Method of manufacturing semiconductor device
By using reflective layer structures with different refractive indexes and melt laser annealing process in DRAM device manufacturing, amorphous silicon is converted into polysilicon, solving the problem of electrical characteristics deterioration caused by silicon movement, and achieving higher process margins and performance improvements .
Patent Information
- Application Number
- CN202410584961.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
During the manufacturing of DRAM devices, as the feature size decreases and the integration degree increases, there is a problem that silicon moves into the barrier pattern in the bit line structure to generate gaps, resulting in deterioration of electrical characteristics, and the existing melt laser annealing process is at a high integration degree It is difficult to execute.
Using a reflective layer structure with different refractive indices, amorphous silicon is converted to by forming the first and second reflective layers on the cell region and peripheral circuit region of the substrate and performing a melt laser annealing (MLA) process thereon. Polysilicon, thereby forming a stable contact plug layer, limiting and preventing silicon from moving, increasing process margin.
Effectively prevent the generation of voids in the bit line structure, improve electrical characteristics, and through increased process margin, the execution of the MLA process under high integration is simplified and the performance of semiconductor devices is improved.
Smart Images

Figure CN118946144A_ABST
Abstract
Description
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application claims the priority of Korean Patent Application No. 10-2023-0061727 filed in the Korean Intellectual Property Office on May 12, 2023, the entire contents of which are incorporated herein by reference. Technical Field
[0003] Example embodiments of the present disclosure relate to a method of manufacturing a semiconductor device. More specifically, example embodiments of the present disclosure relate to a method of manufacturing a DRAM device. Background Art
[0004] In a DRAM device, the DRAM device may include a cell region having a structure different from that in a peripheral circuit region of the DRAM device. As feature sizes decrease and integration increases, research is being developed to manufacture DRAM devices with superior performance while solving problems caused by the integration of DRAM devices. Summary of the invention
[0005] Example embodiments provide a method of manufacturing a semiconductor device having improved electrical characteristics.
[0006] According to an example embodiment of the inventive concept, a method for manufacturing a semiconductor device may include: forming a first gate structure on a first region of a substrate, the substrate including a first region and a second region; forming a bit line structure on the first gate structure; forming a preliminary contact plug layer including amorphous silicon on the substrate; forming a reflective layer structure on the preliminary contact plug layer, the reflective layer structure including a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, the second refractive index being greater than the first refractive index, and a thickness of a portion of the second reflective layer located on the first region of the substrate being different from a thickness of a portion of the second reflective layer located on the second region of the substrate; forming a contact plug layer from the preliminary contact plug layer, the forming of the contact plug layer including performing a molten laser annealing (MLA) process of irradiating a laser on the reflective layer structure so that the amorphous silicon of the preliminary contact plug layer is converted into polycrystalline silicon; and forming a capacitor on the contact plug layer.
[0007] According to an example embodiment of the present invention, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first gate structure on a cell region of a substrate, the substrate comprising a cell region and a peripheral circuit region. Forming a bit line structure on the first gate structure; forming a preliminary contact plug layer comprising amorphous silicon on the substrate; forming a reflective layer structure on the preliminary contact plug layer, the reflective layer structure comprising a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, the second refractive index being greater than the first refractive index; forming a contact plug layer from the preliminary contact plug layer, the forming of the contact plug layer comprising performing a molten laser annealing (MLA) process of irradiating laser on the reflective layer structure, so that the amorphous silicon of the preliminary contact plug layer is converted into polysilicon; and forming a capacitor on the contact plug layer. The reflectance ratio of light in the peripheral circuit region of the substrate is greater than the reflectance ratio of light in the cell region of the substrate.
[0008] According to an example embodiment of the present invention, a method for manufacturing a semiconductor device is provided, the method comprising: forming a first gate structure on a cell region of a substrate, the substrate comprising a cell region and a peripheral circuit region; forming a bit line structure and a second gate structure on the cell region and the peripheral circuit region of the substrate, respectively; forming a preliminary contact plug layer comprising amorphous silicon on the substrate to cover the bit line structure and the second gate structure; forming a reflective layer structure on the preliminary contact plug layer, the reflective layer structure comprising a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, the second refractive index being greater than the first refractive index, and a portion of the second reflective layer located on the cell region of the substrate having a thickness different from a portion of the second reflective layer located on the peripheral circuit region of the substrate; performing a molten laser annealing (MLA) process, the MLA process comprising irradiating a laser on the reflective layer structure so that the preliminary contact plug layer is converted into a contact plug layer comprising polysilicon; planarizing the contact plug layer to form a lower contact plug; forming an upper contact plug on the lower contact plug; and forming a capacitor on the upper contact plug.
