Electrode material, preparation method thereof and lithium ion battery

By coating carbon, nitrogen and nitrogen carbon layers on the surface of bismuth sulfide, the problem of volume change and low conductivity of bismuth sulfide negative electrode material in lithium-ion batteries is solved, and the cycle stability and energy density of the battery are improved.

CN118943339AActive Publication Date: 2024-11-12SOUTHERN UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411269230.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12
Estimated Expiration
2044-09-11

AI Technical Summary

Technical Problem

The volume change of bismuth sulfide negative electrode material in existing lithium-ion batteries is too large during the cycle process and the electronic conductivity is too low, resulting in low utilization and rapid capacity attenuation.

Method used

The surface of bismuth sulfide is coated with carbon layer, nitrogen layer and nitrogen carbon layer in turn, and electrode material is formed through hydrothermal treatment and annealing treatment. The carbon layer relieves stress, the nitrogen layer reduces side reactions, and the nitrogen carbon layer increases the charge transfer rate.

Benefits of technology

It improves the cycle stability and energy density of bismuth sulfide, extends battery life, and improves conductivity and structural stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943339A_ABST
    Figure CN118943339A_ABST
Patent Text Reader

Abstract

The invention discloses an electrode material, a preparation method thereof and a lithium ion battery. The electrode material comprises bismuth sulfide, a carbon layer coated on the surface of the bismuth sulfide, a nitrogen layer coated on the surface of the carbon layer and a nitrogen-carbon layer coated on the surface of the nitrogen layer. The surface of the bismuth sulfide is sequentially coated with the carbon layer, the nitrogen layer and the nitrogen-carbon layer to form the electrode material, the carbon layer serves as a framework support and can effectively relieve huge stress of the bismuth sulfide during charging and discharging, the volume change of the bismuth sulfide is reduced, and therefore the cycling stability of the bismuth sulfide is improved; the nitrogen layer can effectively reduce side reaction of bismuth sulfide and electrolyte, so that the self-discharge rate of the battery is reduced, the energy density is improved, and the battery has more stable and lasting service life; the nitrogen-carbon layer can improve the charge transfer rate in the charge-discharge process, and facilitates the improvement of the conductivity and the structural stability of bismuth sulfide in the repeated lithiation / lithium removal process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an electrode material and a preparation method thereof, and a lithium ion battery. Background Art

[0002] With the rapid development of society, the application of new energy as the key technology has gradually grown and developed, including aerospace, military, medical, electric vehicles, etc. However, new energy has the problem of uneven temporal and spatial distribution, and energy storage provides a more ideal solution for "peak shaving and valley filling". Therefore, finding energy storage devices with high energy density is the main trend of future development. Among various electrochemical energy storage devices, lithium-ion batteries have been widely studied due to their high energy density, long cycle life, and low pollution. Nowadays, graphite-type carbon negative electrode materials have been widely used in commercial lithium-ion batteries. However, the theoretical specific capacity of graphite (372mAh·g -1 ) is low, and it is impossible to achieve the high energy density required by some modern electronic devices. The exploration and development of negative electrode materials with high specific capacity and high safety has become a research hotspot in the field of lithium-ion batteries.

[0003] Metal sulfides, as active materials for rechargeable lithium-ion batteries, have higher specific capacity and higher operational safety than traditional graphite negative electrodes, and have attracted extensive research. Such as iron sulfide, tin sulfide and bismuth sulfide. In particular, bismuth sulfide, as a nested indirect bandgap semiconductor with a bandgap of 1.3eV, this layered structure can provide a safe lithium intercalation potential (0.5-0.8V vs.Li) and a mass specific capacity of 625mAh / g, and is considered to be one of the excellent candidates for lithium-ion batteries. However, when studying the storage application of bismuth sulfide negative electrode lithium-ion batteries, there are still some problems, including excessive volume change during the cycle, low electronic conductivity, and the precipitation and dissolution of polysulfide intermediates in the electrolyte during charge and discharge, resulting in low utilization of negative electrode materials and rapid capacity decay.

[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention

[0005] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide an electrode material and a preparation method thereof and a lithium-ion battery, aiming to solve the problems of excessive volume change and low electronic conductivity of existing electrode materials during the cycle process.

[0006] The technical solution of the present invention is as follows:

[0007] In a first aspect of the present invention, an electrode material is provided. The electrode material includes bismuth sulfide, a carbon layer coated on the surface of the bismuth sulfide, a nitrogen layer coated on the surface of the carbon layer, and a nitrogen-carbon layer coated on the surface of the nitrogen layer.

[0008] Preferably, the bismuth sulfide is spherical in shape, and the diameter of the bismuth sulfide is 1-2 μm.

[0009] Preferably, the thickness of the carbon layer is 5-10 nm.

[0010] Preferably, the thickness of the nitrogen layer is 5-10 nm.

[0011] Preferably, the thickness of the nitrogen-carbon layer is 10-20 nm.

[0012] Preferably, in the nitrogen-carbon layer, the mass ratio of nitrogen to carbon is 0.2.

[0013] A second aspect of the present invention provides a method for preparing an electrode material, the method comprising the following steps:

[0014] Preparation of bismuth sulfide;

[0015] The bismuth sulfide and the carbon source are dissolved in a first solvent, and a hydrothermal treatment and a first annealing treatment are performed in sequence, so that carbon is coated on the surface of the bismuth sulfide, which is recorded as C@Bi2S3;

[0016] The C@Bi2S3 and the nitrogen source are dissolved in a second solvent, and a first deposition process and a second annealing process are sequentially performed, so that nitrogen is coated on the surface of the C@Bi2S3, which is recorded as CN@Bi2S3;

[0017] The CN@Bi2S3 is dissolved in a third solvent, the pH value is adjusted to 7.5-9.5, and then a nitrogen and carbon source is added, and a second deposition treatment and a third annealing treatment are performed in sequence, so that nitrogen and carbon are coated on the surface of the CN@Bi2S3 to obtain the electrode material, which is recorded as CN-NC@Bi2S3.

