Method for improving graphite boat marks
Through the combination of dry etching and deionized water cleaning, the safety hazards of graphite boat cleaning and the problems of defective products are solved, and the cleaning effect of graphite boat and the yield of battery cells are improved.
Patent Information
- Application Number
- CN202411002285.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, graphite boat cleaning has safety hazards and problems of defective products with block marking, resulting in low yield on the production line.
Using a combination of dry etching and deionized water cleaning, nitrogen trifluoride etching and argon etching, followed by overflow bubble treatment with deionized water, further intrinsic silicon plating boat is carried out to enhance the graphite boat cleaning effect.
Effectively reduce chemical consumption, enhance the cleaning degree of graphite boats, reduce electric field abnormalities, reduce the generation of EL bad card dot printing, and improve the yield of battery cells.
Smart Images

Figure CN118943242A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of semiconductor equipment technology, and in particular to a method for improving graphite boat printing. Background Art
[0002] Monocrystalline silicon solar cells are an important type of solar cell. They are made from high-purity monocrystalline silicon rods through a series of processes. The conventional preparation process of monocrystalline silicon solar cells is: texturing → diffusion → selective emitter (SE) laser doping → dephosphorized silicon glass (PSG) / polishing → annealing oxidation → PE-POLY coating → laser grooving → screen printing → sintering → testing. The graphite boat in the PE-POLY process needs to be cleaned regularly, otherwise it is easy to cause abnormal electric field during the process, causing poor EL (electroluminescence). In the process of cleaning the poly graphite boat, high concentration of nitric acid is required, which poses a safety hazard and increases the cost of waste liquid treatment. As the industry moves forward, dry cleaning boats have been gradually developed. This boat cleaning method can effectively reduce the amount of chemicals used and the cost of waste liquid treatment. However, after long-term use of dry cleaning boats, it is easy to cause abnormal discharge during the subsequent use of graphite boats, resulting in EL-poly card point printing of poor films and reducing the yield of the production line.
[0003] Therefore, there is an urgent need to improve a method for graphite boat printing to solve the safety hazards of graphite boat cleaning, avoid printing defective products at stuck points, and improve the yield of the production line. Summary of the invention
[0004] The purpose of the present application is to provide a method for improving graphite boat printing, which can solve the safety hazards of graphite boat cleaning, avoid printing defective products at stuck points, and improve the yield of the production line.
[0005] To solve the above problems, the technical solution adopted by the present invention is:
[0006] The present application provides a method for improving graphite boat printing, comprising the following steps:
[0007] S1, dry etching the graphite boat;
[0008] S2. Rinse the etched graphite boat with deionized water for 1-3 times, with the overflow bubbling time being 20-40 minutes each time.
[0009] In some embodiments of the present application, the above-mentioned dry etching includes the following steps: using nitrogen trifluoride as an etching gas, introducing nitrogen trifluoride into a reaction chamber, ionizing to generate plasma, and then cleaning.
[0010] In some embodiments of the present application, argon gas is also introduced during the dry etching, and the gas flow rate of argon gas is 270-630 sccm; the gas flow rate of nitrogen trifluoride is 3000-3700 sccm.
[0011] In some embodiments of the present application, the above-mentioned deionized water cleaning is specifically to place the etched graphite boat into a water washing tank, spray it for 5-15 minutes, drain the liquid, use water overflow bubbling treatment in the water washing tank for 20-40 minutes, and then dry it.
[0012] In some embodiments of the present application, after draining the liquid, the water capacity in the washing tank is 850-950L.
[0013] In some embodiments of the present application, the above also includes step S3: subjecting the cleaned graphite boat to intrinsic silicon plating.
