Wide-temperature-range aqueous electrolyte and preparation method and application thereof
By introducing DMF and CPDs into the electrolyte of aqueous zinc ion battery, the problem of degradation of battery performance and dendrite growth in water-based zinc ion battery is solved, stable operation and high cycling stability are achieved, and the electrochemical window is broadened.
Patent Information
- Application Number
- CN202411269413.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
AI Technical Summary
The battery performance of water-based zinc ion batteries declines under extreme temperature environments. The dendrite growth and corrosion problems of zinc metal negative electrodes limit their wide temperature range, and the electrochemical stability window of water is narrow, limiting the operating voltage range of the battery.
The co-solvent N,N-dimethylformamide (DMF) and functional additive carbonated polymer points (CPDs) are introduced into the aqueous electrolyte. The freezing point and active water content are reduced through the hydrogen bonding of DMF to water. CPDs are compatible with each other. Zincity and cosolvents jointly inhibit dendrites' growth and regulate the deposition morphology of zinc.
The stable operation and high cycle stability of aqueous zinc ion batteries in a wide temperature range are achieved, which significantly improves the conductivity and electrochemical performance of the electrolyte, extends the cycle life of the battery, and broadens the electrochemical window.
Smart Images

Figure CN118943525A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery electrolytes, and in particular to a wide temperature range aqueous electrolyte and a preparation method and application thereof. Background Art
[0002] As a new generation of energy storage devices with great development prospects, aqueous zinc-ion batteries have attracted widespread attention due to the wide range of electrode materials, safety, environmental friendliness and high energy density. However, the side reactions and dendrite growth occurring at the interface between the zinc metal anode and the electrolyte severely reduce the coulombic efficiency and cycle life of the battery, limiting the application scale and scenarios of aqueous zinc-ion batteries. With the intensification of global extreme temperature environments and the continuous increase in energy storage demand, the demand for energy storage equipment in special environmental scientific research activities such as polar expeditions, aerospace, and daily use in cold and tropical regions is also increasing year by year. Therefore, solving the problems of dendrite growth and corrosion of zinc metal anodes is of great significance to the wide temperature range application of aqueous zinc-ion batteries.
[0003] Aqueous zinc-ion batteries that use water as a solvent are safer than batteries that use flammable, volatile organic solvents as electrolyte solvents. However, aqueous zinc-ion battery electrolytes also face some challenges. The electrochemical stability window of water is narrow, which limits the operating voltage range of the battery. In low-temperature environments, water will crystallize or even solidify, reducing conductivity, resulting in reduced battery performance.
[0004] In order to solve the above problems, people try to start with the electrolyte additive strategy. The co-solvent strategy of mixing water and low-melting-point organic solvents is an effective way to achieve stable and safe operation of aqueous zinc-ion batteries under a wide temperature range. Organic solvent molecules interact with water molecules to form intermolecular hydrogen bonds, destroying the hydrogen bond network between water molecules, thereby lowering the freezing point of the electrolyte and increasing the conductivity of the electrolyte. The freezing point of the mixed electrolyte can be lower than the freezing points of the two solvents themselves, making it possible for aqueous zinc-ion batteries to be used in a wide temperature range.
[0005] DMF is a common organic solvent with a low freezing point and good water solubility. It is widely used as an antifreeze for animal cell cryopreservation and has a good application prospect as an aqueous electrolyte additive. 2+The formation of a complex effectively inhibits the occurrence of hydrogen evolution reaction on the Zn negative electrode. The hydrogen bonding between DMF and water molecules reduces the desolvation activation energy, accelerates the removal of H2O molecules from hydrated zinc ions, and significantly reduces the interface voltage polarization. The introduction of DMF greatly increases the energy barrier for water decomposition and effectively inhibits the hydrogen evolution reaction. The introduction of DMF significantly reduces the freezing point of the aqueous electrolyte and improves the electrolyte conductivity at low temperatures. The introduction of high-donor-number organic small molecules as co-solvents for aqueous electrolytes regulates the solvation sheath to inhibit side reactions and prolongs the cycle life of the battery in a wide temperature range, but the co-solvent does not have a significant inhibitory effect on zinc dendrites. In response to this problem, a method of adding a trace amount of additives on the basis of a co-solvent is provided to induce uniform zinc deposition and further broaden the electrochemical window and temperature window of aqueous zinc-ion batteries. This aqueous co-solvent electrolyte can be applied to aqueous zinc-ion batteries in a wide temperature range, and the electrochemical performance of the battery is significantly improved at low temperatures. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a wide temperature range aqueous electrolyte and its preparation method and application. A co-solvent N,N-dimethylformamide (DMF) and a functional additive carbonized polymer dots (CPDs) are introduced into the traditional aqueous electrolyte. The raw materials required for the preparation method are easy to obtain, the operation is simple, and the preparation conditions are mild. DMF, which is miscible with water, is used as a co-solvent. While significantly reducing the freezing point of the electrolyte, it also shows the effect of adjusting the Zn 2+ Due to the solvation structure and the effect of reducing the active water content, the zinc affinity exhibited by the introduced functionalized additive CPDs synergistically inhibits dendrite growth with the co-solvent.
