Lithium composite oxide

By controlling the atomic ratio relationship between nickel, boron and other metal elements in lithium composite oxides, forming a coating with a specific gradient distribution, the stability of the positive electrode active material in lithium secondary batteries is solved, and the lithium secondary batteries are improved Capacity and lifespan characteristics.

CN118943357APending Publication Date: 2024-11-12ECOPRO BM CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410983613.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-10-31
Filing Date
2020-10-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The demand for positive electrode active materials in lithium secondary batteries is constantly changing, especially in electric vehicle applications. The existing materials have problems with small capacity, poor high temperature characteristics and structural instability, resulting in insufficient efficiency and life characteristics of lithium secondary batteries. .

Method used

By controlling the atomic ratio relationship between nickel, boron and other metal elements in the lithium composite oxide, a coating with a specific gradient distribution is formed, the stability of the lithium composite oxide is improved, thereby improving the capacity and life characteristics of the lithium secondary battery.

Benefits of technology

The high efficiency and long life characteristics of lithium secondary batteries are achieved, and the atomic ratio gradient distribution between boron and nickel is confirmed through XPS analysis, which improves structural stability and reduces the problems of reduced battery capacity and rising resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943357A_ABST
    Figure CN118943357A_ABST
Patent Text Reader

Abstract

The present invention relates to a lithium composite oxide capable of improving the capacity characteristics and life characteristics of a lithium secondary battery. The lithium composite oxide includes: primary particles capable of occluding and releasing lithium; and secondary particles, the primary particles being formed by aggregating, a boron-containing oxide being present in at least a part of a region selected from the interface between the primary particles and the surface of the secondary particles, the boron-containing oxide having a concentration gradient that decreases from the surface of the secondary particles toward the center of the secondary particles.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application with an application date of October 10, 2020, application number 202011077894.6, and invention name “Lithium composite oxide and lithium secondary battery comprising the same”. Technical Field

[0002] The present invention relates to a lithium composite oxide capable of improving the capacity characteristics and life characteristics of a lithium secondary battery. Background Art

[0003] Batteries store electricity using materials capable of electrochemical reactions at the positive and negative electrodes. A representative example of such batteries is a lithium secondary battery that stores electrical energy by changes in chemical potential during the insertion / extraction of lithium ions at the positive and negative electrodes.

[0004] The lithium secondary battery is manufactured by using a material that can reversibly intercalate or deintercalate lithium ions as a positive electrode active material and a negative electrode active material, and filling an organic electrolyte or a polymer electrolyte between the positive electrode and the negative electrode.

[0005] As a positive electrode active material of a lithium secondary battery, a lithium composite oxide has been used, and for example, composite oxides of LiCoO 2 , LiMN 2 O 4 , LiNiO 2 , LiMnO 2 , and the like are being studied.

[0006] Among the above-mentioned positive electrode active materials, although LiCoO 2 having excellent lifespan and charge and discharge efficiency is widely used, the above-mentioned material has limitations in price competitiveness due to the limited resources of cobalt used as a raw material and high price.

[0007] Although lithium manganese oxides such as LiMnO2 and LiMN2O4 have the advantages of good thermal stability and low price, they have problems such as small capacity and poor high temperature characteristics. In addition, although LiNiO2-based positive electrode active materials have battery characteristics of high discharge capacity, they are very difficult to synthesize due to the cation mixing problem between lithium and transition metals, and there are great problems in rate characteristics.

[0008] In addition, according to the degree of the above-mentioned cation mixing, a large amount of lithium by-products are generated, and since most of the lithium by-products are composed of LiOH and Li2CO3 compounds, there are problems of gelation when manufacturing positive electrode slurry and gas generation during charge and discharge after manufacturing electrodes. Residual Li2CO3 increases the expansion of the battery, not only reducing the cycle, but also causing the battery to expand.

[0009] In order to compensate for these shortcomings, the demand for nickel-rich positive active materials with a nickel content of 60% or more as secondary battery positive active materials has begun to increase. However, although the above-mentioned nickel-rich positive active materials exhibit high capacity characteristics, there is the following problem: as the nickel content in the positive active material increases, structural instability is caused by the mixing of lithium / nickel cations. Due to the structural instability of the above-mentioned positive active materials, lithium secondary batteries will deteriorate rapidly not only at high temperatures but also at room temperature.

[0010] Therefore, there is a need to develop a positive electrode active material for compensating for the above-mentioned problems of the nickel-rich positive electrode active material. Summary of the invention

[0011] Technical issues

[0012] In the lithium secondary battery market, the growth of lithium secondary batteries for electric vehicles plays a leading role in the market, and the demand for positive electrode active materials used in lithium secondary batteries is also changing.

[0013] For example, conventionally, lithium secondary batteries using LFP have been mainly used from the viewpoint of ensuring safety, but recently, the use of nickel-based lithium composite oxides having a larger energy capacity per unit weight than LFP has been expanding.

[0014] Therefore, an object of the present invention is to provide a nickel-rich positive electrode active material capable of improving the efficiency characteristics and life characteristics of a lithium secondary battery.

[0015] Furthermore, another object of the present invention is to provide a lithium secondary battery using a positive electrode comprising the lithium composite oxide defined herein.

[0016] The purpose of the present invention is not limited to the purpose mentioned above (for example, electric vehicle use), and other purposes and advantages of the present invention not mentioned can be understood through the following description, and can be more clearly understood through the embodiments of the present invention. In addition, it can be easily understood that the purpose and advantages of the present invention can be achieved by the means and combinations thereof in the claims.

[0017] Solutions to the problem

[0018] In the past, as for light elements generally present in lithium composite oxides, such as representative elements such as boron, their content in the above-mentioned lithium composite oxides could only be predicted by the content of boron-containing raw materials added when preparing the above-mentioned lithium composite oxides, but it was impossible to specifically confirm the content of light elements in the above-mentioned lithium composite oxides relative to other elements.

[0019] Furthermore, observing the results obtained by repeated experiments by the inventors of the present invention, it is found that the content of the light element-containing raw material added when preparing the above-mentioned lithium composite oxide is also important, but it is found that the position where the above-mentioned light element mainly exists in the above-mentioned lithium composite oxide as the final product or the correlation (for example, content ratio or atomic ratio) of the metal elements different from the above-mentioned light element in the specific area of ​​the above-mentioned lithium composite oxide is particularly important.