[0014] In some embodiments of the present application, the intrinsic silicon plating boat comprises the following steps:
[0015] S31, placing the cleaned graphite boat into the boat under nitrogen conditions, and heating it to 440-460°C, reducing the N2 and temperature, evacuating and cooling it to 420-430°C, leak checking and evacuating again;
[0016] S32, pre-introducing N2 and SiH4 gases, reducing the pressure, and then performing deposition while keeping the gas flow rate and pressure constant, repeating the deposition 3-5 times;
[0017] S33, after the temperature treatment, N2 is introduced for cleaning, and then vacuum treatment is performed;
[0018] S34. Break the vacuum under N2 atmosphere, pressurization and temperature increase conditions, then reduce the N2 flow rate and exit the boat.
[0019] In some embodiments of the present application, the above-mentioned step S31 specifically includes placing the cleaned graphite boat into the boat under the conditions of 9000-11000Pa and N2 flow rate of 24000-26000L / min, and heating it to 440-460℃ for treatment for 2100-2300s, reducing the N2 flow rate to 9000-11000L / min, reducing the temperature to 430-440℃ for treatment for 1900-2100s, evacuating the vessel and cooling it to 420-430℃ for treatment for 750s-850s, checking for leaks and evacuating the vessel again.
[0020] In some embodiments of the present application, the above-mentioned step S32 specifically pre-introduces N2 and SiH4 gases, with N2 flow rate of 10000-10500L / min and SiH4 flow rate of 3000-3500L / min, and reduces the pressure to 3000-4500Pa for treatment for 55-65s, and then deposits for 750-850s at a power of 13000-14500W while keeping the gas flow rate and pressure unchanged, and repeats 3-5 times. During each deposition, pulse treatment is performed twice, and each pulse treatment is turned on for 30ms and off for 480ms.
[0021] In some embodiments of the present application, the above step S33 specifically comprises heating to 460-480°C, treating for 25-35s, introducing N2 for cleaning for 10-20s, with an N2 flow rate of 24000-26000L / min, and vacuuming for 25-35s.
[0022] Compared with the prior art, the invention of this application has at least the following advantages or beneficial effects:
[0023] The present application can effectively reduce chemical consumption by combining dry etching and deionized water cleaning on the one hand; on the other hand, after the dry cleaning of the boat, a water washing process is added to clean off the poly dust generated by the dry etching, thereby enhancing the cleaning degree of the graphite boat, thereby reducing the electric field anomaly caused by the boat being put into use online, further reducing the generation of EL bad card point printing, and improving the battery cell yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0025] Figure 1 This is a card point printing trend diagram of an embodiment of the present application. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the embodiments of the present application clearer, the technical scheme in the embodiments of the present application will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to the conventional conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0027] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present application will be described in detail below with reference to specific embodiments.
[0028] The present application provides a method for improving graphite boat printing, comprising the following steps:
[0029] S1, dry etching the graphite boat;
[0030] S2. Rinse the etched graphite boat with deionized water for 1-3 times, with the overflow bubbling time being 20-40 minutes each time.
[0031] This application combines dry etching and deionized water cleaning, which can effectively reduce chemical consumption on the one hand; on the other hand, after the dry cleaning of the boat, adding a water washing process can clean the poly dust generated by dry etching, enhance the cleaning degree of the graphite boat, and thus reduce the electric field anomaly caused by the boat being used online, further reduce the generation of EL bad card point printing, and improve the cell yield. In addition, the graphite boat is overflowed and bubbling for 20-40 minutes, which can improve the cleaning effect and the removal effect of poly dust.
[0032] In some embodiments of the present application, the above-mentioned dry etching includes the following steps: using nitrogen trifluoride as etching gas, introducing nitrogen trifluoride into the reaction chamber, the chamber pressure is 40-45mT, ionization generates plasma, and the dry etching treatment is 55-60s to achieve the purpose of cleaning and etching.
[0033] The poly silicon attached to the surface of the graphite boat blade and the graphite boat block can be effectively removed by dry etching to ensure the surface flatness.
[0034] In some embodiments of the present application, the above-mentioned deionized water cleaning is specifically to place the etched graphite boat into a water washing tank, spray it for 5-15 minutes, drain the liquid, use water overflow bubbling treatment in the water washing tank for 20-40 minutes, and then dry it.
[0035] In some embodiments of the present application, after draining the liquid, the water capacity in the washing tank is 850-950L.
