Non-aqueous electrolyte and high-nickel silicon-based lithium ion battery
By using film-forming additives and cyclosulfonic acid lactone compounds in the nonaqueous electrolyte, a stable battery interface and structure is formed, which solves the problem of performance degradation of high-nickel silicon-based lithium-ion batteries under high temperature conditions, and significantly improves the battery loop and storage performance.
Patent Information
- Application Number
- CN202411220549.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
High-nickel silicon-based lithium-ion batteries have problems such as poor interface stability, low structural stability and poor thermal stability, especially under high temperature conditions, cycling and storage performance are degraded.
Add film-forming additives, lipid heterocyclic sulfonate lactone compounds and aromatic heterocyclic sulfonate lactone compounds as composite additives to the nonaqueous electrolyte solution, and synergistic effects are exerted through specific combinations to form a stable SEI film and passivation film, which improves the Interface and structural stability, inhibit high temperature gas production.
It effectively improves the interface and structural stability of high-nickel silicon-based lithium-ion batteries, improves high-temperature circulation and storage performance, extends the battery's cycle life and suppresses high-temperature gas production.
Smart Images

Figure BDA0005022889900000101 
Figure BDA0005022889900000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a non-aqueous electrolyte and a high-nickel silicon-based lithium ion battery. Background Art
[0002] Lithium-ion batteries are widely favored for their high energy density, long cycle life, and no memory effect. Among them, the positive electrode material is a key factor in determining battery performance and cost. In the layered structure NCM (ternary nickel-cobalt-manganese positive electrode material), nickel is the main redox reaction element, so increasing the nickel content can effectively increase the specific capacity of NCM. High-nickel material NCM material (Ni molar fraction ≥ 0.6) has the characteristics of high specific capacity and low cost, but also has disadvantages such as low capacity retention rate and poor thermal stability. Silicon-based negative electrodes have attracted much attention due to their high theoretical specific capacity, but their huge volume expansion during lithium ion embedding brings challenges, so the application of silicon materials also leads to a reduction in the cycle and storage life of the battery.
[0003] In summary, developing a new type of non-aqueous electrolyte is one of the important research directions to improve the comprehensive performance of high-nickel silicon-based lithium-ion batteries. Summary of the invention
[0004] In view of the deficiencies of the prior art, the object of the present invention is to provide a non-aqueous electrolyte and a high-nickel silicon-based lithium-ion battery. The present invention adds a film-forming additive, an aliphatic heterocyclic sultone compound and an aromatic heterocyclic sultone compound as a composite additive to the non-aqueous electrolyte, and simultaneously utilizes a specific combination of the three additives to exert a synergistic effect, thereby effectively improving the interface stability and structural stability of the high-nickel silicon-based lithium-ion battery, inhibiting the high-temperature gas production of the battery, and improving its high-temperature cycle performance and high-temperature storage performance.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a non-aqueous electrolyte, the non-aqueous electrolyte comprising a non-aqueous organic solvent, a lithium salt and a composite additive;
[0007] The composite additive comprises a film-forming additive, an aliphatic heterocyclic sultone compound and an aromatic heterocyclic sultone compound;
[0008] Based on the mass of the non-aqueous electrolyte, the mass content of the film-forming additive is recorded as W1, the mass content of the aliphatic heterocyclic sultone compound is recorded as W2, and the mass content of the aromatic heterocyclic sultone compound is recorded as W3, W1:W2:W3=(0.5-20):(0.5-10):(0.1-5).
[0009] In high-nickel silicon-based lithium-ion batteries, the continuous destruction and regeneration of the SEI film, as well as the pulverization and crushing of particles, cause the continuous consumption of electrolyte, which indicates that the surface of the silicon material is not effectively passivated, thereby causing the battery performance to decline. Based on this, the present invention introduces a film-forming additive into the non-aqueous electrolyte to reduce the film at the negative electrode, and the dense SEI film formed reduces the internal resistance. At the same time, a fatty heterocyclic sultone compound is introduced to inhibit gas production and improve high-temperature cycle performance. At the same time, an aromatic heterocyclic sultone compound is introduced to form a passivation film at the negative electrode to assist film formation. The three additives work synergistically to stabilize the interface chemical stability and physical structure stability of the battery, improve the high-temperature cycle and high-temperature storage performance of the battery, and inhibit gas production.