[0018] Preferably, the carbon source is selected from one or more of glucose, sodium acetate and methanol;

[0019] The nitrogen source is selected from one or more of urea, boron nitride and cyanide;

[0020] The nitrogen and carbon source is selected from one or more of melamine, ethylenediamine, and dopamine hydrochloride;

[0021] The first solvent, the second solvent and the third solvent are each independently selected from deionized water or ethanol.

[0022] Preferably, the temperature of the hydrothermal treatment is 120-150°C, and the time of the hydrothermal treatment is 10-12h;

[0023] The temperature of the first annealing treatment is 400-500° C., and the time of the first annealing treatment is 1-5 hours;

[0024] The temperature of the second annealing treatment is 400-500°C, and the time of the second annealing treatment is 1-5h;

[0025] The temperature of the third annealing treatment is 400-500° C., and the time of the third annealing treatment is 1-5 hours;

[0026] The first deposition process and the second deposition process are each independently selected from spin coating, dipping, and spraying.

[0027] According to a third aspect of the present invention, a lithium-ion battery is provided. The lithium-ion battery comprises a negative electrode material. The negative electrode material comprises the above-mentioned electrode material or an electrode material prepared by the above-mentioned preparation method.

[0028] Beneficial effects: The present invention provides an electrode material, a preparation method thereof and a lithium-ion battery. The present invention sequentially coats a carbon layer, a nitrogen layer and a nitrogen-carbon layer on the surface of bismuth sulfide to form an electrode material, wherein the carbon layer as a skeleton support can effectively alleviate the huge stress of bismuth sulfide during charging and discharging, reduce the volume change of bismuth sulfide, and thus improve the cycle stability of bismuth sulfide; the nitrogen layer can effectively reduce the side reaction between bismuth sulfide and the electrolyte, thereby reducing the self-discharge rate of the battery and increasing the energy density, so that the battery has a more stable and long-lasting life; the nitrogen-carbon layer can increase the charge transfer rate during charging and discharging, and help bismuth sulfide to improve the conductivity and structural stability during repeated lithiation / delithiation. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 It is a schematic diagram of the assembly structure of a lithium-ion battery prepared in a preferred application example of the present invention.

[0030] Figure 2 It is an XRD comparison diagram of the negative electrode materials prepared in Example 1 and Comparative Example 1 of the present invention as negative electrodes of lithium ion batteries.

[0031] Figure 3 It is an XPS image of the negative electrode material prepared in Example 1 of the present invention.

[0032] Figure 4 is a SEM image of the negative electrode material prepared in Example 1 of the present invention.

[0033] Figure 5 This is a charge and discharge curve diagram of the negative electrode material prepared in Example 1 of the present invention as a negative electrode of a lithium ion battery.

[0034] Figure 6 It is a charge and discharge curve diagram of the negative electrode material prepared in Comparative Example 1 of the present invention as the negative electrode of a lithium ion battery.

[0035] Figure 7It is a test chart of the cycle performance of the negative electrode materials prepared in Example 1 and Comparative Example 1 of the present invention as negative electrodes of lithium-ion batteries.

[0036] Figure 8 This is a rate performance test diagram of the negative electrode materials prepared in Example 1 and Comparative Example 1 of the present invention as negative electrodes of lithium-ion batteries. DETAILED DESCRIPTION

[0037] The present invention provides an electrode material and a preparation method thereof and a lithium ion battery. To make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0038] An embodiment of the present invention provides an electrode material, which includes bismuth sulfide, a carbon layer coated on the surface of the bismuth sulfide, a nitrogen layer coated on the surface of the carbon layer, and a nitrogen-carbon layer coated on the surface of the nitrogen layer.

[0039] In the embodiment of the present invention, a carbon layer, a nitrogen layer and a nitrogen-carbon layer are sequentially coated on the surface of bismuth sulfide to form an electrode material, wherein the carbon layer as a skeleton support can effectively alleviate the huge stress of bismuth sulfide during charging and discharging, reduce the volume change of bismuth sulfide, and thus improve the cycle stability of bismuth sulfide; the nitrogen layer can effectively reduce the side reaction of bismuth sulfide with the electrolyte, thereby reducing the self-discharge rate of the battery and increasing the energy density, so that the battery has a more stable and long-lasting life; the nitrogen-carbon layer can increase the charge transfer rate during the charging and discharging process, and help bismuth sulfide to improve the conductivity and structural stability during repeated lithiation / delithiation.

[0040] In some embodiments, the bismuth sulfide is spherical in shape, and the diameter of the bismuth sulfide is 1-2 μm.

[0041] This intercalation structure of spherical bismuth sulfide stores Li via a fast transport pathway +, will not react electrochemically with the electrode, and spherical bismuth sulfide has a high specific surface area and good particle distribution. The high specific surface area can promote the conduction of more electrons and lithium ions on the surface and inside of the electrode, thereby improving the overall conductivity and electrochemical performance of the battery. Among them, when the size of the bismuth sulfide nanospheres is between 1-2μm, it has the following advantages: 1. Increase the specific surface area: The size range of 1-2 microns is moderate, which can not only maintain a large specific surface area to improve the activity of the electrode, increase the insertion and extraction rate of lithium ions, but also reduce the side reactions and excessive formation of SEI film caused by excessive surface. 2. Maintain a stable structure: The micron-level size can provide a more stable structure, avoid large volume changes during charging and discharging, and thus reduce the pulverization and failure of the material. 3. Good conductivity and ion diffusion: The size of 1-2 microns can ensure the balance between the conductivity and ion diffusion of the material, avoiding the problem of high interface resistance under nanometer size and the problem of too long diffusion path caused by excessive particle size.