[0020] As a result, the inventors of the present invention confirmed that the correlation between the atomic ratios of nickel, boron, and metal elements M1 and M2 in the surface of the above-mentioned lithium composite oxide can not only contribute to the stability of the lithium composite oxide, but also help improve the electrochemical properties such as efficiency characteristics and life characteristics of the lithium secondary battery prepared using the above-mentioned lithium composite oxide.

[0021] According to one aspect of the present invention, a lithium composite oxide is provided, which includes: primary particles capable of absorbing and releasing lithium; and secondary particles, which are formed by agglomeration of the primary particles, and boron-containing oxide exists in at least a portion of a region selected from interfaces between the primary particles and surfaces of the secondary particles, and the boron-containing oxide presents a concentration gradient that decreases from the surface of the secondary particles toward the center of the secondary particles.

[0022] In one embodiment, the atomic ratio of boron to nickel in the lithium composite oxide measured by XPS analysis of the lithium composite oxide may have a gradient decreasing from the surface portion of the secondary particle toward the center portion of the secondary particle.

[0023] In one embodiment, the atomic ratio of boron to nickel in the overall composition of the secondary particles measured by XPS analysis of the lithium composite oxide may be 0.0013 or more and 0.0192 or less.

[0024] In one embodiment, an atomic ratio of boron to nickel in the surface portion of the secondary particle measured by XPS analysis of the lithium composite oxide may be 0.21 or more and 28.8 or less.

[0025] In one embodiment, the ratio of the atomic ratio of boron to nickel in the surface portion of the secondary particle determined by XPS analysis of the lithium composite oxide and the atomic ratio of boron to nickel in the overall composition of the secondary particle is greater than 160 and less than 1500, and the atomic ratio of boron to nickel in the surface portion of the secondary particle is calculated as the atomic ratio of boron to nickel existing from the outermost surface of the secondary particle to a depth of 10 nm.

[0026] In one embodiment, the lithium composite oxide may include i) nickel and cobalt, ii) at least one selected from manganese and aluminum, and iii) boron.

[0027] In one embodiment, the lithium composite oxide may be represented by the following chemical formula 1:

[0028] [Chemical formula 1]

[0029] Li w Ni 1-(x+y+z) Co x B y M1 z M2 z' O2

[0030] Wherein, M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0 <y≤0.20,0≤z≤0.20,0≤z'≤0.20。

[0031] In one embodiment, the boron-containing oxide may be represented by the following chemical formula 2-1:

[0032] [Chemical formula 2-1]

[0033] Li a B b M4 b' O c

[0034] Among them, M4 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, 0≤a≤6, 0≤b≤8, 0≤b'≤8, 2≤c≤13.

[0035] In one embodiment, at least a portion of a region selected from the interface between the primary particles and the surface of the secondary particles may further include at least one metal oxide represented by the following Chemical Formula 2:

[0036] [Chemical formula 2]

[0037] Li a M3 b O c

[0038] Among them, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, 0≤a≤6, 0≤b≤8, 2≤c≤13.

[0039] In one embodiment, the boron-containing oxide and the metal oxide may be present in the same layer, or may be present in separate layers.

[0040] Therefore, according to one aspect of the present invention, a lithium composite oxide can be provided, which includes primary particles capable of absorbing and releasing lithium and secondary particles formed by agglomerating the primary particles, wherein the lithium composite oxide includes i) nickel (Ni) and cobalt (Co), ii) at least one selected from manganese (Mn) and aluminum (Al), and iii) boron (B), and the atomic ratio of boron (B) and nickel (Ni) in the surface portion of the lithium composite oxide exists within a specific range.

[0041] In one embodiment, the lithium composite oxide may be represented by Chemical Formula 1 below.

[0042] [Chemical formula 1]

[0043] Li w Ni 1-(x+y+z) Co x B y M1 z M2 z' O2

[0044] (Wherein, M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0 <y≤0.20,0≤z≤0.20,0≤z'≤0.20)

[0045] In another embodiment of the present invention, the atomic ratio of boron (B) to the metal elements M1 and M2 in the surface portion of the lithium composite oxide may be within a specific range.

[0046] According to another aspect of the present invention, a lithium secondary battery using a positive electrode including the lithium composite oxide can be provided.

[0047] Effects of the Invention

[0048] According to the present invention, the atomic ratio of boron (B) and nickel (Ni) in the surface portion of a lithium composite oxide including primary particles capable of absorbing and releasing lithium and secondary particles formed by agglomerating the primary particles exists within a specific range, thereby improving the stability of the lithium composite oxide, thereby improving the capacity characteristics and life characteristics of a lithium secondary battery using the lithium composite oxide as a positive electrode active material.

[0049] Specific matters for implementing the invention will be described below, and specific effects of the present invention and the above-mentioned effects will be described. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figures 1 to 7 is a graph showing the XPS analysis results of lithium composite oxides prepared according to Examples and Comparative Examples.

[0051] Figure 8 is a graph showing the XRD analysis results of the lithium composite oxides prepared according to Examples and Comparative Examples. DETAILED DESCRIPTION

[0052] In order to easily understand the present invention, specific terms are appropriately defined in this application. Unless otherwise defined herein, the scientific terms and technical terms used in the present invention have the meanings commonly understood by those skilled in the art to which the present invention belongs. In addition, unless the context requires otherwise, the terms in the singular form shall include the plural form and the terms in the plural form shall include the singular form.

[0053] Next, the lithium composite oxide according to the present invention and a lithium secondary battery using a positive electrode including the lithium composite oxide will be described in further detail.

[0054] Lithium composite oxide

[0055] According to one aspect of the present invention, there is provided a lithium composite oxide, comprising: primary particles capable of absorbing and releasing lithium; and secondary particles formed by agglomeration of the primary particles. The lithium composite oxide can be used as a positive electrode active material for a lithium secondary battery.

[0056] The primary particle refers to a crystal grain (grain or crystallite), and the secondary particle refers to an aggregate formed by agglomeration of a plurality of primary particles. The primary particle may have a rod-like, elliptical and / or irregular shape. There may be gaps and / or grain boundaries between the primary particles constituting the secondary particles.

[0057] For example, the primary particles may be spaced apart from adjacent primary particles in the secondary particles to form internal voids. In addition, the primary particles may form a surface present inside the secondary particles by contacting with the internal voids, without forming a grain boundary by contacting with adjacent primary particles. On the other hand, the surface of the primary particles present on the outermost surface of the secondary particles exposed to the external air forms the surface of the secondary particles.