[0036] In some embodiments of the present application, the above also includes step S3: subjecting the cleaned graphite boat to intrinsic silicon plating.
[0037] In some embodiments of the present application, the intrinsic silicon plating boat comprises the following steps:
[0038] S31, placing the cleaned graphite boat into the boat under nitrogen conditions, and heating it to 440-460°C, reducing the N2 and temperature, evacuating and cooling it to 420-430°C, leak checking and evacuating again;
[0039] S32, pre-introducing N2 and SiH4 gases, reducing the pressure, and then performing deposition while keeping the gas flow rate and pressure constant, repeating the deposition 3-5 times;
[0040] S33, after the temperature treatment, N2 is introduced for cleaning, and then vacuum treatment is performed;
[0041] S34. Break the vacuum under N2 atmosphere, pressurization and temperature increase conditions, then reduce the N2 flow rate and exit the boat.
[0042] In the intrinsic silicon boat plating step, N2 and SiH4 are used to discharge and deposit on the graphite boat surface under a plasma electric field, so that the coating has good insulation and the film layer is uniform and dense.
[0043] In some embodiments of the present application, the above-mentioned step S31 specifically includes placing the cleaned graphite boat into the boat under the conditions of 9000-11000Pa and N2 flow rate of 24000-26000L / min, and heating it to 440-460℃ for treatment for 2100-2300s, reducing the N2 flow rate to 9000-11000L / min, reducing the temperature to 430-440℃ for treatment for 1900-2100s, evacuating the vessel and cooling it to 420-430℃ for treatment for 750s-850s, checking for leaks and evacuating the vessel again.
[0044] Preferably, S31 is to put the cleaned graphite boat into the boat under the conditions of 10000Pa and N2 flow rate of 25000L / min, and heat it to 450℃ for 2200s, reduce the N2 flow rate to 10000L / min, reduce the temperature to 430-440℃ for 2000s, evacuate and reduce the temperature to 420-430℃ for 800s, check for leaks and evacuate again.
[0045] In some embodiments of the present application, the above-mentioned step S32 specifically pre-introduces N2 and SiH4 gases, with N2 flow rate of 10000-10500L / min and SiH4 flow rate of 3000-3500L / min, and reduces the pressure to 3000-4500Pa for treatment for 55-65s, and then deposits for 750-850s at a power of 13000-14500W while keeping the gas flow rate and pressure unchanged, and repeats 3-5 times. During each deposition, pulse treatment is performed twice, and each pulse treatment is turned on for 30ms and off for 480ms.
[0046] Preferably, step S32 is to pre-introduce N2 and SiH4 gases, with N2 flow rate of 10000-10500L / min and SiH4 flow rate of 3000-3500L / min, reduce the pressure to 3000-4500Pa and treat for 60s, then deposit for 800s at a power of 13000-14500W while keeping the gas flow rate and pressure unchanged, and repeat 3-5 times. During each deposition, pulse treatment is performed twice, with each pulse treatment being on for 30ms and off for 480ms.
[0047] More preferably, during the first deposition, the power is 1440 W, the pulse treatment is on for 30 ms and off for 480 ms; during the second deposition, the power is 13500 W, the pulse treatment is on for 30 ms and off for 480 ms; during the third deposition, the power is 13000 W, the pulse treatment is on for 30 ms and off for 480 ms.
[0048] In some embodiments of the present application, the above step S33 specifically comprises heating to 460-480°C, treating for 25-35s, introducing N2 for cleaning for 10-20s, with an N2 flow rate of 24000-26000L / min, and vacuuming for 25-35s.
[0049] Preferably, step S33 is to heat to 460-480°C, treat for 30 seconds, then introduce N2 for cleaning for 15 seconds, with an N2 flow rate of 25000L / min, and vacuum treat for 30 seconds.
[0050] In some embodiments of the present application, the above step S34 is specifically to break the vacuum for 110-130s under the conditions of N2 flow rate 45000-55000L / min, pressure 9000-11000Pa, and 460-480℃, and then reduce the N2 flow rate to 24000-2600L / min and exit the boat.
