Composite positive electrode material, preparation method thereof and sodium ion battery
By introducing a hydrophobic coating of fluorinated silicon oxide on the surface of the layered positive electrode material of sodium ion battery, the problems of poor air stability and high surface residual alkali content are solved, and better electrochemical performance and battery safety are achieved.
Patent Information
- Application Number
- CN202411278854.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-12
- Publication Date
- 2024-11-12
AI Technical Summary
The existing sodium ion battery layered cathode materials have problems such as poor air stability and high residual alkali content on the surface, which leads to an increase in storage and transportation costs and increases the risk of battery thermal runaway during the circulation.
Using composite positive electrode material, including the hydrophobic coating of the matrix material NaNiaFebMncO2 and fluorinated silicon oxide (F-SiO2), prepared by high-temperature calcination treatment and high-speed centrifugal drying, the surface of the fluorinated silicon oxide is in close contact with the layered oxide matrix material, reducing the surface of the Surface activity and CEI membrane is constructed through Na-F interaction to improve air stability.
It effectively reduces the surface activity of the material, improves air stability and electrochemical performance, reduces the risk of thermal runaway during battery circulation, and controls the amount of residual alkali on the surface, improving the high and low temperature performance of the battery.
Smart Images

Figure CN118943340A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of material technology, and in particular relates to a composite positive electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Compared with lithium-ion batteries, sodium-ion batteries have developed more slowly. However, in practical applications, due to the scarcity and uneven distribution of lithium resources, many researchers and companies have turned their attention to sodium-ion batteries in recent years. The working principle and preparation process of sodium-ion batteries are basically the same as those of lithium-ion batteries, and sodium resources are rich and evenly distributed. Therefore, sodium-ion batteries have the potential for large-scale production.
[0003] At present, the layered cathode materials of sodium-ion batteries have good high and low temperature performance, but their high surfactant content greatly increases the storage and transportation costs. The increase of residual alkali on the surface of the material not only accelerates capacity decay, but also decomposes and produces gas during the cycle, which also increases the risk of thermal runaway of the battery.
[0004] It can be seen that the existing layered positive electrode materials for sodium ion batteries have the problems of poor air stability and high residual alkali content on the material surface. Summary of the invention
[0005] The purpose of the embodiments of the present application is to provide a composite positive electrode material, aiming to solve the problems of poor air stability and high residual alkali content on the surface of the existing sodium ion battery layered positive electrode materials.
[0006] The embodiment of the present application is implemented as follows: a composite positive electrode material, the composite positive electrode material comprising a base material and a hydrophobic coating coated on the surface of the base material;
[0007] Wherein, the matrix is NaNi a Fe b Mn c O2, a+b+c=1, 0≤a<1, 0≤b<1, 0≤c<1;
[0008] The hydrophobic coating is fluorinated silicon oxide.
[0009] The present application also provides a method for preparing the composite positive electrode material, comprising:
[0010] The precursor obtained by mixing the sodium source, the nickel source, the iron source and the manganese source is subjected to high temperature calcination treatment to obtain a matrix material;
[0011] Add tetraethyl orthosilicate to the mixed solvent of ammonia water and anhydrous ethanol and mix well, then add C 16 F 17 H 19O3Si is reacted, and after high-speed centrifugation, it is dried at a temperature below 300°C to obtain fluorinated silicon oxide;
[0012] The matrix material is added into an ethanol solution of fluorinated silicon oxide and stirred, and dried at a temperature below 300° C. to obtain a composite positive electrode material.
[0013] An embodiment of the present application further provides a sodium ion battery, which includes the above-mentioned composite positive electrode material or the composite positive electrode material prepared by the above-mentioned method for preparing the composite positive electrode material.
