Silicon-carbon composite material with stable conductive network and enhanced elastic copper nano welding structure as well as preparation method and application of silicon-carbon composite material

By introducing an elastic copper nano-welded structure into silicon-carbon composite materials, the problem of conductive network damage caused by silicon particle volume expansion was solved, achieving high capacity and stable electrode performance. The preparation method is simple and low-cost.

CN118943350APending Publication Date: 2024-11-12MONTA VISTA ENERGY TECH CORP (ANHUI)

Patent Information

Application Number
CN202310542300.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing silicon-carbon composite materials suffer from electrode failure due to the volume expansion of silicon particles during charging and discharging, which damages the conductive network and makes it difficult to achieve high capacity and long-term stability.

Method used

An elastic copper nano-welding structure is used to enhance the conductive network. By coating the surface of silicon particles with copper nano-thin layers and carbon nano-thin layers, copper nano-welding points are formed to accommodate volume expansion and maintain the stability of the conductive network.

Benefits of technology

A high-capacity silicon-carbon composite material is obtained by maintaining a good and stable conductive network during electrochemical charging and discharging. The preparation method is simple, low-cost, and easy to scale up.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943350A_ABST
    Figure CN118943350A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-carbon composite material with an elastic copper nano welding structure enhanced and a stable conductive network and a preparation method of the silicon-carbon composite material. The silicon-carbon composite material has a copper nano welding structure, and the copper nano welding structure generates elastic deformation when the volume of the silicon-containing particles is expanded to keep the contact between the silicon-containing particles and the carbon material and maintain the electrode performance. The preparation method comprises the following steps: depositing copper hydroxide on the surfaces of silicon-containing particles, then reducing the copper hydroxide into a copper nano thin layer, mixing the copper nano thin layer with a carbon material, removing oxygen atoms in copper in a high-temperature hydrogen and argon atmosphere, melting the copper nano thin layer into liquid at a low temperature, shrinking the copper metal liquid to a contact point, and catalyzing the surface of the copper metal liquid to generate a carbon wrapping layer after introducing carbon source gas. The silicon-carbon composite material provided by the invention ensures that a good conductive network is kept during volume expansion of silicon-containing particles, and high-reversible high-capacity negative electrode performance is obtained. The preparation method has high conductive stability and low cost, and is beneficial to popularization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of lithium-ion batteries, and specifically relates to a silicon-carbon composite material with an elastic copper nano-welding structure to enhance the stability of the conductive network, and a preparation method and application thereof. Background Art

[0002] High-capacity lithium-ion battery silicon-carbon composite materials are a type of new energy material that has been focused on in recent years. Silicon as a silicon-carbon composite material has an ultra-high theoretical capacity of 4200mAh / g, but the silicon material undergoes huge volume changes during the process of lithium insertion and removal during charging and discharging, and its volume expansion is greater than 300%, resulting in the internal structure of the silicon-based negative electrode being relaxed after repeated charge and discharge cycles, the conductive network being destroyed, the contact between the active particles and the conductive agent being destroyed, the active components no longer participating in the charge and discharge process, and the electrode completely failing after several cycles. Therefore, it is of great practical significance to overcome this problem and develop silicon-based silicon-carbon composite materials with good structural stability.

[0003] To solve this problem, researchers have tried many technical solutions, mainly focusing on three aspects: (1) Nano-silicon technology, which obtains small-sized electrochemically active particles through nano-processing of silicon and its oxides, so that their volume expansion does not cause the active particles to rupture, thereby maintaining the integrity of their basic units; (2) Silicon surface coating technology, which enhances the conductive network by coating with an inorganic layer and makes it more resistant to the expansion and contraction of the particles; (3) Spatial structure regulation strategy, which constructs a porous spatial structure so that its volume expansion is offset by the pore space reserved inside, reducing the macroscopic internal stress of the active particles caused by the expansion, thereby improving the stability of the negative electrode.

[0004] In terms of nano-silicon technology, the most successful one is silicon nanowire technology. Silicon nanowires have extremely stable reversible volume expansion and can still retain 83.6% of the reversible capacity after 1,000 cycles of charge and discharge. However, silicon nanowires are extremely expensive, and their low-cost large-scale production has not yet been realized. There are many invention patents for other nano-silicon particles, but there are currently no successful high-capacity and high-stability products produced based on these patents. The main reason is that after the nano-silicon particles are processed into the negative electrode, the densely stacked negative electrode layer will still produce considerable volume expansion. Even if the particles themselves do not break, the accumulated stress of these macroscopic volume expansions will still cause cracks in the negative electrode active layer, and the conductive network cannot be effectively maintained. It will eventually fail and does not have long-term cycle stability.