[0058] The average major axis length of the primary particles is in the range of 0.01 μm to 5 μm, preferably 0.01 μm to 2 μm, so that the optimal density of the positive electrode prepared using the positive electrode active material of various embodiments of the present invention can be achieved. In addition, the average particle size of the secondary particles may vary depending on the number of agglomerated primary particles, but may be 0.1 μm to 30 μm.

[0059] In one embodiment, the lithium composite oxide may be a compound including i) nickel (Ni) and cobalt (Co), ii) at least one selected from manganese (Mn) and aluminum (Al), and iii) boron (B). More specifically, the lithium composite oxide may be represented by the following Chemical Formula 1.

[0060] [Chemical formula 1]

[0061] Li w Ni 1-(x+y+z) Co x B y M1 z M2 z' O2

[0062] (Wherein, M1 is at least one selected from Mn and Al, M2 is at least one selected from Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements, 0.5≤w≤1.5, 0≤x≤0.50, 0 <y≤0.20,0≤z≤0.20,0≤z'≤0.20)

[0063] In the past, as for light elements generally present in lithium composite oxides, such as representative elements such as boron, their content in the above-mentioned lithium composite oxides could only be predicted by the content of boron-containing raw materials added when preparing the above-mentioned lithium composite oxides, but it was impossible to specifically confirm the content of light elements in the above-mentioned lithium composite oxides relative to other elements.

[0064] Therefore, the content of the light element-containing raw material added when preparing the above-mentioned lithium composite oxide is also important, but the position where the above-mentioned light element mainly exists in the above-mentioned lithium composite oxide as the final product or the correlation (for example, content ratio or atomic ratio) of the metal elements different from the above-mentioned light element in the specific region of the above-mentioned lithium composite oxide is particularly important.

[0065] In one embodiment of the present invention, the atomic ratio of boron (B) to nickel (Ni) in the surface of the lithium composite oxide measured by XPS analysis of the lithium composite oxide may satisfy the following Formula 1.

[0066] [Formula 1]

[0067] 0.2≤B / Ni≤29

[0068] At this time, when B / Ni in the surface of the lithium composite oxide is less than 0.2, the life characteristics may be deteriorated. When B / Ni in the surface of the lithium composite oxide exceeds 29.0, the battery efficiency is reduced and the discharge capacity is reduced.

[0069] Furthermore, the atomic ratio (B / Ni) of boron (B) to nickel (Ni) in the lithium composite oxide may have a gradient decreasing from the surface portion of the lithium composite oxide toward the center portion of the lithium composite oxide.

[0070] As described above, the gradient of the atomic ratio of boron to nickel from the surface of the lithium composite oxide toward the center of the lithium composite oxide can improve the structural stability of the lithium composite oxide and prevent problems such as a decrease in battery capacity and an increase in resistance.

[0071] Furthermore, the lithium composite oxide may include a coating layer covering at least a portion of the surface of the primary particles (eg, interfaces between the primary particles) and / or secondary particles formed by agglomerating the primary particles.

[0072] For example, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle. In particular, the coating layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle.

[0073] Thus, the coating layer may exist as a layer that continuously or discontinuously coats the surface of the primary particles and / or the secondary particles formed by agglomerating the primary particles. When the coating layer exists discontinuously, it may exist in the form of islands.

[0074] Furthermore, depending on circumstances, the oxide may exist not only at the interface between the primary particles and at least a portion of the surface of the secondary particles, but also in internal voids formed in the secondary particles.

[0075] The presence of the coating as above can help improve the physical and electrochemical characteristics of the positive electrode active material.

[0076] At this time, the coating layer may exist in the form of a solid solution without forming a boundary with the primary particles and / or the secondary particles formed by agglomerating the primary particles, but the present invention is not limited thereto.

[0077] Boron (B)-containing oxide may exist in the above-mentioned coating layer. That is, the above-mentioned coating layer may be defined as a region where the boron-containing oxide exists.

[0078] Furthermore, in another embodiment, at least one oxide represented by the following Chemical Formula 2 may also exist in the above-mentioned coating layer.

[0079] [Chemical formula 2]

[0080] Li a M3 b O c

[0081] (Wherein, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, B, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd, and 0≤a≤6, 0≤b≤8, 2≤c≤13)

[0082] When at least one oxide represented by Chemical Formula 2 is further present in the coating layer, the oxide may be an oxide different from the boron-containing oxide.

[0083] The oxide represented by the above chemical formula 2 is an oxide formed by combining lithium and an element represented by M3 or an oxide of M3. Examples of the above oxide may be Li a W b O c , Li a Zr b O c , Li a Ti b O c , Li a Ni b O c , Li a Co b O c , Li a Alb O c 、Co b O c 、Al b O c , W b O c 、Zr b O c or Ti b O c However, the above examples are only described for ease of understanding, and the above oxides defined in this article are not limited to the above examples.

[0084] In another embodiment, the oxide represented by the above chemical formula 2 may be an oxide formed by compounding lithium and at least two elements represented by M3 or further includes an oxide formed by compounding lithium and at least two elements represented by M3. An example of an oxide formed by compounding lithium and at least two elements represented by M3 may be Li a (W / Ti) b O c , Li a (W / Zr) b O c , Li a (W / Ti / Zr) b O c Li a (W / Ti / B) b O c Etc., but the present invention is not limited thereto.

[0085] At this time, the boron-containing oxide may be a borate ester compound or a lithium borate (LBO) compound represented by the following chemical formula 3, or a composite oxide of the compound represented by the following chemical formula 3 and other compounds (eg, an oxide represented by chemical formula 2).

[0086] [Chemical formula 3]

[0087] Li a B b M4 b' O c

[0088] (Wherein, M4 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Ce, Gd and Nd, and 0≤a≤6, 0≤b≤8, 0≤b'≤8, 2≤c≤13)

[0089] Non-limiting examples of the above-mentioned boron-containing oxides include B2O3, Li2O-B2O3, Li3BO3, Li2B4O7, Li2B2O7, Li2B8O 13 wait.

[0090] Also, the coating layer may have a form in which the oxide containing boron and the oxide represented by Chemical Formula 2 exist simultaneously in one layer, or a form in which the oxide containing boron and the oxide represented by Chemical Formula 2 exist in separate layers.

[0091] For example, the coating layer may include a first oxide layer and a second oxide layer, the first oxide layer including at least one oxide represented by the chemical formula 2, and the second oxide layer including a boron-containing oxide.

[0092] At this time, the first oxide layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle at the outermost periphery of the secondary particle (i.e., the surface of the secondary particle). Furthermore, the second oxide layer may exist in a manner of covering at least a portion of the exposed surface of the primary particle not covered by the first oxide layer and the surface of the first oxide layer.

