Electrolyte for aqueous battery, preparation method of electrolyte and aqueous battery
By using electrolytes containing strong acid salts, weak acid salts, stabilizers, antioxidants and surfactants in aqueous batteries, the limitations and corrosion problems of electrolytes and current collectors are solved, extending battery life and improving electrochemistry performance.
Patent Information
- Application Number
- CN202411418807.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-10-12
AI Technical Summary
The matching between the electrolyte of existing water-based batteries and amphoteric current collectors is limited, which leads to the problem that the electrolyte is prone to corrosive current collectors and damages the battery.
Provide an electrolyte for aqueous batteries, including solvents, strong acid salts, weak acid salts, stabilizers, antioxidants and surfactants. By adjusting the pH value and ion concentration of the electrolyte, it prevents current collector corrosion and increases the electrolyte. stability.
It effectively improves the ionic conductivity of the electrolyte, extends the cycle life of the battery, slows down the corrosion of the current collector, expands the application range of the current collector types, and improves the electrochemical performance of the battery.
Smart Images

Figure CN118943524A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of aqueous batteries, and in particular to an electrolyte for aqueous batteries, a preparation method thereof, and an aqueous battery. Background Art
[0002] The electrochemical performance of aqueous batteries is closely related to their electrolytes, and the components of the electrolytes determine the type and life of the current collectors. The components and pH of the electrolytes of aqueous batteries vary with their types, which limits the selection and protection of the current collectors. Sometimes, due to factors such as the type of aqueous batteries and the overpotential of the current collectors, the selection of electrolytes is full of limitations. For example, it is necessary to change the type of solute, reduce the ionic conductivity of the electrolyte, increase the freezing point of the solution, change the pH value, etc., in order to match the selected current collectors, which greatly limits the development of aqueous batteries. Summary of the invention
[0003] In view of the above situation, the present invention aims to provide an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery, which are used to solve one of the following technical problems: the matching limitations of the electrolyte and the amphoteric current collector of the existing aqueous battery, and the problem that the electrolyte is easy to corrode the amphoteric current collector, resulting in easy damage to the battery.
[0004] The purpose of the present invention is mainly achieved through the following technical solutions: On the one hand, the present invention provides an electrolyte for an aqueous battery, the components of which include: a solvent, an electrolyte salt, an additive and an acid-base buffer; wherein the electrolyte salt includes a strong acid radical salt and a weak acid radical salt, and the additive includes a stabilizer, an antioxidant and a surfactant.
[0005] Furthermore, the solvent includes water and an organic solvent.
[0006] Furthermore, the strong acid salt is one or more of sulfate, nitrate, sulfamate, trifluoromethylsulfonate, fluoride, chlorate, perchlorate and permanganate.
[0007] Furthermore, the weak acid salt is one or more of carbonate, bicarbonate, acetate, sulfite, bisulfite, phosphate, hydrogen phosphate, dihydrogen phosphate, oxalate and silicate.
[0008] Furthermore, the stabilizer is one or more of phosphate, sodium citrate, tartrate, glycinate, polyvinyl alcohol, polyacrylic acid, magnesium succinate and sodium dehydrocholate.
[0009] Furthermore, the antioxidant is one or more of ascorbic acid, tea polyphenols, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone, tert-butylhydroquinone, citric acid, EDTA, and ascorbyl palmitate.
[0010] Furthermore, the concentration of the strong acid salt is 0.5~18 mol / L.
[0011] Furthermore, the concentration of the weak acid salt is 0.1~6 mol / L.
[0012] On the other hand, the present invention also provides a method for preparing the above aqueous battery electrolyte, comprising: Step 1, mixing water and an organic solvent to obtain a mixed solvent; Step 2, adding electrolyte salt into the mixed solvent and mixing to obtain solution A; Step 3, adding a stabilizer, an antioxidant and a surfactant to solution A in sequence and mixing them to obtain solution B; Step 4: Add an acid-base buffer to solution B and adjust the pH of solution B to neutral to obtain an electrolyte for an aqueous battery.
[0013] The present invention also provides an aqueous battery, which includes the above-mentioned aqueous battery electrolyte.
[0014] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects: a) The electrolyte salt of the aqueous battery electrolyte of the present invention includes a strong acid salt and a weak acid salt. The main salt of the electrolyte is a strong acid salt, which can be completely ionized after being completely dissolved, providing a rich ion concentration for the electrolyte, thereby increasing the ion conductivity and ion transfer rate of the electrolyte, further accelerating the electrochemical reaction rate, and to a certain extent reducing the adverse effects of concentration polarization; the secondary salt of the electrolyte is a weak acid salt, which can be partially hydrolyzed after being completely dissolved. When the aqueous battery uses amphoteric metals as the current collector, the weak acid hydrated ions formed by the solvation of the weak acid can act as the current collector and react with H 2 O, isolating the direct contact between the metal hydrated ions in the electrolyte and the current collector, thereby avoiding the corrosion of the current collector and slowing down the gas evolution of the electrolyte without affecting the ion exchange, thereby extending the cycle life of the battery.
[0015] b) By adding an appropriate amount of stabilizer to the aqueous battery electrolyte of the present invention, the balance between solvents and between solvents and solutes in the electrolyte can be ensured, and at the same time, the liquid tension can be reduced, so that the electrolyte can better infiltrate the inside of the electrode, making ion shuttling and reaction smoother, the DCR value of the battery smaller, and more conducive to improving the cycle reversibility of the battery.