[0010] In the present invention, the selection range of W1 "0.5-20" can be, for example, 0.5, 1, 3, 5, 7, 9, 11, 13, 15, 17 or 19, the selection range of W2 "0.5-10" can be, for example, 0.5, 1, 3, 5, 7 or 9, and the selection range of W3 "0.1-5" can be, for example, 0.1, 0.5, 1, 2, 3, 4 or 5. Within the above range, the side reactions at the electrochemical energy storage interface can be effectively suppressed, and the interface stability of the battery can be increased. Among them, when the ratio of W1 to W2 is within a suitable range, the electrochemical stability is enhanced and the cycle life is increased; when the ratio of W1 to W3 is within a suitable range, the capacity retention rate and coulomb efficiency are improved; and when the ratio of W2 to W3 is within a suitable range, it is beneficial to suppress gas production and improve the cycle and high temperature stability of the battery.
[0011] In the present invention, if the ratio of W1 to W2 is too small, that is, the mass content of the aliphatic heterocyclic sultone compound is too large, the internal resistance increases, the capacity and efficiency of the battery are reduced, and the cycle life is reduced; if the ratio of W1 to W2 is too large, that is, the mass content of the aliphatic heterocyclic sultone compound is too small, it will cause battery bloating and seriously reduce battery performance.
[0012] In the present invention, if the ratio of W1 to W3 is too small, that is, the mass content of the aromatic heterocyclic sultone compound is too large, the output voltage is reduced and the internal resistance is increased; if the ratio of W1 to W3 is too large, that is, the mass content of the aromatic heterocyclic sultone compound is too small, the degree of battery cracking is accelerated, causing battery failure.
[0013] In the present invention, if the ratio of W2 to W3 is too small, the internal resistance increases and the battery performance decreases; if the ratio of W2 to W3 is too large, the battery rate and power performance are affected.
[0014] Preferably, the value interval of W1 is 3-20%, for example, it can be 3%, 5%, 7%, 9%, 11%, 13%, 15%, 17% or 19%, etc., preferably 4-15%.
[0015] Preferably, the value interval of W2 is 1-5%, for example, it can be 1%, 2%, 3%, 4% or 5%.
[0016] Preferably, the value interval of W3 is 0.2-1%, for example, it can be 0.2%, 0.4%, 0.6%, 0.8% or 1%.
[0017] In the present invention, the HOMO energy level and LUMO energy level of fluoroethylene carbonate are lower than EC (ethylene carbonate), so its oxidation stability is improved, while its reduction stability is reduced; at low potential, fluoroethylene carbonate is easily reduced at the negative electrode and has good film-forming properties; and fluoroethylene carbonate can reduce the loss of active Li and Si after battery cycling, and the negative electrode impedance changes less after cycling. However, if used alone, gas generation is serious during cycling and storage.
[0018] Preferably, the film-forming additive includes any one of fluoroethylene carbonate, trifluoromethylethylene carbonate or difluoroethylene carbonate, or a combination of at least two thereof.
[0019] Preferably, the aliphatic heterocyclic sultone compound includes 1,3-propane sultone and / or 1,4-butane sultone.
[0020] Preferably, the aromatic heterocyclic sultone compound comprises a monocyclic heterocyclic sultone compound and / or a condensed heterocyclic sultone compound.
[0021] Preferably, the monoheterocyclic sultone compound comprises 1,3-propene sultone and / or 1,4-butene sultone.
[0022] Preferably, the fused heterocyclic sultone compound includes any one of 1,3-propane sultone, 4-hydroxybutane-1-sultone-δ-sultone or 1,3,2-dioxazolethiophene-2,2-dioxide or a combination of at least two thereof.
[0023] Preferably, the lithium salt includes any one of LiPF6, LiBF4, LiFSI, LiBOB, LiDFOB, LiPO2F2, LiDFOP, LiTFOP, LiAsF6 or LiClO4, or a combination of at least two thereof.
[0024] Preferably, the concentration of the lithium salt in the non-aqueous electrolyte is 0.8-2 mol / L, for example, 0.8 mol / L, 1 mol / L, 1.2 mol / L, 1.4 mol / L, 1.6 mol / L, 1.8 mol / L or 2 mol / L.
[0025] In the present invention, the concentration of the lithium salt in the non-aqueous electrolyte is within the above range to have good viscosity and excellent ion conductivity.