[0009] In example embodiments, in a method of manufacturing a semiconductor device, a phenomenon in which silicon included in a conductive pattern of a bit line structure moves into a barrier pattern to generate a void can be limited and / or prevented. In addition, an MLA process in which a preliminary lower contact plug layer is melted to be converted into a lower contact plug layer including polysilicon can have an increased margin and can therefore be easily performed. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figures 1 to 43 are plan views and cross-sectional views illustrating a method of manufacturing a semiconductor device according to example embodiments.
[0011] Fig.44 It shows Fig.24 and Fig.25FIG. 2 is a graph showing a reflectance ratio (reflectivity) of light obtained by simulation, wherein the light is incident on a first region I and a second region II of a substrate having a preliminary lower contact plug layer and a lower structure thereon.
[0012] Fig.45 It shows Fig.24 and 25 FIG. 1 is a graph of a reflectance ratio of light obtained by simulation, wherein light is incident on a first region I and a second region II of a substrate having a preliminary lower contact plug layer, a first reflective layer and a second reflective layer, and a lower structure thereon.
[0013] Figure 46 to Figure 48 is a graph showing the reflectance ratio of light obtained by simulation according to Comparative Example 1, Comparative Example 2 and Comparative Example 3, wherein the light is incident on the first region I and the second region II of the substrate 100 having the preliminary lower contact plug layer 470, the reflective layer structure and the lower layer structure thereon.
[0014] Fig.49 and Fig.50 are cross-sectional views showing a method of manufacturing a semiconductor device according to example embodiments, which respectively correspond to Fig.26 and Fig. 27 . DETAILED DESCRIPTION
[0015] With reference to the accompanying drawings, according to the following specific implementation, the above and other aspects and features of the decoupling capacitor structure and the method for forming the decoupling capacitor structure according to the example embodiment, as well as the semiconductor device including the decoupling capacitor structure and the method for manufacturing the semiconductor device will become easy to understand. It will be understood that although the terms "first", "second" and / or "third" can be used in this article to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present invention, the first element, component, region, layer or part discussed below may also be referred to as the second or third element, component, region, layer or part.
[0016] Expressions such as "at least one of..." when following a list of elements modify the entire list of elements rather than modifying the individual elements in the list. For example, "at least one of A, B, and C" and similar language (e.g., "at least one selected from the group consisting of A, B, and C") can be interpreted as only A, only B, only C, or any combination of two or more of A, B, and C, such as ABC, AB, BC, and AC.
[0017] When the term "about" or "substantially" is used in conjunction with a numerical value in this specification, the associated numerical value is intended to include a manufacturing or operating tolerance (e.g., ±10%) around the numerical value. In addition, when the words "generally" and "substantially" are used in conjunction with a geometric shape, the intention is not to require the accuracy of the geometric shape, but the tolerance of the shape is within the scope of the present disclosure. In addition, regardless of whether a numerical value or shape is modified to "about" or "substantially", it should be understood that these values and shapes should be interpreted as including a manufacturing or operating tolerance (e.g., ±10%) around the numerical value or shape.
[0018] Although the term "equal to" is used in the description of the example embodiments, it should be understood that some imprecision may exist. Therefore, when an element is referred to as being "equal to" another element, it should be understood that the element or value may be "equal to" the other element within a desired manufacturing or operating tolerance range (e.g., ±10%).
[0019] Figures 1 to 43 1 is a plan view and a cross-sectional view showing a method of manufacturing a semiconductor device according to an example embodiment. Specifically, Figure 1 , Figure 4 , Figure 7 , Fig.13 , Fig.18 , Fig.29 , Fig.33 , Fig.37 and Fig.40 It is a floor plan. Figure 2 , Figure 5 , Figure 8 , Fig.11 , Fig.14 , Fig.17 , Fig.19 , Fig. 22 , Fig.30 , Figure 34 to Figure 35 , Fig.38 and Fig.41 are cross-sectional views taken along the line AA' of the corresponding plane view, Fig. 9 , Fig.12 , Fig.15 , Fig. 20 , Fig.23 , Figure 31 to Figure 32 , Fig.36 , Fig.39 and Fig.42 are cross-sectional views taken along line BB' of the corresponding plane view, Figure 3 , Figure 6 , Fig.10 , Fig.16 , Fig.21 , Fig.24 , Fig.26 and Fig.43 are cross-sectional views taken along line CC' of the corresponding plan view, and Fig.25 as well as Figure 27 to Figure 28 They are cross-sectional views taken along line EE' of the corresponding plan view, respectively.