[0016] c) By adding an appropriate amount of antioxidant to the aqueous battery electrolyte of the present invention, the volatilization or deterioration of the polar organic solvent in the electrolyte can be effectively prevented, and the concentration of the electrolyte can be ensured not to deviate greatly during the use of the battery. By adding an appropriate amount of surfactant, the reduction of the solvation sheath bond energy of the ions can be promoted, the energy loss in the kinetics of ion reactions can be reduced, and the reversibility of the electrode material and the coulombic efficiency of the battery can be improved. The initial pH of the electrolyte is adjusted to about neutral by an acid-base buffer, in order to prevent the occurrence of hydrogen evolution reaction (HER) or oxygen evolution reaction (OER) on the surface of the amphoteric metal current collector during electrochemical characterization, and during the cycle of the battery, due to the presence of the acid-base buffer and the weak acid salt, the pH of the electrolyte can be adjusted in time to prevent the corrosion of the amphoteric metal current collector, thereby avoiding the aggravation of side reactions or damage to the aqueous battery.
[0017] d) The present invention aims to be able to widely apply amphoteric metals in the current collectors of aqueous batteries, and to slow down or even avoid the corrosion of amphoteric metals in aqueous electrolytes, and to a certain extent, expand the types of current collectors that can be used in aqueous batteries. The electrolyte of the present invention can make the current collector and the electrolyte more fully matched, and minimize the impact of changing electrolyte factors on the electrochemical performance of the battery, so that the electrochemical performance of the aqueous battery can be fully utilized, and promote the rapid development of aqueous batteries.
[0018] e) The aqueous battery using the electrolyte of the present invention can adapt to more types of amphoteric metals, thereby effectively alleviating or even avoiding the corrosion of the amphoteric metal current collector, and further extending the cycle life of the aqueous battery.
[0019] Other features and advantages of the present invention will be described in the following description, and part of them will become obvious from the description, or will be understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the contents particularly pointed out in the written description and the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The accompanying drawings are only used for the purpose of illustrating specific embodiments and are not to be considered as limiting the present invention. In the entire drawings, the same reference symbols represent the same components; Figure 1 The conductivity diagram of the electrolyte of Example 1 and Comparative Example 1; Figure 2 The conductivity diagram of the electrolyte of Example 2 and Comparative Example 2; Figure 3 A comparison diagram of the current collectors of the aqueous sodium battery after cycling between Example 1 and Comparative Example 1; Figure 4 A comparison diagram of the current collectors of the aqueous lithium battery after cycles of Example 2 and Comparative Example 2; Figure 5 is the percentage of electrolyte concentration of the aqueous sodium battery after cycling of Example 1 and Comparative Example 1 (before cycling is 100%); Figure 6 is the percentage of electrolyte concentration of the aqueous lithium battery of Example 2 and Comparative Example 2 after cycling (the electrolyte concentration before cycling is 100%); Figure 7 The DCR diagrams of aqueous sodium batteries of Example 1 and Comparative Example 1; Figure 8 The DCR diagram of the aqueous lithium battery of Example 2 and Comparative Example 2; Fig. 9 The cycle performance diagram of the aqueous sodium battery of Example 1 and Comparative Example 1; Fig.10 It is a cycle performance diagram of the aqueous lithium battery of Example 2 and Comparative Example 2. DETAILED DESCRIPTION
[0021] Preferred embodiments of the present invention will be described in detail below in conjunction with the accompanying drawings, wherein the accompanying drawings constitute a part of the present invention and are used to explain the principles of the present invention together with the embodiments of the present invention.
[0022] The present invention provides an electrolyte for an aqueous battery. The components of the electrolyte for an aqueous battery include: a solvent, an electrolyte salt, an additive and an acid-base buffer; wherein the electrolyte salt includes a strong acid radical salt and a weak acid radical salt, and the additive includes a stabilizer, an antioxidant and a surfactant.
[0023] Specifically, the solvent can provide a place for electrochemical reactions and ensure the normal progress of redox reactions during charging and discharging; specifically, the solvent includes water and organic solvents.
[0024] Specifically, in order to prevent contamination by impurities, the water can be deionized water; the organic solvent can be a polar organic solvent, and the polar organic solvent can be one or more of alcohols, acetonitrile, chloroform, DMSO, pyridine, acetone, formamide, triethylamine, tributylamine, trioctylamine, hexamethylphosphoramide, tetramethylethylenediamine, trifluoroacetic acid, ethyl acetate, dioxane and tetrahydrofuran, etc. The above polar organic solvents can be miscible with deionized water in a certain proportion, and after the solute is completely dissolved, they can undergo solvation with the deionized water. For example, the polar organic solvent can be alcohols and acetonitrile, and the volume ratio of alcohols to acetonitrile is 1~2:1; the polar organic solvent can be triethylamine and dioxane, and the volume ratio of triethylamine to dioxane is 1~2:1; the polar organic solvent can be DMSO and acetone, and the volume ratio of DMSO to acetone is 2~3:1; the polar organic solvent can be pyridine and tetramethylethylenediamine, and the volume ratio of pyridine to tetramethylethylenediamine is 1.5~3:1.
[0025] Specifically, considering that too much polar organic solvent may cause the electrolyte ion conductivity to be too low, affecting the electrochemical reaction rate, too little organic solvent may cause serious hydrogen evolution / oxygen evolution reaction under high voltage. Therefore, in order to maintain a high ionic conductivity of the electrolyte and provide a reaction site for the strong dynamic movement of ions, the volume ratio of water to polar organic solvent is controlled to be (2-20):1, such as 5:1, 8:1, 10:1, 13:1, 15:1, 18:1, preferably (5-15):1.