[0014] An embodiment of the present application provides a composite positive electrode material, which reduces the surface activity of the matrix material by anchoring fluorinated silicon oxide on the surface of a layered oxide matrix material, thereby making it have better air stability; wherein the fluorinated functional groups in the fluorinated silicon oxide coordinate sodium ions through Na-F interaction, so that the fluorinated silicon oxide is in close contact with the material surface, and the outward fluorinated functional groups construct a CEI film during the battery cycle to accelerate the transmission of lithium ions. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a SEM image of the composite positive electrode material provided in Example 1 of the present application;
[0016] Figure 2 The SEM image of the substrate material provided for Comparative Example 1 of the present application;
[0017] Figure 3 A contact angle test diagram of the base material provided in Comparative Example 1 of the present application;
[0018] Figure 4 This is a contact angle test diagram of the composite positive electrode material provided in Example 1 of the present application. DETAILED DESCRIPTION
[0019] In order to make the purpose, technical solution and advantages of the present application more clearly understood, the present application is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.
[0020] The present application provides a composite positive electrode material, which includes a base material and a hydrophobic coating applied on the surface of the base material; wherein the base material is NaNi a Fe b Mn c O2 (a+b+c=1, 0≤a<1, 0≤b<1, 0≤c<1); the hydrophobic coating is fluorinated silicon oxide (F-SiO2).
[0021] In the embodiments of the present application, the composite positive electrode material has a block-like or spherical morphology.
[0022] In the embodiment of the present application, the single crystal particle size of the composite positive electrode material is 2 to 10 nm.
[0023] In the embodiment of the present application, the residual alkali CO3 of the composite positive electrode material 2- <5000ppm,OH - <4000ppm.
[0024] In the embodiment of the present application, the specific surface area of the composite positive electrode material is 0.5 to 5 m 2 ·g -1 .
[0025] The present application also provides a method for preparing the composite positive electrode material, comprising:
[0026] The precursor obtained by mixing the sodium source, the nickel source, the iron source and the manganese source is subjected to high temperature calcination treatment to obtain a matrix material;
[0027] Add tetraethyl orthosilicate to the mixed solvent of ammonia water and anhydrous ethanol and mix well, then add C 16 F 17 H 19 O3Si is reacted, and after high-speed centrifugation, it is dried at a temperature below 300°C to obtain fluorinated silicon oxide;
[0028] The matrix material is added into an ethanol solution of fluorinated silicon oxide and stirred, and dried at a temperature below 300° C. to obtain a composite positive electrode material.
[0029] In the embodiments of the present application, the sodium source, nickel source, iron source, and manganese source are halide salts, nitrates, or sulfates corresponding to sodium, nickel, iron, and manganese, respectively. For example, the sodium source can be sodium chloride, sodium bromide, sodium fluoride, sodium iodide, sodium nitrate, sodium sulfate, etc. Those skilled in the art can determine the type of each metal source according to the ratio. Although the following specific embodiments only take chloride as an example, this should not limit the scope of protection of the present application.
[0030] In the embodiment of the present application, in the step of calcining the precursor obtained by mixing the sodium source, the nickel source, the iron source and the manganese source at high temperature to obtain the matrix material, if the calcination temperature is too low, the crystallinity of the material will be poor and it will not be a pure phase; if the calcination temperature is too high, the primary particles may aggregate seriously, so that the Na + The migration distance increases, both of which will affect the final electrochemical performance. Therefore, the temperature of the high-temperature calcination treatment should be controlled at 920-1050°C and the time should be 8-12h.
[0031] Optionally, the step of subjecting a precursor obtained by mixing a sodium source, a nickel source, an iron source and a manganese source to a high-temperature calcination treatment to obtain a matrix material includes: mixing the sodium source, the nickel source, the iron source and the manganese source in a solvent such as water or an alcohol solvent and then transferring the mixture to an atomizer for atomization, and using a hot air flow to instantly volatilize water vapor to obtain a positive electrode material precursor; then, the precursor is calcined at a high temperature to form a layered single crystal matrix material.
[0032] In the embodiment of the present application, after adding tetraethyl orthosilicate to the mixed solvent of ammonia water and anhydrous ethanol and mixing evenly, C 16 F 17 H 19 O3Si is reacted, and after high-speed centrifugation, it is dried at a temperature below 300°C to obtain fluorinated silicon oxide. The reaction temperature is 60-80°C, the reaction time is 5-7h, and the rotation speed of high-speed centrifugation is not less than 10000r / min, preferably 10000-12000r / min.