[0026] Preferably, the non-aqueous organic solvent includes any one of ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate or propyl propionate, or a combination of at least two thereof.
[0027] In a second aspect, the present invention provides a high-nickel silicon-based lithium-ion battery, comprising a positive electrode, a negative electrode, a separator and the non-aqueous electrolyte as described in the first aspect, wherein the separator is arranged between the positive electrode and the negative electrode.
[0028] Preferably, the positive electrode comprises a positive electrode material layer, and the chemical formula of the active material in the positive electrode material layer is LiNi x Co y Mn z L (1-x-y-z) O2, wherein L is any one of Al, Sr, Mg, Ti, Ca, Zr, Zn, Si or Fe or a combination of at least two thereof, 0.6≤x≤1, 0≤y≤1, 0≤z≤1.
[0029] In the present invention, 0.6≤x≤1, for example, it can be 0.6, 0.7, 0.8, 0.9 or 1, 0≤y≤1, for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1, and 0≤z≤1, for example, it can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9 or 1, etc.
[0030] Preferably, the negative electrode comprises a negative electrode material layer, and the active material in the negative electrode material layer is a silicon-based material.
[0031] Preferably, the silicon-based material includes nano-silicon or silicon-carbon material. Exemplarily, the silicon-carbon material can be prepared by combining silicon oxide and graphite.
[0032] Preferably, the diaphragm comprises a polymer diaphragm or a ceramic diaphragm.
[0033] Preferably, the material of the polymer membrane includes polyethylene and / or polypropylene.
[0034] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] The present invention adds a film-forming additive, an aliphatic heterocyclic sultone compound and an aromatic heterocyclic sultone compound as a composite additive to a non-aqueous electrolyte, and simultaneously utilizes a specific combination of the three additives to exert a synergistic effect, thereby effectively improving the interface stability and structural stability of a high-nickel silicon-based lithium-ion battery, inhibiting the high-temperature gas production of the battery, and improving its high-temperature cycle performance and high-temperature storage performance. DETAILED DESCRIPTION
[0037] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0038] Example 1
[0039] This embodiment provides a non-aqueous electrolyte, which includes a non-aqueous organic solvent, a lithium salt and a composite additive;
[0040] The composite additive comprises a film-forming additive, an aliphatic heterocyclic sultone compound and an aromatic heterocyclic sultone compound;
[0041] Based on the mass of the non-aqueous electrolyte, the mass content of the film-forming additive is recorded as W1, the mass content of the aliphatic heterocyclic sultone compound is recorded as W2, and the mass content of the aromatic heterocyclic sultone compound is recorded as W3, W1:W2:W3=3:1:0.2;
[0042] The film-forming additive is fluoroethylene carbonate, the aliphatic heterocyclic sultone compound is 1,3-propane sultone, and the aromatic heterocyclic sultone compound is 1,4-butene sultone;
[0043] The lithium salt is LiPF6, and the concentration of the lithium salt in the non-aqueous electrolyte is 1 mol / L;
[0044] The non-aqueous organic solvent is a mixed solvent of ethylene carbonate, diethyl carbonate and ethyl methyl carbonate in a volume ratio of 3:2:5.
[0045] This embodiment also provides a high-nickel silicon-based lithium-ion battery, the high-nickel silicon-based lithium-ion battery comprising a positive electrode, a negative electrode, a separator and the non-aqueous electrolyte as described above, the separator being arranged between the positive electrode and the negative electrode;
[0046] The positive electrode includes a positive electrode material layer, and the chemical formula of the active material in the positive electrode material layer is LiNi 0.8 Co 0.1 Mn 0.1 O2;
[0047] The negative electrode comprises a negative electrode material layer, and the active material in the negative electrode material layer is nano-silicon;
[0048] The diaphragm is a polyethylene diaphragm.
[0049] Example 2
[0050] The difference between this embodiment and embodiment 1 is that W1:W2:W3=5:1:0.2.
[0051] The rest of the preparation methods and parameters were the same as those in Example 1.
[0052] Example 3
[0053] The difference between this embodiment and embodiment 1 is that W1:W2:W3=8:1:0.2.
[0054] The rest of the preparation methods and parameters were the same as those in Example 1.
[0055] Example 4
[0056] The difference between this embodiment and embodiment 2 is that W1:W2:W3=5:2:0.2.
[0057] The rest of the preparation methods and parameters were the same as those in Example 2.
