Positive pole piece, preparation method and lithium ion battery
By setting the conductive layer and active material layer in the positive electrode sheet of the lithium-ion battery, the structure of the optical foil layer and the conductive layer is optimized, and the problem of the current collector thickness affecting the battery capacity is solved, the battery performance and stability are improved, and the battery is reduced. cost.
Patent Information
- Application Number
- CN202411021301.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
The current collector thickness of the positive electrode sheet in existing lithium-ion batteries is relatively large, which affects the ductility of the current collector and the battery design capacity, and the increased cost of conductive coating and processing costs are relatively high.
A positive electrode sheet is designed, including an optical foil layer and a conductive layer. The conductive layer is arranged on one side of the optical foil layer and an active material layer is arranged on both sides. By optimizing the surface roughness, surface density and Thickness, combined with the mass ratio of conductive agent and adhesive, uniformly distribute current and mechanical stress, reduce the overall volume of the current collector, and ensure conductivity and adhesiveness.
The performance and stability of the battery are improved, the mechanical stress of the active material is evenly distributed, the volume of the current collector is reduced, the design space of the active material layer is increased, thereby improving the overall capacity of the battery and reducing cost loss.
Smart Images

Figure CN118943380A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of battery materials, and specifically relates to a positive electrode plate and a preparation method, and a lithium-ion battery. Background Art
[0002] Among lithium-ion batteries, lithium iron phosphate batteries are widely used due to their high safety, stable cycle performance, low price, stable discharge platform, and environmental friendliness. At present, lithium-ion batteries often use aluminum foil as the current collector in the positive electrode. Due to the defects of lithium iron phosphate materials such as low electronic and ionic conductivity, relatively small mass density and tap density, they have problems such as poor conductivity and poor adhesion in practical applications. Therefore, in the preparation process of lithium iron phosphate battery current collectors, a certain thickness of conductive carbon layer is often coated on both sides of the plain foil to make carbon-coated aluminum foil. The conductive carbon layer on its surface is used to increase the surface tension of the plain foil, so that the positive active material can be evenly and stably attached to the surface of the current collector, solving the problems of poor adhesion and high contact resistance.
[0003] However, due to the limitations of the coating process, the conductive coating usually has a higher surface density and a thicker thickness, which compresses the thickness of the active material to a certain extent, reduces the design capacity of the battery, and affects the ductility of the current collector; in addition, the increased cost of the conductive coating slurry and coating processing costs, and the added primer step cause process losses, which increase the cost by 40% compared to plain foil.
[0004] Therefore, how to reduce the total volume of the current collector while maintaining the adhesion and conductivity of the current collector of the lithium-ion battery is a problem that needs to be solved at present. Summary of the invention
[0005] The present invention provides a positive electrode plate and a preparation method thereof, and a lithium ion battery, aiming to solve the problem that the overall thickness of the current collector in the positive electrode plate of the existing lithium ion battery is relatively thick, which affects the ductility of the current collector and the designed capacity of the battery.
[0006] The first embodiment of the present application provides a positive electrode sheet, including a current collector and an active material layer disposed on the current collector;
[0007] Wherein, the current collector comprises a light foil layer and a conductive layer, and the conductive layer is arranged on one side of the light foil layer;
[0008] The active material layer includes a first active material layer and a second active material layer, the first active material layer is connected to the conductive layer, and the second active material layer is connected to the optical foil layer.
[0009] In some embodiments, the optical foil layer includes a first surface and a second surface, the first surface is located on a side of the optical foil layer close to the conductive layer, and the second surface is located on a side of the optical foil layer close to the second active material layer;
[0010] Wherein, the surface roughness of the first surface is 0.08-0.13 μm, and the dyne value is 24-28 dyn;
[0011] The surface roughness of the second surface is 0.15 to 0.4 μm, and the dyne value is 32 to 38 dyn.
[0012] In some embodiments, the surface density of the conductive layer is 0.2 to 0.5 g / m 2 .