[0093] In particular, the second oxide layer exists in a manner that does not cover the exposed surface of the primary particle not covered by the first oxide layer and the surface of the first oxide layer as a whole, thereby improving lithium ion conduction efficiency.

[0094] As described above, the lithium composite oxide according to the present embodiment includes a coating layer, and the coating layer covers at least a portion of the surface of the primary particles (e.g., the interface between the primary particles) and / or the secondary particles formed by agglomerating the primary particles, thereby improving structural stability. In addition, when the lithium composite oxide is used as a positive electrode active material for a lithium secondary battery, life and capacity characteristics can be improved.

[0095] Furthermore, the coating layer not only reduces the residual lithium in the lithium composite oxide but also serves as a migration path (diffusion path) for lithium ions, thereby improving the efficiency characteristics of the lithium secondary battery.

[0096] Furthermore, the oxide may have a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle. Thus, the concentration of the oxide may decrease from the outermost surface of the secondary particle toward the center of the secondary particle.

[0097] As described above, the oxide presents a concentration gradient that decreases from the surface of the secondary particle toward the center of the secondary particle, thereby effectively reducing the residual lithium present on the surface of the positive electrode active material to prevent side reactions caused by unreacted residual lithium. In addition, the oxide can also prevent the crystallinity of the inner region of the surface of the positive electrode active material from decreasing. In addition, the oxide can prevent the overall structure of the positive electrode active material from collapsing during the electrochemical reaction.

[0098] Lithium secondary battery

[0099] According to another aspect of the present invention, a positive electrode including a positive electrode collector and a positive electrode active material layer formed on the positive electrode collector may be provided, wherein the positive electrode active material layer may include the lithium composite oxide according to various embodiments of the present invention as a positive electrode active material.

[0100] Therefore, detailed description of the lithium composite oxide will be omitted, and only the remaining components not described above will be described below. In addition, below, the above lithium composite oxide is referred to as a positive electrode active material for convenience.

[0101] The positive electrode collector is not particularly limited as long as it has conductivity without causing chemical changes in the battery, and examples thereof may include: stainless steel, aluminum, nickel, titanium, sintered carbon, or aluminum or stainless steel whose surface has been treated with carbon, nickel, titanium, silver, etc. In addition, the positive electrode collector may generally have a thickness of 3 μm to 500 μm, or the adhesion of the positive electrode active material may be increased by forming micro-concave and convex on the surface of the collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0102] The positive electrode active material layer may be prepared by coating a positive electrode slurry composition on the positive electrode current collector. The positive electrode slurry composition includes the positive electrode active material and a conductive material, and optionally includes a binder as required.

[0103] The content of the positive electrode active material may be 80 wt % to 99 wt %, more specifically 85 wt % to 98.5 wt %, relative to the total weight of the positive electrode active material layer. When the content of the positive electrode active material is within the above range, the positive electrode active material may have excellent capacity characteristics, but the present invention is not necessarily limited thereto.

[0104] The above-mentioned conductive material is used to provide conductivity to the electrode, and can be used without limitation, as long as it has electronic conductivity and does not cause chemical changes in the assembled battery. Specific examples thereof may include: graphite such as natural graphite or artificial graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black or carbon fiber; metal powder or metal fiber such as copper, nickel, aluminum or silver; conductive whiskers such as zinc oxide whiskers, potassium titanate whiskers; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc., and these substances can be used as a single one or as a mixture of two or more. The content of the above-mentioned conductive material can be 0.1 wt% to 15 wt% relative to the total weight of the positive electrode active material layer.

[0105] The above-mentioned binder serves to adhere the positive electrode active material particles to each other and improve the adhesion of the positive electrode active material and the collector. Specific examples thereof may include: polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile (polyacrylonitrile), carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber or its various copolymers, etc., and these substances can be used as a single or as a mixture of two or more. Relative to the total weight of the positive electrode active material layer, the content of the above-mentioned binder can be 0.1% by weight to 15% by weight.

[0106] In addition to using the above-mentioned positive electrode active material, the above-mentioned positive electrode can be prepared using a common positive electrode preparation method. Specifically, the above-mentioned positive electrode can be prepared by coating a positive electrode slurry composition prepared by dissolving or dispersing the above-mentioned positive electrode active material and a selective binder and a conductive material in a solvent onto a positive electrode collector, and then drying and rolling the obtained product.

[0107] The above-mentioned solvent may be a solvent commonly used in the art, and may include dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, water, etc., and these substances may be used alone as a substance, or as a mixture of two or more. Considering the coating thickness and preparation yield of the slurry, as long as the above-mentioned solvent can dissolve or disperse the above-mentioned positive electrode active material, conductive material and binder and has a viscosity sufficient to obtain excellent thickness uniformity when it is used to prepare the positive electrode coating thereafter, the amount of the solvent used is sufficient.

[0108] Furthermore, in another embodiment, the positive electrode may be prepared by casting the positive electrode slurry composition on a separate support, and then laminating a film obtained by peeling off the support on a positive electrode collector.

[0109] In addition, according to another aspect of the present invention, an electrochemical device including the positive electrode may be provided. The electrochemical device may be specifically a battery, a capacitor, etc., and more specifically, may be a lithium secondary battery.

[0110] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode positioned opposite to the positive electrode, and a separator and an electrolyte between the positive electrode and the negative electrode. Since the positive electrode is the same as the positive electrode described above, a detailed description will be omitted for convenience, and only the remaining components not described above will be described in detail below.

[0111] The lithium secondary battery may further include a battery container for accommodating an electrode assembly including the positive electrode, the negative electrode, and the separator, and a sealing member for sealing the battery container.

[0112] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.

[0113] The above-mentioned negative electrode collector is not particularly limited as long as it has high conductivity without causing chemical changes in the battery, and examples thereof may include: copper, stainless steel, aluminum, nickel, titanium, sintered carbon, or copper or stainless steel, aluminum-cadmium alloy, etc., whose surface is treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode collector may generally have a thickness of 3 μm to 500 μm, or, like the positive electrode collector, may increase the adhesion of the negative electrode active material by forming tiny concave-convex shapes on the surface of the above-mentioned collector. For example, various forms such as films, sheets, boxes, nets, porous materials, foams, and non-woven fabrics may be used.

[0114] The negative electrode active material layer may be prepared by coating a negative electrode slurry composition on the negative electrode current collector. The negative electrode slurry composition includes the negative electrode active material and a conductive material, and optionally includes a binder as required.