[0005] Silicon surface coating technology has been a key research and development direction in recent years. After silicon is nano-processed, it no longer cracks and can be charged and discharged multiple times. Carbon coating allows silicon nanoparticles to obtain a certain degree of adjacent conductive network enhancement during repeated expansion and contraction. For example, Chinese patent CN113998702A pickles microsilicon powder, ball-mills it, mixes it with an organic precursor, dries it, and carbonizes it to obtain a SiO2 / C composite material, which is then reduced by low-temperature magnesium heat, pickled, centrifuged, and dried to obtain a Si / C composite material. Although this material achieves carbon coating on the surface of silicon particles, the particle size distribution is wide and the particles are dense, leaving no space for silicon to expand in volume during the charge and discharge process, resulting in a loose and damaged structure, and it has no use value for lithium-ion batteries.

[0006] The spatial structure control strategy overcomes the overall volume expansion through structural design. For example, the Chinese invention patent CN107565136A uses silicon dioxide reduction to prepare porous silicon technology, combined with chemical vapor deposition carbon coating process, to obtain a carbon-encapsulated porous silicon composite structure with rich internal pores, which can provide a certain space during the charge and discharge process. However, the reserved space for large-sized carbon-encapsulated particles with high silicon content is often insufficient, and the volume expansion will eventually lead to the fragmentation of large-sized particles. The Chinese invention patent CN114105145A forms Si / Mg3N2 by high-temperature reaction of nitrogen-containing gas with the prepared Si / Mg powder, and then obtains composite secondary particles of carbon-encapsulated porous silicon nanoparticles through chemical vapor deposition carbon coating combined with acid washing to remove Mg3N2. The composite secondary particles have a large number of pores inside, which reserve sufficient space for the volume expansion of small-size silicon particles of about 100 nanometers, which is extremely beneficial to the charge and discharge stability. However, the large amount of nitrogen-containing gas consumed produces serious nitrate pollution emissions, and long-term corrosion to equipment, which will also increase production costs and safety risks, making it difficult to mass-produce in China.

[0007] Therefore, by designing the spatial structure of silicon-carbon composite materials, so that they can maintain a good and stable conductive network during the repeated volume expansion during the electrochemical charge and discharge process, the electrochemically active particles continue to combine with the conductive network to obtain high-capacity silicon-carbon composite materials. The preparation process of the material is easy to scale up and the cost is acceptable to the market. This is an urgent problem to be solved in carbon-silicon composite materials. Summary of the invention

[0008] The purpose of the present invention is to provide a silicon-carbon composite material with an elastic copper nano-welding structure and a stable conductive network and a preparation method thereof, which utilizes the elastic enhancement property brought by the nano-size effect to enable the copper nanoparticles to act as elastic contact points to adapt to the stress generated by the volume expansion of silicon-containing nanoparticles without the conductive contact points falling off, maintain a good and stable conductive network, ensure the electron transmission inside the electrode, and obtain highly reversible large-capacity negative electrode performance. The preparation method thereof takes into account both high conductive stability and low cost, and is conducive to promotion.

[0009] In order to achieve the above technical effects, the present invention provides the following technical solutions:

[0010] The present invention provides a silicon-carbon composite material with an elastic copper nano-welding structure to enhance the stability of the conductive network. The silicon-carbon composite material has a copper nano-welding structure, and the copper nano-welding structure includes silicon-containing particles, carbon materials, and elastic copper nano-welding points connecting the two.

[0011] The copper nano-welded structure generates elastic deformation when the silicon-containing particles expand in volume, so that the silicon-containing particles maintain contact with the carbon material, so that during the repeated volume expansion generated during the electrochemical charge and discharge process, the silicon-carbon composite material maintains a good and stable conductive network.

[0012] Furthermore, the elastic copper nano-welding points in the copper nano-welding structure are formed by the copper nano-thin layer wrapped on the surface of the silicon-containing particles shrinking to the contact part between the silicon-containing particles and the carbon material;

[0013] The elastic copper nano-welding point has electrochemical inertness, and is a silicon-metal copper-carbon structure formed by surface chemical reaction between the metallic copper of the copper nano-thin layer and the silicon-containing particles and the carbon material, and the silicon-metal copper-carbon structure is bonded by chemical bonds. The elastic copper nano-welding point has electrochemical inertness, and is a silicon-metal copper-carbon structure formed by surface chemical reaction between the metallic copper of the copper nano-thin layer and the silicon-containing particles and the carbon material, and the silicon-metal copper-carbon structure is bonded by chemical bonds.