[0013] In some embodiments, the thickness of the optical foil layer is 6-12 μm.
[0014] In some embodiments, the thickness of the conductive layer is 0.5-2 μm.
[0015] In some embodiments, the first active material layer has a thickness of 85-100 μm.
[0016] In some embodiments, the second active material layer has a thickness of 85-100 μm.
[0017] In some embodiments, the conductive layer includes a conductive agent and an adhesive;
[0018] Wherein, the mass ratio of the conductive agent to the adhesive is (0.8-1.2):1.
[0019] In some embodiments, the conductive agent includes one or a combination of conductive graphite, conductive carbon black, carbon nanotubes, graphene and conductive fibers.
[0020] The adhesive includes one or a combination of polyacrylic acid, polyvinylidene fluoride, and polyvinyl alcohol.
[0021] The second embodiment of the present application provides a method for preparing a positive electrode sheet, which is used to prepare the positive electrode sheet in any of the above embodiments, comprising the following steps:
[0022] Providing a current collector, the current collector comprising a light foil layer and a conductive layer, wherein the conductive layer is arranged on one side of the light foil layer;
[0023] An active material layer is provided, wherein the active material layer includes a first active material layer and a second active material layer, wherein the first active material layer is connected to the conductive layer, and the second active material layer is connected to the optical foil layer.
[0024] In some embodiments, the optical foil layer is prepared by the following steps:
[0025] Providing a cast-rolled billet, and rolling the cast-rolled billet multiple times to obtain a single foil;
[0026] stacking two of the single foils to obtain a coil, and double-closing the coil on a coil closing machine to obtain an intermediate product;
[0027] The intermediate product is finely pressed, rolled and cut through a double rolling process to obtain the smooth foil layer.
[0028] In some embodiments, the thickness of the cast-rolled billet is 0.22-0.26 mm, and the rolling thickness is 0.02-0.03 mm.
[0029] In some embodiments, the coining has a compression amount of 50-60%.
[0030] A third embodiment of the present application provides a lithium-ion battery, comprising the positive electrode sheet in any of the above embodiments.
[0031] The present application provides a positive electrode sheet, including a current collector and an active material layer arranged on the current collector; wherein the current collector includes a light foil layer and a conductive layer, and the conductive layer is arranged on one side of the light foil layer; the active material layer includes a first active material layer and a second active material layer, and the first active material layer is connected to the conductive layer, and the second active material layer is connected to the light foil layer. The light foil layer and the conductive layer form the current collector, and by arranging the active material layer on both sides of the current collector, the current can be evenly distributed, the performance and stability of the battery can be improved, and the mechanical stress of the active material can be evenly distributed; the conductive layer is arranged only on one side of the light foil layer, and the overall volume of the current collector can be reduced while ensuring the conductivity and adhesion of the current collector, providing a larger design space for the active material layer, thereby improving the overall capacity of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] The technical solution and other beneficial effects of the present application will be made apparent by describing in detail the specific implementation methods of the present application in conjunction with the accompanying drawings.
[0033] Figure 1 A schematic diagram of the structure of a positive electrode sheet provided in Example 1 of the present application;
[0034] Figure 2 A schematic diagram of the structure of a positive electrode sheet provided in Comparative Example 1 of the present application;
[0035] Figure 3 A performance test result diagram of the current collector in the positive electrode sheet provided in Example 1 and Comparative Example 1 of the present application;
[0036] Reference numerals:
[0037] 100 - current collector, 101 - optical foil layer, 102 - conductive layer, 200 - active material layer, 201 - first active material layer, 202 - second active material layer. DETAILED DESCRIPTION
[0038] The technical solutions in the embodiments of the present application will be described clearly and completely below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of the present application.
[0039] In the description of the present application, it should be noted that, unless otherwise clearly specified and limited, the terms "connected" and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be directly connected, or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to the specific circumstances. In the description of the present application, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined. In addition, the terms "first" and "second" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more features.
