Negative pole piece, secondary battery and electric device
By setting an acute angle opening in the film layer of the negative electrode sheet, the problem of insufficient electrolyte infiltration caused by expansion of the negative electrode sheet of the battery is solved, and the cycle life and safety performance of the battery are improved.
Patent Information
- Application Number
- CN202310530900.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-05-11
AI Technical Summary
During the charging and discharging of the battery, the expansion of the negative electrode sheet leads to insufficient infiltration of the electrolyte, which affects the cycle life and safety performance.
The opening is provided in the membrane layer of the negative electrode sheet. The angle between the axis of the opening and the lower surface of the membrane layer is an acute angle, providing an embedded and disengagement channel for active ions, reducing internal resistance and polarization losses, and increasing the elasticity of the electrode sheet. , alleviate the expansion problem.
It improves the wetting and capacity performance of the electrolyte in the negative electrode sheet, extends the cycle life of the battery, and improves safety performance and utilization.
Smart Images

Figure CN118943280A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of battery technology, and in particular to a negative electrode plate, a secondary battery and an electrical device. Background Art
[0002] With the rapid development of the battery field, the application scope of batteries is becoming more and more extensive. For example, they are used in energy storage power systems such as hydropower, thermal power, wind power and solar power stations, as well as power tools, electric bicycles, electric motorcycles, electric vehicles, military equipment, aerospace and other fields. At the same time, higher requirements are also put forward for the energy density, cycle performance and safety performance of batteries. Among them, during the use of the battery, the negative electrode plate will expand, thereby affecting the infiltration of the electrolyte, and thus affecting the cycle life and safety performance of the battery. Summary of the invention
[0003] The present application is made in view of the above-mentioned problems, and its purpose is to provide a negative electrode plate, a secondary battery and an electrical device. The negative electrode plate can be used in a battery to improve the cycle life and safety performance of the battery.
[0004] A first aspect of the present application provides a negative electrode plate, which includes: a current collector and a film layer arranged on at least one side of the current collector, wherein the film layer is provided with a plurality of openings, and an angle θ between the axis of the opening and the lower surface of the film layer satisfies: 0°<θ<90°, and the lower surface of the film layer is a surface of the film layer close to the current collector.
[0005] In the embodiment of the present application, by setting an opening in the film layer of the negative electrode plate, a channel can be provided for the embedding and extraction of active ions, which can reduce internal resistance, reduce polarization loss, and help improve the infiltration and capacity performance of the electrolyte in the negative electrode plate; at the same time, it can also increase the elasticity of the negative electrode plate and slow down the expansion of the negative electrode plate, which is beneficial to extend the cycle life of the battery and improve the utilization rate of the battery; in addition, the angle between the opening and the lower surface of the film layer is set to an acute angle, which can slow down the expansion of the negative electrode plate along the thickness direction of the film layer, which is beneficial to reduce the expansion of the negative electrode plate and the polarization caused by stress during the charge and discharge process, thereby improving the safety, quality assurance performance and cycle life of the battery.
[0006] In combination with the first aspect, in a possible implementation manner, θ satisfies: 20°≤θ≤70°, optionally, θ satisfies: 30°≤θ≤60°.
[0007] Based on the above embodiments, the angle between the axis of the opening and the lower surface of the membrane layer is within a suitable range, which can ensure the structural stability of the negative electrode plate while taking into account the improvement of the electrolyte infiltration problem in the negative electrode plate and the expansion problem of the negative electrode plate.
[0008] In combination with the first aspect, in a possible embodiment, there is a partial film layer between one end of the opening close to the current collector and the surface of the current collector. That is, the depth of the opening is less than the thickness of the film layer, which can be understood as the opening being a closed hole. In the case where the opening is a closed hole, the contact area between the film layer and the surface of the current collector is larger than that of the through hole. Therefore, the film layer with closed holes has a greater bonding force with the current collector than the film layer with through holes, which can reduce the risk of peeling of the film layer.
[0009] In combination with the first aspect, in another possible implementation, the opening includes a through hole that penetrates the membrane layer. Based on this embodiment, the provision of the through hole is conducive to the embedding and extraction of active ions, which can further reduce the internal resistance and polarization loss; in addition, compared with the closed hole, the through hole can slow down the expansion of the negative electrode sheet. In summary, the through hole can further extend the cycle life of the battery and improve the utilization rate of the secondary battery.
[0010] In combination with the first aspect, in a possible implementation, the aperture of the end of the opening close to the current collector is a first aperture, the aperture of the end of the opening away from the current collector is a second aperture, and the first aperture is smaller than the second aperture.
[0011] Based on the above embodiment, the first aperture at one end close to the current collector is smaller, and the second aperture at the end away from the current collector is larger, which is beneficial to reducing the extreme difference in active ion concentration between the surface and the interior of the negative electrode plate, thereby further improving the utilization rate of the secondary battery; when the opening is a through hole, the above aperture is set to facilitate the embedding and release of active ions while improving the bonding force between the membrane layer and the current collector.
[0012] In combination with the first aspect, in a possible implementation, the first aperture D1 satisfies 10 μm≤D1≤60 μm, and / or the second aperture D2 satisfies: 40 μm≤D2≤120 μm. Optionally, 0.25≤D1 / D2<1.
[0013] Optionally, 30 μm≤D1≤60 μm, and / or 60 μm≤D2≤120 μm. Optionally, 0.25≤D1 / D2≤0.5.
[0014] Based on the above embodiment, setting the first pore size and the second pore size within the above appropriate range can take into account both the improvement of the electrolyte infiltration problem in the negative electrode plate and the improvement of the bonding force between the membrane layer and the current collector.
[0015] In combination with the first aspect, in a possible implementation manner, the aperture of the opening gradually increases from a first aperture to a second aperture from an end close to the current collector to an end far from the current collector.