[0007] In order to achieve the above object, the present invention adopts the following technical solution:
[0008] The present invention first provides a method for preparing a wide temperature range aqueous electrolyte, the preparation method comprising the following steps:
[0009] Step 1: Preparation of carbonized polymer dots (CPDs);
[0010] Step 2: Evenly mix DMF and ZnSO4 electrolyte to prepare a mixed electrolyte;
[0011] Step 3: Add the carbonized polymer dots CPDs from step 1 to the mixed electrolyte from step 2 to obtain a wide temperature range aqueous electrolyte.
[0012] Preferably, the method for preparing carbonized polymer dots CPDs in step 1 comprises:
[0013] Dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction. After filtering, dialysis and freeze-drying, carbonized polymer dots CPDs are obtained.
[0014] Preferably, the molar ratio of citric acid to ethylenediamine is 1:1.
[0015] Preferably, the reaction temperature is 180° C. and the reaction time is 5 h.
[0016] Preferably, the volume fraction of DMF in step 2 is 10-50%.
[0017] Preferably, the concentration of the ZnSO4 electrolyte in step 2 is 2 mol / L.
[0018] Preferably, in step 3, the amount of carbonized polymer dots CPDs added is 0.1-0.4 mg / mL.
[0019] Preferably, the volume fraction of DMF in step 2 is 30%, and the amount of carbonized polymer dots CPDs added is 0.2 mg / mL.
[0020] The present invention also provides a wide temperature range aqueous electrolyte obtained by the above preparation method.
[0021] The present invention also provides application of the above-mentioned wide temperature range aqueous electrolyte in aqueous zinc ion batteries.
[0022] Beneficial Effects of the Invention
[0023] The wide temperature range aqueous electrolyte provided by the present invention mainly utilizes the large solubility of DMF in water. At the same time, CPDs has a hard carbonized crystal core, and the carbon-based core is wrapped with a polymer chain rich in functional groups. The rich functional groups such as aldehyde and carbonyl in the chain structure and the nitrogen and oxygen elements in DMF ensure the stability and uniformity of the electrolyte system through hydrogen bonds and other forces. The wide temperature range aqueous electrolyte provided by the present invention is stable, with a freezing point below -61°C and a boiling point above 153°C.
[0024] The wide temperature range aqueous electrolyte provided by the present invention is applied to zinc ion batteries. DMF has a strong electron donating ability and can replace Zn 2+The water molecules in the solvated structure reduce the content of active water, thereby inhibiting the decomposition of water molecules and side reactions. Although the introduction of DMF has successfully broadened the application temperature window of aqueous zinc-ion batteries, due to the high reduction stability of DMF, it is unable to form a solid electrolyte interface (SEI) film, which inhibits side reactions to a certain extent, but the induction effect on the uniform growth of zinc dendrites is not obvious. Therefore, on this basis, the present invention uses functional additives to regulate the deposition morphology of zinc. CPDs are nanoscale carbon materials composed of a rigid core structure wrapped in a flexible chain structure. It has the characteristics of a wide source of synthetic materials, a simple process, and easy adjustment of structural composition. It has been widely introduced into the field of electrochemical energy storage and has shown excellent electrochemical performance. There are abundant functional groups on the short-chain polymers with yarn ball orientation in CPDs, which promote the uniform distribution of the electric field by alleviating the "tip effect", limit the formation of dendrites, and accelerate the uniform deposition of zinc, thereby improving the cycle stability and specific capacity of zinc-based batteries. The rich hydrophilic oxygen-containing groups attached to CPDs can jointly regulate Zn with DMF. 2+ Solvation structure, its oxygen-containing groups and Zn 2+ It has a strong adsorption effect, which can reduce the nucleation barrier and induce Zn to deposit evenly and smoothly, thereby achieving a long cycle life of aqueous zinc-ion batteries and providing key support for expanding the application scenarios of aqueous zinc-ion batteries.