[0014] Furthermore, the size of the elastic copper nano-welding point is 2-30 nm as observed by scanning electron microscopy.

[0015] Furthermore, the elastic copper nano-welding points account for 5-10% of the theoretical mass percentage of the silicon-carbon composite material.

[0016] The present invention also provides a method for preparing the above-mentioned silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability: silicon-containing particles are mixed with a copper salt solution, and copper hydroxide is deposited on the surface of the silicon-containing particles under alkaline conditions; a carbon material is then added to the mixture, a reducing gas is introduced to reduce the copper hydroxide, and a carbon source is introduced after annealing to obtain a silicon-carbon composite material with an elastic copper nano-welding structure coated with a carbon nano-thin layer. Specifically, the preparation steps include:

[0017] S1. dispersing the silicon-containing particles in a copper salt solution, adding an alkaline solution, and depositing copper hydroxide on the surface of the silicon-containing particles to form a Si / Cu(OH)2 dispersion;

[0018] S2. adding the carbon material to the Si / Cu(OH)2 dispersion and spray drying to obtain Si / Cu(OH)2 / C material;

[0019] S3. The Si / Cu(OH)2 / C material is subjected to a reduction reaction in the reducing gas, and dried to obtain a Si / Cu(0) / C material;

[0020] S4. Annealing the Si / Cu(0) / C material in a hydrogen-argon mixed atmosphere, and then carbon-coating it with the carbon source gas to obtain a Si / Cu / C silicon-carbon composite material having an elastic copper nano-welding structure.

[0021] Furthermore, the copper salt solution includes any one of copper chloride, copper acetate monohydrate, copper nitrate, and copper sulfate, or a combination of two or more thereof.

[0022] Furthermore, the alkaline solution includes any one of ammonia water or urea solution.

[0023] Furthermore, the silicon-containing particles include: nano silicon powder.

[0024] Furthermore, the particle size of the silicon-containing particles is between 10 and 200 nanometers.

[0025] Furthermore, the carbon nanomaterial includes: any one of carbon nanotubes, graphene oxide, activated carbon, or a combination of two or more thereof.

[0026] Furthermore, the reducing gas described in S3 includes hydrazine hydrate vapor, the reduction temperature is 80° C.-120° C., and the reduction time is 60-180 minutes.

[0027] Furthermore, the drying temperature in S3 is 40°C-80°C.

[0028] Furthermore, the active nanoparticle powder coated with the copper nano-thin layer is annealed in a mixed gas atmosphere of hydrogen and argon.

[0029] Furthermore, the volume ratio of hydrogen to argon in the hydrogen-argon mixed gas in S4 is 5:95.

[0030] Furthermore, the carbon source gas in S4 includes any one of methane and natural gas, or a combination of the two.

[0031] Furthermore, the volume fraction of the carbon source gas in S4 is 1%-5%.

[0032] Furthermore, the annealing time in S4 is 60-180 minutes.

[0033] Furthermore, the annealing temperature in S4 is 800° C. and the annealing time is 60-180 minutes.

[0034] Application of the above-mentioned elastic copper nano-welded structure enhanced conductive network stable silicon-carbon composite material or the elastic copper nano-welded structure enhanced conductive network stable silicon-carbon composite material prepared according to the preparation method provided by the present invention in the negative electrode of lithium ion battery.

[0035] Compared with the prior art, the present invention has the following beneficial effects:

[0036] The elastic copper nano-welding structure provided by the present invention enhances the conductive network stability of the silicon-carbon composite material, and successively coats the copper nano-thin layer and the carbon nano-thin layer on the surface of the silicon-containing particles, and forms an elastic copper nano-welding structure where the copper nano-thin layer and the carbon nano-thin layer contact each other. The copper nano-welding structure can deform when the volume of the silicon-containing particles expands, thereby maintaining the stability of the conductive network and obtaining a high-capacity silicon-carbon composite material.

[0037] The preparation method provided by the invention has clear and simple whole preparation process, and the raw materials and equipment are common and can be promoted. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 Schematic diagram of the preparation method of the silicon-carbon composite material prepared in Example 1 of the present invention.

[0040] Figure 2 This is a scanning electron microscope (SEM) image of the silicon-carbon composite material prepared in Example 1 of the present invention.

