the aqueous ammonia in the solution is 0.1-1.0 mol / L.

[0019] Optionally, the anion of the ammonium salt comprises CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of; and

[0020] The molar concentration of the ammonium salt in the solution is 0.01-0.1 mol / L.

[0021] Optionally, the designated temperature is 65-90° C., and the predetermined time is 8-30 min.

[0022] According to another aspect of the present invention, a CZTSSe solar cell is provided, comprising a CZTSSe absorption layer and a CdS buffer layer on the CZTSSe absorption layer, wherein the CdS buffer layer is prepared according to the aforementioned method for preparing a buffer layer of a CZTSSe solar cell.

[0023] The preparation method of the buffer layer of the CZTSSe solar cell provided by the present invention introduces an alkali metal salt into the solution of chemical water bath deposition to assist in regulating the growth process of the CdS buffer layer. Alkali metal ions can not only eliminate the deep energy level defects on the surface of CZTSSe, but more importantly, alkali metals can promote the "ion-ion" CdS growth mode in the solution, and ultimately greatly reduce the defect density at the CZTSSe / CdS interface, so that a highly crystalline and highly uniform CdS film can be prepared. The method is simple to operate, and can solve the crystallinity and uniformity problems of large-area growth of CdS films, meet the needs of high-quality CZTSSe / CdS films, and are suitable for large-scale applications. It will greatly promote the industrialization process of CZTSSe solar cells.

[0024] Furthermore, in the method for preparing the buffer layer of the CZTSSe solar cell provided by the present invention, cadmium salts and alkali metal salts with good solubility are used, which is beneficial to improving the deposition rate and deposition uniformity of CdS and avoiding the introduction of undesirable impurities and harmful doping, thereby further ensuring the high quality of the CdS film.

[0025] Furthermore, in the method for preparing the buffer layer of the CZTSSe solar cell provided by the present invention, a preferred thiourea and Cd 2+The molar ratio of , thereby achieving a faster film deposition rate and taking into account large-area uniformity, while further inhibiting the loss of S element in the CdS film.

[0026] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention, it can be implemented according to the contents of the specification. In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are listed below.

[0027] Based on the following detailed description of specific embodiments of the present invention in conjunction with the accompanying drawings, those skilled in the art will become more aware of the above and other objects, advantages and features of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present invention. Moreover, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:

[0029] Figure 1 A schematic diagram showing a process of preparing a buffer layer of a CZTSSe solar cell according to an embodiment of the present invention;

[0030] Figure 2 is an X-ray photoelectron spectrum of Se element on the surface of CZTSSe provided by Example 1 of the present invention and the comparative example;

[0031] Figure 3 is a scanning electron microscope image of cadmium sulfide prepared in Example 1 of the present invention;

[0032] Figure 4 is a scanning electron microscope image of cadmium sulfide prepared in a comparative example;

[0033] Figure 5 1 is a Raman spectrum of cadmium sulfide prepared in Example 1 of the present invention and in the comparative example;

[0034] Figure 6 It is a trend diagram of the ratio of the S element to the Cd element in the cadmium sulfide provided in Example 1 of the present invention and the comparative example as a function of the chemical water bath deposition time. DETAILED DESCRIPTION

[0035] The exemplary embodiments of the present disclosure will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present disclosure are shown in the accompanying drawings, it should be understood that the present disclosure can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided to enable a more thorough understanding of the present disclosure and to fully convey the scope of the present disclosure to those skilled in the art.

[0036] In order to solve the technical problem of generating a large number of deep energy level defects and leakage channels at the heterojunction interface when CdS is deposited on the surface of a CZTSSe thin film using a chemical water bath deposition method, the present invention provides a method for preparing a buffer layer of a CZTSSe solar cell.

[0037] Figure 1 FIG. 1 is a schematic diagram showing a process of preparing a buffer layer of a CZTSSe solar cell according to an embodiment of the present invention. Figure 1 As shown, a method for preparing a buffer layer of a CZTSSe solar cell provided in an embodiment of the present invention comprises the following steps:

[0038] Step S1: immersing the CZTSSe thin film in a solution containing a cadmium salt of a first concentration while maintaining stirring, wherein the solution also contains an ammonia water-ammonium salt buffer system and an alkali metal salt.