[0025] The wide temperature range aqueous electrolyte provided by the present invention is applied to the stable operation of aqueous zinc ion batteries under a wide temperature range, has high ionic conductivity, and still has good long cycle stability at low temperatures, and has broad application prospects in energy storage devices under extreme environments. Experimental results show that in the application of the wide temperature range aqueous electrolyte provided by the present invention, at room temperature, at a current density of 2 mA cm -2 、Area specific capacity 1mAh cm -2 The constant current charge-discharge cycle performance test was carried out under the condition of 3DMF-0.2CPDs, which can ensure that the symmetrical battery can operate stably for more than 200 hours at a stable polarization voltage of about 0.13V. -2 、Area capacity 1mAh cm -2 Under the conditions, the average Coulombic efficiency of 3DMF-0.2CPDs can reach 99.29% after 300 cycles.
[0026] The wide-temperature-range aqueous electrolyte provided by the present invention has a streamlined preparation process, good quality stability and low preparation cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The constant current charge-discharge cycle performance, rate performance and coulombic efficiency diagram of the mixed electrolyte prepared in Example 1.
[0028] Figure 2This is a constant current charge-discharge cycle performance diagram of the mixed electrolyte prepared in Example 1.
[0029] Figure 3 Digital photos of ZnSO4-DMF-CPDs mixed electrolytes of different concentrations prepared in Example 2;
[0030] Figure 4 The constant current charge-discharge cycle performance diagram of the 3DMF mixed electrolyte with different CPDs concentrations prepared in Example 2 and the coulombic efficiency diagram in the Zn / / Cu battery.
[0031] Figure 5 For Zn / / Zn symmetric cells, 0DMF (a), 3DMF (b), and 3DMF-0.2CPDs (c) prepared in Example 1 were used at a current density of 0.5 mA cm -2 、Area capacity 3mAh cm -2 Morphology of zinc deposition under . DETAILED DESCRIPTION
[0032] The present invention first provides a method for preparing a wide temperature range aqueous electrolyte, the preparation method comprising the following steps:
[0033] Step 1: Prepare carbonized polymer dots CPDs; the specific preparation is preferably as follows: dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction, preferably at 180°C for 5 hours. After the reaction is completed, the reactor is naturally cooled to room temperature and the solution is filtered. The filtered solution is dialyzed with a dialysis bag, and the dialysis time is preferably 24 hours. The dialyzed solution is divided into small beakers and freeze-dried to obtain carbonized polymer dots CPDs powder; the molar ratio of citric acid and ethylenediamine is preferably 1:1.
[0034] Step 2: Evenly mix DMF and ZnSO4 electrolyte to obtain a mixed electrolyte; the concentration of ZnSO4 electrolyte is preferably 2 mol / L, and the volume fraction of DMF is preferably 10-50%, more preferably 30%;
[0035] Step 3: Add the carbonized polymer dots CPDs from step 1 to the mixed electrolyte from step 2 to obtain a wide temperature range aqueous electrolyte. The amount of carbonized polymer dots CPDs added is preferably 0.1-0.4 mg / mL, more preferably 0.2 mg / mL.
[0036] The present invention also provides a wide temperature range aqueous electrolyte obtained by the above preparation method.
[0037] The wide temperature range aqueous electrolyte provided by the present invention is stable, has a freezing point lower than -61°C, and a boiling point higher than 153°C.
[0038] The wide temperature range aqueous electrolyte provided by the present invention is preferably an electrolyte when the volume fraction of the co-solvent DMF is 30% and the amount of CPDs added is 0.2 mg / mL, recorded as 3DMF-0.2CPDs, and its stability and synergistic effect are more significant.
[0039] The present invention also provides application of the above-mentioned wide temperature range aqueous electrolyte in aqueous zinc ion batteries.