[0115] The above-mentioned negative electrode active material can use a compound that can reversibly embed and deintercalate lithium. Specific examples thereof may include: carbon materials such as artificial graphite, natural graphite, graphitized carbon fiber and amorphous carbon; metal compounds that can be alloyed with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy or Al alloy; metal oxides that can be doped and dedoped with lithium such as SiOβ (0<β<2), SnO2, vanadium oxide and lithium vanadium oxide; or a composite containing a metal compound and a carbon compound such as a Si-C composite or a Sn-C composite, and any one of these substances or a mixture of two or more thereof can be used. In addition, a metallic lithium film can be used as a negative electrode active material. In addition, the carbon material can use both low-crystalline carbon and high-crystalline carbon. Low crystalline carbon generally includes soft carbon and hard carbon, and high crystalline carbon generally includes: amorphous, plate-like, scaly, spherical or fibrous natural graphite or artificial graphite, and high-temperature sintered carbon such as Kish graphite, pyrolytic carbon, mesophase pitch based carbon fiber, mesophase carbon microbeads, mesophase pitch, and petroleum or coal tar pitch derived cokes.

[0116] The negative electrode active material may be included in an amount of 80 wt % to 99 wt % based on the total weight of the negative electrode active material layer.

[0117] The binder is a component that helps to bind the conductive material, the active material and the current collector, and its content is generally 0.1 wt % to 10 wt % based on the total weight of the negative electrode active material layer. Examples of the binder may include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber and various copolymers thereof.

[0118] The above conductive material is a component for further improving the conductivity of the negative electrode active material, and the content of the conductive material can be 10% by weight or less, preferably 5% by weight or less, based on the total weight of the negative electrode active material layer. The above conductive material is not subject to any restrictions as long as it has conductivity and does not cause chemical changes in the battery, and conductive materials such as graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black or thermal black can be used; conductive fibers such as carbon fibers or metal fibers; metal powders such as fluorocarbons, aluminum or nickel powders; conductive whiskers such as zinc oxide or potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.

[0119] In one embodiment, the negative electrode active material layer can be prepared by: coating a negative electrode slurry composition prepared by dissolving or dispersing a negative electrode active material and a selective binder and a conductive material in a solvent on a negative electrode collector and drying the obtained product; or by casting the negative electrode slurry composition on a separate carrier and then laminating a film obtained by peeling off the carrier on the negative electrode collector.

[0120] On the other hand, in the above-mentioned lithium secondary battery, the separator separates the negative electrode and the positive electrode, and provides a migration channel for lithium ions, and there is no particular limitation, as long as it is generally used as a separator in a lithium secondary battery. In particular, a separator with low resistance to electrolyte ion migration and excellent ability to contain electrolyte liquid moisture is preferred. Specifically, it is possible to use: a porous polymer film, for example, a porous polymer film prepared from a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a laminated structure of more than two layers thereof. In addition, commonly used porous non-woven fabrics such as non-woven fabrics made of high melting point glass fibers or polyethylene terephthalate fibers can be used. In addition, in order to ensure heat resistance and mechanical strength, a coated separator comprising a ceramic component or a polymer material can also be used, and can be selectively used in a single-layer or multilayer structure.

[0121] In addition, the electrolyte used in the present invention may include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel polymer electrolytes, solid inorganic electrolytes, molten inorganic electrolytes, etc. that can be used in the preparation of lithium secondary batteries, but the present invention is not limited thereto.

[0122] Specifically, the electrolyte may include an organic solvent and a lithium salt.

[0123] The above-mentioned organic solvent can be used without particular limitation as long as it can function as a medium through which ions participating in the electrochemical reaction of the battery can migrate. Specific examples of the organic solvent may include: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone or ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene or fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methylethyl carbonate (MEC), ethylmethyl carbonate (EMC), ethylene carbonate (EC) or propylene carbonate (PC); alcohol solvents such as ethanol or isopropanol; nitrile solvents such as R-CN (R is C2 to C 20 Straight chain, branched or cyclic hydrocarbon group, and may contain double bond aromatic ring or ether bond); amide such as dimethylformamide; dioxolane such as 1,3-dioxolane; sulfolane, etc. Among them, carbonate solvents are preferred, and a mixture of cyclic carbonates (such as ethylene carbonate, propylene carbonate, etc.) with high ion conductivity and high dielectric constant that can enhance the charging and discharging performance of the battery and low viscosity linear carbonate compounds (such as ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, mixing cyclic carbonates and chain carbonates in a volume ratio of about 1:1 to 1:9 can produce excellent electrolyte performance.

[0124] The above-mentioned lithium salt can be used without particular limitation, as long as it is a compound capable of providing lithium ions in a lithium secondary battery. Specific examples of lithium salts may include LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, LiB(C2O4)2, etc. Lithium salts can be advantageously used in a concentration range of 0.1M to 2.0M. When the lithium salt concentration is included in the above range, the electrolyte has appropriate conductivity and viscosity, thereby being able to exhibit excellent electrolyte performance, and lithium ions can be effectively migrated.

[0125] In the above electrolyte, in order to increase the battery life property, inhibit the decline of battery capacity, improve the battery discharge capacity, etc., in addition to the above electrolyte forming components, one or more additives may be further included, including, for example: halogenated alkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N, N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride. Wherein, relative to the total weight of the electrolyte, the content of the above additives can be 0.1% by weight to 5% by weight.

[0126] The lithium secondary battery containing the positive electrode active material according to the present invention as described above stably exhibits excellent discharge capacity, output characteristics and life characteristics, and is therefore used in the following fields: the field of portable devices such as mobile phones, laptop computers and digital cameras; and the field of electric vehicles such as hybrid electric vehicles (HEV) and the like.

[0127] The shape of the lithium secondary battery according to the present invention is not particularly limited, but may have a cylindrical, angular, pouch or coin shape using a can. And, preferably, the lithium secondary battery can be used as a battery cell for a power source of a small device, and can also be used as a unit battery of a medium and large battery module including a plurality of battery cells.

[0128] According to another aspect of the present invention, a battery module including the above-mentioned lithium secondary battery as a unit battery and / or a battery pack including the same may be provided.

[0129] The battery module or the battery pack may be used in power tools (Power Tool); electric vehicles including electric vehicles (EV), hybrid vehicles and plug-in hybrid electric vehicles (PHEV); or as a power source for one or more medium and large devices in a system for storing electricity.