[0026] Specifically, electrolyte salts are used to provide the main ions required for electrochemical reactions. Different electrolyte salts can be ionized or hydrolyzed after dissolution, wherein the ionized ions can play a role in ion transport, and the hydrolyzed H - or OH - The pH of the electrolyte can be adjusted, and the appropriate electrolyte salt concentration can greatly reduce the concentration polarization in the electrochemical reaction while ensuring high ionic conductivity.
[0027] Specifically, the electrolyte salt includes a strong acid salt and a weak acid salt, wherein the strong acid salt is the main salt of the electrolyte, and the strong acid salt can be one or more of sulfate, nitrate, aminosulfonate, trifluoromethanesulfonate, fluoride, chlorate, perchlorate and permanganate; for example, the strong acid salt can be sulfate and perchlorate, and the molar ratio of sulfate to perchlorate is 1-2:4-5; for example, the strong acid salt can be nitrate and aminosulfonate; the weak acid salt is the secondary salt of the electrolyte, which can be The weak acid salt may be one or more of carbonate, bicarbonate, acetate, sulfite, bisulfite, phosphate, hydrogen phosphate, dihydrogen phosphate, oxalate and silicate; for example, the weak acid salt may be dihydrogen phosphate and acetate, and the molar ratio of dihydrogen phosphate to acetate is 1-2:2; the weak acid salt may be carbonate and oxalate, and the molar ratio of carbonate to oxalate is 1-2:3-4; the cation of the electrolyte salt may be Li + 、Na + , K + Mg 2+ 、Zn 2+ , Ca 2+ 、Al 3+ , Fe 2+ , Fe 3+ , Cu 2+ 、Ag + , Pb 2+ Sn 2+ NH 4 + NR 4 + and C 5 H 5 NH+ Wait for one of them.
[0028] Specifically, in order to ensure that more ions and higher ionic conductivity can be provided and the normal redox reaction rate can be met, the concentration of the strong acid salt in the above-mentioned electrolyte salt is 0.5~18 mol / L, for example, 1 mol / L, 3 mol / L, 5 mol / L, 7 mol / L, 10 mol / L, 13 mol / L, 15 mol / L, preferably 1~10 mol / L.
[0029] Specifically, in order to effectively balance the ion concentration of the electrolyte and adjust the pH value of the electrolyte to a certain extent, the concentration of the weak acid salt in the electrolyte salt is controlled to be 0.1~6 mol / L, for example, 0.3 mol / L, 0.5 mol / L, 1 mol / L, 1.5 mol / L, 2 mol / L, 3 mol / L, 5 mol / L, preferably 0.3~4 mol / L.
[0030] Specifically, stabilizers can increase the bond energy between water and organic solvents, slow down the volatilization of organic solvents, thereby ensuring that the concentration of the electrolyte remains unchanged and preventing safety hazards caused by volatilized organic solvents; antioxidants can prevent the electrolyte from deteriorating and extend the service life of the electrolyte; surfactants can improve the solid-liquid interfacial tension, reduce the ion solvation sheath energy, and accelerate the electrochemical reaction rate. Acid-base buffers are used to adjust the final pH of the electrolyte after the electrolyte volume is fixed to meet the battery injection standards, thereby ensuring the battery formation results and subsequent performance.
[0031] Specifically, the stabilizer can be one or more of phosphate, sodium citrate, tartrate, glycine, polyvinyl alcohol, polyacrylic acid, magnesium succinate and sodium dehydrocholate.
[0032] Considering that too much stabilizer is easy to preempt the electrochemical reaction, resulting in aggravation of side reactions; too little stabilizer is easy to cause weak bond energy of solvated molecules, uneven distribution of electrolyte solvent or excessive volatilization of solvent, etc. Therefore, the mass of the stabilizer is controlled to account for 0.01% to 0.1% of the total mass of the electrolyte salt in the electrolyte, such as 0.02%, 0.03%, 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, 0.09%, preferably 0.01 to 0.05%.
[0033] Specifically, the antioxidant can be one or more of ascorbic acid, tea polyphenols, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone, tert-butylhydroquinone, citric acid, EDTA, ascorbyl palmitate, and the like.
[0034] Considering that too much antioxidant may cause a reduction reaction of part of the electrolyte salt, resulting in changes in the electrolyte components; too little antioxidant may not guarantee the antioxidant capacity of the electrolyte, which may cause the electrolyte to deteriorate and fail. Therefore, the content of the antioxidant is controlled to account for 0.05% to 1% of the total mass of the electrolyte salt in the electrolyte, such as 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, preferably 0.05% to 0.5%.
[0035] Specifically, the surfactant can be one or more of sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, stearic acid, lauric acid, lecithin, alkyl glucoside, sorbitan fatty acid, coconut acid monoethanolamide, coconut acid diethanolamide, fatty alcohol polyoxyethylene ether ammonium sulfate, potassium lauryl ether phosphate and disodium lauryl sulfosuccinate.
[0036] Considering that too much surfactant can easily lead to increased interfacial tension and make ion / electron exchange difficult, too little surfactant can not reduce the ion solvation sheath energy and reduce the coulombic efficiency of the battery. Therefore, the content of surfactant is controlled to account for 0.01% to 0.5% of the total mass of electrolyte salt in the electrolyte, such as 0.05%, 0.08%, 0.1%, 0.2%, 0.3%, 0.4%, preferably 0.02% to 0.3%.