[0042] In some embodiments, the carbon layer has a thickness of 5-10 nm.

[0043] The embodiment of the present invention controls the thickness of the carbon layer within this range, which has the following three benefits: 1. Improving electronic conductivity: The carbon layer is a good conductive material, and a suitable thickness can significantly improve the electronic conductivity of the electrode and reduce the internal resistance. 2. Preventing volume expansion and structural collapse: A moderate carbon layer can provide a buffering effect during the insertion and extraction of lithium ions, reduce the volume change of the negative electrode material, and prevent the collapse of the electrode structure. 3. The impact of being too thick or too thin: If the thickness of the carbon layer exceeds 10 nanometers, it may increase the overall thickness of the electrode, resulting in an increase in the transmission distance of electrons and ions and a reduction in rate performance; if the thickness of the carbon layer is less than 5 nanometers, it is difficult to form an effective protective layer, and the occurrence of side reactions cannot be effectively avoided.

[0044] In some embodiments, the thickness of the nitrogen layer is 5-10 nm.

[0045] The embodiment of the present invention controls the thickness of the nitrogen layer within this range, which has the following three benefits: 1. Increase electronic conductivity: Nitrogen doping can improve the electronic conductivity of the material because nitrogen atoms can introduce additional electrons and increase conductivity. The appropriate thickness (5-10 nanometers) ensures sufficient electron transport without affecting the overall conductivity of the material. 2. Stabilize the SEI film: A moderate thickness of the nitrogen layer can reduce the direct contact between the electrolyte and the negative electrode material, thereby helping to form a stable solid electrolyte interface (SEI) film and reduce electrolyte decomposition and side reactions. 3. The impact of being too thick or too thin: If the thickness of the nitrogen layer exceeds 10 nanometers, it will increase the diffusion path of electrons and ions and reduce the rate performance of the battery; if the thickness is less than 5 nanometers, the coating effect is not obvious and it is difficult to form a stable interface protection layer.

[0046] In some embodiments, the carbon nitride layer has a thickness of 10-20 nm.

[0047] The embodiment of the present invention controls the thickness of the nitrogen-carbon layer within this range, which has the following three benefits: 1. Improving electrical conductivity and ionic conductivity: The nitrogen-rich carbon layer combines the advantages of nitrogen doping and carbon materials, and can simultaneously improve electronic conductivity and ionic conductivity, thereby improving the overall performance of the battery. 2. Stabilizing the SEI film: The nitrogen-rich carbon layer can promote the formation of a uniform SEI film, reduce electrolyte decomposition and side reactions, and extend the cycle life of the battery. 3. The impact of being too thick or too thin: If the thickness of the nitrogen-rich carbon layer exceeds 10 nanometers, it may cause the overall thickness of the electrode to increase, thereby affecting the transmission rate of electrons and ions; if the thickness is less than 5 nanometers, it cannot provide sufficient conductivity and SEI film stability, affecting battery performance.

[0048] In summary, appropriate coating thickness and nanosphere size can optimize the performance of lithium-ion battery anodes, while too thick or too thin coatings will cause an imbalance between conductivity, ion transfer rate and structural stability, affecting the overall performance of the battery.

[0049] In some embodiments, in the nitrogen-carbon layer, the mass ratio of nitrogen to carbon is 0.2.

[0050] The embodiment of the present invention controls the mass ratio of nitrogen to carbon to 0.2, which has the following benefits: 1. Optimizing electronic conductivity: In the nitrogen-carbon layer, nitrogen doping can effectively introduce additional free electrons and improve the conductivity of the material. When the nitrogen doping ratio is 0.2, a balance point can be reached, and the overall conductivity can be significantly improved without significantly damaging the conductivity of the carbon layer. This conductivity enhancement is mainly due to the enrichment of π electrons and the introduction of defects caused by nitrogen doping, and this change can improve the charge transfer ability of carbon-based materials. 2. Promoting lithium ion diffusion: Nitrogen doping can produce certain defects and active sites in the carbon network, which are conducive to the adsorption and diffusion of lithium ions. Therefore, when N:C=0.2, this moderate doping can maintain the structural stability of the carbon material to the greatest extent, while introducing more active sites, improving the rate performance and reversible capacity of the electrode material. 3. Improving SEI film stability: The nitrogen-doped layer can provide a uniform electron distribution and chemical environment, which helps to form a uniform solid electrolyte interface (SEI) film on the electrode surface. A moderate doping ratio (such as 0.2) can optimize interface stability, reduce the occurrence of side reactions, and improve cycle stability.

[0051] In summary, a nitrogen-carbon ratio of 0.2 can achieve a good balance in terms of electronic conductivity, lithium ion diffusivity and SEI film stability, and improve the electrochemical performance of bismuth sulfide nanosphere negative electrode materials. Too high or too low nitrogen doping ratios will lead to imbalances in conductivity, structural stability and electrochemical reactions, thus affecting the overall performance of the battery.