[0020] Hereinafter, in this specification (but not necessarily in the claims), two directions substantially parallel to the upper surface of the substrate 100 and substantially perpendicular to each other may be referred to as a first direction D1 and a second direction D2, respectively, and a direction substantially parallel to the upper surface of the substrate 100 and having an acute angle with respect to the first direction D1 and the second direction D2 may be referred to as a third direction D3. A substantially identical or similar direction perpendicular to the upper surface of the substrate 100 may be referred to as a vertical direction.
[0021] refer to Figures 1 to 3 , the first active pattern 101 and the second active pattern 105 may be formed on the substrate 100 including the first region I and the second region II.
[0022] The substrate 100 may include silicon, germanium, silicon-germanium, or a III-V compound semiconductor such as GaP, GaAs, or GaSb. In some example embodiments, the substrate 100 may be a silicon-on-insulator (SOI) substrate or a germanium-on-insulator (GOI) substrate.
[0023] The first region I of the substrate 100 may be a cell region on which a memory cell is formed, and the second region II of the substrate 100 surrounding the first region I of the substrate 100 may be a peripheral circuit region on which a circuit for driving the memory cell is formed. Figures 1 to 3 A portion of the first region I and a portion of the second region II adjacent to the first region I in the first direction D1 and the second direction D2 are respectively shown.
[0024] The first active pattern 101 and the second active pattern 105 may be formed by removing the upper portion of the substrate 100 to form a groove structure. The first active pattern 101 may extend along the third direction D3 on the first region I, and a plurality of first active patterns 101 may be spaced apart from each other in each of the first direction D1 and the second direction D2. In addition, a plurality of second active patterns 105 may be spaced apart from each other in each of the first direction D1 and the second direction D2.
[0025] The groove structure may include a first groove 102, a second groove 104, and a third groove 106. The first groove 102 may be formed between the first active patterns 101 spaced apart from each other by a relatively small distance, the second groove 104 may be formed between the first active patterns 101 spaced apart from each other by a relatively large distance, and the third groove 106 may be formed on the second region II of the substrate 100 or between the first region I and the second region II of the substrate 100.
[0026] In example embodiments, the third groove 106 may have a width and / or depth greater than that of the second groove 104 , and the second groove 104 may have a width and / or depth greater than that of the first groove 102 .
[0027] The isolation structure 110 may be formed to cover sidewalls of the first and second active patterns 101 and 105 .
[0028] In example embodiments, the isolation structure 110 may include a first isolation pattern 112, a second isolation pattern 114, and a third isolation pattern 116 sequentially stacked on an inner wall of the third groove 106. However, the first isolation pattern 112 and the second isolation pattern 114 may be formed in the second groove 104 having a smaller width than the third groove 106, and the first isolation pattern 112 may be formed in the first groove 102 having a smaller width than the second groove 104.
[0029] Each of the first isolation pattern 112 and the third isolation pattern 116 may include oxide (eg, silicon oxide), and the second isolation pattern 114 may include insulating nitride (eg, silicon nitride).
[0030] refer to Figures 4 to 6 An etching process may be performed on the first active pattern 101 and the isolation structure 110 on the first region I of the substrate 100 and a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100 to form a fourth groove 40 .
[0031] In example embodiments, during the etching process, the first active pattern 101 including a semiconductor material may be less etched than the isolation structure 110 including an insulating material due to etching selectivity. Therefore, the fourth groove 40 may have a concave upper surface on an upper surface of the first active pattern 101.
[0032] The first gate insulating layer and the first conductive layer may be sequentially stacked on the inner wall of the fourth groove 40 and the upper surfaces of the first and second active patterns 101, 105 and the isolation structure 110, the first gate insulating layer and the first conductive layer may be planarized until the upper surfaces of the first and second active patterns 101, 105 and the isolation structure 110 are exposed, and the upper portion of the first conductive layer may be removed by, for example, an etch-back process.
[0033] The planarization process may include a chemical mechanical polishing (CMP) process and / or an etch-back process.
[0034] The first gate insulating pattern 120 may be formed on the inner wall of the fourth groove 40 through a planarization process, and the first conductive pattern 140 may be formed on the first gate insulating pattern 120 to fill a lower portion of the fourth groove 40 through an etch-back process.