[0040] The disclosure below provides many different embodiments or examples to realize the different structures of the present application. In order to simplify the disclosure of the present application, the parts and settings of specific examples are described below. Of course, they are only examples, and the purpose is not to limit the present application.
[0041] The first embodiment of the present application provides a positive electrode sheet, including a current collector 100 and an active material layer 200 disposed on the current collector 100;
[0042] The current collector 100 includes a light foil layer 101 and a conductive layer 102, and the conductive layer 102 is arranged on one side of the light foil layer 101;
[0043] The active material layer 200 includes a first active material layer 201 and a second active material layer 202 . The first active material layer 201 is connected to the conductive layer 102 , and the second active material layer 202 is connected to the optical foil layer 101 .
[0044] The light foil layer 101 and the conductive layer 102 form the current collector 100. By respectively arranging the first active material layer 201 and the second active material layer 202 on the two side surfaces of the current collector 100, the current can be evenly distributed, the performance and stability of the battery can be improved, and at the same time, the mechanical stress generated by the volume change of the active material during the battery charging and discharging process can be evenly distributed on both sides of the current collector 100, thereby improving the stability and cycle life of the active material; arranging the conductive layer only on one side of the light foil layer can reduce the overall volume of the current collector 100 while ensuring the conductivity and adhesion of the current collector 100, thereby providing a larger design space for the active material layer, thereby improving the overall capacity of the battery.
[0045] In some embodiments, the optical foil layer 101 includes a first surface and a second surface, the first surface is located on a side of the optical foil layer 101 close to the conductive layer 102, and the second surface is located on a side of the optical foil layer 101 close to the second active material layer 202;
[0046] The surface roughness of the first surface is 0.08 to 0.13 μm, and the dyne value is 24 to 28 dyn;
[0047] The surface roughness of the second surface is 0.15 to 0.4 μm, and the dyne value is 32 to 38 dyn.
[0048] It can be understood that the value of the surface roughness of the first surface (unit: μm) can be any value among 0.08, 0.09, 0.1, 0.12, 0.13 or a range between any two values; the value of the dyne value of the first surface (unit: dyn) can be any value among 24, 25, 26, 27, 28 or a range between any two values; the value of the surface roughness of the second surface (unit: μm) can be any value among 0.15, 0.2, 0.25, 0.3, 0.35, 0.4 or a range between any two values; the value of the dyne value of the second surface (unit: dyn) can be any value among 32, 33, 34, 35, 36, 37, 38 or a range between any two values.
[0049] The first surface is directly in contact with the roller for rolling, and its surface tension is low and the adhesion is poor. By coating the conductive layer 102 on the first surface, the surface tension can be increased, the contact resistance can be reduced, and the slurry of the first active material layer 201 can be uniformly and stably attached to the surface of the current collector 100; the second surface has a high surface roughness and dyne value, and has good adhesion and surface tension. Therefore, it is not necessary to add an additional conductive layer 102 to achieve good adhesion with the slurry of the second active material layer 30. When the surface roughness and dyne value of the first surface and the second surface meet the above value range, the surface tension and conductivity of the two sides of the light foil layer 101 can be balanced, so that it has good performance in terms of overall volume and adhesion.
[0050] In some embodiments, the surface density of the conductive layer 102 is 0.2-0.5 g / m 2 It is understood that the surface density of the conductive layer 102 (unit: g / m 2 ) can be any value among 0.2, 0.3, 0.4, 0.5 or a range between any two values. When the surface density of the conductive layer 102 meets the above value range, it can have a good bonding effect and a certain conductivity, thereby reducing the contact resistance of the battery.
[0051] In some embodiments, the thickness of the light foil layer 101 is 10-15 μm. It is understood that the value (unit: μm) of the thickness of the light foil layer 101 can be any value among 10, 11, 12, 13, 14, 15 or a range between any two values. When the thickness of the light foil layer 101 meets the above value range, the stability of the pole piece rolling stage can be guaranteed. In addition, the thicker the thickness of the light foil layer 101, the lower the rolling break rate, which can reduce cost loss.