[0037] Specifically, the acid-base buffer can be one or more of ammonia water, acetic acid, oxalic acid, phosphoric acid, boric acid, citric acid and barbituric acid.
[0038] Specifically, the amount of the acid-base buffer used is based on the adjusted pH value of the electrolyte, and the buffer is added dropwise to the electrolyte until the pH is 6.9-7.1.
[0039] The present invention also provides a method for preparing the aqueous battery electrolyte, comprising the following steps: Step 1, mixing water and an organic solvent to obtain a mixed solvent; Step 2, adding electrolyte salt into the mixed solvent and mixing to obtain solution A; Step 3, adding a stabilizer, an antioxidant and a surfactant to solution A in sequence to dissolve them completely, thereby obtaining solution B; Step 4: Add an acid-base buffer to solution B and adjust the pH of solution B to neutral to obtain an aqueous battery electrolyte.
[0040] Specifically, in step 1, stirring can be used to accelerate the mixing process during the mixing process. If the stirring speed is too high, it is easy to cause the solution to splash, the shear force is too large, and the electrolyte demulsification or stratification occurs; if the stirring speed is too low, the solute dissolution time will be too long, and the electrolyte components will be uneven in all directions. Therefore, in order to ensure that a suitable shear force can be provided and that the solvation bond energy between the polar organic solvent and water is not destroyed during the electrolyte preparation process, thereby causing stratification, the stirring speed in step 1 is controlled to be 50~280r / min, such as 80r / min, 100r / min, 150r / min, 180r / min, 200r / min, 250r / min, preferably 100~250r / min.
[0041] Specifically, in step 2, stirring can be used to accelerate the mixing process during the mixing process, and the stirring speed is 50~280r / min, for example, 80r / min, 100r / min, 150r / min, 180r / min, 200r / min, 250r / min, preferably 100~250r / min.
[0042] Specifically, in step 3, considering the stability of the solvated molecular structure after the electrolyte salt is dissolved, adding a stabilizer first can ensure that the bond energy of the solvated molecule is not broken, and then adding an antioxidant can slow down the volatilization and deterioration of the electrolyte, and finally adding a surfactant, whose molecules can provide efficient interface reaction ability for the ions in the electrolyte and improve the electrochemical performance of the battery. Therefore, the stabilizer, antioxidant and surfactant are added to solution A in sequence.
[0043] The present invention also provides an aqueous battery comprising the aqueous battery electrolyte.
[0044] Specifically, the aqueous battery can be one of an aqueous lithium ion battery, an aqueous sodium ion battery, an aqueous potassium ion battery, an aqueous zinc ion battery, an aqueous magnesium ion battery, an aqueous aluminum ion battery, an aqueous zinc-nickel secondary battery, a supercapacitor and an aqueous dual-ion battery.
[0045] Specifically, the preparation method of the aqueous battery includes the following steps: S1. Select the current collector according to the aqueous battery to be assembled, cut it into a suitable size, and clean the surface of the current collector with anhydrous ethanol; S2. Assemble the electrode, separator, current collector, etc. required for the aqueous battery into a battery cell and put them into a shell. After injecting a proper amount of the above-mentioned electrolyte, seal and let it stand to obtain an aqueous battery.
[0046] After formation and capacity separation, the electrochemical performance test of the aqueous battery can be carried out.
[0047] Specifically, the current collector in the above S1 can be one or more of Al foil, Zn foil, Sn foil, Ni foil, foam Ni, Ti foil, Ti mesh, stainless steel foil, stainless steel mesh, foam Fe, carbon cloth, carbon paper, AC paper and graphite paper, among which Al foil, Zn foil and Sn foil are amphoteric metal current collectors.
[0048] Specifically, in the above S1, the types of current collectors used in the positive and negative electrodes of the aqueous battery may be different, and only the current collector of one electrode may be an amphoteric metal, or the current collectors of both the positive and negative electrodes may be amphoteric metals.
[0049] Compared with the prior art, the electrolyte salt of the aqueous battery electrolyte of the present invention includes a strong acid root salt and a weak acid root salt. The main salt of the electrolyte is a strong acid root salt, which can be completely ionized after being completely dissolved, providing a rich ion concentration for the electrolyte, thereby increasing the ion conductivity and ion transfer rate of the electrolyte, further accelerating the electrochemical reaction rate, and to a certain extent reducing the adverse effects of concentration polarization; the secondary salt of the electrolyte is a weak acid root salt. After being completely dissolved, the weak acid root can be partially hydrolyzed. When the aqueous battery uses amphoteric metals as the current collector, the weak acid root hydrated ions formed by the solvation of the weak acid root enable the weak acid root to act as the current collector and react with H 2 O, isolating the direct contact between the metal hydrated ions in the electrolyte and the current collector, thereby avoiding the corrosion of the current collector and slowing down the gas evolution of the electrolyte without affecting the ion exchange, thereby extending the cycle life of the battery.
[0050] By adding a proper amount of stabilizer to the aqueous battery electrolyte of the present invention, the balance between solvents and between solvent and solute in the electrolyte can be ensured, and at the same time, the liquid tension can be reduced, so that the electrolyte can better infiltrate the inside of the electrode, so that ion shuttle and reaction are smoother, the DCR value of the battery is smaller, and it is more conducive to improving the cycle reversibility of the battery.