[0058] Example 5
[0059] The difference between this embodiment and embodiment 2 is that W1:W2:W3=5:3:0.2. The rest of the preparation methods and parameters are the same as those in embodiment 2.
[0060] Example 6
[0061] The difference between this embodiment and embodiment 2 is that W1:W2:W3=5:5:0.2. The other preparation methods and parameters are the same as those in embodiment 2.
[0062] Example 7
[0063] The difference between this embodiment and embodiment 4 is that W1:W2:W3=5:2:0.1. The other preparation methods and parameters are the same as those in embodiment 4.
[0064] Example 8
[0065] The difference between this embodiment and embodiment 4 is that W1:W2:W3=5:2:0.5. The other preparation methods and parameters are the same as those in embodiment 4.
[0066] Example 9
[0067] The difference between this embodiment and embodiment 4 is that W1:W2:W3=5:2:1. The other preparation methods and parameters are the same as those in embodiment 4.
[0068] Example 10
[0069] The difference between this embodiment and embodiment 1 is that the value of W1 is 20%. The other preparation methods and parameters are the same as those in embodiment 1.
[0070] Embodiment 11
[0071] The difference between this embodiment and embodiment 1 is that the value of W1 is 3%. The other preparation methods and parameters are the same as those in embodiment 1.
[0072] Example 12
[0073] The difference between this embodiment and embodiment 1 is that the value of W2 is 8%. The other preparation methods and parameters are the same as those in embodiment 1.
[0074] Example 13
[0075] The difference between this embodiment and embodiment 1 is that the value of W2 is 0.5%.
[0076] The rest of the preparation methods and parameters were the same as those in Example 1.
[0077] Embodiment 14
[0078] The difference between this embodiment and embodiment 1 is that the value of W3 is 3%.
[0079] The rest of the preparation methods and parameters were the same as those in Example 1.
[0080] Embodiment 15
[0081] The difference between this embodiment and embodiment 1 is that the value of W3 is 0.1%.
[0082] The rest of the preparation methods and parameters were the same as those in Example 1.
[0083] Comparative Example 1
[0084] The difference between this comparative example and Example 8 is that 1,4-butene sultone is not added, that is, W3 is 0.
[0085] The rest of the preparation methods and parameters were the same as those in Example 8.
[0086] Comparative Example 2
[0087] The difference between this comparative example and Example 8 is that 1,3-propane sultone is not added, that is, W2 is 0.
[0088] The rest of the preparation methods and parameters were the same as those in Example 8.
[0089] Comparative Example 3
[0090] The difference between this comparative example and Example 8 is that no fluoroethylene carbonate is added, that is, W1 is 0.
[0091] The rest of the preparation methods and parameters were the same as those in Example 8.
[0092] Comparative Example 4
[0093] The difference between this comparative example and Example 8 is that the mass contents of fluoroethylene carbonate and 1,3-propane sultone are adjusted so that W1:W2=0.1:10.
[0094] The rest of the preparation methods and parameters were the same as those in Example 8.
[0095] Comparative Example 5
[0096] The difference between this comparative example and Example 8 is that the mass contents of fluoroethylene carbonate and 1,3-propane sultone are adjusted so that W1:W2=25:0.5.
[0097] The rest of the preparation methods and parameters were the same as those in Example 8.
[0098] Comparative Example 6
[0099] The difference between this comparative example and Example 8 is that the mass contents of fluoroethylene carbonate and 1,4-butene sultone are adjusted so that W1:W3=0.5:10.
[0100] The rest of the preparation methods and parameters were the same as those in Example 8.
[0101] Comparative Example 7
[0102] The difference between this comparative example and Example 8 is that the mass contents of fluoroethylene carbonate and 1,4-butene sultone are adjusted so that W1:W3=25:0.1.
[0103] The rest of the preparation methods and parameters were the same as those in Example 8.
[0104] Comparative Example 8
[0105] The difference between this comparative example and Example 8 is that the mass contents of 1,3-propane sultone and 1,4-butene sultone are adjusted so that W2:W3=0.5:10.
[0106] The rest of the preparation methods and parameters were the same as those in Example 8.
[0107] Comparative Example 9
[0108] The difference between this comparative example and Example 8 is that the mass contents of 1,3-propane sultone and 1,4-butene sultone are adjusted so that W2:W3=15:0.1.
[0109] The rest of the preparation methods and parameters were the same as those in Example 8.