[0016] In combination with the first aspect, in a possible embodiment, on a plane parallel to the film layer, the spacing between adjacent openings includes a first spacing d1, and / or a second spacing d2, and / or a third spacing d3, wherein the first spacing d1 satisfies 800μm≥d1≥173μm, the second spacing d2 satisfies 500μm≥d2≥100μm, and the third spacing d3 satisfies 500μm≥d3≥100μm; optionally, 433μm≥d1≥260μm, 250μm≥d2≥150μm, and 250μm≥d3≥150μm.
[0017] Based on the above embodiment, the first distance d1, the second distance d2 and the third distance d3 are set within the above appropriate range, so that the difficulty of electrolyte infiltration in the negative electrode plate can be effectively reduced.
[0018] In combination with the first aspect, in a possible embodiment, the first spacing is the spacing between adjacent openings in the first direction, the second spacing is the spacing between adjacent openings in the second direction, and the third spacing is the spacing between adjacent openings in the third direction, wherein the first direction is perpendicular to the second direction, and the third direction intersects with the first direction and the second direction respectively.
[0019] Based on the above embodiments, the pore spacing is controlled in multiple directions, which can better ensure the uniformity of pore distribution, thereby further alleviating the uneven embedding of active ions caused by uneven pore spacing.
[0020] In combination with the first aspect, in a possible embodiment, the membrane layer includes a first membrane layer and a second membrane layer, the first membrane layer is arranged on the surface of the current collector, and the second membrane layer is arranged on the surface of the first membrane layer away from the current collector, and the opening includes a first opening arranged in the first membrane layer and a second opening arranged in the second membrane layer, wherein the pore size of the first opening is smaller than the pore size of the second opening.
[0021] In combination with the first aspect, in a possible implementation manner, the membrane layer includes an active material layer disposed on a surface of the current collector.
[0022] In combination with the first aspect, in a possible embodiment, the membrane layer includes an active material layer and a conductive polymer layer, the number of layers of the active material layer and the conductive polymer layer are both multi-layer, the multi-layer active material layer and the multi-layer conductive polymer layer are stacked on each other, and the outermost layer away from the current collector is the conductive polymer layer.
[0023] The second aspect of the present application provides a secondary battery, comprising the negative electrode sheet in any embodiment of the first aspect of the present application. Optionally, the battery can be a battery or a battery cell.
[0024] A third aspect of the present application provides an electrical device, comprising a secondary battery in any embodiment of the second aspect of the present application, wherein the secondary battery is used to supply power to the electrical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the following briefly introduces the drawings required for use in the embodiments of the present application. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on the drawings without creative work. In the drawings, the drawings are not drawn according to the actual scale.
[0026] Figure 1 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application;
[0027] Figure 2 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application;
[0028] Figure 3 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application;
[0029] Figure 4 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application;
[0030] Figure 5 is a schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application;
[0031] Figure 6 is a schematic top view of a negative electrode sheet according to an embodiment of the present application;
[0032] Figure 7 is a schematic diagram of a secondary battery according to an embodiment of the present application;
[0033] Figure 8 is an exploded view of a secondary battery according to an embodiment of the present application;
[0034] Fig. 9 is a schematic diagram of a battery module according to an embodiment of the present application;
[0035] Fig.10 is a schematic diagram of a battery pack according to an embodiment of the present application;
[0036] Fig.11 is an exploded view of a battery pack according to an embodiment of the present application;
[0037] Fig.12 It is a schematic diagram of an electrical device according to an embodiment of the present application. DETAILED DESCRIPTION
[0038] Below, the embodiments of the negative electrode plate, secondary battery and electric device of the present application are specifically disclosed in detail with appropriate reference to the drawings. However, there may be cases where unnecessary detailed descriptions are omitted. For example, there are cases where detailed descriptions of well-known matters and repeated descriptions of actually the same structure are omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate the understanding of those skilled in the art. In addition, the drawings and the following descriptions are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0039] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0040] If not otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0041] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0042] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0043] At present, secondary batteries have been widely used in various fields. In secondary batteries, the battery cell usually includes a shell, an electrode assembly and an electrolyte solution. The electrode assembly and the electrolyte solution are both contained in the shell. The electrode assembly usually includes a positive electrode sheet, a negative electrode sheet and a separator between the positive electrode sheet and the negative electrode sheet. When the battery is charged, active ions, such as lithium ions, sodium ions, magnesium ions, etc., are deintercalated from the positive electrode and then re-intercalated into the negative electrode through the separator.
[0044] During the charge and discharge process of a secondary battery, active ions can be in a state of movement from positive electrode → negative electrode → positive electrode. When charging a secondary battery, active ions are generated on the positive electrode of the secondary battery, and the generated active ions can move to the negative electrode through the electrolyte. The active ions that reach the negative electrode are embedded in the negative electrode. The more active ions are embedded in the negative electrode, the higher the charging capacity. When the secondary battery is discharged (for example, when using the secondary battery to discharge an electrical device), the active ions embedded in the negative electrode can escape and move back to the positive electrode.
[0045] In the electrochemical reaction of the secondary battery, due to the structural changes of the electrode active material during the deintercalation of the active ions, the side reactions of the active materials and other factors, the negative electrode of the battery will expand during the cycle. Due to various factors such as ion dynamics and battery energy density, the spacing between the positive electrode and the negative electrode is very small, which is usually not enough to accommodate the expansion of the electrode active material or structural damage. Therefore, the electrolyte, especially the liquid electrolyte, will be squeezed out between the positive and negative electrode sheets, affecting the infiltration of the electrolyte, so that there is not enough electrolyte for ion conduction between the positive and negative electrode sheets, and the battery will be severely polarized, which greatly affects the cycle performance and service life of the battery. If the expansion force generated cannot be effectively released, it will greatly deteriorate the performance of the battery cell, and even damage the electrode sheet and cause the battery to short-circuit, causing safety hazards. Especially in the wound electrode assembly, the electrode sheet is wound into a cylindrical electrode assembly, and the middle area of the electrode sheet forms the middle part of the electrode assembly after winding. Due to structural reasons, it is difficult to infiltrate the middle part of the cylindrical electrode assembly, and the stored electrolyte is limited.