[0051] By adding an appropriate amount of antioxidant to the aqueous battery electrolyte of the present invention, the volatilization or deterioration of the polar organic solvent in the electrolyte can be effectively prevented, and the concentration of the electrolyte can be ensured not to deviate greatly during the use of the battery. By adding an appropriate amount of surfactant, the reduction of the solvation sheath bond energy of the ions can be promoted, the energy loss in the kinetics of the ion reaction can be reduced, and the reversibility of the electrode material and the coulombic efficiency of the battery can be improved. The initial pH of the electrolyte is adjusted to about neutral by an acid-base buffer, in order to prevent the occurrence of hydrogen evolution reaction (HER) or oxygen evolution reaction (OER) on the surface of the amphoteric metal current collector during electrochemical characterization, and during the cycle of the battery, due to the presence of the acid-base buffer and the weak acid salt, the pH of the electrolyte can be adjusted in time to prevent the corrosion of the amphoteric metal current collector, thereby avoiding the aggravation of side reactions or damage to the aqueous battery.
[0052] The present invention aims to be able to widely apply amphoteric metals in the current collectors of aqueous batteries, and to slow down or even avoid the corrosion of amphoteric metals in aqueous electrolytes, so that the electrochemical performance can be characterized normally, and at the same time, to a certain extent, the types of current collectors that can be used in aqueous batteries are expanded. The electrolyte of the present invention can make the current collector and the electrolyte more fully matched, and minimize the impact of changing electrolyte factors on the electrochemical performance of the battery, so that the electrochemical performance of the aqueous battery can be fully utilized, and promote the rapid development of aqueous batteries.
[0053] The aqueous battery using the electrolyte of the present invention can adapt to more types of amphoteric metals, thereby effectively alleviating or even avoiding the corrosion of the amphoteric metal current collector, and further extending the cycle life of the aqueous battery.
[0054] The technical solution of the present invention is further explained below in conjunction with specific examples. It should be noted that the data in the examples are all exemplary descriptions, and the dosage can be determined according to actual needs during the production process.
[0055] Embodiment 1: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0056] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, isopropanol and acetonitrile into the container at a volume ratio of 9:0.5:0.5, a total of 20 mL, and stir continuously at a rate of 240 r / min at room temperature to make it fully uniform to obtain a mixed solvent; 2. Weigh 6.88 g of sodium trifluoromethanesulfonate as a strong acid salt and 1.64 g of sodium acetate as a weak acid salt, respectively, and add them to the mixed solvent in sequence, and continue to stir at a rate of 240 r / min to completely dissolve them to obtain solution A; 3. Weigh 0.0026 g of sodium dihydrogen phosphate, 0.0213 g of EDTA, and 0.0128 g of sodium dodecyl sulfate, respectively, and add them to solution A in sequence to dissolve them completely to obtain solution B; 4. Add an appropriate amount of acetic acid to solution B and adjust the pH of solution B to 6.95 to obtain the electrolyte prepared in this embodiment.
[0057] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous sodium ion battery to be assembled, Al foil is used as the current collector for both the positive and negative electrodes, and is cut into appropriate sizes, and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, diaphragm, current collector, etc. required for the aqueous sodium ion battery into a battery cell and put them into a shell. After injecting an appropriate amount of the above-mentioned electrolyte, seal and let it stand to obtain an aqueous sodium ion battery.
[0058] After formation and capacity separation, the electrochemical performance test of aqueous sodium-ion batteries can be carried out.
[0059] Embodiment 2: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0060] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, triethylamine and dioxane into a container at a volume ratio of 14:1:1, a total of 16 mL, and stir continuously at a rate of 150 r / min at room temperature to make them fully uniform to obtain a mixed solvent; 2. Weigh 15.3 g of lithium perchlorate as a strong acid salt, 1.664 g of lithium dihydrogen phosphate, and 2.112 g of lithium acetate as a weak acid salt, respectively, and add them to the mixed solvent in sequence, continue stirring at a rate of 150 r / min to completely dissolve them, and obtain solution A; 3. Weigh 0.0038 g of magnesium succinate, 0.0286 g of ascorbic acid and 0.0153 g of coconut oil diethanolamide respectively, and add them to solution A in sequence to dissolve them completely, thereby obtaining solution B; 4. Add an appropriate amount of aqueous ammonia to solution B and adjust the pH of solution B to 7.05 to obtain the electrolyte prepared in this embodiment.
[0061] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous lithium-ion battery to be assembled, Al foil is used as the positive electrode and Cu foil is used as the negative electrode as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, separator, current collector, etc. required for the aqueous lithium-ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand to obtain an aqueous lithium-ion battery.
[0062] After formation and capacity separation, the electrochemical performance test of aqueous lithium-ion batteries can be carried out.
[0063] Embodiment three: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0064] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, DMSO and acetone into the container at a volume ratio of 24:1.5:0.5, a total of 26 mL, and stir continuously at a rate of 180 r / min at room temperature to make it fully uniform to obtain a mixed solvent; 2. Weigh 6.29 g of zinc sulfate and 27.2 g of zinc perchlorate as strong acid salts, 1.09 g of sodium bicarbonate and 4.04 g of zinc dihydrogen phosphate as weak acid salts, respectively, and add them to the mixed solvent in sequence, continue stirring at a rate of 180 r / min to completely dissolve them, and obtain solution A; 3. Weigh 0.0155 g of sodium tartrate, 0.1352 g of butylated hydroxytoluene and 0.0966 g of alkyl glucoside respectively, and add them to solution A in sequence to dissolve them completely, thereby obtaining solution B; 4. Add an appropriate amount of aqueous ammonia to solution B and adjust the pH of solution B to 7 to obtain the electrolyte prepared in this embodiment.