[0052] When the N:C is above and below the range of 0.2, 1. The effect of exceeding 0.2 (higher nitrogen content): Reduced conductivity: Excessive nitrogen doping may destroy the original structure of the carbon layer, resulting in a decrease in the delocalization of π electrons in the carbon network, thereby reducing electronic conductivity. This will increase the internal resistance of the battery and reduce the rate performance of the electrode; Negative effects of too many defects: Too high a nitrogen content will introduce too many structural defects. Although these defects can serve as active sites, they will also accelerate the decay of the electrode material, resulting in faster capacity decay. 2. The effect of less than 0.2 (lower nitrogen content): The doping effect is not obvious: When the nitrogen content is too low (such as N:C < 0.1), the electronic structure and conductivity of the carbon layer cannot be effectively improved. The lack of sufficient active sites may slow down the kinetics of the lithium ion insertion and extraction process, reducing the specific capacity and cycle performance of the battery; SEI film instability: Too low nitrogen doping will reduce the stability of the SEI film, which may cause uneven contact between the electrolyte and the electrode surface, thereby causing uneven electrochemical reactions and affecting the cycle life of the battery.

[0053] An embodiment of the present invention provides a method for preparing an electrode material, the method comprising the following steps:

[0054] Preparation of bismuth sulfide;

[0055] The bismuth sulfide and the carbon source are dissolved in a first solvent, and a hydrothermal treatment and a first annealing treatment are performed in sequence, so that carbon is coated on the surface of the bismuth sulfide, which is recorded as C@Bi2S3;

[0056] The C@Bi2S3 and the nitrogen source are dissolved in a second solvent, and a first deposition process and a second annealing process are sequentially performed, so that nitrogen is coated on the surface of the C@Bi2S3, which is recorded as CN@Bi2S3;

[0057] The CN@Bi2S3 is dissolved in a third solvent, the pH value is adjusted to 7.5-9.5, and then a nitrogen and carbon source is added, and a second deposition treatment and a third annealing treatment are performed in sequence, so that nitrogen and carbon are coated on the surface of the CN@Bi2S3 to obtain the electrode material, which is recorded as CN-NC@Bi2S3.

[0058] In some embodiments, the pH adjusting substance used to adjust the pH value is at least one of trisamine methane, trishydroxymethylaminomethane, and phosphate buffer.

[0059] The preparation method provided by the embodiment of the present invention is simple, low in cost and has good application prospects.

[0060] In some embodiments, the step of preparing bismuth sulfide specifically includes:

[0061] The bismuth salt and the sulfur source were dissolved in deionized water at a molar ratio of 2:3, and then stirred in a magnetic stirrer for 2 hours to obtain a mixed solution;

[0062] The mixed solution was placed in a homogeneous reactor with a PTFE liner and reacted at 120°C for 12 hours; after cooling to room temperature, a black precipitate was obtained by washing and filtration;

[0063] The black precipitate was dried in an oven at a drying temperature of 60° C. for a drying time of 4 h to obtain bismuth sulfide.

[0064] In some embodiments, the bismuth salt is selected from at least one of bismuth acetate, bismuth nitrate, bismuth sulfate, and bismuth chloride, and the sulfur source is selected from at least one of glutathione, thioether, and thiol.

[0065] In some embodiments, the carbon source is selected from one or more of glucose, sodium acetate, and methanol;

[0066] The nitrogen source is selected from one or more of urea, boron nitride and cyanide;

[0067] The nitrogen and carbon source is selected from one or more of melamine, ethylenediamine, and dopamine hydrochloride;

[0068] The first solvent, the second solvent and the third solvent are each independently selected from deionized water or ethanol.

[0069] In some embodiments, the temperature of the hydrothermal treatment is 120-150° C., and the time of the hydrothermal treatment is 10-12 h;

[0070] The temperature of the first annealing treatment is 400-500° C., and the time of the first annealing treatment is 1-5 hours;

[0071] The temperature of the second annealing treatment is 400-500°C, and the time of the second annealing treatment is 1-5h;

[0072] The temperature of the third annealing treatment is 400-500° C., and the time of the third annealing treatment is 1-5 hours;

[0073] The first deposition process and the second deposition process are each independently selected from spin coating, dipping, and spraying.

[0074] The first annealing treatment, the second annealing treatment and the third annealing treatment of the present invention are all carried out in an inert gas environment. Under the action of high temperature annealing, the three-layer interface (carbon layer, nitrogen layer and nitrogen-carbon layer) is in close contact with the surface gap of the Bi2S3 nanosphere, thereby improving the conductivity and stability of the Bi2S3 nanosphere.

[0075] An embodiment of the present invention provides a method for preparing an electrode material, comprising the following steps:

[0076] The bismuth salt and the sulfur source were dissolved in deionized water at a molar ratio of 2:3, and then stirred in a magnetic stirrer for 2 hours to obtain a mixed solution;

[0077] The mixed solution was placed in a homogeneous reactor with a PTFE liner and reacted at 120°C for 12 hours. After cooling to room temperature, a black precipitate was obtained by washing and filtration.

[0078] The black precipitate was dried in an oven at 60°C for 4 h to obtain Bi2S3 nanospheres.

[0079] Bismuth sulfide nanospheres were dispersed in deionized water, glucose was added and stirred for 5 h to obtain a suspension;

[0080] The suspension was placed in a homogeneous reactor with a PTFE liner and reacted at 150°C for 12 hours. After cooling to room temperature, a black precipitate was obtained by washing and filtration.

[0081] The black precipitate was dried in an oven at 60°C for 4 hours, and then subjected to heat treatment to obtain C@Bi2S3 nanospheres.