[0046] In view of this, the embodiment of the present application provides a negative electrode plate, a secondary battery and an electric device. Among them, an opening is set in the film layer of the negative electrode plate, and the angle between the axis of the opening of the film layer in the negative electrode plate and the lower surface of the film layer is an acute angle. The opening can provide a channel for the embedding and extraction of active ions, thereby effectively improving the infiltration and capacity performance of the electrolyte in the negative electrode plate, and alleviating the problems of insufficient electrolyte infiltration and surface lithium precipitation; the angle between the axis and the lower surface of the film layer is an acute angle, which can increase the elasticity of the electrode plate, slow down the expansion of the electrode plate along the thickness direction of the film layer, and is conducive to reducing the polarization caused by the expansion of the electrode plate and stress during the charging and discharging process, thereby improving the safety quality assurance performance and cycle life of the battery. It should be understood that lithium-ion batteries are only an example of secondary batteries, and the secondary batteries described in this application can also be sodium-ion batteries, potassium-ion batteries, magnesium-ion batteries, etc.
[0047] [Negative electrode]
[0048] An embodiment of the present application provides a negative electrode plate, which includes: a current collector and a film layer arranged on at least one side of the current collector, wherein the film layer is provided with a plurality of openings, and an angle θ between the axis of the opening and a surface of the film layer close to the current collector satisfies: 0°<θ<90°.
[0049] The opening may be along the thickness direction of the film layer, and the axis is a line passing through the geometric center of the opening along the thickness direction of the film layer. The surface of the film layer close to the current collector may be referred to as the lower surface of the film layer. There is an angle between the above axis and the lower surface of the film layer, and θ is the smaller angle between the axis and the lower surface of the film layer.
[0050] θ satisfies 0°<θ<90°, in other words, the angle between the axis of the opening and the lower surface of the film layer is an acute angle. For example, the cross section of the opening can be circular, nearly circular, polygonal, etc.
[0051] Figure 1 Schematic cross-sectional view of a negative electrode sheet of an embodiment of the present application. Figure 1 As shown, Figure 1 It is a cross-sectional view of the negative electrode plate along the thickness direction, and the z direction is the thickness direction of the film layer. The negative electrode plate 100 of an embodiment of the present application includes a current collector 110 and a film layer 120, wherein the film layer 120 is arranged on the upper surface of the current collector 110, wherein an opening 121 is arranged in the film layer 120, and the angle θ between the axis of the opening 121 and the surface of the current collector 110 satisfies: 0°<θ<90°, in other words, the angle between the axis of the opening 121 and the surface of the current collector 110 is an acute angle. Exemplarily, θ can be 20°, 30°, 45°, 60°, 70°, 85°, and a range value between any two of the above.
[0052] Figure 2This is a schematic cross-sectional view of a negative electrode sheet according to another embodiment of the present application. Figure 2 The angle between the axis of the middle opening 121 and the surface of the current collector 110 is 90°, that is, a right angle.
[0053] In the embodiment of the present application, an opening is provided in the film layer of the negative electrode plate, and the angle between the axis of the opening of the film layer in the negative electrode plate and the lower surface of the film layer is an acute angle. The opening can provide a channel for the embedding and extraction of active ions, thereby effectively improving the infiltration and capacity performance of the electrolyte in the negative electrode plate, and alleviating the problems of insufficient electrolyte infiltration and surface lithium precipitation; in addition, in the negative electrode plate, the film layer usually expands along the thickness direction of the film layer and the plane direction of the film layer, that is, expansion in the vertical direction and expansion in the horizontal direction. When the angle between the axis of the opening and the lower surface of the film layer is an acute angle, for example Figure 1 The opening in the film can relieve the expansion of the film in both the horizontal and vertical directions. When the angle between the axis of the opening and the lower surface of the film is 90°, Figure 2 The opening shown in the figure can only alleviate the expansion of the film layer in the horizontal direction. It can be seen that when the angle between the axis of the opening and the lower surface of the film layer is an acute angle, the expansion of the film layer in the horizontal direction and the vertical direction can be alleviated at the same time, thereby further alleviating the expansion of the negative electrode sheet, which is beneficial to reduce the polarization caused by the expansion of the negative electrode sheet during the charge and discharge process, thereby improving the safety quality assurance performance and cycle life.
[0054] Optionally, in some embodiments, the angle θ between the axis of the opening and the lower surface of the film layer satisfies 20°≤θ≤70°. Optionally, in some embodiments, θ satisfies 30°≤θ≤60°. In this way, the angle between the axis of the opening and the lower surface of the film layer is in a suitable range, which can ensure the structural stability of the electrode while taking into account the improvement of the electrolyte infiltration problem in the electrode and the electrode expansion problem.
[0055] Optionally, in some embodiments, the angle θ between the axis of the opening and the lower surface of the film layer can be 45°. When the angle between the axis of the opening and the lower surface of the film layer is 45°, the greatest balance can be achieved between the structural stability of the negative electrode plate and the improvement of the electrolyte infiltration problem in the plate and the plate expansion problem.
[0056] Optionally, in some embodiments of the present application, a portion of or all of the openings may have a partial film layer between one end of the current collector and the current collector surface. It can be understood that the depth of the opening is less than the thickness of the film layer, that is, the openings on the film layer may be closed holes.