[0051] Preferably, step S34 is to break the vacuum for 120s under the conditions of N2 flow rate 50000L / min, pressure 10000Pa, and 460-480°C, then reduce the N2 flow rate to 25000L / min, and exit the boat.
[0052] The features and performance of the present application are further described in detail below in conjunction with the embodiments.
[0053] Example 1
[0054] A method for improving graphite boat printing, comprising the following steps:
[0055] S1, dry etching the graphite boat;
[0056] S2, washing the etched graphite boat with deionized water once, specifically, placing it in a water washing tank, spraying it for 5 minutes, draining the liquid, and then bubbling it with water overflow in the water washing tank for 20 minutes, and then drying it;
[0057] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0058] S31, put the cleaned graphite boat into the boat under the conditions of 10000Pa and N2 flow rate of 25000L / min, and heat it to 450℃ for 2200s, reduce the N2 flow rate to 10000L / min, reduce the temperature to 430-440℃ for 2000s, evacuate and reduce the temperature to 420℃ for 800s, check for leaks and evacuate again;
[0059] S32, pre-introduce N2 and SiH4 gas, N2 flow rate 10000L / min, SiH4 flow rate 3000L / min, reduce the pressure to 3000Pa for 60s, then deposit at a power of 13000W for 800s while keeping the gas flow rate and pressure unchanged, repeat 3 times;
[0060] S34, heating to 460°C, treating for 30 seconds, then introducing N2 for cleaning for 15 seconds, N2 flow rate 25000L / min, vacuum treatment for 30 seconds;
[0061] S35. Break the vacuum for 120 seconds at a N2 flow rate of 50,000 L / min, a pressure of 10,000 Pa, and 460°C, then reduce the N2 flow rate to 25,000 L / min and exit the boat.
[0062] Example 2
[0063] A method for improving graphite boat printing, comprising the following steps:
[0064] S1, dry etching the graphite boat;
[0065] S2. Wash the etched graphite boat with deionized water once, specifically, put it into a water washing tank, drain the liquid, and then treat it with overflow bubbling water in the water washing tank for 30 minutes, and then dry it;
[0066] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0067] S31, put the cleaned graphite boat into the boat under the conditions of 10000Pa and N2 flow rate of 25000L / min, and heat it to 450℃ for 2200s, reduce the N2 flow rate to 10000L / min, reduce the temperature to 430℃ for 2000s, evacuate and reduce the temperature to 420℃ for 800s, check for leaks and evacuate again;
[0068] S32, pre-introduce N2 and SiH4 gas, N2 flow rate 10000L / min, SiH4 flow rate 3000L / min, reduce the pressure to 3000Pa for 60s, then deposit at a power of 13000W for 800s while keeping the gas flow rate and pressure unchanged, repeat 3 times;
[0069] S34, heating to 460°C, treating for 30 seconds, then introducing N2 for cleaning for 15 seconds, N2 flow rate 25000L / min, vacuum treatment for 30 seconds;
[0070] S35. Break the vacuum for 120 seconds at a N2 flow rate of 50,000 L / min, a pressure of 10,000 Pa, and 460°C, then reduce the N2 flow rate to 25,000 L / min and exit the boat.
[0071] Example 3
[0072] This embodiment is basically the same as embodiment 2, except that the washing is performed twice and the spraying is performed for 10 minutes before washing.