[0052] In some embodiments, the thickness of the conductive layer 102 is 0.5 to 2 μm. It is understood that the thickness of the conductive layer 102 (unit: μm) can be any value of 0.5, 1, 1.5, 2, or a range between any two values. When the thickness of the conductive layer 102 satisfies the above value range, it can ensure that the overall volume and conductivity of the positive electrode plate are in an ideal state.
[0053] In some embodiments, the thickness of the first active material layer 201 is 85-100 μm. It is understood that the thickness of the first active material layer 201 (unit: μm) can be any value among 85, 90, 95, 100 or a range between any two values.
[0054] In some embodiments, the thickness of the second active material layer 202 is 85-100 μm. It is understood that the thickness of the second active material layer 202 (unit: μm) can be any value among 85, 90, 95, 100 or a range between any two values.
[0055] In some embodiments, the conductive layer 102 includes a conductive agent and an adhesive;
[0056] The mass ratio of the conductive agent to the adhesive is 0.8 to 1.2: 1. When the mass ratio of the conductive agent to the adhesive satisfies the above value range, the bonding strength and conductivity of the conductive layer 102 and the light foil layer 101 can be further balanced.
[0057] In some embodiments, the conductive agent includes one or a combination of conductive graphite, conductive carbon black, carbon nanotubes, graphene, and conductive fibers.
[0058] The adhesive includes one or a combination of polyacrylic acid, polyvinylidene fluoride and polyvinyl alcohol.
[0059] The second embodiment of the present application provides a method for preparing a positive electrode sheet, which is used to prepare the positive electrode sheet in any of the above embodiments, comprising the following steps:
[0060] A current collector 100 is provided, wherein the current collector 100 comprises a light foil layer 101 and a conductive layer 102, wherein the conductive layer 102 is disposed on one side of the light foil layer 101;
[0061] An active material layer 200 is provided. The active material layer 200 includes a first active material layer 201 and a second active material layer 202 . The first active material layer 201 is connected to the conductive layer 102 , and the second active material layer 202 is connected to the optical foil layer 101 .
[0062] In some embodiments, the optical foil layer 101 is prepared by the following steps:
[0063] Providing a cast-rolled billet, and rolling the cast-rolled billet multiple times to obtain a single foil;
[0064] stacking two of the single foils to obtain a coil, and double-closing the coil on a coil closing machine to obtain an intermediate product;
[0065] The intermediate product is finely pressed, rolled, and cut through a double rolling process to obtain the smooth foil layer 101 .
[0066] Specifically, the preparation of the light foil layer 101 can be achieved by the following steps:
[0067] a. Rolling the cast billet through three passes to obtain a single foil;
[0068] b. Double-fold the rolls of the same width and thickness obtained in step a on a roll-folding machine to synthesize aluminum foil with a thickness twice that of a single roll;
[0069] c. The aluminum foil obtained in step b is put into a finishing mill and rolled through a double rolling process. After rolling, an aluminum foil having a thickness of 50 to 60% of the thickness of the aluminum foil in step b is obtained from the outlet of the finishing mill;
[0070] d. Roll and cut the aluminum foil obtained in step c to obtain a finished product.
[0071] In some embodiments, the thickness of the cast-rolled billet is 0.22-0.26 mm, the rolling passes are distributed as 0.24 mm→0.11 mm→0.051 mm→0.024 mm, and the rolling thickness is 0.02-0.03 mm.
[0072] A third embodiment of the present application provides a lithium-ion battery, comprising the positive electrode sheet in any of the above embodiments.