[0035] The second conductive pattern 150 may be formed on the first conductive pattern 140, a first gate mask layer may be formed on the second conductive pattern 150, the first and second active patterns 101 and 105, and the isolation structure 110 to fill the fourth groove 40, and the first gate mask layer may be planarized until the upper surfaces of the first and second active patterns 101 and 105 and the isolation structure 110 are exposed, so that the first gate mask 160 may be formed to fill the upper portion of the fourth groove 40. The first conductive pattern 140 and the second conductive pattern 150 may jointly form a gate electrode, and a first barrier pattern may be further formed between the first gate insulating pattern 120 and the first conductive pattern 140.
[0036] The first gate insulating pattern 120 may include an oxide (e.g., silicon oxide), the first barrier pattern may include a metal nitride (e.g., titanium nitride, tantalum nitride, etc.), the first conductive pattern 140 may include a metal, a metal nitride, a metal silicide, doped polysilicon, etc., the second conductive pattern 150 may include doped polysilicon, and the first gate mask 160 may include a nitride (e.g., silicon nitride).
[0037] The first gate insulating pattern 120, the first barrier pattern, the first conductive pattern 140, the second conductive pattern 150, and the first gate mask 160 in the fourth groove 40 may collectively form a first gate structure 170. In example embodiments, the first gate structure 170 may extend along the first direction D1 on the first region I of the substrate 100 and a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100, and a plurality of first gate structures 170 may be spaced apart from each other in the second direction D2. Ends of the first gate structures 170 in the first direction D1 may be aligned with each other in the second direction D2 on the portion of the second region II of the substrate 100.
[0038] refer to Figures 7 to 10 The insulating layer structure 210 may be formed on the first region I and the second region II of the substrate 100 , and a portion of the insulating layer structure 210 located on the second region II of the substrate 100 except a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100 may be removed.
[0039] For example, a thermal oxidation process may be performed on the second active pattern 105 on the second region II of the substrate 100 to form the second gate insulating layer 220 .
[0040] The insulating layer structure 210 may be patterned, and the first active pattern 101, the isolation structure 110, and the first gate mask 160 of the first gate structure 170 may be partially etched using the patterned insulating layer structure 210 as an etching mask to form a first opening 230. In example embodiments, the patterned insulating layer structure 210 may have a circular or elliptical shape in a plan view, and a plurality of insulating layer structures 210 may be spaced apart from each other along the first direction D1 and the second direction D2 on the first region I of the substrate 100 and a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100. Each insulating layer structure 210 may overlap opposite ends of the first active pattern 101 in the third direction D3 in a vertical direction substantially perpendicular to the upper surface of the substrate 100.
[0041] refer to Fig.11 and Fig.12 , a third conductive layer 240, a second barrier layer 250, a fourth conductive layer 260, and a second mask layer 270 may be sequentially stacked on the insulating layer structure 210, the first active pattern 101, the isolation structure 110, and the upper surface of the first gate structure 170 exposed by the first opening 230 on the first region I of the substrate 100, and the second gate insulating layer 220 and the isolation structure 110 on the second region II of the substrate 100, which may jointly form a conductive structure layer. The third conductive layer 240 may fill the first opening 230.
[0042] The third conductive layer 240 may include doped polysilicon, the second barrier layer 250 may include metal silicon nitride (eg, titanium silicon nitride), the fourth conductive layer 260 may include metal (eg, tungsten), and the second mask layer 270 may include nitride (eg, silicon nitride).
[0043] refer to Figures 13 to 16 , the conductive structure layer may be patterned to form a second gate structure 330 on the second region II of the substrate 100 .
[0044] The second gate structure 330 may include a second gate insulating pattern 280, a third conductive pattern 290, a second barrier pattern 300, a fourth conductive pattern 310 and a second gate mask 320 sequentially stacked in a vertical direction substantially perpendicular to the upper surface of the substrate 100, and the third conductive pattern 290, the second barrier pattern 300 and the fourth conductive pattern 310 may jointly form a second gate electrode.
[0045] The second gate structure 330 may at least partially overlap the second active pattern 105 in a vertical direction on the second region II of the substrate 100 .
[0046] A portion of the conductive structure layer located on an edge portion of the first region I of the substrate 100 and adjacent to the second region II of the substrate 100 can also be removed, thereby partially exposing the insulating layer structure 210 and the upper surfaces of the active pattern 101, the isolation structure 110 and the first gate structure 170 exposed by the first opening 230.