[0040] In the application of the wide temperature range aqueous electrolyte provided by the present invention, preferably, the wide temperature range aqueous electrolyte is used as an aqueous zinc ion battery electrolyte. The ionic conductivity of 3DMF-0.2CPDs is calculated to be 9.15mS / cm, which is greater than the ionic conductivity of 3DMF and significantly improved compared with the ionic conductivity of 0DMF. This shows that the co-solvent DMF can improve the ionic conductivity, but the improvement effect is not significant. The introduction of CPDs and DMF synergistically regulates the Zn 2+ The solvated structure increases the active sites while enhancing the charge transfer capacity of the electrolyte, further improving the ionic conductivity of the co-solvent electrolyte.
[0041] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0042] Example 1
[0043] Synthesis of CPDs: Weigh 1.921g of citric acid and absorb 670μL of ethylenediamine and dissolve them in 60mL of distilled water. After stirring at room temperature to fully dissolve them, transfer the above uniform solution to a 100mL polytetrafluoroethylene reactor and perform a constant temperature hydrothermal reaction at 180°C for 5h. After the reaction is completed and the hydrothermal reactor is naturally cooled to room temperature, the resulting liquid is filtered using a 5mL syringe with a modified filter head. After the filtration is completed, dialyze in a dialysis cylinder for 24h using a dialysis bag with a molecular weight cutoff of 200D. The dialyzed solution is divided into 50mL small beakers, frozen in the refrigerator, and dried in a vacuum freeze dryer for 48h to obtain CPDs powder;
[0044] Preparation of ZnSO4-DMF aqueous co-solvent electrolyte: First, prepare a certain amount of 2mol / L ZnSO4 electrolyte with pure water as a standby. Secondly, mix DMF with water according to a certain volume fraction as a solvent and mix it with ZnSO4 electrolyte to prepare an electrolyte of the same concentration. The prepared mixed electrolyte is recorded as 1DMF, 2DMF, 3DMF, 4DMF, and 5DMF according to the DMF volume fraction of 10%, 20%, 30%, 40%, and 50%. The 2mol / L ZnSO4 electrolyte without DMF is recorded as 0DMF.
[0045] Figure 1 The mixed electrolyte prepared in Example 1 (a, b) constant current charge-discharge cycle performance and rate performance of DMF mixed electrolyte with different volume fractions; (c) coulombic efficiency of DMF mixed electrolyte with different volume fractions in Zn / / Cu battery. Figure 1 As shown in (a), at a current density of 1 mA cm -2 Area capacity 1mAh cm -2 Under the condition of 2DMF and 3DMF, both can ensure stable battery cycle for more than 250h, and the battery voltage fluctuation of 3DMF is only about 0.05V lower than that of 0DMF. Figure 1 As shown in (b), the addition of DMF can effectively improve the rate performance of the battery. When the current density increases to 2 mA cm -2 When the current density is further increased to 3 mA cm -2 When the co-solvent is used, the overpotential of the battery can be reduced from 0.6V to 0.02V at most while ensuring the stable operation of the battery, and the voltage does not fluctuate significantly. This shows that DMF with a volume fraction of 30% can be well dissolved in 2M ZnSO4 electrolyte and participates in the Zn 2+ The solvation structure reconstruction effectively reduces the severity of side reactions. Figure 1 (c) shows that at a current density of 3 mA cm -2 Area capacity 1mAh cm -2 Under the condition of , the coulombic efficiency of 3DMF can still be maintained at more than 96% after 400 cycles, while the coulombic efficiency of 0DMF without DMF began to fluctuate greatly after 200 cycles and could not continue to operate stably, which confirmed that the introduction of co-solvent DMF helps to form a strong solid electrolyte interface (SEI) and ensure the reversibility of Zn deposition / stripping. Combined with the above cycle performance test and the test of Zn deposition / stripping coulombic efficiency, 3DMF has the best improvement on the comprehensive electrochemical performance of the battery. The introduction and optimization of functional additives based on Example 1 can be based on this concentration of 3DMF.