[0065] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous zinc ion battery to be assembled, the positive electrode uses Ti mesh and the negative electrode uses Zn foil as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the pole pieces, diaphragms, current collectors, etc. required for the aqueous zinc ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand to obtain an aqueous zinc ion battery.
[0066] After formation and capacity separation, the electrochemical performance test of aqueous zinc-ion batteries can be carried out.
[0067] Embodiment 4: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0068] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, pyridine and tetramethylethylenediamine into a container at a volume ratio of 30:6:4, a total of 40 mL, and stir continuously at a rate of 170 r / min at room temperature to make them fully uniform to obtain a mixed solvent; 2. Weigh 6.8 g of sodium nitrate and 9.52 g of sodium sulfamate as strong acid salts, 8.52 g of disodium hydrogen phosphate and 2.68 g of sodium oxalate as weak acid salts, respectively, and add them to the mixed solvent in sequence, continue stirring at a rate of 170 r / min to completely dissolve them, and obtain solution A; 3. Weigh 0.0028 g of sodium citrate, 0.0137 g of tea polyphenols and 0.0083 g of sodium dodecylbenzene sulfonate respectively, and add them to solution A in sequence to dissolve them completely, thereby obtaining solution B; 4. Add an appropriate amount of phosphoric acid to solution B and adjust the pH of solution B to 7.0 to obtain the electrolyte prepared in this embodiment.
[0069] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous sodium ion battery to be assembled, Al foil is used as the current collector for both the positive and negative electrodes, and is cut into appropriate sizes, and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, diaphragm, current collector, etc. required for the aqueous sodium ion battery into a battery cell and put them into a shell. After injecting an appropriate amount of the above-mentioned electrolyte, seal and let it stand to obtain an aqueous sodium ion battery.
[0070] After formation and capacity separation, the electrochemical performance test of aqueous sodium-ion batteries can be carried out.
[0071] Embodiment five: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0072] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, formamide, and hexamethylphosphoramide into a container at a volume ratio of 18:2:1, a total of 21 mL, and stir continuously at a rate of 130 r / min at room temperature to make them fully uniform to obtain a mixed solvent; 2. Weigh 3.32 g of sodium permanganate as a strong acid salt, 6.89 g of sodium acetate, and 2.23 g of sodium carbonate as a weak acid salt, and add them to the mixed solvent in sequence, and continue to stir at a rate of 130 r / min to completely dissolve them to obtain solution A; 3. Weigh 0.0075 g of sodium dehydrocholate, 0.0249 g of tert-butylhydroquinone and 0.0062 g of disodium lauryl sulfosuccinate respectively, and add them to solution A in sequence to dissolve them completely, thereby obtaining solution B; 4. Add an appropriate amount of barbituric acid to solution B and adjust the pH of solution B to 6.95 to obtain the electrolyte prepared in this example.
[0073] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous sodium ion battery to be assembled, Al foil is used as the current collector for both the positive and negative electrodes, and is cut into appropriate sizes, and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, diaphragm, current collector, etc. required for the aqueous sodium ion battery into a battery cell and put them into a shell. After injecting an appropriate amount of the above-mentioned electrolyte, seal and let it stand to obtain an aqueous sodium ion battery.
[0074] After formation and capacity separation, the electrochemical performance test of aqueous sodium-ion batteries can be carried out.
[0075] Embodiment six: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0076] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, ethanol and ethyl acetate into the container at a volume ratio of 30:0.5:1.5, a total of 32 mL, and stir continuously at a rate of 210 r / min at room temperature to make it fully uniform to obtain a mixed solvent; 2. Weigh 40.7 g of lithium perchlorate, 6.6 g of lithium sulfamate as strong acid salts, 6.33 g of lithium acetate, and 3.68 g of lithium phosphate as weak acid salts, respectively, and add them to the mixed solvent in sequence, continue stirring at a rate of 210 r / min to completely dissolve them, and obtain solution A; 3. Weigh 0.043 g of polyvinyl alcohol, 0.172 g of ascorbyl palmitate and 0.1146 g of coconut oil monoethanolamide respectively, and add them to solution A in sequence to dissolve them completely to obtain solution B; 4. Add an appropriate amount of ammonia water to solution B and adjust the pH of solution B to 7.05 to obtain the electrolyte prepared in this embodiment.
[0077] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous lithium-ion battery to be assembled, Al foil is used as the positive electrode and Cu foil is used as the negative electrode as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, separator, current collector, etc. required for the aqueous lithium-ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand to obtain an aqueous lithium-ion battery.
[0078] After formation and capacity separation, the electrochemical performance test of aqueous lithium-ion batteries can be carried out.
[0079] Embodiment seven: This embodiment provides an electrolyte for an aqueous battery, a preparation method thereof, and an aqueous battery.
[0080] The method for preparing the aqueous battery electrolyte of this embodiment comprises the following steps: 1. Add deionized water, propylene glycol and dioxane into a container at a volume ratio of 18:0.5:0.5, a total of 19 mL, and stir continuously at a rate of 110 r / min at room temperature to make them fully uniform to obtain a mixed solvent; 2. Weigh 1.16 g of lithium chlorate as a strong acid salt, 0.36 g of lithium sulfite, and 0.78 g of lithium dihydrogen phosphate as a weak acid salt, respectively, and add them to the mixed solvent in sequence, continue stirring at a rate of 110 r / min to completely dissolve them, and obtain solution A; 3. Weigh 0.0021 g of polyacrylic acid, 0.0104 g of citric acid and 0.0092 g of lecithin respectively, and add them to solution A in sequence to dissolve them completely, thereby obtaining solution B; 4. Add an appropriate amount of aqueous ammonia to solution B and adjust the pH of solution B to 6.95 to obtain the electrolyte prepared in this embodiment.