[0057] Figure 3 Schematic cross-sectional view of a negative electrode sheet of an embodiment of the present application. Figure 5As shown, the depth of the opening 121 is less than the thickness of the film layer, that is, Figure 3 The open cells shown are closed cells.
[0058] When the opening is a closed hole, the contact area between the membrane layer and the current collector surface is larger than that of the through hole. Therefore, the membrane layer with closed holes has a greater bonding force with the current collector than that with through holes, which can reduce the risk of membrane layer peeling.
[0059] Optionally, in some embodiments of the present application, the openings of the film layer may include through holes that penetrate the film layer. Figure 1 The opening shown is a through hole. The through hole can also be called a collector through hole, which can be understood as the through hole being able to directly reach the surface of the collector. The setting of the through hole is conducive to the embedding and extraction of active ions, which can further reduce the internal resistance and polarization loss; in addition, compared with the closed hole, the through hole can slow down the expansion of the pole piece. In summary, the through hole can further extend the cycle life of the secondary battery and improve the utilization rate of the secondary battery.
[0060] Different active materials have different expansion forces, and thus different membrane layers of active materials also have different expansion forces. When the expansion force of the active material in the membrane layer is small, the expansion force of the membrane layer is also small, and closed cells can be used; when the expansion force of the active material in the membrane layer is large, the expansion force of the membrane layer is also large, and through holes can be used.
[0061] Optionally, in some embodiments of the present application, closed pores may be provided in the film layer with a relatively small expansion force. For some film layers with a relatively small expansion force, for example, when the expansion force of the active material in the film layer is not particularly large, closed pores may be provided to help increase the bonding force between the film layer and the current collector, thereby reducing the risk of peeling of the film layer.
[0062] Optionally, in some embodiments of the present application, through holes can be provided in the film layer with greater expansion force. For some film layers with greater expansion force, for example, when the expansion force of the active material in the film layer is relatively large, the first thing to improve is the expansion problem of the pole piece. Since the depth of the opening has a relatively large impact on the expansion problem, in this case, through holes can be used, which can provide a greater degree of relief for the expansion problem.
[0063] Optionally, in some embodiments of the present application, the aperture of the opening in the film layer may vary along the thickness direction of the film layer. Specifically, in some embodiments of the present application, the aperture of the end of the opening in the film layer close to the current collector is a first aperture, and the aperture of the end of the opening away from the current collector is a second aperture, and the first aperture may be set to be smaller than the second aperture.
[0064] Based on the above embodiment, the first aperture at one end close to the current collector is smaller, and the second aperture at the end away from the current collector is larger, which can reduce the extreme difference in active ion concentration between the surface and the interior of the electrode, thereby further improving the utilization rate of the secondary battery; when the opening is a through hole, the above aperture is set to facilitate the embedding and release of active ions, while improving the bonding force between the membrane layer and the current collector.
[0065] Optionally, in some embodiments of the present application, the first aperture D1 ≥ 10 μm, and / or the second aperture D2 ≤ 120 μm. Further, in some embodiments of the present application, the first aperture D1 ≤ 60 μm, and / or the second aperture D2 ≥ 40 μm, optionally 30 μm ≤ D1 ≤ 60 μm, 60 μm ≤ D2 ≤ 120 μm. Exemplarily, D1 can be 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 60 μm, and a range value between any two of the above. Exemplarily, D2 can be 60 μm, 75 μm, 90 μm, 100 μm, 110 μm, 120 μm, and a range value between any two of the above. Setting the first aperture and the second aperture in the above-mentioned appropriate range can take into account the improvement of the wetting problem of the electrolyte in the pole piece and the improvement of the bonding force between the membrane layer and the current collector.
[0066] Optionally, in some embodiments of the present application, D1 and D2 may also satisfy 0.25≤D1 / D2<1. Exemplarily, D1 / D2 may be 0.25, 0.3, 0.5, 0.6, 0.7, 0.8, and a range value between any two of the above. Optionally, 0.25≤D1 / D2≤0.5.
[0067] Optionally, in some embodiments of the present application, the aperture of the opening may gradually increase from the first aperture to the second aperture from the end close to the current collector to the end away from the current collector. Exemplarily, the first aperture may increase to the second aperture with a gradient. Exemplarily, the first aperture may increase to the second aperture with a slope change. Based on this embodiment, it is possible to ensure that the complexity and difficulty of hole making are not too large.
[0068] For example, Figure 4 Schematic cross-sectional view of a negative electrode sheet according to an embodiment of the present application, wherein the opening 121 is a closed hole, and the aperture of the opening 121 increases in a slope from an end close to the current collector to an end away from the current collector.
[0069] For example, Figure 5 Schematic diagram of a negative electrode sheet according to an embodiment of the present application. Figure 5 The middle opening 121 is a through hole, and the aperture of the opening 121 increases in a slope from an end close to the current collector to an end far from the current collector.
[0070] Optionally, in some embodiments of the present application, the openings may be evenly distributed on a plane parallel to the film layer. Based on the above embodiments, evenly distributed openings in the film layer can alleviate uneven active ion embedding caused by uneven pore spacing, and for example, when the active ions are lithium ions, lithium utilization can be improved.