[0046] Figure 2 The mixed electrolyte prepared in Example 1 has a current density of 0.5 mA cm -2 The area capacity is 0.5 mAh cm -2 The constant current charge-discharge cycle performance of 0DMF and 3DMF mixed electrolyte at -5°C, -15°C, and -25°C under the conditions (a, b, c). The mixed electrolyte of this embodiment is as follows Figure 2 As shown, at a current density of 0.5 mA cm -2Area capacity 0.5mAhcm -2 Under the conditions of , 0DMF and 3DMF were tested at -5℃, -15℃, and -25℃ respectively. Figure 2 As shown in (a), 3DMF can cycle for nearly 800 h at a stable voltage of about 0.1 V at -5°C, which is in sharp contrast to the cycling of 0DMF. Figure 2 As shown in (b), the 3DMF cycle voltage at -15°C is nearly 10 times lower than the 0DMF cycle voltage. Figure 2 As shown in (c), 3DMF can support the battery to stably cycle for 500 h at -25 °C. This confirms that DMF, as a co-solvent, can participate in the reorganization of the hydrogen bond network, reduce the freezing point of the mixed aqueous electrolyte, and ensure that the battery can still operate stably at -25 °C.
[0047] Example 2
[0048] The synthesis of CPDs was the same as in Example 1;
[0049] The DMF and 2 mol / L ZnSO4 electrolyte were mixed evenly to prepare a mixed electrolyte; the volume fraction of DMF was 30%;
[0050] Preparation of ZnSO4-DMF-CPDs wide temperature range aqueous electrolyte: CPDs were mixed evenly with ZnSO4-DMF aqueous co-solvent electrolyte at mass concentrations of 0.1 mg / mL, 0.2 mg / mL, 0.3 mg / mL, and 0.4 mg / mL to prepare ZnSO4-DMF-CPDs aqueous co-solvent electrolyte. The carbon dots added in 3DMF were 0.1 mg / mL, 0.2 mg / mL, 0.3 mg / mL, and 0.4 mg / mL, respectively named 3DMF-0.1CPDs, 3DMF-0.2CPDs, 3DMF-0.3CPDs, and 3DMF-0.4CPDs.
[0051] Figure 3 The digital photos of the ZnSO4-DMF-CPDs mixed electrolytes with different concentrations prepared in Example 2; Figure 3 As shown, 0.4 mg / mL of carbon dots can also be well dissolved in 3DMF. As the concentration of carbon dots in 3DMF increases from 0.1 mg / mL to 0.4 mg / mL, the color of the co-solvent electrolyte gradually deepens. The ZnSO4-DMF-CPDs wide temperature range aqueous electrolytes of various concentrations configured in this embodiment have good stability and are qualified as aqueous zinc ion battery electrolytes.
[0052] Figure 4(a) Constant current charge-discharge cycle performance of 3DMF mixed electrolyte with different CPDs concentrations prepared in Example 2; (b) Coulomb efficiency of 3DMF mixed electrolyte with different CPDs concentrations in Zn / / Cu battery. The aqueous co-solvent of this example uses a wide temperature range aqueous electrolyte with different CPDs concentrations at a current density of 2 mA cm -2 、Area capacity 1mAh cm -2 The constant current charge and discharge cycle performance test is carried out under the conditions of Figure 4 As shown in (a), the introduction of CPDs in 30% DMF can ensure that the symmetrical battery can operate stably at a stable polarization voltage of about 0.13 V for more than 200 h. 3DMF-0.4CPDs began to show a large voltage hysteresis after 160 h of cycling, which is attributed to the fact that excessive CPDs increase the viscosity of the electrolyte system, thereby hindering the Zn 2+ transmission. Figure 4 As shown in (b), at a current density of 4 mA cm -2 、Area capacity 1mAh cm -2 Under the conditions of , after 200 stable cycles, the coulombic efficiency of 3DMF without carbon dots was higher than 100%, which may indicate that side reactions occurred in the battery, resulting in an increase in the coulombic efficiency of the battery. The mixed electrolyte after adding CPDs can ensure that the battery can stably cycle 300 cycles with a coulombic efficiency close to 100%, among which the average coulombic efficiency of 3DMF-0.2CPDs can reach 99.29% after 300 cycles, which is still higher than the average coulombic efficiency of 98.27% of 3DMF before 300 cycles. This shows that the addition of carbon dots can enhance the inhibitory effect on side reactions, and the irreversible capacity loss in the galvanizing / stripping process is small.