[0081] The aqueous battery of this embodiment includes the above aqueous battery electrolyte, and the preparation method of the aqueous battery includes the following steps: 5. According to the aqueous lithium-ion battery to be assembled, Al foil is used as the positive electrode and Cu foil is used as the negative electrode as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the electrode, separator, current collector, etc. required for the aqueous lithium-ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand to obtain an aqueous lithium-ion battery.
[0082] After formation and capacity separation, the electrochemical performance test of aqueous lithium-ion batteries can be carried out.
[0083] Comparative Example 1: This comparative example provides an electrolyte, a preparation method thereof, and an aqueous battery.
[0084] The electrolyte salt of this comparative example does not contain a weak acid salt, and the preparation method of the electrolyte comprises the following steps: 1. Add deionized water, isopropanol and acetonitrile into the container at a volume ratio of 9:0.5:0.5, a total of 20 mL, and stir continuously at a rate of 240 r / min at room temperature to make it fully uniform to obtain a mixed solvent; 2. Weigh 6.88 g of sodium trifluoromethanesulfonate as a strong acid salt and add it to the mixed solvent, and continue to stir at a rate of 240 r / min to completely dissolve it to obtain solution A; 3. Weigh 0.0026 g of sodium dihydrogen phosphate, 0.0213 g of EDTA and 0.0128 g of sodium dodecyl sulfate respectively, and add them to solution A in sequence to dissolve them completely to obtain solution B; 4. Add an appropriate amount of ammonia water to solution B and adjust the pH of solution B to 6.95 to obtain the electrolyte; 5. According to the aqueous sodium ion battery to be assembled, Al foil is used as the current collector for both the positive and negative electrodes, and is cut into appropriate sizes, and the surface of the current collector is cleaned with anhydrous ethanol; 6. Assemble the pole pieces, diaphragms, current collectors, etc. required for the aqueous sodium ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand; 7. After formation and capacity separation, the electrochemical performance test of aqueous sodium ion battery can be carried out.
[0085] Comparative Example 2: This comparative example provides an electrolyte, a preparation method thereof, and an aqueous battery.
[0086] The electrolyte of this comparative example does not contain any additives, and the remaining steps of the preparation method of the electrolyte are the same as those of Example 2, which will not be repeated here.
[0087] According to the aqueous lithium-ion battery to be assembled, Al foil is used as the positive electrode and Cu foil is used as the negative electrode as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; the pole pieces, diaphragms, current collectors, etc. required for the aqueous lithium-ion battery are assembled into a battery cell and incorporated into a shell, and an appropriate amount of the above-mentioned electrolyte is injected and then sealed and allowed to stand; after formation and volume separation, the electrochemical performance test of the aqueous lithium-ion battery can be carried out.
[0088] Comparative Example 3: This comparative example provides an electrolyte, a preparation method thereof, and an aqueous battery.
[0089] The electrolyte of this comparative example does not contain weak acid salts and additives, and the preparation method of the electrolyte comprises the following steps: 1. Add deionized water, DMSO and acetone into the container at a volume ratio of 24:1.5:0.5, a total of 26 mL, and stir continuously at a rate of 180 r / min at room temperature to make it fully uniform to obtain a mixed solvent; 2. Weigh 6.29 g of zinc sulfate and 27.2 g of zinc perchlorate as strong acid salts, add them into the mixed solvent, and continue to stir at a rate of 180 r / min to completely dissolve them to obtain solution A; 3. Add an appropriate amount of ammonia water to solution A and adjust the pH of solution A to 7 to obtain the electrolyte prepared by the present invention; 4. According to the aqueous zinc ion battery to be assembled, the positive electrode uses Ti mesh and the negative electrode uses Zn foil as the current collector, which are cut into appropriate sizes and the surface of the current collector is cleaned with anhydrous ethanol; 5. Assemble the pole pieces, diaphragms, current collectors, etc. required for the aqueous zinc ion battery into a battery cell and put them into a shell, inject an appropriate amount of the above-mentioned electrolyte, and then seal and let it stand; 6. After formation and capacity separation, the electrochemical performance test of aqueous zinc ion battery can be carried out.
[0090] The performance tests of the embodiments and comparative examples are shown in Table 1 below. It can be seen that the voltage window of the electrolyte of the present invention is widened. For example, the voltage window of the electrolyte is above 2.5V, such as 2.55~2.8V; the corrosion potential of the current collector is improved, indicating that the current collector is more corrosion-resistant in the electrolyte of the present invention; the electrolyte provided by the present invention can effectively alleviate the volatilization of the solvent in the electrolyte during the cycle, and ensure that the physical and chemical properties of the electrolyte remain unchanged to the greatest extent. For example, the solute concentration of the electrolyte after the cycle is 102%~111%, providing a good place for electrochemical reactions. The DCR of the aqueous battery of the present invention is low, for example, the DCR is 15~27 mΩ; the discharge specific capacity of the aqueous battery of the present invention is improved, for example, the discharge specific capacity reaches 70 mAh / g or more, for example, 70~340 mAh / g; the cycle life is extended, for example, the cycle life reaches more than 240 cycles.