[0041] Figure 3This is a Cu Mapping image of the silicon-carbon composite material prepared in Example 2 of the present invention.

[0042] Figure 4 This is the charge and discharge curve of the first cycle of the silicon-carbon composite material prepared in Example 1 of the present invention.

[0043] Figure 5 This is the cycle curve of the first 100 cycles of the silicon-carbon composite material prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0044] The present invention will be more fully understood through the following detailed description, which should be read in conjunction with the accompanying drawings. Detailed embodiments of the present invention are disclosed herein; however, it should be understood that the disclosed embodiments are only exemplary of the present invention, which can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis of the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in virtually any appropriate detailed embodiment.

[0045] The present invention provides a silicon-carbon composite material with an elastic copper nano-welding structure to enhance the stability of the conductive network. The silicon-carbon composite material has a copper nano-welding structure, and the copper nano-welding structure includes silicon-containing particles, carbon materials, and elastic copper nano-welding points connecting the two. The elastic copper nano-welding points are formed by shrinking a copper nano-thin layer wrapped on the surface of the silicon-containing particles to the contact position between the silicon-containing particles and the carbon materials. Specifically, the elastic copper nano-welding points are formed by adsorbing and depositing a copper hydroxide nano-thin layer on the surface of the silicon-containing nano-particles, and then chemically reducing the copper hydroxide nano-thin layer to form a copper nano-thin layer, which is then liquefied at high temperature, and using capillary action to transfer the liquefied metal Copper shrinks to the surface where silicon-containing particles contact with carbon materials to form elastic copper nano-welding points, and then carbon source gas is introduced to catalyze the formation of a carbon nano-thin layer on the surface of the elastic copper nano-welding structure; the elastic copper nano-welding structure is limited to the area between the silicon-containing nano-particles and the carbon materials in contact with them and the surrounding 2-30nm range, and the elastic copper nano-welding points do not react with the two to form an alloy, but only form a strong chemical bond of silicon-metal-carbon through surface chemical action, the elastic copper nano-welding points are electrochemically inert, do not participate in the composite powder as the negative electrode charging and discharging process of the lithium ion battery, and the mass percentage of the elastic copper nano-welding points is adjustable in the range of 5-10%. During the charging and discharging process of the lithium ion battery, the silicon-carbon negative electrode material can stabilize the contact between the silicon-containing particles and the conductive carbon material during the volume expansion and contraction process of the silicon-containing particles by using the electrochemically inert elastic copper nano-welding points, without causing failure of the contact points, thereby stabilizing the performance of the battery negative electrode and obtaining a highly reversible charging and discharging capacity.

[0046] The present invention also provides a method for preparing the silicon-carbon composite material, which comprises depositing copper hydroxide on the surface of silicon-containing nanoparticles by a chemical method, then reducing the copper hydroxide to a copper nanolayer, and compounding the silicon-containing particles wrapped with the copper nanolayer with a carbon material, further removing oxygen atoms inside the copper in a high-temperature reducing hydrogen and argon atmosphere, melting the elemental metallic copper into liquid metallic copper at a low temperature by utilizing the nano effect, shrinking the copper metal liquid to the contact point by utilizing the capillary action of the contact interface between the silicon-containing nanoparticles and the carbon material, and catalyzing the generation of a carbon coating layer on the surface after introducing a carbon source gas, thereby further enhancing the stability of the silicon-carbon composite material, and finally forming an elastic copper nano-welding structure with an enhanced conductive network stability.

[0047] Example 1

[0048] See also Figure 1 , is a schematic diagram of the preparation method of the silicon-carbon composite material of this embodiment, firstly, the silicon-containing particles are dispersed in water, then copper acetate monohydrate and ammonia water are added, after washing, graphene oxide dispersion is added, sprayed to obtain Si / Cu(OH)2 / GO material, and then annealed in a hydrogen and argon mixed gas atmosphere to obtain Si / Cu / rGO material. Specifically, the preparation steps are as follows:

[0049] (1) Preparation of Si / Cu(OH)2 materials

[0050] 1 g of silicon powder (50 nm) was weighed and ultrasonically dispersed in 200 ml of deionized water, and 312 mg of copper acetate monohydrate was added thereto to obtain a dispersion having a Cu:Si mass ratio of 0.1:1. The dispersion was rapidly stirred and 1 mL of ammonia water (25 wt%) was slowly added dropwise, and then stirred for 8 h and aged overnight to obtain a Si / Cu(OH)2 dispersion, which was centrifuged and washed with deionized water to remove excess components for later use.