[0082] Dissolve C@Bi2S3 nanospheres and nitrogen source in a suitable solvent and stir for 4 h to obtain a suspension, the suitable solvent being ethanol or deionized water;

[0083] The suspension is subjected to a sedimentation method, and a black precipitate is obtained after washing and filtration;

[0084] The black precipitate was dried in an oven at 60°C for 4 h, and then subjected to heat treatment to obtain CN@Bi2S3 nanospheres.

[0085] The CN@Bi2S3 nanospheres were dispersed in deionized water and stirred for 5 h. pH adjusting substances were continuously added to adjust the pH value of the solution to about 8.5. Nitrogen and carbon sources were added and stirred for 12 h before filtering to obtain a black precipitate.

[0086] The black precipitate was dried in an oven at a temperature of 60°C for a drying time of 4 h. After drying, the CN-NC@Bi2S3 nanospheres were obtained by heat treatment.

[0087] An embodiment of the present invention further provides a lithium ion battery, wherein the lithium ion battery comprises a negative electrode material, wherein the negative electrode material comprises the above-mentioned electrode material or an electrode material prepared by the above-mentioned preparation method.

[0088] The negative electrode material provided in the embodiment of the present invention is applied to a lithium ion battery, so that the negative electrode material has good cycle stability and rate performance.

[0089] In some embodiments, the lithium-ion battery includes a positive electrode, a negative electrode, a gasket, a spring, a separator and an electrolyte, and the negative electrode is prepared from the above-mentioned electrode materials.

[0090] In some embodiments, the negative electrode further includes a conductive agent (carbon black) and a binder (2% CMC), and the mass ratio of the negative electrode material, the conductive agent and the binder is 7:2:1 or 8:1:1.

[0091] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments, and are only for illustrating the present invention but not limiting the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0092] Example 1

[0093] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0094] The electrode materials were prepared as follows:

[0095] Step 1: Dissolve Bi(NO3)3·5H2O and glutathione (GSH) in deionized water at a molar ratio of 2:3, then stir in a magnetic stirrer for 2 hours to obtain a mixed solution, transfer the mixed solution to a homogeneous reactor with a PTFE liner, and react at 120°C for 12 hours. After cooling to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry it at 60°C for 4 hours to obtain Bi2S3 nanospheres.

[0096] Step 2: Disperse the Bi2S3 nanospheres obtained in step 1 in deionized water, add 0.2 g of glucose and stir for 5 h to obtain a suspension, transfer the suspension to a homogeneous reactor with a PTFE liner, and react at 150°C for 12 h, then cool to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60°C for 4 h, and anneal at 500°C in an Ar atmosphere for 1 h to obtain C@Bi2S3 nanospheres.

[0097] Step 3: Dissolve the C@Bi2S3 nanospheres obtained in step 2 and 0.2 g of boron nitride in deionized water, stir for 4 hours to obtain a suspension, and use a sedimentation method to wash and filter to obtain a black precipitate. Transfer the black precipitate to an oven and dry it at 60°C for 4 hours, then anneal it at 500°C in an Ar atmosphere for 1 hour to obtain CN@Bi2S3 nanospheres.

[0098] Step 4: Disperse the CN@Bi2S3 nanospheres (0.306 g) obtained in step 3 in 750 mL of deionized water and stir for 5 h, then continuously add 0.15 g of triaminemethane, and when the pH value is adjusted to 8.5, add 0.034 g of dopamine hydrochloride, stir overnight, wash and filter to obtain a black precipitate, filter with deionized water and alcohol to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60 ° C for 4 h, and anneal at 500 ° C for 1 h in Ar atmosphere to obtain CN-NC@Bi2S3 nanospheres.

[0099] The negative electrode was prepared as follows:

[0100] The CN-NC@Bi2S3 nanosphere material prepared above was used as the negative electrode active material of the lithium ion battery, carbon black was used as the conductive agent, sodium carboxymethyl cellulose was used as the binder, and deionized water was used as the solvent. The negative electrode active material, the conductive agent, and the binder were mixed evenly at a mass ratio of 7:2:1, and a uniform slurry was formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0101] Example 2

[0102] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0103] The electrode materials were prepared as follows:

[0104] Step 1: Dissolve Bi(NO3)3·5H2O and glutathione (GSH) in deionized water at a molar ratio of 2:3, then stir in a magnetic stirrer for 2 hours to obtain a mixed solution, transfer the mixed solution to a homogeneous reactor with a PTFE liner, and react at 120°C for 12 hours. After cooling to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry it at 60°C for 4 hours to obtain Bi2S3 nanospheres.

[0105] Step 2: Disperse the Bi2S3 nanospheres obtained in step 1 in deionized water, add 0.2 g of glucose and stir for 5 h to obtain a suspension, transfer the suspension to a homogeneous reactor with a PTFE liner, and react at 150°C for 12 h, then cool to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60°C for 4 h, and anneal at 500°C in an Ar atmosphere for 1 h to obtain C@Bi2S3 nanospheres.

[0106] Step 3: Dissolve the C@Bi2S3 nanospheres obtained in step 2 and 0.2 g of boron nitride in deionized water, stir for 4 hours to obtain a suspension, and use a sedimentation method to wash and filter to obtain a black precipitate. Transfer the black precipitate to an oven and dry it at 60°C for 4 hours, then anneal it at 500°C in an Ar atmosphere for 1 hour to obtain CN@Bi2S3 nanospheres.

[0107] Step 4: Disperse the CN@Bi2S3 nanospheres (0.153 g) obtained in step 3 in 750 mL of deionized water and stir for 5 h, then continuously add 0.15 g of triaminemethane, and when the pH value is adjusted to 8.5, add 0.017 g of dopamine hydrochloride, stir overnight, wash and filter to obtain a black precipitate, filter with deionized water and alcohol to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60 ° C for 4 h, and anneal at 500 ° C for 1 h in Ar atmosphere to obtain CN-NC@Bi2S3 nanospheres.