[0130] Hereinafter, the present invention will be described in more detail with reference to Examples. However, it should be understood that these Examples are for illustrative purposes only and should not be construed as limiting the scope of the present invention.

[0131] Experimental Example 1. Preparation of lithium composite oxide

[0132] (1) Embodiment 1

[0133] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a precursor is synthesized by coprecipitation reaction, LiOH is added to the synthesized precursor, and then fired to prepare a lithium composite oxide. Specifically, after mixing LiOH with the precursor, an O2 atmosphere is maintained in a sintering furnace and the temperature is increased to 790°C at 1°C per minute, heat-treated for 10 hours, and then naturally cooled to obtain a lithium composite oxide.

[0134] Next, distilled water was added to the above lithium composite oxide, and then washed with water for 1 hour, and the washed lithium composite oxide was filtered and dried.

[0135] Then, the lithium composite oxide and the boron-containing raw material (H3BO3) were mixed together using a heating stirrer and heat-treated. The boron-containing raw material (H3BO3) was mixed so that its content was 0.3% by weight relative to the total weight of the lithium composite oxide, the temperature was raised at 1°C per minute under an O2 atmosphere, and the mixture was heat-treated for 5 hours while being stirred, and then naturally cooled to obtain the lithium composite oxide.

[0136] (2) Embodiment 2

[0137] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a precursor is synthesized by coprecipitation reaction, LiOH and H3BO3 are added to the synthesized precursor, and then fired to prepare a lithium composite oxide. Specifically, after LiOH and H3BO3 are mixed with the precursor, an O2 atmosphere is maintained in a sintering furnace and the temperature is increased to 790°C at 1°C per minute, heat-treated for 10 hours, and then naturally cooled to obtain a lithium composite oxide.

[0138] Next, distilled water was added to the above lithium composite oxide, and then washed with water for 1 hour, and the washed lithium composite oxide was filtered and dried.

[0139] Then, the lithium composite oxide and the boron-containing raw material (H3BO3) were mixed together using a heating stirrer and heat-treated. The boron-containing raw material (H3BO3) was mixed so that its content was 0.3% by weight relative to the total weight of the lithium composite oxide, the temperature was raised at 1°C per minute under an O2 atmosphere, and the mixture was heat-treated for 5 hours while being stirred, and then naturally cooled to obtain the lithium composite oxide.

[0140] (3) Embodiment 3

[0141] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a precursor is synthesized by coprecipitation reaction, LiOH, Al2O3, TiO2 and ZrO2 are added to the synthesized precursor, and then fired to prepare a lithium composite oxide. Specifically, after LiOH, Al2O3, TiO2 and ZrO2 are mixed with the precursor, an O2 atmosphere is maintained in a sintering furnace and the temperature is increased to 790°C at 1°C per minute, heat-treated for 10 hours, and then naturally cooled to obtain a lithium composite oxide.

[0142] Next, distilled water was added to the above lithium composite oxide, and then washed with water for 1 hour, and the washed lithium composite oxide was filtered and dried.

[0143] Then, the lithium composite oxide and the boron-containing raw material (H3BO3) were mixed together using a heating stirrer and heat-treated. The boron-containing raw material (H3BO3) was mixed so that its content was 0.3% by weight relative to the total weight of the lithium composite oxide, the temperature was raised at 1°C per minute under an O2 atmosphere, and the mixture was heat-treated for 5 hours while being stirred, and then naturally cooled to obtain the lithium composite oxide.

[0144] (4) Embodiment 4

[0145] First, nickel sulfate, cobalt sulfate and manganese sulfate are prepared, and a precursor is synthesized by coprecipitation reaction, LiOH is added to the synthesized precursor, and then fired to prepare a lithium composite oxide. Specifically, after mixing LiOH with the precursor, an O2 atmosphere is maintained in a sintering furnace and the temperature is increased to 790°C at 1°C per minute, heat-treated for 10 hours, and then naturally cooled to obtain a lithium composite oxide.

[0146] Next, distilled water was added to the above lithium composite oxide, and then washed with water for 1 hour, and the washed lithium composite oxide was filtered and dried.

[0147] Then, the lithium composite oxide and the boron-containing raw material (H3BO3), the aluminum-containing raw material (Al2O3), the titanium-containing raw material (TiO2) and the zirconium-containing raw material (ZrO2) are mixed together using a heating stirrer and heat-treated. The boron-containing raw material (H3BO3) is mixed so that its content is 0.3% by weight relative to the total weight of the lithium composite oxide, the temperature is raised at 1°C per minute in an O2 atmosphere, and the heat treatment is performed for 5 hours while stirring, and then naturally cooled to obtain the lithium composite oxide.

[0148] (5) Embodiment 5

[0149] The lithium composite oxide was prepared in the same manner as in Example 1 except that the content of the boron-containing raw material (H3BO3) was 0.06 wt% relative to the total weight of the lithium composite oxide.

[0150] (6) Embodiment 6

[0151] The lithium composite oxide was prepared in the same manner as in Example 1 except that the content of the boron-containing raw material (H3BO3) was 0.55 wt% relative to the total weight of the lithium composite oxide.

[0152] (7) Embodiment 7

[0153] The lithium composite oxide was prepared in the same manner as in Example 1 except that the content of the boron-containing raw material (H3BO3) was 0.9 wt% relative to the total weight of the lithium composite oxide.

[0154] (8) Comparative Example 1

[0155] The lithium composite oxide is prepared in the same manner as in Example 1, except that after the washed lithium composite oxide is filtered and dried, the above-mentioned lithium composite oxide and the boron-containing raw material (H3BO3) are mixed together using a mixer, and then the heat treatment is carried out for 5 hours in a sintering furnace while maintaining an O2 atmosphere and heating at 2°C per minute, followed by natural cooling.

[0156] (9) Comparative Example 2

[0157] The lithium composite oxide was prepared in the same manner as in Example 2, except that after the washed lithium composite oxide was filtered and dried, the above-mentioned lithium composite oxide and the boron-containing raw material (H3BO3) were mixed together using a mixer, and then the heat treatment was carried out for 5 hours in a sintering furnace while maintaining an O2 atmosphere and heating at 2°C per minute, and then naturally cooled.

[0158] (10) Comparative Example 3

[0159] The lithium composite oxide was prepared in the same manner as in Example 3, except that the lithium composite oxide and the boron-containing raw material (H3BO3) were mixed together using a mixer after the washed lithium composite oxide was filtered and dried, and then the mixture was heated at 2°C per minute in a sintering furnace while maintaining an O2 atmosphere for 5 hours, and then cooled naturally. In addition, during the mixing, the content of the boron-containing raw material (H3BO3) was mixed to be 1.0% by weight relative to the total weight of the lithium composite oxide.