[0051] (2) Preparation of Si / Cu(OH)2 / GO

[0052] Weigh 200 mg of graphene oxide and ultrasonically disperse it in 100 ml of deionized water. Quickly stir the graphene oxide dispersion and slowly inject the Si / Cu(OH)2 dispersion into it. After 8 hours of stirring and dispersion, spray dry to obtain Si / Cu(OH)2 / GO material. The spray drying conditions are: inlet temperature of 220°C, outlet temperature of 120°C, and feed rate of 10 mL / min.

[0053] (3) Preparation of Si / Cu(0) / rGO

[0054] The Si / Cu(OH)2 / GO material was reduced in hydrazine hydrate vapor at 90°C for 120 min, and then dried in a vacuum oven at 60°C to obtain the Si / Cu(0) / rGO material.

[0055] (4) Preparation of Si / Cu / rGO materials

[0056] The Si / Cu(0) / rGO material obtained in the above step (3) is annealed in a mixed gas atmosphere of hydrogen and argon, Ar:H2 (95:5 Vol%), and the high-temperature furnace is heated to 800°C at a heating rate of 5°C / min, and the temperature is kept constant at 800°C for 120 minutes to further remove the oxygen atoms inside the copper. After cooling, CH4 gas (ethylene can also be used) is introduced to catalyze carbon coating, and the high-temperature furnace is heated to 800°C at a heating rate of 5°C / min, and the temperature is kept constant at 800°C for 120 minutes. The sample is cooled to room temperature in the furnace and then taken out to obtain the Si / Cu / rGO material.

[0057] Example 2

[0058] The only difference between Example 2 and Example 1 is that 642 mg of copper acetate monohydrate is added, and 5 mL of urea solution (40 wt %) is slowly added in step (1). The other conditions remain the same as in Example 1.

[0059] Example 3

[0060] The only difference between Example 3 and Example 1 is that 156 mg of copper acetate monohydrate is added. The other conditions are the same as those in Example 1.

[0061] Example 4

[0062] The only difference between Example 4 and Example 1 is that 1.56 g of copper acetate monohydrate is added. The other conditions are the same as those in Example 1.

[0063] Example 5

[0064] The only difference between Example 5 and Example 1 is that 0.208 mg of copper chloride is added. The other conditions are the same as those in Example 1.

[0065] Example 6

[0066] The only difference between Example 6 and Example 1 is that 0.348 of copper nitrate is added. The other conditions are the same as those of Example 1.

[0067] Example 7

[0068] The only difference between Example 7 and Example 1 is that 290 mg of copper nitrate is added. The other conditions are the same as those of Example 1.

[0069] Example 8

[0070] The only difference between Example 8 and Example 1 is that the amount of GO added is 50 mg. The other conditions are the same as those of Example 1.

[0071] Example 9

[0072] The only difference between Example 9 and Example 1 is that the amount of GO added is 100 mg. The other conditions are the same as those of Example 1.

[0073] Example 10

[0074] The only difference between Example 10 and Example 1 is that the amount of GO added is 400 mg. The other conditions are the same as those of Example 1.

[0075] Embodiment 11

[0076] The only difference between Example 11 and Example 1 is that the reduction time in hydrazine hydrate vapor is 60 min. The other conditions remain the same as in Example 1.

[0077] Example 12

[0078] The only difference between Example 12 and Example 1 is that the reduction time in hydrazine hydrate vapor is 180 min. The other conditions remain the same as in Example 1.

[0079] Embodiment 13

[0080] The only difference between Example 13 and Example 1 is that the reduction temperature in hydrazine hydrate vapor is 80° C. The other conditions remain the same as in Example 1.

[0081] Embodiment 14

[0082] The only difference between Example 14 and Example 1 is that the reduction temperature in hydrazine hydrate vapor is 120° C. The other conditions remain the same as in Example 1.

[0083] Embodiment 15

[0084] The only difference between Example 15 and Example 1 is that the reduction time in the hydrogen-argon mixed gas is 60 minutes. The other conditions are the same as those in Example 1.

[0085] Example 16

[0086] The only difference between Example 16 and Example 1 is that the reduction time in the hydrogen-argon mixed gas is 180 min. The other conditions remain the same as in Example 1.

[0087] Embodiment 17

[0088] The only difference between Example 17 and Example 1 is that the second reducing gas is maintained for 60 minutes, and the other conditions remain the same as in Example 1.

[0089] Embodiment 18

[0090] The only difference between Example 18 and Example 1 is that the second reducing gas is maintained for 180 minutes, and the other conditions remain the same as those of Example 1.