[0108] The negative electrode was prepared as follows:

[0109] The CN-NC@Bi2S3 nanosphere material prepared above was used as the negative electrode active material of the lithium ion battery, carbon black was used as the conductive agent, sodium carboxymethyl cellulose was used as the binder, and deionized water was used as the solvent. The negative electrode active material, the conductive agent, and the binder were mixed evenly at a mass ratio of 7:2:1, and a uniform slurry was formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0110] Example 3

[0111] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0112] The electrode materials were prepared as follows:

[0113] Step 1: Dissolve Bi(NO3)3·5H2O and glutathione (GSH) in deionized water at a molar ratio of 2:3, then stir in a magnetic stirrer for 2 hours to obtain a mixed solution, transfer the mixed solution to a homogeneous reactor with a PTFE liner, and react at 120°C for 12 hours. After cooling to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry it at 60°C for 4 hours to obtain Bi2S3 nanospheres.

[0114] Step 2: Disperse the Bi2S3 nanospheres obtained in step 1 in deionized water, add 0.2 g of glucose and stir for 5 h to obtain a suspension, transfer the suspension to a homogeneous reactor with a PTFE liner, and react at 150°C for 12 h, then cool to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60°C for 4 h, and anneal at 500°C in an Ar atmosphere for 1 h to obtain C@Bi2S3 nanospheres.

[0115] Step 3: Dissolve the C@Bi2S3 nanospheres obtained in step 2 and 0.2 g of boron nitride in deionized water, stir for 4 hours to obtain a suspension, and use a sedimentation method to wash and filter to obtain a black precipitate. Transfer the black precipitate to an oven and dry it at 60°C for 4 hours, then anneal it at 500°C in an Ar atmosphere for 1 hour to obtain CN@Bi2S3 nanospheres.

[0116] Step 4: Disperse the CN@Bi2S3 nanospheres (0.306 g) obtained in step 3 in 750 mL of deionized water and stir for 5 h, then continuously add 0.15 g of triaminemethane, and when the pH value is adjusted to 9.5, add 0.034 g of dopamine hydrochloride, stir overnight, wash and filter to obtain a black precipitate, filter with deionized water and alcohol to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60 ° C for 4 h, and anneal at 500 ° C for 1 h in Ar atmosphere to obtain CN-NC@Bi2S3 nanospheres.

[0117] The negative electrode was prepared as follows:

[0118] The CN-NC@Bi2S3 nanosphere material prepared above was used as the negative electrode active material of the lithium ion battery, carbon black was used as the conductive agent, sodium carboxymethyl cellulose was used as the binder, and deionized water was used as the solvent. The negative electrode active material, the conductive agent, and the binder were mixed evenly at a mass ratio of 7:2:1, and a uniform slurry was formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0119] Example 4

[0120] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0121] The electrode materials were prepared as follows:

[0122] Step 1: Dissolve Bi(NO3)3·5H2O and glutathione (GSH) in deionized water at a molar ratio of 2:3, then stir in a magnetic stirrer for 2 hours to obtain a mixed solution, transfer the mixed solution to a homogeneous reactor with a PTFE liner, and react at 120°C for 12 hours. After cooling to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry it at 60°C for 4 hours to obtain Bi2S3 nanospheres.

[0123] Step 2: Disperse the Bi2S3 nanospheres obtained in step 1 in deionized water, add 0.2 g of glucose and stir for 5 h to obtain a suspension, transfer the suspension to a homogeneous reactor with a PTFE liner, and react at 150°C for 12 h, then cool to room temperature, wash and filter to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60°C for 4 h, and anneal at 500°C in an Ar atmosphere for 1 h to obtain C@Bi2S3 nanospheres.

[0124] Step 3: Dissolve the C@Bi2S3 nanospheres obtained in step 2 and 0.2 g of boron nitride in deionized water, stir for 4 hours to obtain a suspension, and use a sedimentation method to wash and filter to obtain a black precipitate. Transfer the black precipitate to an oven and dry it at 60°C for 4 hours, then anneal it at 500°C in an Ar atmosphere for 1 hour to obtain CN@Bi2S3 nanospheres.

[0125] Step 4: Disperse the CN@Bi2S3 nanospheres (0.306 g) obtained in step 3 in 750 mL of deionized water and stir for 5 h, then continuously add 0.15 g of triaminemethane, and when the pH value is adjusted to about 8.5, add 0.034 g of dopamine hydrochloride, stir overnight, wash and filter to obtain a black precipitate, filter with deionized water and alcohol to obtain a black precipitate, transfer the black precipitate to an oven and dry at 60 ° C for 4 h, and anneal at 500 ° C for 1 h in Ar atmosphere to obtain CN-NC@Bi2S3 nanospheres.

[0126] The negative electrode was prepared as follows:

[0127] The CN-NC@Bi2S3 nanosphere material prepared above was used as the negative electrode active material of the lithium ion battery, carbon black was used as the conductive agent, sodium carboxymethyl cellulose was used as the binder, and deionized water was used as the solvent. The negative electrode active material, the conductive agent, and the binder were mixed evenly at a mass ratio of 7:2:1, and a uniform slurry was formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0128] Comparative Example 1

[0129] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0130] The electrode materials were prepared as follows:

[0131] Step 1: Dissolve 0.2425 g of bismuth nitrate pentahydrate (Bi(NO3)3·5H2O) in 30 mL of deionized water and stir rapidly for 1 h to obtain solution A;

[0132] Step 2: Add 0.3073 g of glutathione (GSH) to solution A and stir for 1 h to obtain turbid solution B;

[0133] Step 3: Transfer the turbid liquid B to a 50 mL homogeneous reactor with a polytetrafluoroethylene liner and react at 120°C for 12 hours. After cooling to room temperature, filter with deionized water and alcohol to obtain a black precipitate, place the black precipitate in an oven and keep it at 60°C for 12 hours to obtain Bi2S3 nanospheres.