[0071] Optionally, in some embodiments of the present application, on a plane parallel to the film layer, the spacing between adjacent openings may include a first spacing d1, and / or a second spacing d2, and / or a third spacing d3. Optionally, the first spacing d1 satisfies 800μm≥d1≥173μm, the second spacing d2 satisfies 500μm≥d2≥100μm, and the third spacing d3 satisfies 500μm≥d3≥100μm. Exemplarily, the first spacing d1 may be 175μm, 260μm, 295μm, 330μm, 400μm, 700μm, 800μm, and a range value between any two of the above. Exemplarily, the second spacing d2 may be 100μm, 150μm, 170μm, 190μm, 210μm, 250m, 300μm, 350μm, 400μm, 500μm, and a range value between any two of the above. Exemplarily, the third spacing d3 may be 100 μm, 150 μm, 170 μm, 190 μm, 210 μm, 250 μm, 300 μm, 350 μm, 400 μm, 450 μm, 500 μm, or a range between any two of the above. Optionally, in some embodiments, 433 μm ≥ d1 ≥ 260 μm, 250 μm ≥ d2 ≥ 150 μm, and 250 μm ≥ d3 ≥ 150 μm.
[0072] Based on the above embodiment, the first spacing d1, the second spacing d2 and the third spacing d3 are set within the above appropriate range, so that the difficulty of electrolyte infiltration in the electrode sheet can be effectively reduced.
[0073] Optionally, in some embodiments of the present application, the first spacing may be the spacing between adjacent openings in the first direction, the second spacing may be the spacing between adjacent openings in the second direction, and the third spacing may be the spacing between adjacent openings in a third direction, wherein the first direction is perpendicular to the second direction, and the third direction intersects with the first direction and the second direction, respectively.
[0074] For example, Figure 6 FIG. 1 is a schematic top view of a negative electrode sheet according to an embodiment of the present application. Figure 6As shown, the opening 1 has adjacent openings in the first direction S1, the second direction S2, and the third direction S3, wherein the first direction S1 is perpendicular to the second direction S2, and the third direction S3 intersects the first direction S1 and the second direction S2, respectively. The spacing between adjacent openings in the first direction is a first spacing d1, the spacing between adjacent openings in the second direction is a second spacing d2, and the spacing between adjacent openings in the third direction is a third spacing d3.
[0075] Based on the above embodiments, the pore spacing is controlled in multiple directions to ensure the uniformity of pore distribution. For example, when the active ions are not lithium ions, the uneven lithium insertion caused by uneven pore spacing can be further alleviated.
[0076] Optionally, in some embodiments of the present application, the membrane layer may include a first membrane layer and a second membrane layer, wherein the first membrane layer is disposed on the surface of the current collector, and the second membrane layer is disposed on the surface of the first membrane layer away from the current collector, and the opening includes a first opening disposed in the first membrane layer and a second opening disposed in the second membrane layer, wherein the pore size of the first opening is smaller than the pore size of the second opening.
[0077] Optionally, in some embodiments of the present application, the membrane layer may include an active material layer disposed on the surface of the current collector, and the active material layer includes a negative electrode active material. Exemplarily, the negative electrode active material may include at least one of natural graphite, artificial graphite, soft carbon, hard carbon, silicon-based materials, and metal oxides.
[0078] In some embodiments, the negative electrode active material may be natural graphite, so that high capacity and high adhesion of the active material can be achieved. In some embodiments, the negative electrode active material is artificial graphite, so that high porosity of the active material can be achieved.
[0079] In some embodiments, the film layer may further include other materials, such as a conductive polymer. Exemplarily, the film layer may include an active material layer and a conductive polymer layer, wherein the active material layer may be disposed on the current collector surface, and the conductive polymer layer may be disposed on the surface of the active material layer away from the current collector.
[0080] A conductive polymer layer is set in the membrane layer. Taking lithium ions as an example, after the active ions are treated with lithium supplementation, the contact area between lithium and the active material layer can be reduced, thereby slowing down the speed of lithium insertion in the negative electrode plate and reducing the heat generation of the plate.
[0081] Furthermore, in some embodiments of the present application, the number of active material layers and conductive polymer layers can be multiple layers, and the multiple active material layers and the multiple conductive polymer layers can be stacked on each other, wherein the outermost layer away from the current collector can be a conductive polymer layer.
[0082] Alternatively, the negative electrode current collector may be a metal foil or a composite current collector. For example, as the metal foil, a copper foil may be used. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material substrate. The composite current collector may be formed by forming a metal material (copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0083] Optionally, the negative electrode active material may be a negative electrode active material for a battery known in the art. As an example, the negative electrode active material may include at least one of the following materials: artificial graphite, natural graphite, soft carbon, hard carbon, silicon-based materials, tin-based materials, lithium titanate, etc. The silicon-based material may be selected from at least one of elemental silicon, silicon oxide compounds, silicon-carbon composites, silicon-nitrogen composites, and silicon alloys. The tin-based material may be selected from at least one of elemental tin, tin oxide compounds, and tin alloys. However, the present application is not limited to these materials, and other traditional materials that can be used as negative electrode active materials for batteries may also be used. These negative electrode active materials may be used alone or in combination of two or more.
[0084] Optionally, the negative electrode film layer further includes a binder. The binder may be selected from at least one of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA) and carboxymethyl chitosan (CMCS).
[0085] Optionally, in one embodiment, the negative electrode film layer further includes a conductive agent, which can be selected from at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene and carbon nanofibers.
[0086] Optionally, the negative electrode film layer further includes other additives, such as a thickener (such as sodium carboxymethyl cellulose (CMC-Na)) and the like.
[0087] In some embodiments, the negative electrode sheet can be prepared in the following manner: the components for preparing the negative electrode sheet are formed into a negative electrode slurry. For example, the negative electrode active material, the conductive agent, the binder and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a negative electrode slurry. Then, the negative electrode slurry is coated on the current collector 1, and after drying, cold pressing and other processes, the negative electrode sheet can be obtained.
[0088] [Positive electrode]
[0089] The positive electrode sheet generally includes a positive electrode current collector and a positive electrode film layer disposed on at least one surface of the positive electrode current collector, wherein the positive electrode film layer includes a positive electrode active material.