[0091] Embodiment 19

[0092] The only difference between Example 19 and Example 1 is that the particle size of the silicon nanoparticles is 30 nm, and the other conditions remain the same as in Example 1.

[0093] Embodiment 20

[0094] The only difference between Example 20 and Example 1 is that the particle size of the silicon nanoparticles is 100 nm, and the other conditions remain the same as those of Example 1.

[0095] Embodiment 21

[0096] The only difference between Example 21 and Example 1 is that the particle size of the silicon nanoparticles is 200 nm, and the other conditions remain the same as those of Example 1.

[0097] Comparative Example 1

[0098] The only difference between Comparative Example 1 and Example 1 is that 100 mg of copper acetate monohydrate is added, and the other conditions are the same as those of Example 1.

[0099] Comparative Example 2

[0100] The only difference between Comparative Example 2 and Example 1 is that 2 g of copper acetate monohydrate is added, and the other conditions are the same as those of Example 1.

[0101] Comparative Example 3

[0102] The only difference between Comparative Example 2 and Example 1 is that 10 mg of graphene oxide is added, and the other conditions remain the same as those of Example 1.

[0103] Comparative Example 4

[0104] The only difference between Comparative Example 4 and Example 1 is that 1 g of graphene oxide is added, and the other conditions remain the same as those of Example 1.

[0105] Comparative Example 5

[0106] The only difference between Comparative Example 5 and Example 1 is that the reduction is carried out in hydrazine hydrate vapor for 30 minutes, and the other conditions are the same as those in Example 1.

[0107] Comparative Example 6

[0108] The only difference between Comparative Example 6 and Example 1 is that the annealing is performed in an argon atmosphere without hydrogen, and the other conditions are the same as those of Example 1.

[0109] Performance Characterization and Data Analysis

[0110] 1. Morphological characteristics and first cycle charge and discharge performance

[0111] The morphology of the Si / Cu / rGO material prepared in Example 1 was observed using a scanning electron microscope. Figure 2 , is a scanning electron microscope (SEM) image of the silicon-carbon composite material prepared in Example 1 of the present invention, Figure 2 It is intuitively shown that the silicon-containing nanoparticles are combined with the graphene nanosheets (in the dotted circle), and the graphene forms a continuous stretching network to adapt to the volume expansion of the silicon-containing particles during the charge and discharge process. Furthermore, the rough morphology of the silicon-containing particle surface also proves the formation of the copper nano-welding structure. The size of the elastic copper nano-welding point is 2-30nm under the scanning electron microscope, and the elastic copper nano-welding point accounts for 1-30% of the theoretical mass percentage of the silicon-carbon composite material.

[0112] See also Figure 3 , is the Cu Mapping image of the silicon-carbon composite material prepared in Example 2 of the present invention, Figure 3 It shows that copper is mainly distributed around silicon-containing particles.

[0113] The first cycle charge and discharge performance of the Si / Cu / rGO material prepared in Example 1 was tested (under 0.2C lithium removal / 0.2C lithium insertion conditions), see Figure 4 , is the charge-discharge curve of the first cycle of the silicon-carbon composite material prepared in Example 1 of the present invention, Figure 4 It shows that the first-cycle charge and discharge capacities of Si / Cu / rGO materials are 1109.04 mAh / g and 894.6 mAh / g, respectively, corresponding to a first-cycle coulombic efficiency of 80.66%.

[0114] Figure 5 The first 100 cycles of the silicon-carbon composite material prepared in Example 1 of the present invention show a weak peak at 0.75 V during lithium insertion, which corresponds to the beginning of SEI formation. In addition, there is an obvious stripping or stripping voltage platform regardless of lithium insertion or stripping. Figure 5 It shows that the composite material still has a reversible capacity of 559.56 mAh / g after 30 cycles, and an irreversible capacity of 568.56 mAh / g (with 500 mAh / g as a reference value).

[0115] 2. Mass fraction and lithium storage performance

[0116] The electrochemical properties of the silicon-carbon composite materials prepared in Examples 1-21 and Comparative Examples 1-6 were tested by assembling CR2025 type button half-cells.

[0117] The specific assembly process is as follows: lithium metal sheet is used as the counter electrode; 1M Li PF6 / EC:DEC:DMC (1:1:1) is used as the electrolyte; polypropylene microporous membrane is used as the separator; the active material, CE-300j, sodium carboxymethyl cellulose (CMC), and styrene-butadiene latex (SBR) are prepared into a slurry according to a mass ratio of 8:1:0.5:0.5, and the slurry is evenly coated on the carbon-coated copper foil and placed in a vacuum drying oven at 80°C for 4 hours to form an electrode sheet. The battery is assembled in a glove box filled with argon. The model of the battery test system is LANDCT3002A, and the voltage range is 0.001~1.5V.