[0160] (11) Comparative Example 4

[0161] The lithium composite oxide was prepared in the same manner as in Example 4 except that the lithium composite oxide and the boron-containing raw material (H3BO3), the aluminum-containing raw material (Al2O3), the titanium-containing raw material (TiO2) and the zirconium-containing raw material (ZrO2) were mixed together using a mixer after filtering and drying the washed lithium composite oxide, and then the mixture was heat-treated for 5 hours in a sintering furnace while maintaining an O2 atmosphere and heating at 2°C per minute, and then naturally cooled. In addition, during the mixing, the content of the boron-containing raw material (H3BO3) was mixed to be 1.2% by weight relative to the total weight of the lithium composite oxide.

[0162] The compositions of the lithium composite oxides prepared according to the respective Examples and Comparative Examples are shown in Table 1. The compositions of the lithium composite oxides were derived by ICP analysis.

[0163] Table 1

[0164]

[0165] Experimental Example 2. XPS Analysis Results of Lithium Composite Oxide

[0166] The lithium composite oxides prepared according to the examples and comparative examples were subjected to XPS analysis to confirm the composition of the elements in the surface portion of the lithium composite oxides. XPS analysis was performed using Quantum 2000 (Physical Electronics) (accelerating voltage: 0.5-15 keV, 300 W, energy resolution: about 1.0 eV, minimum analysis area: 10 micro, sputtering rate: 0.1 nm / min).

[0167] Table 2 below shows the composition of elements in the surface of the lithium composite oxide prepared according to each of the examples and comparative examples according to the XPS analysis. The composition of elements in the surface of the lithium composite oxide described in Table 2 below shows the composition of elements present from the outermost surface of the lithium composite oxide to a depth of 10 nm.

[0168] Table 2

[0169]

[0170]

[0171] Using the XPS depth profile analysis method (ion energy: 2000eV, spot size: 200μm), about 25nm was etched from the outermost surface of the lithium composite oxide according to Examples 1 to 4, and then the atomic ratio of boron and nickel was analyzed by XPS analysis in the same manner. Similarly, the atomic ratio of boron and nickel was analyzed by XPS analysis by etching the lithium composite oxide that had undergone a surface etching once again in the same manner to confirm whether the B / Ni value changes from the surface portion of the lithium composite oxide toward the center portion. The above XPS analysis results are shown in Table 3 below.

[0172] Table 3

[0173] Classification 1st time - B / Ni 2nd - B / Ni Example 1 0.86 0.52 Example 2 0.91 0.59 Example 3 0.84 0.49 Example 4 0.75 0.44

[0174] Referring to the results of Table 3, it can be confirmed that the B / Ni in the lithium composite oxide confirmed by XPS analysis has a concentration gradient that decreases from the surface portion toward the center portion of the lithium composite oxide. As described above, the concentration gradient direction of B / Ni can minimize the reduction in battery capacity of a lithium secondary battery using the lithium composite oxide and improve life characteristics.

[0175] Table 4

[0176] Classification X Y Y / X Example 1 0.0062 3.54 570.97 Example 2 0.0103 3.89 377.67 Example 3 0.0064 3.46 540.63 Example 4 0.0064 3.70 578.13 Example 5 0.0013 0.21 161.54 Example 6 0.0113 10.5 929.20 Example 7 0.0192 28.8 1500.00 Comparative Example 1 0.0006 0.06 100.00 Comparative Example 2 0.0011 0.17 154.55 Comparative Example 3 0.0202 32.84 1625.74 Comparative Example 4 0.0255 49.63 1946.27

[0177] Table 4 shows the ratio of the atomic ratio X of boron to nickel in the overall composition of the lithium composite oxide described in Table 1 and the atomic ratio Y of boron to nickel in the surface portion of the lithium composite oxide described in Table 2.

[0178] With reference to Table 4, it can be confirmed that the atomic ratio of boron to nickel in the surface portion of the lithium composite oxide is greater than the atomic ratio of boron to nickel in the overall composition of the lithium composite oxide. In particular, it can be confirmed that the ratio of the atomic ratio of boron to nickel in the surface portion of the lithium composite oxide to the atomic ratio of boron to nickel in the overall composition of the lithium composite oxide is at least 160 or more and 1500 or less.

[0179] As described above, the ratio of the atomic ratio of boron to nickel in the surface portion of the above-mentioned lithium composite oxide to the atomic ratio of boron to nickel in the overall composition of the above-mentioned lithium composite oxide is greater than 100 and less than 1500, thereby minimizing the reduction in battery capacity of a lithium secondary battery using the above-mentioned lithium composite oxide and improving life characteristics.

[0180] and, Figure 1 Graph showing XPS analysis results of the lithium composite oxides prepared according to Example 1 and Comparative Example 1, Figure 2 Graph showing XPS analysis results of lithium composite oxides prepared according to Example 2 and Comparative Example 2, Figure 3 Graph showing XPS analysis results of lithium composite oxides prepared according to Example 3 and Comparative Example 3, Figures 4 to 7 Graph showing XPS analysis results of lithium composite oxides prepared according to Example 4 and Comparative Example 4.

[0181] Reference Figures 1 to 3 The lithium composite oxides prepared according to Examples 1 to 3 and Comparative Examples 1 to 3 all showed a B1s peak, thereby confirming that a boron oxide coating was formed on the surface of the lithium composite oxides prepared according to each of the Examples and Comparative Examples.

[0182] On the other hand, referring to Figures 4 to 7 The lithium composite oxides prepared according to Example 4 and Comparative Example 4 further show Al 2p peak, Ti 2p peak and Zr 3d peak, thereby confirming that in addition to the boron oxide coating, aluminum oxide, titanium oxide and zirconium oxide coatings are also formed on the surface of the lithium composite oxides prepared according to Example 4 and Comparative Example 4.

[0183] Experimental Example 3. XRD analysis results of lithium composite oxide

[0184] The lithium composite oxides prepared according to Examples 1 to 4 and Comparative Examples 1 to 4 were subjected to XRD analysis.

[0185] In the XRD analysis, a Cu-Kαα1 radiation source was used as the X-ray source, and the measurement was performed in the range of 10° to 70° (2θ) with a step size of 0.02° by a θ-2θ scanning method (Bragg-Brentano parafocusing geometry).