[0039] Step S2: adding thiourea to the solution and dissolving the thiourea completely.

[0040] Step S3: placing the solution in a water bath environment at a specified temperature for chemical water bath deposition for a predetermined time to deposit a CdS film as a buffer layer on the surface of the CZTSSe film.

[0041] In step S3, a high temperature water bath is used for chemical water bath deposition. Specifically, the specified temperature of the water bath can be set to 65-90°C, such as 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C. The predetermined time for water bath deposition can be 8-30min, such as 10min, 13min, 15min, 17min, 20min, 22min, 25min, 27min, 29min, which can be determined according to the thickness of the deposited CdS film.

[0042] The inventors of this application have found through research that when CdS is deposited on the surface of CZTSSe thin film using chemical water bath deposition, a large number of interface defects often exist at the CZTSSe / CdS interface. The main reason is that there is a CdS film with poor lattice fit and coverage and low crystallinity at the interface. On the one hand, there are a large number of Se-Se bonds on the surface of untreated CZTSSe crystals, which produce deep energy level defects at the interface and are not conducive to the formation of CdS. 2+ On the other hand, thiourea spontaneously hydrolyzes into S 2- present in solution, which will promote Cd 2+ With S 2- Directly precipitate in the solution to form CdS nanoparticles, i.e., the "cluster-cluster" growth mode, and eventually make the CdS film deposited on the surface of CZTSSe full of holes and poor in crystal quality. After the introduction of alkali metal salts during the water bath deposition process, the alkali metal can use its strong bonding ability with Se to open the Se-Se bond on the surface of CZTSSe, and at the same time make the surface of CZTSSe produce more -2 valence Se, which is more conducive to the adsorption of Cd 2+ During the water bath deposition process, alkali metals can coordinate with thiourea, inhibiting the spontaneous hydrolysis reaction of thiourea, allowing thiourea to react more with Cd adsorbed on the surface of CZTSSe. 2+ Coordinate to form a metastable complex [Cd(OH)2SC(NH2)2] abs , that is, promoting the "ion-ion" CdS growth mode, so that a CdS film with high crystalline quality and high coverage can be formed in situ on the CZTSSe surface.

[0043] Therefore, the method for preparing the buffer layer of the CZTSSe solar cell provided by the embodiment of the present invention introduces an alkali metal salt into the solution of chemical water bath deposition to assist in regulating the growth process of the CdS buffer layer. Alkali metal ions can not only eliminate the deep energy level defects on the surface of CZTSSe, but more importantly, alkali metals can promote the "ion-ion" CdS growth mode in the solution, and ultimately greatly reduce the defect density at the CZTSSe / CdS interface, thereby being able to prepare a highly crystalline and highly uniform CdS film. The method is simple to operate, and can solve the problems of crystallinity and uniformity of large-area growth of CdS films, meet the needs of high-quality CZTSSe / CdS films, and are suitable for large-scale applications. It will greatly promote the industrialization process of CZTSSe solar cells.

[0044] In some embodiments of the present invention, before executing step S1, a step of preparing the solution for immersing the CZTSSe thin film may be performed. In a specific embodiment, an appropriate amount of cadmium salt and alkali metal salt may be added to a container containing deionized water, and stirred until they are completely dissolved, thereby obtaining a solution containing alkali metal salt and a first concentration of cadmium salt. Then, an appropriate amount of ammonia water and ammonium salt are added to the solution to form an ammonia water-ammonium salt buffer system, wherein after adding ammonia water and ammonium salt, attention is paid to keep stirring to avoid the generation of Cd(OH)2 precipitation.

[0045] In some embodiments of the present invention, after completing step S3, a post-processing step of the CdS film may be further included. Specifically, the CZTSSe film on which CdS is deposited obtained in step 3 is taken out, washed with deionized water, and dried.

[0046] In some embodiments of the present invention, cadmium salts with good solubility (specifically solubility in water) are preferably used, which is beneficial to improving the deposition rate and deposition uniformity of CdS and avoiding the introduction of impurity phases into the solution, thereby affecting the quality of the prepared CdS.