[0118] The mass fraction of Si and the lithium storage performance of the samples prepared in Examples 1-21 and Comparative Examples 1-6 are shown in Table 1.

[0119] Table 1 Statistics of Si mass fraction and lithium storage capacity in silicon-carbon composite materials prepared in Examples 1-21 and Comparative Examples 1-6

[0120]

[0121]

[0122] Compared with Comparative Examples 1-2, Examples 1-4 regulate the number of copper nano-welding points by changing the content of copper salt. In Comparative Example 1, a low copper salt ratio results in a small number of copper nano-welding structures, which leads to a poor composite effect of silicon powder and graphene and poor overall electrochemical performance. In Comparative Example 2, an excessively high copper salt ratio results in an increase in the inert layer on the surface of the active substance, which is not conducive to the embedding and de-embedding of lithium ions. An appropriate copper salt ratio can not only form unique copper nano-welding sites, but also form strong silicon-copper-carbon chemical bonds between silicon-containing particles, copper nano-thin layers, and carbon nano-thin layers, thereby promoting the combination of silicon-containing particles, silicon and carbon materials, and the copper nano-welding sites have excellent conductivity, thereby reducing the charge transfer resistance and improving the overall electrochemical performance.

[0123] Compared with Examples 8-10 and Comparative Examples 3-4, the distribution of active particles therein is adjusted by changing the content of graphene. In Comparative Example 3, the graphene content is relatively low, resulting in a low first coulombic efficiency; however, in Comparative Example 4, the excessive graphene is prone to produce too many irreversible Li storage sites during sintering, which also causes a low first coulombic efficiency.

[0124] In summary, the results in Table 1 show that copper, as a metal nano-welding point, has a crucial influence on the comprehensive electrochemical properties of the silicon-carbon composite material when its content is within an appropriate range.

[0125] Table 1 also shows that the reduction conditions play an important role in the synthesis of silicon-carbon (Cu) composite materials. Since the main component of the nano-welding site in the present invention is copper, the control of the reduction conditions is particularly important. In Examples 11-16 and Comparative Examples 5-6, the hydrazine hydrate reduction time, temperature, annealing time in a hydrogen-argon mixed gas, and hydrogen content are controlled respectively. Sufficient hydrazine hydrate reduction and hydrogen-containing annealing conditions are necessary. The former forms a precursor of the welding structure, and the latter ensures that the combination of graphene, silicon and nano-copper is tighter. If the hydrazine hydrate reaction time is too short and hydrogen-free sintering is performed, the oxygen content in the system is too high, which affects the conductivity and structure of the material, increases the mass transfer resistance, and reduces its capacity and first coulomb efficiency, but the cycle stability is slightly increased.

[0126] At the same time, referring to the silicon-carbon composite materials prepared in the embodiments and comparative examples of the present invention, their lithium storage capacity, first effect, and cycle stability are all limited by the material synthesis path.

[0127] In summary, the present invention provides a silicon-carbon composite material with an elastic copper nano-welding structure to enhance the stability of the conductive network, and the silicon-carbon composite material has a copper nano-welding structure. The copper nano-welding structure is formed by the copper nano-thin layer wrapped on the surface of the silicon-containing particles shrinking to the contact point formed by the silicon-containing particles and the carbon nano-thin layer. The copper nano-welding structure generates elastic deformation when the silicon-containing particles expand in volume to maintain the contact between the silicon-containing particles and the carbon nano-thin layer, maintain the electrode performance, and can maintain a good and stable conductive network in the repeated volume expansion during the electrochemical charge and discharge process, so as to obtain a high-capacity silicon-carbon composite material. The preparation method provided by the present invention is simple, low-cost, and easy to promote.

[0128] It should be understood that the above examples are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A silicon-carbon composite material with an elastic copper nano-welded structure and a stable conductive network, characterized in that: The silicon-carbon composite material has a copper nano-welding structure; the copper nano-welding structure includes silicon-containing particles, carbon material and elastic copper nano-welding points connecting the two; The copper nano-welded structure generates elastic deformation when the silicon-containing particles expand in volume, so that the silicon-containing particles maintain contact with the carbon material, so that during the repeated volume expansion generated during the electrochemical charge and discharge process, the silicon-carbon composite material maintains a good and stable conductive network.