[0134] The negative electrode was prepared as follows:

[0135] The Bi2S3 nanosphere material prepared above is used as the negative electrode active material of the lithium ion battery, carbon black is used as the conductive agent, sodium carboxymethyl cellulose is used as the binder, and deionized water is used as the solvent. The negative electrode active material, the conductive agent, and the binder are mixed evenly at a mass ratio of 7:2:1, and a uniform slurry is formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0136] Comparative Example 2

[0137] A preparation method for a negative electrode of a lithium ion battery comprises the following steps:

[0138] The electrode materials were prepared as follows:

[0139] Step 1: 10 mmol of melamine was dissolved in 30 mL of ethanol and stirred for 30 min, then 3 mL of formaldehyde solution was added dropwise thereto and stirred for 1 h to obtain a mixed solution A, 1 mmol of citric acid was added to the solution A and stirred for 1 h, then the solution was transferred to a high-pressure reactor, the high-pressure reactor was placed in a blast dryer, reacted at 200° C. for 10 h, the obtained product was washed with water and ethanol, and then placed in a vacuum drying oven at 60° C. for 8 h to obtain a powder sample B;

[0140] Step 2: Place the powder sample B obtained in step 1 in a tube furnace and anneal it in an Ar atmosphere at a temperature of 750°C and a heating rate of 5°C min. -1 , annealing time is 2h, and finally NC material is obtained.

[0141] The negative electrode was prepared as follows:

[0142] The Bi2S3 nanosphere material prepared above is used as the negative electrode active material of the lithium ion battery, carbon black is used as the conductive agent, sodium carboxymethyl cellulose is used as the binder, and deionized water is used as the solvent. The negative electrode active material, the conductive agent, and the binder are mixed evenly at a mass ratio of 7:2:1, and a uniform slurry is formed by stirring for 12 hours, and then coated on the copper foil with a 16μm scraper, dried in a vacuum drying oven at 80°C for 12 hours, and then cut into discs with a diameter of 12mm.

[0143] Application Examples

[0144] The lithium-ion battery used the negative electrode prepared in the above examples 1-4 and comparative examples 1 and 2 as the working electrode, lithium metal foil as the counter electrode, Whatman GF / A glass fiber filter as the separator, and 1.0 mol L electrolyte. -1 LiPF6, the solution is ethylene carbonate-dimethyl carbonate (1:1 vol%), and the assembly process is as follows Figure 1 All batteries were assembled in a glove box and then placed in a 25°C thermostat for 6 h before electrochemical performance testing.

[0145] Electrochemical performance test methods

[0146] Using LAND CT2001A battery tester system, 0.01-3.0V vs.Li / Li + The constant current charge and discharge processes were carried out under a voltage range and different current densities. At the same time, the cyclic voltammetry (CV) curves and electrochemical impedance spectroscopy (EIS) were recorded on a CS2350H electrochemical workstation at ambient temperature (~25°C).

[0147] Performance testing experiment

[0148] X-ray diffraction test was performed on the negative electrode materials of Example 1 and Comparative Example 1. The test results are as follows: Figure 2 shown.

[0149] The diffraction peaks of Example 1 and Comparative Example 1 both match well with the standard comparison card (PDF#17-0320), showing good crystallinity.

[0150] The negative electrode material prepared in Example 1 was tested by scanning electron microscope. The test results are as follows: Figure 3 shown.

[0151] The high-resolution XPS spectra of Bi 4f and S2p of the samples are shown in Figure 2. Figure 3 As shown in a, Bi 4f 7 / 2 and 4f 5 / 2 The peaks are located at around 159eV and 164eV respectively. There are also two weak peaks at 158.61 and 159.88eV, which belong to S 2- Substance S2p 3 / 2 and S2p 1 / 2 The presence of these elements indicates that sulfur atoms are bound to bismuth. Figure 3 Figure b shows the presence of CC (283.30 eV), CN (284.87 eV) and C=O (287.20 eV)11,29. CC and CN may originate from the decomposition of dopamine hydrochloride. The high-resolution XPS spectrum of N 1s is shown in Figure 2. Figure 3 As shown in Figure c, the N 1s peak consists of two main peaks. The peak at 395.6 eV belongs to pyridinic nitrogen, while the peak at 397.5 eV belongs to graphitic nitrogen, and the peaks at 402.8 eV and 404.3 eV belong to pyrrolic nitrogen and N-oxide, respectively. The presence of four types of nitrogen indicates that nitrogen atoms are successfully doped into the amorphous carbon layer during the carbonization process. The results show that the types of nitrogen are mainly highly active pyridinic nitrogen and N-oxide with high electronic conductivity. The abundant nitrogen elements in the amorphous carbon layer provide more lithium reaction sites and improve the adsorption capacity of polysulfides due to the increase in polarity, which plays an important role in improving electrode kinetics and maintaining structural integrity.

[0152] The negative electrode material prepared in Example 1 was tested by scanning electron microscope. The test results are as follows: Figure 4 shown.

[0153] The morphology of the negative electrode material is nanospheres, and the thickness of the CN-CN layer is about 20nm.