[0073] A method for improving graphite boat printing, comprising the following steps:
[0074] S1, dry etching the graphite boat;
[0075] S2, washing the etched graphite boat with deionized water twice, specifically, placing it in a water washing tank, spraying it for 10 minutes, draining the liquid, and then bubbling it with water overflow in the water washing tank for 30 minutes, and then drying it;
[0076] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0077] S31, put the cleaned graphite boat into the boat under the conditions of 10000Pa and N2 flow rate of 25000L / min, and heat it to 450℃ for 2200s, reduce the N2 flow rate to 10000L / min, reduce the temperature to 430℃ for 2000s, evacuate and reduce the temperature to 420℃ for 800s, check for leaks and evacuate again;
[0078] S32, pre-introduce N2 and SiH4 gas, N2 flow rate 10000L / min, SiH4 flow rate 3000L / min, reduce the pressure to 3000Pa for 60s, then deposit at a power of 13000W for 800s while keeping the gas flow rate and pressure unchanged, repeat 3 times;
[0079] S34, heating to 460°C, treating for 30 seconds, then introducing N2 for cleaning for 15 seconds, N2 flow rate 25000L / min, vacuum treatment for 30 seconds;
[0080] S35. Break the vacuum for 120 seconds at a N2 flow rate of 50,000 L / min, a pressure of 10,000 Pa, and 460°C, then reduce the N2 flow rate to 25,000 L / min and exit the boat.
[0081] Example 4
[0082] This embodiment is basically the same as embodiment 2, except that the washing is performed 3 times and spraying is performed for 10 minutes before washing.
[0083] A method for improving graphite boat printing, comprising the following steps:
[0084] S1, dry etching the graphite boat;
[0085] S2, washing the etched graphite boat with deionized water for 3 times, specifically, placing it in a water washing tank, spraying it for 10 minutes, draining the liquid, and then bubbling it with water overflow in the water washing tank for 30 minutes, and then drying it;
[0086] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0087] S31, put the cleaned graphite boat into the boat under the conditions of 10000Pa and N2 flow rate of 25000L / min, and heat it to 450℃ for 2200s, reduce the N2 flow rate to 10000L / min, reduce the temperature to 430℃ for 2000s, evacuate and reduce the temperature to 420℃ for 800s, check for leaks and evacuate again;
[0088] S32, pre-introduce N2 and SiH4 gas, N2 flow rate 10000L / min, SiH4 flow rate 3000L / min, reduce the pressure to 3000Pa for 60s, then deposit at a power of 13000W for 800s while keeping the gas flow rate and pressure unchanged, repeat 3 times;
[0089] S34, heating to 460°C, treating for 30 seconds, then introducing N2 for cleaning for 15 seconds, N2 flow rate 25000L / min, vacuum treatment for 30 seconds;
[0090] S35. Break the vacuum for 120 seconds at a N2 flow rate of 50,000 L / min, a pressure of 10,000 Pa, and 460°C, then reduce the N2 flow rate to 25,000 L / min and exit the boat.
[0091] Example 5
[0092] A method for improving graphite boat printing, comprising the following steps:
[0093] S1, dry etching the graphite boat;
[0094] S2. Wash the etched graphite boat with deionized water once, specifically, put it into a water washing tank, drain the liquid, and then treat it with overflow bubbling water in the water washing tank for 30 minutes, and then dry it;
[0095] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0096] S31, put the cleaned graphite boat into the boat under the conditions of 9000Pa and N2 flow rate of 24000L / min, and heat it to 440℃ for 2100s, reduce the N2 flow rate to 9000L / min, reduce the temperature to 435℃ for 1900s, evacuate and reduce the temperature to 430℃ for 750s, check for leaks and evacuate again;
[0097] S32, pre-introducing N2 and SiH4 gas, N2 flow rate 10500L / min, SiH4 flow rate 3300L / min, reducing the pressure to 3200Pa for 55s, then keeping the gas flow rate and pressure unchanged, depositing for 850s at a power of 14500W for the first time, 850s at a power of 13500W for the second time, and 850s at a power of 13000W for the third time. During each deposition, pulse treatment was performed twice, each pulse treatment was on for 30ms and off for 480ms;
[0098] S34, heating to 470°C, treating for 25 seconds, then introducing N2 for cleaning for 10 seconds, N2 flow rate 24000L / min, vacuum treatment for 25 seconds;
[0099] S35. Break the vacuum for 110 seconds at a N2 flow rate of 45,000 L / min, a pressure of 9,000 Pa, and 470°C, then reduce the N2 flow rate to 24,000 L / min and exit the boat.