[0053] The morphology of zinc deposition of 0DMF, 3DMF prepared in Example 1 and 3DMF-0.2CPDs prepared in Example 2 was characterized using a scanning electron microscope (SEM). Figure 5 For Zn / / Zn symmetric cells, 0DMF (a), 3DMF (b), and 3DMF-0.2CPDs (c) prepared in Example 1 were used at a current density of 0.5 mA cm -2 、Area capacity 3mAh cm -2 The zinc deposition morphology. Figure 5 (a) shows the 0DMF at a current density of 0.5 mA cm -2 、Area capacity 3mAh cm -2 The zinc deposition morphology under the microscope shows the formation of large zinc dendrites and the direction of zinc deposition is very chaotic. Figure 5 The zinc deposition in (b) is more uniform and flatter than that in (a), with a small amount of zinc dendrite growth. Figure 5No obvious Zn dendrites were observed in (c). CPDs can be preferentially adsorbed on the Zn surface and act as nucleation sites to induce uniform Zn deposition. It is also speculated that CPDs and DMF may participate in the construction of the SEI film, further inhibiting the growth of Zn dendrites and the corrosion of the Zn negative electrode.
[0054] The above examples illustrate that the wide temperature range aqueous electrolyte provided by the present invention broadens the operating temperature window of aqueous zinc ion batteries. 2+ Adjustment of the solvation structure improves the electrochemical performance of aqueous zinc ions over a wide temperature range.
[0055] The wide temperature range aqueous electrolyte provided by the present invention can inhibit the growth of zinc dendrites and induce uniform zinc deposition, thereby improving the electrochemical performance of aqueous zinc ion batteries, and can be used as an electrolyte for constructing dendrite-free aqueous zinc ion batteries. DMF, as a co-solvent, can effectively regulate the growth of Zn 2+ Solvation structure, inhibiting the occurrence of side reactions, and widening the battery electrochemical window. As a functional additive, CPDs can reduce the nucleation barrier and regulate the Zn 2+ CPDs adsorb on the high potential tip of the Zn negative electrode due to the Zn 2+ It has a stronger adsorption effect with the oxygen-containing groups of carbon dots, thus being able to inhibit the growth of zinc dendrites and obtain a lower nucleation overpotential, thereby guiding the uniform and regular deposition of Zn.
Claims
1. A method for preparing a wide temperature range aqueous electrolyte, characterized in that: The preparation method comprises the following steps: Step 1: Preparation of carbonized polymer dots (CPDs); Step 2: Evenly mix DMF and ZnSO4 electrolyte to prepare a mixed electrolyte; Step 3: Add the carbonized polymer dots CPDs from step 1 to the mixed electrolyte from step 2 to obtain a wide temperature range aqueous electrolyte.
2. The method for preparing a wide temperature range aqueous electrolyte according to claim 1, characterized in that: Step 1: The method for preparing carbonized polymer dots (CPDs) comprises: Dissolve citric acid and ethylenediamine in deionized water, stir evenly, and then transfer the mixture to a polytetrafluoroethylene reactor for reaction. After filtering, dialysis and freeze-drying, carbonized polymer dots CPDs are obtained.
3. The method for preparing a wide temperature range aqueous electrolyte according to claim 2, characterized in that: The molar ratio of the citric acid to ethylenediamine is 1:
1.
4. The method for preparing a wide temperature range aqueous electrolyte according to claim 2, characterized in that: The reaction temperature is 180°C and the reaction time is 5 hours.
5. The method for preparing a wide temperature range aqueous electrolyte according to claim 1, characterized in that: The volume fraction of DMF in step 2 is 10-50%.
6. The method for preparing a wide temperature range aqueous electrolyte according to claim 1, characterized in that: The concentration of the ZnSO4 electrolyte in step 2 is 2 mol / L.
7. The method for preparing a wide temperature range aqueous electrolyte according to claim 1, characterized in that: In step 3, the amount of carbonized polymer dots CPDs added is 0.1-0.4 mg / mL.
8. The method for preparing a wide temperature range aqueous electrolyte according to claim 1, characterized in that: The volume fraction of DMF in step 2 is 30%, and the amount of carbonized polymer dots CPDs added is 0.2 mg / mL.
9. A wide temperature range aqueous electrolyte obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the wide temperature range aqueous electrolyte according to claim 9 in aqueous zinc ion batteries.