[0033] It is worth noting that the embodiment of the present application obtains fluorinated silicon oxide by high-speed centrifugation of the mixed solution and drying at a temperature below 300°C, which can effectively remove the perfluorodecyltriethoxysilane that does not participate in the reaction, thereby improving the purity. In addition, based on a bottom-up method, the present application prepares F-SiO2 powder by grafting fluorinated components on organic silane. Due to the increase in surface roughness and the introduction of fluorinated groups, the particle surface energy of the powder is extremely low and has a certain degree of hydrophobicity.
[0034] In the embodiment of the present application, the concentration of the ethanol solution of fluorinated silicon oxide is 0.05-2 g / L, wherein too high a concentration will affect the dispersion effect of fluorinated silicon oxide, and too low a concentration will affect the distribution effect of fluorinated silicon oxide on the material surface.
[0035] In an embodiment of the present application, the matrix material is added to an ethanol solution of fluorinated silicon oxide for stirring treatment, and dried at a temperature below 300°C to obtain a composite positive electrode material, and the stirring treatment time is 3-5h. Among them, the fluorinated functional groups in F-SiO2 will coordinate sodium ions through Na-F interactions during the stirring process, and the outward fluorinated functional groups can construct a CEI film during the battery cycle. Fluorinated silicon oxide is anchored to the surface of the layered oxide material through a variety of interfacial interaction forces (such as hydrogen bonds or electrostatic interactions), thereby reducing the surface activity of the material and making it have better air stability; the present application exposed the obtained composite positive electrode material to the air for 30 days, and then conducted a cycle performance test again. The electrochemical test results show that the material is not affected by air.
[0036] In addition, the drying temperature needs to be strictly controlled in the above steps. The higher the drying temperature, the more it affects the hydrophobic properties of the coating. For example, when the drying temperature reaches above 270°C, the hydrophobic properties of the coating begin to decrease. When the drying temperature exceeds 300°C, the surface coating will become amorphous, causing the coating to lose a certain degree of hydrophobic properties. At the same time, the organic coating will also react with transition metal ions during the high temperature process, resulting in the loss of active substances. Moreover, high temperature causes the fluorinated silicon oxide to decompose into silicates and hydrogen fluoride. The strong acidity of hydrogen fluoride will cause the transition metal to dissolve.
[0037] The specific examples of the embodiments of the present application are given below. It should be understood that these examples are only used to illustrate the present application and are not used to limit the scope of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present application. Unless otherwise defined, the professional terms used below are consistent with the meanings understood by professional and technical personnel in the field; unless otherwise specified, the raw materials and reagents involved in the present application can be purchased from the market or prepared by known methods.
[0038] In addition, it should be noted that the numerical values given in the following examples are as accurate as possible, but those skilled in the art understand that due to unavoidable measurement errors and experimental operation problems, each number should be understood as an approximate number rather than an absolutely accurate value.
[0039] Example 1
[0040] Weigh 43.2g of nickel chloride, 54g of ferric chloride, 41.82g of manganese chloride, and 64.2g of sodium chloride respectively, pour them into a 3L beaker, add 1L of deionized water, and mechanically stir at a speed of 600r / min for 30min to obtain a uniformly mixed metal salt solution. Transfer the uniform metal salt solution to an atomizer for atomization, and instantly dry the water by spray drying technology to obtain a matrix material precursor. Pour the matrix material precursor into a crucible and calcine in an air atmosphere. The calcination temperature is 1000℃, the calcination time is 12h, and the heating rate is 4℃ / min. After the box furnace is cooled to below 100℃, the matrix material is obtained. The matrix material is sodium nickel copper iron manganese oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0041] Weigh 5 mL of ethyl orthosilicate and add it to 58 mL of ammonia water and 100 mL of anhydrous ethanol, stir for 1 h, then add 0.25 mL of C 16 F 17 H 19O3Si continued to react at 65°C for 6 hours, and finally centrifuged at 10000 r / min and dried at 100°C to obtain F-SiO2.
[0042] 1g of layered single crystal sodium ion battery cathode material was added with 0.2g·L -1 The obtained product was stirred in F-SiO2 ethanol solution for 4 h and then vacuum dried at 100 °C for 1 h to obtain a layered single crystal sodium ion battery composite positive electrode material.