[0110] Performance Testing
[0111] The high nickel silicon-based lithium ion batteries provided in the above examples and comparative examples were tested as follows:
[0112] 1. At 45°C, the formed high nickel silicon-based lithium-ion battery is charged to 4.25V with a 1C constant current and constant voltage, and the cut-off current is 0.05C, and then discharged to 2.75V with a 1C constant current. After such charge / discharge cycles, the capacity retention rate after the 500th cycle is calculated to evaluate its 45°C cycle performance;
[0113] The capacity retention rate after 500 cycles is calculated as follows:
[0114] Capacity retention rate (%) = (500th cycle discharge capacity / 1st cycle discharge capacity) × 100%.
[0115] 2. Test method for capacity retention rate, capacity recovery rate and thickness expansion rate after storage at 60°C for 14 days: Charge the formed high nickel silicon-based lithium-ion battery to 4.25V at room temperature 25°C with 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.75V with 1C constant current, measure the initial discharge capacity of the battery, and then charge it to 4.25V with 1C constant current and constant voltage, with a cut-off current of 0.05C, measure the initial thickness of the battery, and then store the battery at 60°C for 14 days, measure the thickness of the battery, and then discharge it to 2.75V with 1C constant current, measure the battery retention capacity, and then charge it to 2.75V with 1C constant current and constant voltage, with a cut-off current of 0.05C, and then discharge it to 2.75V with 1C constant current, and measure the recovery capacity;
[0116] The calculation formulas for capacity retention rate, capacity recovery rate, and thickness expansion rate are as follows:
[0117] Capacity retention rate (%) = retention capacity / initial capacity × 100%;
[0118] Capacity recovery rate (%) = recovery capacity / initial capacity × 100%;
[0119] Thickness expansion ratio (%) = (thickness after 14 days - initial thickness) / initial thickness × 100%.
[0120] The above test results are shown in Table 1.
[0121] Table 1
[0122]
[0123]
[0124] analyze:
[0125] As can be seen from the above table, the present invention introduces fluoroethylene carbonate into the non-aqueous electrolyte to reduce and form a film at the negative electrode, and the dense SEI film formed reduces the internal resistance. At the same time, the introduction of aliphatic heterocyclic sultone compounds inhibits gas production and improves high-temperature cycle performance. At the same time, the introduction of aromatic heterocyclic sultone compounds forms a passivation film at the negative electrode to assist film formation. The synergistic effect of the three additives can stabilize the interfacial chemical stability and physical structure stability of the battery, improve the high-temperature cycle and high-temperature storage performance of the battery, and inhibit gas production.
[0126] It can be seen from Example 1 and Examples 10-11 that if the amount of fluoroethylene carbonate is large, the battery will produce serious gas, resulting in an increase in the thermal runaway factors of the battery; if the amount of fluoroethylene carbonate is small, the SEI film formed by the battery will be unstable, and the capacity retention rate and capacity recovery rate will be reduced.
[0127] It can be seen from Examples 1 and 12-13 that if the amount of 1,3-propane sultone is large, the DCR will increase and the battery will be severely cracked; if the amount of 1,3-propane sultone is small, the internal interface stability of the battery will be poor and gas generation will occur.
[0128] It can be seen from Example 1 and Examples 14-15 that if the amount of 1,4-butene sultone is large, the DCR will increase and the battery capacity retention and recovery rate will be reduced; if the amount of 1,4-butene sultone is small, the battery high temperature cycle retention rate will be poor.
[0129] It can be seen from Example 8 and Comparative Example 1 that if 1,4-butene sultone is not added, high-temperature flatulence will occur and the capacity retention rate will be low.
[0130] It can be seen from Example 8 and Comparative Example 2 that if 1,3-propane sultone is not added, the capacity retention rate and capacity recovery rate of the battery are both reduced, the DC impedance is greatly increased, and the thickness expansion rate becomes larger.
[0131] It can be seen from Example 8 and Comparative Example 3 that if fluoroethylene carbonate is not added, the capacity retention rate at 45° C. for 500 weeks is poor, as low as 65.8%, and the DC impedance is greatly increased.
[0132] It can be seen from Example 8 and Comparative Examples 4-5 that if the ratio of W1:W2 is too small, the DCR increases, affecting the discharge capacity of the battery; if the ratio of W1:W2 is too large, serious gas production occurs, leading to thermal runaway.