[0100] Example 6
[0101] A method for improving graphite boat printing, comprising the following steps:
[0102] S1, dry etching the graphite boat;
[0103] S2. Wash the etched graphite boat with deionized water once, specifically, put it into a water washing tank, drain the liquid, and then treat it with overflow bubbling water in the water washing tank for 30 minutes, and then dry it;
[0104] S3: Plating the cleaned graphite boat with intrinsic silicon:
[0105] S31, put the cleaned graphite boat into the boat under the conditions of 11000Pa and N2 flow rate of 26000L / min, and heat it to 460℃ for 2300s, reduce the N2 flow rate to 11000L / min, reduce the temperature to 440℃ for 2100s, evacuate and reduce the temperature to 430℃ for 850s, check for leaks and evacuate again;
[0106] S32, pre-introducing N2 and SiH4 gases, with N2 flow rate of 10400L / min and SiH4 flow rate of 3500L / min, reducing the pressure to 3500Pa for 65s, then keeping the gas flow rate and pressure unchanged, depositing for 750s at a power of 14500W for the first time, 750s at a power of 13500W for the second time, and 750s at a power of 13000W for the third time. During each deposition, pulse treatment was performed twice, with each pulse treatment on for 30ms and off for 480ms;
[0107] S34, heating to 480°C, treating for 35 seconds, then introducing N2 for cleaning for 20 seconds, N2 flow rate 26000L / min, vacuum treatment for 35 seconds;
[0108] S35. Break the vacuum for 130 seconds at a N2 flow rate of 55,000 L / min, a pressure of 11,000 Pa, and 480°C, then reduce the N2 flow rate to 26,000 L / min and exit the boat.
[0109] Comparative Example 1
[0110] This comparative example is basically the same as Example 2, except that the graphite boat after etching is not cleaned with deionized water.
[0111] Figure 1 The middle ordinate is the graphite boat printing defective rate, and the abscissa is time. The method of comparative example 1 was used for processing from the daytime of June 1 to the night of June 2; from the daytime of June 3 to the night of June 15, the method of embodiment 2 was used for processing. By comparison, it can be seen that after using the method of embodiment 2, the graphite boat printing defective rate was significantly reduced.
[0112] Comparative Example 2
[0113] This comparative example is basically the same as Example 5, except that only the first deposition is performed.
[0114] Comparative Example 3
[0115] This comparative example is basically the same as Example 5, except that the three deposition powers are 13000W.
[0116] Experimental example
[0117] The boats of Examples 2-3 and Comparative Example 1 were produced on the same production line and in the same path, specifically following the following path: texturing → boron diffusion → back polishing → PE-POLY coating → annealing → RCA → ALD → front coating → back coating → screen printing → sintering → testing. The above paths are all referenced to the prior art. The electrical performance and EL card point data were tracked, and the experimental results are shown in Table 1-2.
[0118] Table 1
[0119]
[0120]
[0121] Referring to Table 1, the electrical performance results show that adding a water wash procedure after dry cleaning the boat can effectively improve the boat cleaning degree, optimize the poly silicon deposition rate of the boat, and thus improve FF; and by comparing Example 5 with Comparative Examples 2-3, it can be seen that deposition twice under corresponding conditions can improve electrical performance.
[0122] Table 2
[0123] Sample Test volume EL card points Proportion Example 2 1756 31 1.77% Example 3 1796 17 0.95% Example 5 1788 16 0.89% Comparative Example 1 1776 74 4.17% Comparative Example 2 1753 34 1.93% Comparative Example 3 1772 19 1.07%
[0124] Referring to Table 2, the EL results show that adding a water washing procedure after the dry cleaning of the boat can further remove the residual poly dust on the boat page, reduce the abnormal frequency of discharge at the graphite boat card point, and effectively reduce the EL card point printing defects; and two depositions at the corresponding power are most effective in reducing the abnormal frequency of discharge at the graphite boat card point.