[0073] The following is a description of the positive electrode sheet and preparation method and lithium-ion battery provided by the present application in combination with specific embodiments:
[0074] Example 1
[0075] This embodiment provides a positive electrode sheet, such as Figure 1 As shown, including:
[0076] Light foil layer 101;
[0077] A conductive layer 102, wherein the conductive layer 102 is disposed on one side of the optical foil layer 101;
[0078] A first active material layer 201, the first active material layer 201 is arranged on a side of the conductive layer 102 away from the optical foil layer 101;
[0079] The second active material layer 202 is disposed on a side of the optical foil layer 101 away from the conductive layer 102 .
[0080] The positive electrode sheet provided in this embodiment can be prepared by the following method:
[0081] 1) A 0.24 mm thick cast billet is subjected to three rolling passes to obtain an aluminum foil with a thickness of 0.024 mm, and the rolling passes are distributed as 0.24 mm→0.11 mm→0.051 mm→0.024 mm. The aluminum foil is rolled into a thickness of 0.048 mm by a coiling machine, and the aluminum foil is subjected to finish rolling with a reduction of 50% to obtain a 0.024 mm double coil, which is then subjected to coiling and slitting to obtain a 12 um single-sided smooth aluminum foil layer 101. The smooth foil layer 101 has a thickness of 12 μm, a surface roughness of the first side (bright side) of 0.12 μm, and a dyne value of 26 dyn; the surface roughness of the second side (dark side) of 0.32 μm, and a dyne value of 34 dyn;
[0082] 2) mixing conductive carbon black, carbon nanotubes and polyacrylic acid in a mass ratio of 1:1:2, and adding deionized water to form a conductive slurry with a solid content of 12%;
[0083] 3) The conductive paste is evenly coated on the first surface of the light foil layer 101 by a micro-gravure roller, and dried to form a current collector 100 having a light foil layer 101 and a conductive layer 102. The coating surface density of the conductive layer 102 is 0.4 g / m 2 ;
[0084] 4) Adding NMP to lithium iron phosphate material, conductive agent (SP) and binder (PVDF) in a mass ratio of 97:1.2:1.8 and mixing them evenly to obtain a positive electrode slurry, and coating the positive electrode slurry evenly on the surfaces of both sides of the current collector 100 by extrusion coating to form a first active material layer (30) and a second active material layer (40), drying, rolling and die-cutting at a compaction density of 2.58 to obtain a positive electrode sheet.
[0085] The above positive electrode sheet is further prepared to form a lithium-ion battery, which specifically includes the following steps:
[0086] Graphite, conductive agent (SP), dispersant (CMC) and binder (SBR) are mixed in a mass ratio of 96:1:1.8:1.2, deionized water is added and mixed thoroughly to obtain a negative electrode slurry, the negative electrode slurry is evenly coated on a 6μm copper foil by extrusion coating, and after drying and roller pressing, it is die-cut into negative electrode sheets, stacked with the above-mentioned positive electrode sheets, and then welded into a shell, an electrolyte is injected, and the battery is packaged to obtain a lithium-ion battery.
[0087] Embodiments 2 to 5
[0088] The positive electrode sheets, lithium-ion batteries and preparation methods thereof provided in Examples 2 to 5 are consistent with those in Example 1, except that only the process parameters of the light foil layer are adjusted, as shown in Table 1.
[0089] Comparative Example 1
[0090] Comparative Example 1 provides a positive electrode sheet, such as Figure 2 As shown, including:
[0091] Light foil layer 101;
[0092] Conductive layer 102, the conductive layer 102 is disposed on both sides of the optical foil layer 101, and forms a current collector 100 with the optical foil layer 101;
[0093] The first active material layer 201 and the second active material layer 202 are disposed on both sides of the current collector 100 , respectively.