[0047] In a specific embodiment, the cation of the cadmium salt is Cd 2+ The anion of the cadmium salt may include, but is not limited to, CH3COO - (acetate ion), SO4 2- (sulfate ion), NO3 - (nitrate), Cl - (chloride ion), Br - (bromide ion), I - (iodide ion), F - (fluoride ion), etc.

[0048] In some embodiments, the first concentration of the cadmium salt in the solution is 0.001-0.01 mol / L, for example, 0.002 mol / L, 0.003 mol / L, 0.004 mol / L, 0.005 mol / L, 0.006 mol / L, 0.007 mol / L, 0.008 mol / L, 0.009 mol / L. This is conducive to obtaining a uniform CdS film.

[0049] In some preferred embodiments, the first concentration of the cadmium salt in the solution is 0.002-0.005 mol / L.

[0050] In some embodiments of the present invention, alkali metal salts with good solubility (specifically solubility in water) are preferably used. Due to their good solubility in aqueous solution, these alkali metal salts are not easily adsorbed onto the CdS layer and introduce harmful doping, thereby further ensuring the high quality of the CdS film.

[0051] In some specific embodiments, the cation of the alkali metal salt may include, but is not limited to, Li + (Li-ion), Na + (sodium ion), K + (potassium ion), Rb + (Rubidium ion), Cs + (cesium ion), etc.

[0052] In some specific embodiments, the anion of the alkali metal salt may include, but is not limited to, CH3COO - (acetate ion), SO4 2- (sulfate ion), NO3 - (nitrate), Cl - (chloride ion), Br - (bromide ion), I - (iodide ion), F - (fluoride ion), etc.

[0053] In some embodiments, the molar concentration of the alkali metal salt in the solution is 0.001-0.01 mol / L, for example, 0.002 mol / L, 0.003 mol / L, 0.004 mol / L, 0.005 mol / L, 0.006 mol / L, 0.007 mol / L, 0.008 mol / L, 0.009 mol / L. At this concentration, the alkali metal ions can form a coordination effect with most of the thiourea, thereby effectively inhibiting the spontaneous hydrolysis of the thiourea and facilitating the acquisition of a dense CdS film.

[0054] In some preferred embodiments, the molar concentration of the alkali metal salt in the solution is 0.02-0.05 mol / L.

[0055] In some embodiments of the present invention, the molar concentration of the ammonia water constituting the ammonia water-ammonium salt buffer system in the solution is 0.1-1.0 mol / L, thereby providing a suitable pH environment for CdS deposition.

[0056] In addition, in some embodiments of the present invention, an ammonia-ammonium salt buffer system is formed by using an ammonium salt with good solubility. The ammonium salt with good solubility can provide a continuous and stable concentration of NH4 +, thereby better stabilizing the pH of the solution. In a specific embodiment, the anion of the ammonium salt may include, but is not limited to, CH3COO - (acetate ion), SO4 2- (sulfate ion), NO3 - (nitrate), Cl - (chloride ion), Br - (bromide ion), I - (iodide ion), F - (fluoride ion), etc.

[0057] Accordingly, the molar concentration of the ammonium salt in the solution may be 0.01-0.1 mol / L, depending on the actual application conditions and the molar concentration of aqueous ammonia.

[0058] In some embodiments of the present invention, thiourea and Cd in solution 2+ The molar ratio of thiourea is 5-50, for example, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, 30, 31, 32, 33, 34, 35, 36, 37, 38, 39, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49. That is, the amount of thiourea used is much higher than that of thiourea and Cd. 2+ Theoretical molar dosage of the reaction. By using a relatively high concentration of thiourea, a faster film deposition rate can be achieved while taking into account large-area uniformity, while further suppressing the loss of S elements in the CdS film, thereby further improving the quality of the deposited CdS film.

[0059] In some preferred embodiments, thiourea and Cd in solution 2+ The molar ratio is 30-40.

[0060] Based on the same technical concept, an embodiment of the present invention further provides a CZTSSe solar cell. The CZTSSe solar cell includes a CZTSSe absorption layer and a CdS buffer layer on the CZTSSe absorption layer, wherein the CdS buffer layer is prepared according to the method for preparing a buffer layer of a CZTSSe solar cell described in any of the foregoing embodiments or combinations of the embodiments.