[0043] Example 2
[0044] Weigh 43.2g of nickel chloride, 54g of ferric chloride, 41.82g of manganese chloride, and 64.2g of sodium chloride respectively, pour them into a 3L beaker, add 1L of deionized water, and mechanically stir at a speed of 600r / min for 30min to obtain a uniformly mixed metal salt solution. Transfer the uniform metal salt solution to an atomizer for atomization, and instantly dry the water by spray drying technology to obtain a matrix material precursor. Pour the matrix material precursor into a crucible and calcine in an air atmosphere. The calcination temperature is 1000℃, the calcination time is 12h, and the heating rate is 4℃ / min. After the box furnace is cooled to below 100℃, the matrix material is obtained. The matrix material is sodium nickel copper iron manganese oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0045] Weigh 5 mL of ethyl orthosilicate and add it to 58 mL of ammonia water and 100 mL of anhydrous ethanol, stir for 1 h, then add 0.25 mL of C 16 F 17 H 19 O3Si continued to react at 65°C for 6 hours, and finally centrifuged at 10000 r / min and dried at 100°C to obtain F-SiO2.
[0046] 1g of layered single crystal sodium ion battery cathode material was added with 0.1g·L -1 The obtained product was stirred in F-SiO2 ethanol solution for 4 h and then vacuum dried at 100 °C for 1 h to obtain a layered single crystal sodium ion battery composite positive electrode material.
[0047] Example 3
[0048] Weigh 43.2g of nickel chloride, 54g of ferric chloride, 41.82g of manganese chloride, and 64.2g of sodium chloride respectively, pour them into a 3L beaker, add 1L of deionized water, and mechanically stir at a speed of 600r / min for 30min to obtain a uniformly mixed metal salt solution. Transfer the uniform metal salt solution to an atomizer for atomization, and instantly dry the water by spray drying technology to obtain a matrix material precursor. Pour the matrix material precursor into a crucible and calcine in an air atmosphere. The calcination temperature is 1000℃, the calcination time is 12h, and the heating rate is 4℃ / min. After the box furnace is cooled to below 100℃, the matrix material is obtained. The matrix material is sodium nickel copper iron manganese oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0049] Weigh 5 mL of ethyl orthosilicate and add it to 58 mL of ammonia water and 100 mL of anhydrous ethanol and stir for 1 h. Then add 0.25 mL of C 16 F 17 H 19 O3Si continued to react at 65°C for 6 hours, and finally centrifuged at 10000 r / min and dried at 100°C to obtain F-SiO2.
[0050] 1g of layered single crystal sodium ion battery cathode material was added with 0.3g·L -1 The obtained product was stirred in F-SiO2 ethanol solution for 4 h and then vacuum dried at 100 °C for 1 h to obtain a layered single crystal sodium ion battery composite positive electrode material.
[0051] Example 4
[0052] After the composite positive electrode material prepared in Example 1 was exposed to air for 30 days, 2032 button batteries were assembled and electrochemical performance tested.
[0053] Comparative Example 1
[0054] Weigh 43.2g of nickel chloride, 54g of ferric chloride, 41.82g of manganese chloride, and 64.2g of sodium chloride respectively, pour them into a 3L beaker, add 1L of deionized water, and mechanically stir at a speed of 600r / min for 30min to obtain a uniformly mixed metal salt solution. Transfer the uniform metal salt solution to an atomizer for atomization, and instantly dry the water by spray drying technology to obtain a matrix material precursor. Pour the matrix material precursor into a crucible and calcine in an air atmosphere. The calcination temperature is 1000℃, the calcination time is 12h, and the heating rate is 4℃ / min. After the box furnace is cooled to below 100℃, the matrix material is obtained. The matrix material is sodium nickel copper iron manganese oxide NaNi 1 / 3 Fe 1 / 3 Mn 1 / 3 O2.
[0055] Comparative Example 2
[0056] After the base material obtained in Comparative Example 1 was exposed to air for 30 days, 2032 button batteries were assembled and electrochemical performance tested.