[0094] The positive electrode sheet provided in this embodiment can be prepared by the following method:
[0095] 1) The 0.24 mm thick cast billet is rolled in 4 passes, and the rolling passes are distributed as 0.24 mm→0.11 mm→0.051 mm→0.024 mm→0.012 mm, to prepare a 12 um double-sided light foil layer 101, the thickness of the light foil layer 101 is 12 μm, the surface roughness of the upper and lower surfaces is 0.11 μm, and the dyne value is 32 dyn;
[0096] 2) mixing conductive carbon black, carbon nanotubes and polyacrylic acid in a mass ratio of 1:1:2, and adding deionized water to form a conductive slurry with a solid content of 12%;
[0097] 3) The conductive paste is evenly coated on the upper and lower surfaces of the light foil layer 101 by a micro-gravure roller, and dried to form a current collector 100 having a light foil layer 101 and a conductive layer 102. The coating surface density of the conductive layer 102 is 0.4 g / m 2 ;
[0098] 4) Adding NMP to lithium iron phosphate material, conductive agent (SP) and binder (PVDF) in a mass ratio of 97:1.2:1.8 and mixing them evenly to obtain a positive electrode slurry, and coating the positive electrode slurry evenly on the surfaces of both sides of the current collector 100 by extrusion coating to form a first active material layer (30) and a second active material layer (40), drying, rolling and die-cutting at a compaction density of 2.58 to obtain a positive electrode sheet.
[0099] The above positive electrode sheet is further prepared to form a lithium-ion battery, which specifically includes the following steps:
[0100] Graphite, conductive agent (SP), dispersant (CMC) and binder (SBR) are mixed in a mass ratio of 96:1:1.8:1.2, deionized water is added and mixed thoroughly to obtain a negative electrode slurry, the negative electrode slurry is evenly coated on a 6μm copper foil by extrusion coating, and after drying and roller pressing, it is die-cut into negative electrode sheets, stacked with the above-mentioned positive electrode sheets, and then welded into a shell, an electrolyte is injected, and the battery is packaged to obtain a lithium-ion battery.
[0101] Comparative Examples 2 to 4
[0102] The positive electrode sheets, lithium-ion batteries and preparation methods thereof provided in Comparative Examples 2 to 4 are consistent with those in Example 1, except that only the process parameters of the light foil layer are adjusted, as shown in Table 1.
[0103] Table 1
[0104]
[0105] The electrical performance of the batteries prepared in Example 1 and Comparative Example 1 was tested. The results are as follows: Figure 3 It can be seen that the positive electrode sheet of the single-sided carbon-coated aluminum foil provided in Example 1 has a similar capacity retention rate in long-term cycles as the positive electrode sheet of the double-sided carbon-coated aluminum foil provided in Comparative Example 1, and the positive electrode sheet provided in Example 1 has a better later performance.
[0106] The current collectors 100 prepared in Examples 1 to 5 and Comparative Examples 1 to 4 were subjected to tension and NMP wiping resistance tests, as well as a rolling stage processing performance test. The test results are shown in Table 2.
[0107] Table 2
[0108]
[0109] According to Table 2, in terms of mechanical properties, the positive electrode plate provided in the embodiment of the present application has NMP wiping resistance and peeling force comparable to that of the double-sided carbon-coated positive electrode plate, and at the same time has better tensile strength and elongation. It can be seen that the positive electrode plate provided in the present application has better processing performance as a whole.
[0110] According to Comparative Example 1, it can be seen that the positive electrode sheet of the double-sided carbon-coated aluminum foil has a large overall volume and thick thickness, resulting in unsatisfactory tensile strength and elongation, and the uneven stress distribution causes the strip to break easily during rolling processing.
[0111] According to Comparative Example 2, when the roughness of the first surface is too small, the bonding force and surface tension between the plain foil layer 101 and the conductive layer 102 are insufficient, resulting in low tensile strength and elongation, and the tape is easily broken during rolling processing.
[0112] According to Comparative Example 3, when the roughness of the first surface is too large, the stress distribution between the plain foil layer 101 and the conductive layer 102 will be uneven, which will also lead to low tensile strength and elongation, and the tape will be easily broken during rolling processing.