[0091] Table 1 Performance test results of embodiments and comparative examples
[0092] Figure 1 The conductivity diagram of the electrolyte of Example 1 and Comparative Example 1, Figure 2 The conductivity diagram of the electrolyte of Example 2 and Comparative Example 2; it can be seen that compared with the comparative example, the conductivity of the electrolyte of the present invention is not much different, indicating that the addition of polar organic solvents can effectively improve the voltage window of the electrolyte without affecting the conductivity.
[0093] Figure 3 This is a comparison of the current collectors of the aqueous sodium battery after cycling of Example 1 and Comparative Example 1. Figure 4 This is a comparison diagram of the current collectors of the aqueous lithium batteries of Example 2 and Comparative Example 2 after cycling; it can be seen that the electrolyte provided by the present invention can effectively alleviate the corrosion of the current collector during the cycling process, greatly extending the cycle life of the aqueous battery.
[0094] Figure 5 is the percentage of electrolyte concentration of the aqueous sodium battery after cycling of Example 1 and Comparative Example 1 (before cycling is 100%); Figure 6The electrolyte concentration percentages of the aqueous lithium batteries of Example 2 and Comparative Example 2 after cycling (the concentration before cycling is 100%) are shown. It can be seen that the electrolyte provided by the present invention can effectively alleviate the volatilization of the solvent in the electrolyte during the cycling process, ensure that the physical and chemical properties of the electrolyte remain unchanged to the greatest extent, and provide a good place for electrochemical reactions.
[0095] Figure 7 : DCR diagram of aqueous sodium battery of Example 1 and Comparative Example 1, Figure 8 The DCR diagram of the aqueous lithium battery of Example 2 and Comparative Example 2; it can be seen that the electrolyte provided by the present invention effectively alleviates the corrosion of the current collector during the cycle, so the DCR of the battery is reduced compared with the comparative example, which greatly reduces the ohmic polarization of the battery.
[0096] Fig. 9 The cycle performance diagram of the aqueous sodium battery of Example 1 and Comparative Example 1; Fig.10 It is a cycle performance diagram of the aqueous lithium battery of Example 2 and Comparative Example 2; it can be seen that the electrolyte provided by the present invention can alleviate the problem of collector corrosion and improve the volatility of the electrolyte, thereby effectively extending the cycle life of the aqueous battery.
[0097] It should be noted that when the aqueous battery electrolyte of the present invention uses polar organic solvents, electrolyte salts, additives and acid-base buffers not mentioned in the above embodiments, it can also be applied to a variety of current collectors, which will not be described one by one here.
[0098] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. An aqueous battery electrolyte, characterized in that: The components of the aqueous battery electrolyte include: a solvent, an electrolyte salt, an additive and an acid-base buffer; wherein the electrolyte salt includes a strong acid radical salt and a weak acid radical salt, and the additive includes a stabilizer, an antioxidant and a surfactant.
2. The aqueous battery electrolyte according to claim 1, characterized in that: The solvent includes water and an organic solvent.
3. The aqueous battery electrolyte according to claim 1, characterized in that: The strong acid salt is one or more of sulfate, nitrate, sulfamate, trifluoromethylsulfonate, fluoride, chlorate, perchlorate and permanganate.
4. The aqueous battery electrolyte according to claim 1, characterized in that: The weak acid salt is one or more of carbonate, bicarbonate, acetate, sulfite, bisulfite, phosphate, hydrogen phosphate, dihydrogen phosphate, oxalate and silicate.
5. The aqueous battery electrolyte according to claim 1, characterized in that: The stabilizer is one or more of phosphate, sodium citrate, tartrate, glycine, polyvinyl alcohol, polyacrylic acid, magnesium succinate and sodium dehydrocholate.
6. The aqueous battery electrolyte according to claim 1, characterized in that: The antioxidant is one or more of ascorbic acid, tea polyphenols, butylated hydroxyanisole, butylated hydroxytoluene, tert-butylhydroquinone, tert-butylhydroquinone, citric acid, EDTA, and ascorbyl palmitate.
7. The aqueous battery electrolyte according to claim 1, characterized in that The concentration of the strong acid salt is 0.5-18 mol / L.
8. The aqueous battery electrolyte according to claim 7, characterized in that The concentration of the weak acid salt is 0.1-6 mol / L.
9. A method for preparing an aqueous battery electrolyte according to any one of claims 1 to 8, characterized in that: include: Step 1, mixing water and an organic solvent to obtain a mixed solvent; Step 2, adding electrolyte salt into the mixed solvent and mixing to obtain solution A; Step 3, adding a stabilizer, an antioxidant and a surfactant to solution A in sequence and mixing them to obtain solution B; Step 4: Add an acid-base buffer to solution B and adjust the pH of solution B to neutral to obtain an electrolyte for an aqueous battery.
10. An aqueous battery, characterized in that: The aqueous battery comprises the aqueous battery electrolyte according to any one of claims 1 to 8 or the aqueous battery electrolyte prepared by the preparation method according to claim 9.
Citation Information
Patent Citations
Aqueous electrolyte for improving reversibility of neutral zinc-manganese battery and preparation method of aqueous electrolyte
CN112086694A
Aqueous mixed ion battery electrolyte and application thereof
CN113823846A
Aqueous electrolyte of zinc metal battery
CN115566281A
Aqueous battery
CN115692718A
Aqueous battery electrolyte and preparation method thereof
CN118099558A