2. The silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 1, characterized in that: The elastic copper nano-welding point in the copper nano-welding structure is formed by the copper nano-thin layer wrapped on the surface of the silicon-containing particle shrinking to the contact position between the silicon-containing particle and the carbon material; The elastic copper nano-welding point is electrochemically inert and is a silicon-metal copper-carbon structure formed by surface chemical reaction between the metal copper of the copper nano-thin layer and the silicon-containing particles and the carbon material, and the silicon-metal copper-carbon structure is bonded by chemical bonds.

3. The silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 2, characterized in that: The elastic copper nano-welding point size is 2-30nm; And / or, the elastic copper nano-welding points account for 1-30% of the theoretical mass percentage of the silicon-carbon composite material.

4. A method for preparing a silicon-carbon composite material with an elastic copper nano-welded structure and a stable conductive network as described in any one of claims 1 to 3, characterized in that include: Silicon-containing particles are mixed with a copper salt solution, and copper hydroxide is deposited on the surface of the silicon-containing particles under alkaline conditions; a carbon material is then added and mixed, and a reducing gas is introduced to reduce the copper hydroxide, and after annealing, a carbon source gas is introduced again to obtain a silicon-carbon composite material with an elastic copper nano-welded structure coated with a carbon nano-thin layer.

5. The method for preparing the silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 4, characterized in that: The preparation steps include: S1. dispersing the silicon-containing particles in a copper salt solution, adding an alkaline solution, and depositing copper hydroxide on the surface of the silicon-containing particles to form a Si / Cu(OH)2 dispersion; S2. adding the carbon material to the Si / Cu(OH)2 dispersion and spray drying to obtain Si / Cu(OH)2 / C material; S3. The Si / Cu(OH)2 / C material is reduced in the reducing gas and dried to obtain a Si / Cu(O) / C material; S4. Annealing the Si / Cu(O) / C material in a hydrogen-argon mixed atmosphere, and then carbon-coating it with the carbon source gas to obtain a Si / Cu / C silicon-carbon composite material having an elastic copper nano-welding structure.

6. The method for preparing the silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 5, characterized in that: The copper salt solution includes any one of copper chloride, copper acetate monohydrate, copper nitrate, and copper sulfate, or a combination of two or more thereof; And / or, the mass ratio of the silicon-containing particles to the copper in the copper salt and the carbon material is 1:0.03-0.7:0.005-0.

4. And / or, the alkaline solution includes any one of aqueous ammonia or urea solution; And / or, the carbon material includes any one of carbon nanotubes, graphene oxide, and activated carbon; And / or, the particle size of the silicon-containing particles is 10-200 nanometers.

7. The method for preparing the silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 5, characterized in that: The reducing gas in S3 includes hydrazine hydrate vapor; and / or, the reduction temperature in hydrazine hydrate vapor is 80° C.-120° C., and the reduction time is 60-180 minutes; And / or, the drying temperature in S3 is 40°C-80°C.

8. The method for preparing the silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 5, characterized in that: The volume ratio of hydrogen to argon in the hydrogen-argon mixed gas in S4 is 5:95; And / or, the carbon source gas is any one of methane and ethylene, or a combination of two or more thereof; And / or, the volume fraction of the carbon source gas is 1%-5%.

9. The method for preparing the silicon-carbon composite material with elastic copper nano-welding structure and enhanced conductive network stability according to claim 5, characterized in that: The annealing temperature in S4 is 800°C; And / or, the annealing time is 60-180 minutes; And / or, the carbon catalysis and coating time in the carbon source gas is 60-180 minutes.

10. Use of the elastic copper nano-welded structure reinforced conductive network-stabilized silicon-carbon composite material as claimed in any one of claims 1 to 2 or the elastic copper nano-welded structure reinforced conductive network-stabilized silicon-carbon composite material prepared by the preparation method as claimed in any one of claims 3 to 9 in lithium-ion battery negative electrodes.

Citation Information

Patent Citations

  • Preparation method of rectorite-based porous silicon carbon composite material and product of rectorite-based porous silicon carbon composite material

    CN107565136A

  • Method for preparing Si / C negative electrode material by taking silica fume as raw material

    CN113998702A

  • Carbon-coated three-dimensional porous silicon negative electrode material as well as preparation method and application thereof

    CN114105145A

Cited By

  • Copper-containing silicon carbon negative electrode material, preparation method thereof and lithium ion battery

    CN119307881A