[0090] As an example, the positive electrode current collector has two surfaces opposite to each other in its thickness direction, and the positive electrode film layer is disposed on any one or both of the two opposite surfaces of the positive electrode current collector.
[0091] In some embodiments, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver and silver alloy, etc.) on a polymer material substrate (such as a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).
[0092] In some embodiments, the positive electrode active material may adopt a positive electrode active material for a battery that is well known in the art. As an example, the positive electrode active material may include at least one of the following materials: a lithium-containing phosphate with an olivine structure, a lithium transition metal oxide, and their respective modified compounds. However, the present application is not limited to these materials, and other traditional materials that can be used as positive electrode active materials for batteries may also be used. These positive electrode active materials may be used alone or in combination of two or more. Among them, examples of lithium transition metal oxides may include, but are not limited to, lithium cobalt oxide (such as LiCoO2), lithium nickel oxide (such as LiNiO2), lithium manganese oxide (such as LiMnO2, LiMn2O4), lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide (such as LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2 (also referred to as NCM333), LiNi 0.5 Co 0.2 Mn 0.3 O2 (also referred to as NCM523), LiNi 0.5 Co 0.25 Mn 0.25 O2 (also referred to as NCM211), LiNi 0.6 Co 0.2 Mn 0.2 O2 (also referred to as NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O2 (also referred to as NCM811), lithium nickel cobalt aluminum oxide (such as LiNi 0.85 Co0.15 Al 0.05 O2) and its modified compounds, etc. Examples of lithium-containing phosphates with an olivine structure may include, but are not limited to, at least one of lithium iron phosphate (such as LiFePO4 (also referred to as LFP)), a composite material of lithium iron phosphate and carbon, lithium manganese phosphate (such as LiMnPO4), a composite material of lithium manganese phosphate and carbon, lithium iron manganese phosphate, and a composite material of lithium iron manganese phosphate and carbon.
[0093] In some embodiments, the positive electrode material may further include a binder. As an example, the binder may include at least one of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer, and fluorine-containing acrylate resin.
[0094] In some embodiments, the positive electrode material layer may further optionally contain a conductive agent. As an example, the conductive agent may include at least one of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.
[0095] In some embodiments, the positive electrode sheet can be prepared in the following manner: the components for preparing the positive electrode sheet, such as the positive electrode active material, the conductive agent, the binder, the additive and any other components are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the current collector, and after drying, cold pressing and other processes, the positive electrode sheet can be obtained.
[0096] [Electrolytes]
[0097] The electrolyte plays the role of conducting ions between the positive electrode and the negative electrode. The present application has no specific restrictions on the type of electrolyte, which can be selected according to needs. For example, the electrolyte can be liquid, gel or all-solid.
[0098] In some embodiments, the electrolyte is an electrolyte solution, which includes an electrolyte salt and a solvent.
[0099] In some embodiments, the electrolyte salt can be selected from at least one of lithium hexafluorophosphate, lithium tetrafluoroborate, lithium perchlorate, lithium hexafluoroarsenate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, lithium trifluoromethanesulfonate, lithium difluorophosphate, lithium difluorooxalatoborate, lithium dioxalatoborate, lithium difluorodioxalatophosphate, and lithium tetrafluorooxalatophosphate.
[0100] In some embodiments, the solvent can be selected from at least one of ethylene carbonate, propylene carbonate, ethyl methyl carbonate, diethyl carbonate, dimethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate, butylene carbonate, fluoroethylene carbonate, methyl formate, methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, methyl butyrate, ethyl butyrate, 1,4-butyrolactone, cyclopentane sulfone, dimethyl sulfone, methyl ethyl sulfone and diethyl sulfone.
[0101] In some embodiments, the electrolyte may further include additives, such as negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high or low temperature performance, etc.
[0102] [Isolator]
[0103] In some embodiments, the secondary battery further includes a separator. The present application has no particular limitation on the type of separator, for example, any known porous structure separator with good chemical stability and mechanical stability can be selected.
[0104] In some embodiments, the material of the isolation membrane can be selected from at least one of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without particular limitation. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without particular limitation.
[0105] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator may be formed into an electrode assembly by a winding process or a lamination process.
[0106] In addition, the secondary battery, battery module, battery pack, and electric device of the present application will be described below with reference to the drawings as appropriate.
[0107] In one embodiment of the present application, a secondary battery is provided.
[0108] Generally, a secondary battery includes a positive electrode sheet, a negative electrode sheet, an electrolyte and a separator. During the battery charging and discharging process, active ions are embedded and released back and forth between the positive electrode sheet and the negative electrode sheet. The electrolyte plays the role of conducting ions between the positive electrode sheet and the negative electrode sheet. The separator is set between the positive electrode sheet and the negative electrode sheet, mainly to prevent the positive and negative electrodes from short-circuiting, while allowing ions to pass through.
[0109] Alternatively, the secondary battery may be a battery or a battery cell.
[0110] In some embodiments, the secondary battery may include an outer package, which may be used to encapsulate the electrode assembly and the electrolyte.
[0111] In some embodiments, the outer packaging of the secondary battery may be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery may also be a soft package, such as a bag-type soft package. The material of the soft package may be plastic, and examples of the plastic include polypropylene, polybutylene terephthalate, and polybutylene succinate.
[0112] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square or any other shape. Figure 7 The secondary battery 700 is a square structure as an example.
[0113] In some embodiments, reference Figure 8 , the outer package may include a shell 81 and a cover plate 83. Among them, the shell 81 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 81 has an opening connected to the receiving cavity, and the cover plate 83 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can form an electrode assembly 82 through a winding process or a lamination process. The electrode assembly 82 is encapsulated in the receiving cavity. The electrode assembly 82 is immersed in the electrolyte. The number of electrode assemblies 82 contained in the secondary battery 700 can be one or more, and those skilled in the art can select according to specific actual needs.