[0133] It can be seen from Example 8 and Comparative Examples 6-7 that if the ratio of W1:W3 is too small, the battery will be severely cracked, and the discharge recovery rate after storage is only 62.3%; if the ratio of W1:W3 is too large, the battery expansion rate reaches 10%, and bloating occurs.
[0134] It can be seen from Example 8 and Comparative Examples 8-9 that if the ratio of W2:W3 is too small, the battery will not bloat, but will be severely cracked, with a capacity recovery of only 60.3%; if the ratio of W2:W3 is too large, the power performance of the battery will be affected, with a capacity retention rate of only 52% after 500 weeks at 45°C.
[0135] The applicant declares that the present invention illustrates the technical solution of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned embodiments, that is, it does not mean that the present invention must rely on the above-mentioned embodiments to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of various raw materials of the product of the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A non-aqueous electrolyte, characterized in that: The non-aqueous electrolyte comprises a non-aqueous organic solvent, a lithium salt and a composite additive; The composite additive comprises a film-forming additive, an aliphatic heterocyclic sultone compound and an aromatic heterocyclic sultone compound; Based on the mass of the non-aqueous electrolyte, the mass content of the film-forming additive is recorded as W1, the mass content of the aliphatic heterocyclic sultone compound is recorded as W2, and the mass content of the aromatic heterocyclic sultone compound is recorded as W3, W1:W2:W3=(0.5-20):(0.5-10):(0.1-5).
2. The non-aqueous electrolyte according to claim 1, characterized in that The value range of W1 is 3-20%, preferably 4-15%; Preferably, the value range of W2 is 1-5%; Preferably, the value interval of W3 is 0.2-1%.
3. The non-aqueous electrolyte according to claim 1 or 2, characterized in that The film-forming additive includes any one of fluoroethylene carbonate, trifluoromethylethylene carbonate or difluoroethylene carbonate or a combination of at least two thereof; Preferably, the aliphatic heterocyclic sultone compound comprises 1,3-propane sultone and / or 1,4-butane sultone; Preferably, the aromatic heterocyclic sultone compound comprises a monocyclic heterocyclic sultone compound and / or a condensed heterocyclic sultone compound; Preferably, the monoheterocyclic sultone compound comprises 1,3-propene sultone and / or 1,4-butene sultone; Preferably, the fused heterocyclic sultone compound includes any one of 1,3-propane sultone, 4-hydroxybutane-1-sultone-δ-sultone or 1,3,2-dioxazolethiophene-2,2-dioxide or a combination of at least two thereof.
4. The non-aqueous electrolyte according to any one of claims 1 to 3, characterized in that: The lithium salt includes any one of LiPF6, LiBF4, LiFSI, LiBOB, LiDFOB, LiPO2F2, LiDFOP, LiTFOP, LiAsF6 or LiClO4, or a combination of at least two thereof; Preferably, the concentration of the lithium salt in the non-aqueous electrolyte is 0.8-2 mol / L.
5. The non-aqueous electrolyte according to any one of claims 1 to 4, characterized in that: The non-aqueous organic solvent includes any one of ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, propylene carbonate, ethylene carbonate or propyl propionate, or a combination of at least two thereof.
6. A high nickel silicon based lithium ion battery, characterized in that: The high-nickel silicon-based lithium-ion battery comprises a positive electrode, a negative electrode, a separator and the non-aqueous electrolyte according to any one of claims 1 to 5, wherein the separator is arranged between the positive electrode and the negative electrode.
7. The high nickel silicon-based lithium ion battery according to claim 6, characterized in that: The positive electrode comprises a positive electrode material layer, and the chemical formula of the active material in the positive electrode material layer is LiNi x Co y Mn z L (1-x-y-z) O2, wherein L is any one of Al, Sr, Mg, Ti, Ca, Zr, Zn, Si or Fe or a combination of at least two thereof, 0.6≤x≤1, 0≤y≤1, 0≤z≤1.
8. The high nickel silicon based lithium ion battery according to claim 6 or 7, characterized in that: The negative electrode comprises a negative electrode material layer, and the active material in the negative electrode material layer is a silicon-based material.
9. The high nickel silicon-based lithium ion battery according to any one of claims 6 to 8, characterized in that: The diaphragm comprises a polymer diaphragm or a ceramic diaphragm; Preferably, the material of the polymer membrane includes polyethylene and / or polypropylene.