[0125] In summary, the present application can effectively reduce chemical consumption by combining dry etching and deionized water cleaning. On the other hand, after the dry cleaning of the boat, adding a water washing process can clean the poly dust generated by dry etching, enhance the cleaning degree of the graphite boat, and thus reduce the electric field anomaly caused by the boat being used online, further reduce the generation of EL bad card point printing, and improve the cell yield. In addition, the overflow bubbling treatment of the graphite boat for 20-40 minutes can improve the cleaning effect and improve the removal effect of poly dust.
[0126] The embodiments described above are part of the embodiments of the present application, rather than all of the embodiments. The detailed description of the embodiments of the present application is not intended to limit the scope of the present application for protection, but merely represents the selected embodiments of the present application. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
Claims
1. A method for improving graphite boat printing, characterized in that: The steps include: S1, dry etching the graphite boat; S2. Rinse the etched graphite boat with deionized water for 1-3 times, with the overflow bubbling time being 20-40 minutes each time.
2. A method for improving graphite boat printing according to claim 1, characterized in that: The dry etching comprises the following steps: using nitrogen trifluoride as etching gas, introducing nitrogen trifluoride into a reaction chamber, ionizing to generate plasma, and then cleaning.
3. A method for improving graphite boat printing according to claim 2, characterized in that: During the dry etching, argon gas is also introduced, and the gas flow rate of argon gas is 270-630 sccm; the gas flow rate of nitrogen trifluoride is 3000-3700 sccm.
4. A method for improving graphite boat printing according to claim 1, characterized in that: The deionized water cleaning is specifically to put the etched graphite boat into a water washing tank, spray it for 5-15 minutes, drain the liquid, and then use water overflow bubbling treatment in the water washing tank for 20-40 minutes, and then dry it.
5. A method for improving graphite boat printing according to claim 3, characterized in that: After draining the liquid, the water capacity in the washing tank is 850-950L.
6. A method for improving graphite boat printing according to claim 1, characterized in that: The step S3 is also included: the cleaned graphite boat is subjected to intrinsic silicon plating.
7. A method for improving graphite boat printing according to claim 6, characterized in that: The intrinsic silicon plating boat comprises the following steps: S31, placing the cleaned graphite boat into the boat under nitrogen conditions, and heating it to 440-460°C, reducing the N2 and temperature, evacuating and cooling it to 420-430°C, leak checking and evacuating again; S32, pre-introducing N2 and SiH4 gases, reducing the pressure, and then performing deposition while keeping the gas flow rate and pressure constant, repeating the deposition 3-5 times; S33, after the temperature treatment, N2 is introduced for cleaning, and then vacuum treatment is performed; S34. Break the vacuum under N2 atmosphere, pressurization and temperature increase conditions, then reduce the N2 flow rate and exit the boat.
8. A method for improving graphite boat printing according to claim 7, characterized in that: The step S31 specifically includes placing the cleaned graphite boat into the boat under the conditions of 9000-11000Pa and N2 flow rate of 24000-26000L / min, heating it to 440-460°C for 2100-2300s, reducing the N2 flow rate to 9000-11000L / min, reducing the temperature to 430-440°C for 1900-2100s, evacuating the boat and reducing the temperature to 420-430°C for 750s, checking for leaks and evacuating the boat again.
9. A method for improving graphite boat printing according to claim 7, characterized in that: The step S32 specifically involves pre-introducing N2 and SiH4 gases, with N2 flow rate of 10000-10500L / min and SiH4 flow rate of 3000-3500L / min, reducing the pressure to 3000-4500Pa and treating for 55-65s, then depositing for 750-850s at a power of 13000-14500W while keeping the gas flow rate and pressure unchanged, and repeating 3-5 times. During each deposition, pulse treatment is performed twice, with each pulse treatment being on for 30ms and off for 480ms.
10. A method for improving graphite boat printing according to claim 7, characterized in that: The step S33 specifically comprises heating to 460-480° C., treating for 25-35 seconds, introducing N2 for cleaning for 10-20 seconds, with an N2 flow rate of 24000-26000 L / min, and vacuuming for 25-35 seconds.