[0114] In some embodiments, the secondary batteries 700 may be assembled into a battery module. The number of secondary batteries contained in the battery module may be one or more, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery module.
[0115] Fig. 9 900 is an example of a battery module. Fig. 9 In the battery module 900, the plurality of secondary batteries 700 may be arranged in sequence along the length direction of the battery module 900. Of course, they may also be arranged in any other manner. Further, the plurality of secondary batteries 700 may be fixed by fasteners.
[0116] Optionally, the battery module 900 may further include a housing having an accommodation space, and the plurality of secondary batteries 700 may be accommodated in the accommodation space.
[0117] In some embodiments, the battery modules described above may also be assembled into a battery pack. The battery pack may contain one or more battery modules, and the specific number may be selected by those skilled in the art according to the application and capacity of the battery pack.
[0118] Fig.10 and Fig.11 1 is a battery pack 1000 as an example. Fig. 9 and Fig.10 The battery pack 1000 may include a battery box and a plurality of battery modules 900 disposed in the battery box. The battery box includes an upper box body 1200 and a lower box body 1300. The upper box body 1200 can be covered on the lower box body 1300 to form a closed space for accommodating the battery modules 900. The plurality of battery modules 900 may be arranged in the battery box in any manner.
[0119] In addition, the present application also provides an electrical device, which includes at least one of the secondary battery, battery module, or battery pack provided in the present application. The secondary battery, battery module, or battery pack can be used as a power source for the electrical device, and can also be used as an energy storage unit for the electrical device. The electrical device may include mobile devices (such as mobile phones, laptops, etc.), electric vehicles (such as pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc., but are not limited thereto.
[0120] As the electrical device, a secondary battery, a battery module or a battery pack may be selected according to its usage requirements.
[0121] Fig.12 The power consumption device is taken as an example. The power consumption device is a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle. In order to meet the high power and high energy density requirements of the power consumption device for the secondary battery, a battery pack or a battery module can be used.
[0122] Another example of a device may be a mobile phone, a tablet computer, a notebook computer, etc. Such a device is usually required to be thin and light, and a secondary battery may be used as a power source.
[0123] [Example]
[0124] Preparation process
[0125] (1) Preparation of positive electrode sheet
[0126] Lithium iron phosphate was selected as the positive electrode active material. The positive electrode active material, conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) were dissolved in a solvent N-methylpyrrolidone (NMP) at a mass ratio of 90:5:5. The mixture was fully stirred and mixed to obtain a slurry. The slurry was evenly coated on the positive electrode current collector aluminum foil, and then dried, cold pressed, and cut to obtain the positive electrode sheet.
[0127] (2) Preparation of negative electrode sheet
[0128] Natural graphite was selected as the negative electrode active material, and the negative electrode active material, conductive agent acetylene black, binder styrene butadiene rubber (SBR), and thickener sodium carboxymethyl cellulose (CMC) were dissolved in deionized water at a mass ratio of 90:4:4:2, and mixed evenly to obtain a negative electrode slurry, which was evenly coated on the negative electrode current collector copper foil, and then dried, cold pressed, and cut to obtain a negative electrode sheet. In the cold pressing process, the negative electrode sheet was placed in two counter-rotating rollers with protrusions to form openings in the membrane layer by mechanical processing.
[0129] (3) Preparation of electrolyte
[0130] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3:7, and lithium hexafluorophosphate (LiPF6) was added to dissolve in the solvent so that the mass fraction of the solute in the electrolyte was 11%. The mixture was stirred evenly to obtain an electrolyte.
[0131] (4) Assembly of lithium secondary batteries
[0132] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is located between the positive electrode sheet and the negative electrode sheet and can separate the positive electrode sheet from the negative electrode sheet; then the stacked components are wound to obtain an electrode assembly; the electrode assembly is placed in a shell, and the electrolyte is injected after drying; and a secondary battery is obtained after processes such as formation and standing.
[0133] Test Method
[0134] Cycle number test method: At 25°C, the secondary battery prepared in each embodiment and comparative example is charged at a constant current of 1C to a charging cut-off voltage V1, V1 can be selected to be 4.4V, then charged at a constant voltage to a current ≤ 0.05C, left to stand for 5 minutes, and then discharged at a constant current of 0.33C to a discharge cut-off voltage V2, V2 can be selected to be 2.5V and left to stand for 5 minutes. This is a charge and discharge cycle. According to this method, the battery is tested for cyclic charge and discharge until the battery capacity decays to 80%. The number of cycles at this time is the cycle life of the battery.
[0135] Charging capacity test method: C is used to indicate the battery charging and discharging capacity ratio. 1C indicates the current intensity when the battery is fully discharged in one hour. For example, if a 18650 battery with a nominal capacity of 2200mA·h is discharged at a 1C intensity for one hour, the discharge current is 2200mA. Charging and discharging ratio = charging and discharging current / rated capacity; for example: when a battery with a rated capacity of 100A·h is discharged at 20A, its discharge ratio is 0.2C.
[0136] At 25° C., the battery cells prepared in each embodiment and comparative example were fully charged, left to stand for 5 minutes, and then discharged. Specifically, the discharge process was to discharge at a constant current of 0.33C to a discharge cut-off voltage V2, and then left to stand for 5 minutes.
[0137] Test Results
[0138] The relevant parameters and test results of the comparative examples and different embodiments are shown in Table 1.
[0139] Table 1: Related parameters and test results of comparative examples and different embodiments
[0140]
[0141]
[0142] In the above table, "angle" is the angle θ between the axis of the opening and the lower surface of the film layer; "thickness" is the thickness of the film layer; "depth" is the depth of the opening in the film layer. If the depth of the opening is less than the thickness of the film layer, it means that the opening is a closed hole. If the depth of the opening is equal to the thickness of the film layer, it means that the opening is a through hole.