[0061] Those skilled in the art should be aware that CZTSSe solar cells can generally also include a back contact electrode (such as a Mo electrode), a window layer (such as a zinc oxide layer), a transparent conductive layer (such as an ITO layer), an Al electrode, etc. The structure of a CZTSSe solar cell should be well known to those skilled in the art, and in order not to obscure the key points of the present invention, it will not be described in detail herein.

[0062] The CZTSSe solar cell provided in an embodiment of the present invention adopts a CdS buffer layer prepared by the method for preparing a buffer layer of a CZTSSe solar cell according to the present invention. Compared with a CZTSSe solar cell with a CdS buffer layer prepared by the existing chemical water bath deposition technology, its open circuit voltage and fill factor are improved, and thus its photoelectric conversion efficiency is greatly improved.

[0063] The following is an explanation of the embodiments of the present invention by specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0064] Example 1

[0065] In this embodiment, the steps of preparing the CdS buffer layer include:

[0066] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0067] Step 2: weigh 0.06 g of CdSO4 and 0.06 g of RbCl, add them into water, and stir until completely dissolved;

[0068] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0069] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0070] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0071] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0072] Example 2

[0073] In this embodiment, the steps of preparing the CdS buffer layer include:

[0074] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0075] Step 2: weigh 0.06 g of CdSO4 and 0.03 g of NaCl, add them into water, and stir until completely dissolved;

[0076] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0077] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0078] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0079] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0080] Example 3

[0081] In this embodiment, the steps of preparing the CdS buffer layer include:

[0082] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0083] Step 2: weigh 0.06 g of CdSO4 and 0.09 g of CsCl, add them into water, and stir until completely dissolved;

[0084] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0085] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0086] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0087] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0088] Example 4

[0089] In this embodiment, the steps of preparing the CdS buffer layer include:

[0090] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0091] Step 2: weigh 0.06 g of CdSO4 and 0.06 g of RbF, add them into water, and stir until completely dissolved;

[0092] Step 3: Add 10 ml of ammonia water and 0.06 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0093] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0094] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0095] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0096] Example 5

[0097] In this embodiment, the steps of preparing the CdS buffer layer include:

[0098] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0099] Step 2: weigh 0.06 g of CdSO4 and 0.024 g of RbCl, add them into water, and stir until completely dissolved;

[0100] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0101] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0102] Step 5, placing the beaker in a 90° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 8 minutes and the deposition thickness is 50 nm;

[0103] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0104] Example 6

[0105] In this embodiment, the steps of preparing the CdS buffer layer include:

[0106] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0107] Step 2: weigh 0.06 g of CdSO4 and 0.24 g of RbCl, add them into water, and stir until completely dissolved;

[0108] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0109] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0110] Step 5, placing the beaker in a 65° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 25 minutes and the deposition thickness is 60 nm;

[0111] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0112] Example 7

[0113] In this embodiment, the steps of preparing the CdS buffer layer include:

[0114] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0115] Step 2: weigh 0.06 g of CdSO4 and 0.06 g of RbCl, add them into water, and stir until completely dissolved;

[0116] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0117] Step 4: Add 0.11 g of thiourea and stir until completely dissolved;

[0118] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0119] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0120] Example 8

[0121] In this embodiment, the steps of preparing the CdS buffer layer include:

[0122] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0123] Step 2: weigh 0.042 g of CdSO4 and 0.06 g of RbCl, add them into water, and stir until completely dissolved;

[0124] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0125] Step 4: Add 0.76 g of thiourea and stir until completely dissolved;

[0126] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0127] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0128] Comparative Example

[0129] In this comparative example, the steps for preparing the CdS buffer layer include:

[0130] Step 1: Add 200 ml of ultrapure water into a 500 ml beaker;

[0131] Step 2: weigh 0.06 g of CdSO4 and add it into water, stirring until it is completely dissolved;

[0132] Step 3: Add 10 ml of ammonia water and 0.12 g of NH4Cl, keep stirring to prevent Cd(OH)2 from precipitating, and immerse the CZTSSe film in the solution;

[0133] Step 4: Add 0.7 g of thiourea and stir until completely dissolved;

[0134] Step 5, placing the beaker in a 70° C. water bath for stirring and heating, and starting chemical water bath deposition, wherein the deposition time is 11 minutes and the deposition thickness is 50 nm;

[0135] Step six, take out the CZTSSe film grown with CdS, rinse it with deionized water, and then dry it.