[0186] Referring to the table showing the XRD analysis results of the lithium composite oxides prepared according to Examples 1 to 4 and Comparative Examples 1 to 4 Figure 8 It can be confirmed that the lithium composite oxides according to each embodiment and comparative example all have a hexagonal lattice structure (hexagonal α-NaFeO2) including an R-3m space group. And, although not shown separately, it can be confirmed that the lithium composite oxides prepared according to Examples 5 to 7 all have a hexagonal lattice structure including an R-3m space group.

[0187] Experimental Example 4. Results of Characteristic Evaluation of Lithium Secondary Batteries

[0188] (1) Preparation of lithium secondary batteries

[0189] The lithium composite oxide prepared according to the above embodiment and comparative example, artificial graphite as a conductive material and polyvinylidene fluoride (PVdF) as a binder were mixed in a weight ratio of 92:4:4 to prepare a slurry. The slurry was uniformly coated on an aluminum foil with a thickness of 15 μm and vacuum dried at 135° C. to prepare a positive electrode for a lithium secondary battery.

[0190] Lithium foil was used as the counter electrode of the above-mentioned positive electrode, a porous polyethylene film (Celgard2300, thickness: 25 μm) was used as the isolation membrane, and a liquid electrolyte containing LiPF6 dissolved at a concentration of 1.15 M in a solvent prepared by mixing ethylene carbonate and ethyl methyl carbonate in a volume ratio of 3:7 was used to prepare a button battery according to a known preparation process.

[0191] (2) Evaluation of capacity characteristics of lithium secondary batteries

[0192] Using an electrochemical analyzer (Toyo, Toscat-3100), a charge / discharge experiment was performed at 25°C, a voltage range of 3.0V to 4.3V, and a discharge rate of 0.1C to 5.0C to determine the charge capacity, discharge capacity, charge / discharge efficiency, and life characteristics of the lithium secondary battery prepared by the above method. Charge / discharge was performed 50 times under the above charge / discharge experimental conditions, and then the ratio of the discharge capacity at the 50th cycle relative to the initial capacity, i.e., the capacity retention rate, was determined. The above measurement results are shown in Table 5 below.

[0193] Table 5

[0194]

[0195]

[0196] Referring to the results in Table 5 above, the charging capacity of the lithium secondary batteries prepared using the lithium composite oxides according to the embodiments and the comparative examples is at a similar level, but in the case of the lithium secondary battery including the positive electrode using the positive electrode active material according to the embodiment, the life characteristics are more excellent than those of Comparative Examples 1 and 2, and the charge / discharge efficiency is higher than that of Comparative Examples 3 and 4.

[0197] Although the embodiments of the present invention are described above, those skilled in the art will understand that various modifications and changes can be made to the present invention by adding, modifying, deleting, increasing, etc., without departing from the scope of the idea of ​​the present invention as described in the claims, and these also fall within the scope of the rights of the present invention.

Claims

1. A lithium composite oxide, wherein: include: Primary particles, capable of occluding and releasing lithium; and Secondary particles, formed by the aggregation of the above primary particles, The boron-containing oxide exists in at least a portion of a region selected from the interface between the primary particles and the surface of the secondary particles, The boron-containing oxide has a concentration gradient that decreases from the surface portion of the secondary particle toward the center portion of the secondary particle.

2. The lithium composite oxide according to claim 1, wherein The atomic ratio of boron to nickel in the lithium composite oxide measured by XPS analysis of the lithium composite oxide has a gradient decreasing from the surface portion of the secondary particle toward the center portion of the secondary particle.

3. The lithium composite oxide according to claim 1, wherein In the overall composition of the secondary particles, the atomic ratio of boron to nickel measured by XPS analysis of the lithium composite oxide is 0.0013 or more and 0.0192 or less.

4. The lithium composite oxide according to claim 1, wherein The atomic ratio of boron to nickel in the surface of the secondary particle measured by XPS analysis of the lithium composite oxide is 0.21 or more and 28.8 or less, The atomic ratio of boron to nickel in the surface portion of the secondary particle was calculated as the atomic ratio of boron to nickel present to a depth of 10 nm from the outermost surface of the secondary particle.

5. The lithium composite oxide according to claim 1, wherein The ratio of the atomic ratio of boron to nickel in the surface of the secondary particle and the atomic ratio of boron to nickel in the overall composition of the secondary particle measured by XPS analysis of the lithium composite oxide is 160 or more and 1500 or less, The atomic ratio of boron to nickel in the surface portion of the secondary particle was calculated as the atomic ratio of boron to nickel present to a depth of 10 nm from the outermost surface of the secondary particle.

6. The lithium composite oxide according to claim 1, wherein The lithium composite oxide includes i) nickel and cobalt, ii) at least one selected from manganese and aluminum, and iii) boron.

7. The lithium composite oxide according to claim 1, wherein The lithium composite oxide is represented by the following chemical formula 1: [Chemical formula 1] The w Nor 1-(x+y+z) Co x B y M1 z M2 z' O2 in, M1 is at least one selected from Mn and Al, M2 is at least one selected from the group consisting of Mn, Ba, Ce, Hf, Ta, Cr, F, Mg, Al, Cr, V, Ti, Fe, Zr, Zn, Si, Y, Nb, Ga, Sn, Mo, W, P, Sr, Ge, Nd, Gd and Cu, M1 and M2 are different elements. 0.5≤w≤1.5,0≤x≤0.50,0 <y≤0.20,0≤z≤0.20,0≤z'≤0.20。 8. The lithium composite oxide according to claim 1, wherein The boron-containing oxide is represented by the following chemical formula 2-1: [Chemical formula 2-1] Li a B b M4 b' Oh c in, M4 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, 0≤a≤6, 0≤b≤8, 0≤b'≤8, 2≤c≤13.

9. The lithium composite oxide according to claim 1, wherein At least a portion of a region selected from the interface between the primary particles and the surface of the secondary particles further includes at least one metal oxide represented by the following Chemical Formula 2: [Chemical formula 2] Read a M3 b Oh c in, M3 is at least one selected from Ni, Mn, Co, Fe, Cu, Nb, Mo, Ti, Al, Cr, Zr, Zn, Na, K, Ca, Mg, Pt, Au, P, Eu, Sm, W, Ce, V, Ba, Ta, Sn, Hf, Gd and Nd, 0≤a≤6, 0≤b≤8, 2≤c≤13.

10. The lithium composite oxide according to claim 9, wherein The boron-containing oxide and the metal oxide may be present in the same layer or in separate layers.