[0057] The composite positive electrode material prepared in Example 1 and the matrix material prepared in Comparative Example 1 were subjected to SEM and hydrophilic performance tests respectively. Figure 1-2 As shown, many small particles are attached to the surface of the composite positive electrode material prepared in Example 1, while the surface of the base material prepared in Comparative Example 1 is very smooth, indicating that F-SiO2 is effectively anchored on the surface of the material. Figure 3-4 The contact angle test results with water show that the composite positive electrode material prepared in Example 1 exhibits certain hydrophobicity.
[0058] The composite positive electrode materials corresponding to Examples 1-4 and the matrix materials corresponding to Comparative Examples 1-2 were used as positive electrode active materials to prepare positive electrode sheets, and metal Na was used as the negative electrode to obtain button batteries. The electrochemical performance of the batteries provided by Examples 1-4 and Comparative Example 1 was tested: the voltage was 2 to 4V, and the rate was 0.1C during the first week of charging and discharging. The first charge and discharge specific capacity was measured to obtain the first efficiency. At the same time, the physical and chemical performance pH of Examples 1-4 and Comparative Examples 1-2 was also tested. The test results are shown in Table 1:
[0059] Table 1
[0060]
[0061]
[0062] In summary, it can be seen from Table 1 that after the introduction of F-SiO2 on the surface of the layered sodium ion positive electrode material in the embodiment of the present application, the pH value of the material can be significantly reduced, indicating that the surface residual alkali is effectively controlled. Due to its high air stability, the composite positive electrode material exhibits a high specific capacity and initial efficiency.
[0063] In addition, although the F-SiO2 coating has a lower surface energy, if its content is too high, it will increase the interfacial impedance and lead to a decrease in capacity; it has been determined through experiments that the electrochemical performance of the composite positive electrode material synthesized at 4%wt is reduced, so its usage should not exceed 4%wt.
[0064] In addition, by comparing the performance of Example 4 and Comparative Example 2, it can be found that the introduction of F-SiO2 coating on the surface of the layered sodium ion positive electrode material in the present application can improve the air stability of the positive electrode material, thereby effectively protecting the base material.
[0065] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the present application. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the present application shall be subject to the attached claims.
[0066] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
Claims
1. A composite positive electrode material, characterized in that: The composite positive electrode material comprises a base material and a hydrophobic coating coated on the surface of the base material; Wherein, the matrix is NaNi a Fe b Mn c O2, a+b+c=1, 0≤a<1, 0≤b<1, 0≤c<1; The hydrophobic coating is fluorinated silicon oxide.
2. The composite positive electrode material according to claim 1, characterized in that The single crystal particle size of the composite positive electrode material is 2 to 10 nm.
3. The composite positive electrode material according to claim 1, characterized in that The residual alkali CO3 of the composite positive electrode material 2- <5000ppm,OH - <4000ppm; the specific surface area of the composite positive electrode material is 0.5 to 5m 2 ·g -1 .
4. A method for preparing the composite positive electrode material according to claim 1, characterized in that: include: The precursor obtained by mixing the sodium source, the nickel source, the iron source and the manganese source is subjected to high temperature calcination treatment to obtain a matrix material; Add tetraethyl orthosilicate to the mixed solvent of ammonia water and anhydrous ethanol and mix well, then add C 16 F 17 H 19 O3Si is reacted, and after high-speed centrifugation, it is dried at a temperature below 300°C to obtain fluorinated silicon oxide; The matrix material is added into an ethanol solution of fluorinated silicon oxide and stirred, and dried at a temperature below 300° C. to obtain a composite positive electrode material.
5. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The sodium source, nickel source, iron source and manganese source are halide salts, nitrates or sulfates corresponding to sodium, nickel, iron and manganese respectively.
6. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The temperature of high temperature calcination treatment is 920-1050°C and the time is 8-12h.
7. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The reaction temperature is 60-80°C and the reaction time is 5-7h.
8. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The rotation speed of high-speed centrifugal treatment is not less than 10000r / min.
9. The method for preparing a composite positive electrode material according to claim 4, characterized in that: The concentration of the fluorinated silicon oxide ethanol solution is 0.05-2 g / L.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the composite positive electrode material according to any one of claims 1 to 3 or a composite positive electrode material prepared by the method for preparing the composite positive electrode material according to any one of claims 4 to 9.