[0136] from Figure 2 It can be seen that after alkali metal treatment, the characteristic peak of the X-ray photoelectron spectrum of Se element on the surface of CZTSSe shifts to the right, indicating that the chemical valence state of Se changes from 0 valence state to -2 valence state, proving that alkali metal successfully breaks the Se-Se bond on the surface of CZTSSe, that is, eliminates the deep energy level defects at the interface. Figure 3 and Figure 4 The comparison results show that compared with the comparative example, the surface of the CdS film obtained in Example 1 is more dense and has no pinholes. Figure 5 The results show that the Raman characteristic peak of CdS obtained in Example 1 is stronger than that of CdS in the comparative example, indicating that its crystallinity is also better. Figure 6 It can be seen that the introduction of alkali metals significantly inhibits the loss of S elements inside the CdS film, which is also beneficial to protecting the crystallinity of the CdS film.

[0137] Table 1 below lists the performance test data of CZTSSe solar cells assembled with CZTSSe thin films deposited with a CdS thin film buffer layer obtained in the aforementioned embodiments and comparative examples.

[0138] Table 1

[0139]

[0140] The test data in Table 1 show that compared with the CZTSSe solar cell using the CdS buffer layer of the comparative example, the open circuit voltage and fill factor of the CZTSSe solar cell using the CdS buffer layer prepared by the preparation method of the CZTSSe solar cell buffer layer according to the present invention are generally improved to varying degrees, and thus their photoelectric conversion efficiency is also greatly improved.

[0141] In summary, the method according to the embodiment of the present invention not only suppresses Se-related deep level defects on the CZTSSe surface, but also greatly improves the coverage and crystallinity of the CdS film, and ultimately greatly reduces the defects at the CZTSSe / CdS interface.

[0142] In the description provided herein, a large number of specific details are described. However, it is understood that embodiments of the present invention can be practiced without these specific details. In some instances, well-known methods, structures and techniques are not shown in detail so as not to obscure the understanding of this description.

[0143] At this point, those skilled in the art should recognize that, although multiple exemplary embodiments of the present invention have been shown and described in detail herein, many other variations or modifications that conform to the principles of the present invention can still be directly determined or derived based on the content disclosed in the present invention without departing from the spirit and scope of the present invention. Therefore, the scope of the present invention should be understood and recognized as covering all these other variations or modifications.

Claims

1. A method for preparing a buffer layer of a CZTSSe solar cell, characterized in that: include: Immersing the CZTSSe film in a solution containing a cadmium salt of a first concentration while stirring, wherein the solution further contains an ammonia-ammonium salt buffer system and an alkali metal salt; adding thiourea to the solution and allowing the thiourea to completely dissolve; The solution is placed in a water bath environment at a specified temperature for chemical water bath deposition for a predetermined time to deposit a CdS film as a buffer layer on the surface of the CZTSSe film.

2. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The cation of the alkali metal salt includes Li + 、Na + , K + , Rb + and Cs + One or more of .

3. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The anion of the alkali metal salt includes CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of .

4. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The molar concentration of the alkali metal salt in the solution is 0.001-0.01 mol / L.

5. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The first concentration of the cadmium salt is 0.001-0.01 mol / L; and The anion of the cadmium salt includes CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of .

6. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: Thiourea and Cd in the solution 2+ The molar ratio is 5-50.

7. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The molar concentration of the ammonia water in the solution is 0.1-1.0 mol / L.

8. The method for preparing a buffer layer of a CZTSSe solar cell according to claim 1, characterized in that: The anion of the ammonium salt includes CH3COO - 、SO4 2- 、NO3 - , Cl - Br - ,I - and F - One or more of; and The molar concentration of the ammonium salt in the solution is 0.01-0.1 mol / L.

9. The method for preparing a buffer layer of a CZTSSe solar cell according to any one of claims 1 to 8, characterized in that: The specified temperature is 65-90° C., and the predetermined time is 8-30 minutes.