[0143] From the performance comparison between Examples 1-5 and Comparative Example 1, it can be seen that by using the negative electrode plate with a special structure provided by the present application, that is, setting the angle between the opening of the negative electrode plate and the lower surface of the membrane layer to an acute angle, the charging capacity and cycle performance of the battery can be effectively improved.
[0144] By comparing Example 1 and Examples 6-8, it can be seen that the depth of the opening has a certain influence on the performance. The opening in Example 1 is a through hole, and the opening in Examples 6-8 is a closed hole. The charging capacity and the number of cycles of Example 1 are better than those of Examples 6-8. By comparing Examples 6-8, it can be seen that as the depth of the opening increases, the performance of the charging capacity and the number of cycles are improved.
[0145] Furthermore, through the performance comparison of Examples 9-17, it can be concluded that setting the pore size of the opening in the membrane layer close to the current collector to be smaller than the pore size at the end away from the current collector can further improve the charging capacity and cycle performance of the battery.
[0146] By comparing Examples 18-22, it can be concluded that the spacing between the openings also has a certain influence on the performance of the battery. As the spacing between the openings increases, the charging capacity and cycle performance of the battery decrease.
[0147] It should be noted that the present application is not limited to the above-mentioned embodiments. The above-mentioned embodiments are only examples, and the embodiments having the same structure as the technical idea and exerting the same effect within the scope of the technical solution of the present application are all included in the technical scope of the present application. In addition, without departing from the scope of the main purpose of the present application, various modifications that can be thought of by those skilled in the art to the embodiments and other methods of combining some of the constituent elements in the embodiments are also included in the scope of the present application.
Claims
1. A pole piece, characterized in that: The negative electrode plate comprises: a current collector and a film layer disposed on at least one side of the current collector, The membrane layer is provided with a plurality of openings, and an angle θ between the axis of the opening and the lower surface of the membrane layer satisfies: 0°<θ<90°, wherein the lower surface of the membrane layer is the surface of the membrane layer close to the current collector.
2. The negative electrode sheet according to claim 1, characterized in that: The θ satisfies: 20°≤θ≤70°. Optionally, the θ satisfies: 30°≤θ≤60°.
3. The negative electrode sheet according to claim 1 or 2, characterized in that: A portion of the film layer is located between one end of the opening close to the current collector and the surface of the current collector.
4. The negative electrode sheet according to claim 1 or 2, characterized in that: The opening comprises a through hole penetrating the membrane layer.
5. The negative electrode sheet according to any one of claims 1 to 4, characterized in that: The aperture of one end of the opening close to the current collector is a first aperture, and the aperture of one end of the opening away from the current collector is a second aperture, and the first aperture is smaller than the second aperture.
6. The negative electrode sheet according to claim 5, characterized in that: The first aperture D1 satisfies: 10 μm ≤ D1 ≤ 60 μm, and / or the second aperture D2 satisfies: 40 μm ≤ D2 ≤ 120 μm; Optionally, 30 μm ≤ D1 ≤ 60 μm, and / or, 60 μm ≤ D2 ≤ 120 μm; And / or, 0.25≤D1 / D2<1.
7. The negative electrode sheet according to claim 5 or 6, characterized in that: From an end close to the current collector to an end far from the current collector, the aperture of the opening gradually increases from the first aperture to the second aperture.
8. The negative electrode sheet according to any one of claims 1 to 7, characterized in that: On a plane parallel to the film layer, the spacing between adjacent openings includes a first spacing d1, and / or a second spacing d2, and / or a third spacing d3, wherein the first spacing d1 satisfies 800 μm ≥ d1 ≥ 173 μm, the second spacing d2 satisfies 500 μm ≥ d2 ≥ 100 μm, and the third spacing d3 satisfies 500 μm ≥ d3 ≥ 100 μm; Optionally, 433 μm ≥ d1 ≥ 260 μm, 250 μm ≥ d2 ≥ 150 μm, 250 μm ≥ d3 ≥ 150 μm; Among them, the first spacing is the spacing between the adjacent openings in the first direction, the second spacing is the spacing between the adjacent openings in the second direction, and the third spacing is the spacing between the adjacent openings in the third direction, wherein the first direction is perpendicular to the second direction, and the third direction intersects with the first direction and the second direction respectively.
9. The negative electrode sheet according to claim 1 or 2, characterized in that: The film layer comprises a first film layer and a second film layer, wherein the first film layer is disposed on the surface of the current collector, and the second film layer is disposed on the surface of the first film layer away from the current collector. The openings include a first opening disposed in the first film layer and a second opening disposed in the second film layer, wherein a diameter of the first opening is smaller than a diameter of the second opening.
10. The negative electrode sheet according to any one of claims 1 to 9, characterized in that: The membrane layer comprises an active material layer and a conductive polymer layer, the number of layers of the active material layer and the conductive polymer layer are both multiple layers, the active material layer and the conductive polymer layer are stacked on each other, and the outermost layer away from the current collector is the conductive polymer layer.
11. A secondary battery, characterized in that: include: The negative electrode sheet according to any one of claims 1 to 10.
12. An electrical device, characterized in that: include: The secondary battery as claimed in claim 11.
Citation Information
Patent Citations
Lithium-ion energy storage battery
CN101867060A
Electrode for secondary battery comprising fine holes
CN108292737A
Current collector, and secondary battery, battery module, and device comprising same
CN214313261U
Collector, and lithium ion secondary battery using the same
JP2013182810A
Power storage device and secondary battery and manufacturing method for electrode
JP2014022102A
Cited By
Composite metal foil and battery
CN120389046A
Composite metal foil and battery
CN120389046B