[0154] The negative electrode materials prepared in Example 1 and Comparative Example 1 were subjected to constant current charge and discharge performance tests. The test results are as follows: Figure 5 , Figure 6 , Figure 7 shown.

[0155] from Figure 5It can be seen that the first cycle discharge capacity of the negative electrode material prepared in Example 1 reached 753 mAh g -1 The charge and discharge curves from the 100th to the 200th cycle almost overlap, indicating that the negative electrode material has good cycle stability; when it cycles to the 200th cycle, the coulomb efficiency is 99.46%, which indicates that the energy loss is small.

[0156] from Figure 6 It can be seen that the first cycle discharge capacity of the negative electrode material prepared in Comparative Example 1 is 830.8 mAh g -1 As the charge and discharge proceed, the discharge specific capacity continues to decay and the stability is poor. The coulomb efficiency of the 100th cycle is 97.03%, and the energy loss is higher than that of the negative electrode material prepared in Example 1.

[0157] like Figure 7 As shown in Figure 2, the reversible specific capacity of the negative electrode material prepared in Comparative Example 1 is finally stabilized at 343.9 mAh g -1 The reversible specific capacity of the negative electrode material prepared in Example 1 was finally stabilized at 636.1 mAh g -1 Compared with the negative electrode material of Comparative Example 1, the cycle stability of the negative electrode material prepared in Example 1 is greatly improved, and the final electrochemical performance is significantly improved.

[0158] The negative electrode materials prepared in Example 1 and Comparative Example 1 were subjected to rate performance tests. Figure 8 As shown in the figure, Comparative Example 1 exhibits poor rate performance. After charging and discharging at a large current density, its structure is destroyed, and its performance cannot be restored when it is discharged at a low current density, indicating that it cannot withstand a fast discharge / charge rate due to its limited conductivity and drastic volume change during the lithiation / degradation reaction. In contrast, the capacity of Example 1 at current densities of 0.1A / g, 0.2A / g, 0.5A / g and 1A / g is 643.9mAh g -1 、536.1mAh g -1 、454.7mAh g -1 and 345.3mAh g -1 When the current density returned to 0.1A / g, the reversible capacity of the negative electrode material gradually recovered to 576.3mAh g-1, which shows that even in the process of rapid lithiation / attenuation, the negative electrode material is tightly fixed on the electrode, showing good rate performance. After high-rate charge and discharge, the battery performance is basically unchanged when it returns to low-rate charge and discharge, and can be restored to the performance of the first charge and discharge at this rate.

[0159] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.

Claims

1. An electrode material, characterized in that: The electrode material includes bismuth sulfide, a carbon layer coated on the surface of the bismuth sulfide, a nitrogen layer coated on the surface of the carbon layer, and a nitrogen-carbon layer coated on the surface of the nitrogen layer.

2. The electrode material according to claim 1, characterized in that The bismuth sulfide has a spherical shape and a diameter of 1-2 μm.

3. The electrode material according to claim 1, characterized in that The thickness of the carbon layer is 5-10 nm.

4. The electrode material according to claim 1, characterized in that The thickness of the nitrogen layer is 5-10 nm.

5. The electrode material according to claim 1, characterized in that The thickness of the nitrogen-carbon layer is 10-20 nm.

6. The electrode material according to claim 1, characterized in that In the nitrogen-carbon layer, the mass ratio of nitrogen to carbon is 0.

2.

7. A method for preparing an electrode material, characterized in that: The preparation method comprises the following steps: Preparation of bismuth sulfide; The bismuth sulfide and the carbon source are dissolved in a first solvent, and subjected to a hydrothermal treatment and a first annealing treatment in sequence, so that carbon is coated on the surface of the bismuth sulfide, which is recorded as C@Bi2S3; The C@Bi2S3 and the nitrogen source are dissolved in a second solvent, and a first deposition process and a second annealing process are sequentially performed, so that nitrogen is coated on the surface of the C@Bi2S3, which is recorded as CN@Bi2S3; The CN@Bi2S3 is dissolved in a third solvent, the pH value is adjusted to 7.5-9.5, and then a nitrogen and carbon source is added, and a second deposition treatment and a third annealing treatment are performed in sequence, so that nitrogen and carbon are coated on the surface of the CN@Bi2S3 to obtain the electrode material, which is recorded as CN-NC@Bi2S3.

8. The method for preparing the electrode material according to claim 7, characterized in that: The carbon source is selected from one or more of glucose, sodium acetate and methanol; The nitrogen source is selected from one or more of urea, boron nitride and cyanide; The nitrogen and carbon source is selected from one or more of melamine, ethylenediamine, and dopamine hydrochloride; The first solvent, the second solvent and the third solvent are each independently selected from deionized water or ethanol.

9. The method for preparing an electrode material according to claim 7, characterized in that: The temperature of the hydrothermal treatment is 120-150°C, and the time of the hydrothermal treatment is 10-12h; The temperature of the first annealing treatment is 400-500° C., and the time of the first annealing treatment is 1-5 hours; The temperature of the second annealing treatment is 400-500°C, and the time of the second annealing treatment is 1-5h; The temperature of the third annealing treatment is 400-500° C., and the time of the third annealing treatment is 1-5 hours; The first deposition process and the second deposition process are each independently selected from spin coating, dipping, and spraying.

10. A lithium ion battery, comprising a negative electrode material, characterized in that: The negative electrode material includes the electrode material according to any one of claims 1 to 6 or an electrode material prepared by the preparation method according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • Bismuth sulfide electrode material with specific morphologic structure and application thereof

    CN106299357A

  • Preparation method of multi-protection stable iron electrode as well as product and application of multi-protection stable iron electrode

    CN117691033A

  • KR20210021756A