[0113] It can be seen from Comparative Example 4 that when the thickness of the light foil layer is too high, the overall volume of the positive electrode plate is too large, resulting in a lower elongation.
[0114] The above is a detailed introduction to a positive electrode plate and a preparation method, and a lithium-ion battery provided in the embodiments of the present application. Specific examples are used in the present application to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the technical solution and its core idea of the present application. Ordinary technicians in this field should understand that they can still modify the technical solutions recorded in the aforementioned embodiments, or replace some of the technical features therein with equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present application.
Claims
1. A positive electrode sheet, characterized in that: It comprises a current collector (100) and an active material layer (200) arranged on the current collector (100); The current collector (100) comprises a light foil layer (101) and a conductive layer (102), and the conductive layer (102) is arranged on one side of the light foil layer (101); The active material layer (200) comprises a first active material layer (201) and a second active material layer (202); the first active material layer (201) is connected to the conductive layer (102), and the second active material layer (202) is connected to the optical foil layer (101).
2. A positive electrode sheet according to claim 1, characterized in that: The optical foil layer (101) comprises a first surface and a second surface, wherein the first surface is located on a side of the optical foil layer (101) close to the conductive layer (102), and the second surface is located on a side of the optical foil layer (101) close to the second active material layer (202); Wherein, the surface roughness of the first surface is 0.08-0.13 μm, and the dyne value is 24-28 dyn; The surface roughness of the second surface is 0.15 to 0.4 μm, and the dyne value is 32 to 38 dyn.
3. A positive electrode sheet according to claim 1, characterized in that: The surface density of the conductive layer (102) is 0.2 to 0.5 g / m 2 .
4. A positive electrode sheet according to claim 1, characterized in that: The thickness of the optical foil layer (101) is 6 to 12 μm; and / or, The thickness of the conductive layer (102) is 0.5 to 2 μm; and / or, The thickness of the first active material layer (201) is 85 to 100 μm; and / or, The thickness of the second active material layer (202) is 85-100 μm.
5. The positive electrode sheet according to claim 1, characterized in that: The conductive layer (102) comprises a conductive agent and an adhesive; Wherein, the mass ratio of the conductive agent to the adhesive is (0.8-1.2):
1.
6. A positive electrode sheet according to claim 5, characterized in that: The conductive agent includes one or a combination of conductive graphite, conductive carbon black, carbon nanotubes, graphene and conductive fibers; and / or, The adhesive includes one or a combination of polyacrylic acid, polyvinylidene fluoride, and polyvinyl alcohol.
7. A method for preparing a positive electrode sheet according to any one of claims 1 to 6, characterized in that: The steps include: A current collector (100) is provided, wherein the current collector (100) comprises a light foil layer (101) and a conductive layer (102), wherein the conductive layer (102) is arranged on one side of the light foil layer (101); An active material layer (200) is provided, wherein the active material layer (200) comprises a first active material layer (201) and a second active material layer (202), wherein the first active material layer (201) is connected to the conductive layer (102), and the second active material layer (202) is connected to the optical foil layer (101).
8. The method for preparing a positive electrode sheet according to claim 7, characterized in that: The optical foil layer (101) is prepared by the following steps: Providing a cast-rolled billet, and rolling the cast-rolled billet multiple times to obtain a single foil; stacking two of the single foils to obtain a coil, and double-closing the coil on a coil closing machine to obtain an intermediate product; The intermediate product is finely pressed, rolled and cut through a double rolling process to obtain the smooth foil layer (101).
9. The method for preparing a positive electrode sheet according to claim 8, characterized in that: The thickness of the cast-rolled billet is 0.22-0.26 mm, and the rolling thickness is 0.02-0.03 mm; and / or, The precision pressing has a pressing amount of 50 to 60%.
10. A lithium ion battery, characterized in that: The invention comprises a positive electrode sheet as claimed in any one of claims 1 to 6 or a positive electrode sheet prepared by a preparation method as claimed in any one of claims 7 to 9.