[0047] The first spacer structure may be formed on the sidewalls of the second gate structure 330, and the second spacer structure may be formed on the sidewalls of the conductive structure layer remaining on the first region I of the substrate 100. The first spacer structure may include a first spacer 340 and a third spacer 350 stacked on the sidewalls of the second gate structure 330 in a horizontal direction substantially parallel to the upper surface of the substrate 100, and the second spacer structure may include a second spacer 345 and a fourth spacer 355 stacked on the sidewalls of the conductive structure layer in a horizontal direction.
[0048] The first spacer 340 and the second spacer 345 may be formed by forming a first spacer layer on the substrate 100 to cover the conductive structure layer and the second gate structure 330 and anisotropically etching the first spacer layer. The third spacer 350 and the fourth spacer 355 may be formed by forming a second spacer layer on the substrate 100 to cover the conductive structure layer, the second gate structure 330, and the first spacer 340 and the second spacer 345 and anisotropically etching the second spacer layer.
[0049] The first spacer 340 and the second spacer 345 may include nitride (eg, silicon nitride), and the third spacer 350 and the fourth spacer 355 may include oxide (eg, silicon oxide).
[0050] However, the first spacer structure and the second spacer structure may not be limited thereto, and each of the first spacer structure and the second spacer structure may include a single spacer or more than two spacers stacked sequentially.
[0051] A first etch stop layer 360 may be formed on the substrate 100 to cover the conductive structure layer, the second gate structure 330, the first and second spacer structures, and the isolation structure 110. The first etch stop layer 360 may include nitride (eg, silicon nitride).
[0052] refer to Fig.17 The first interlayer insulating layer 370 can be formed on the first etch stop layer 360 to a sufficient height, the first interlayer insulating layer 370 can be planarized until the upper surface of the second gate structure 330 and the upper surface of the portion of the first etch stop layer 360 located on the conductive structure layer are exposed, and a capping layer 380 can be formed on the first interlayer insulating layer 370 and the first etch stop layer 360.
[0053] Therefore, the first interlayer insulating layer 370 may fill the space between the first spacer structures on the sidewalls of the second gate structure 330 and the space between the first spacer structures on the sidewalls of the second gate structure 330 and the second spacer structures on the sidewalls of the conductive structure layer.
[0054] The first interlayer insulating layer 370 may include oxide (eg, silicon oxide), and the capping layer 380 may include nitride (eg, silicon nitride).
[0055] refer to Figures 18 to 21 , a portion of the capping layer 380 located on the first region I of the substrate 100 can be etched to form a first capping pattern 385, and the first etch stop layer 360, the second mask layer 270, the fourth conductive layer 260, the second barrier layer 250 and the third conductive layer 240 can be sequentially etched using the first capping pattern 385 as an etching mask.
[0056] In example embodiments, the first capping pattern 385 may extend in the second direction D2 on the first region I of the substrate 100 , and a plurality of first capping patterns 385 may be formed to be spaced apart from each other in the first direction D1 . The capping layer 380 may remain on the second region II of the substrate 100 .
[0057] Through the etching process, on the first region I of the substrate 100, the fifth conductive pattern 245, the third barrier pattern 255, the sixth conductive pattern 265, the second mask 275, the first etch stop pattern 365 and the first capping pattern 385 can be sequentially stacked on the first opening 230, and the third insulating pattern 205, the fifth conductive pattern 245, the third barrier pattern 255, the sixth conductive pattern 265, the second mask 275, the first etch stop pattern 365 and the first capping layer pattern 385 can be sequentially stacked on the second insulating layer 190 of the insulating layer structure 210 at the outside of the first opening 230.
[0058] Hereinafter, the fifth conductive pattern 245, the third barrier pattern 255, the sixth conductive pattern 265, the second mask 275, the first etch stop pattern 365, and the first capping pattern 385, which are sequentially stacked, may be referred to as a bit line structure 395. In example embodiments, the bit line structure 395 may extend in the second direction D2 on the first region I of the substrate 100, and a plurality of the bit line structures 395 may be spaced apart from each other in the first direction D1.
[0059] A dummy bit line structure 397 including a seventh conductive pattern 247, a fourth barrier pattern 257, an eighth conductive pattern 267, a third mask 277, a second etch stop pattern 367, and a second capping pattern 387 sequentially stacked and extending in the second direction D2 may be formed on a portion of the first region I of the substrate 100 adjacent to the second region II of the substrate 100 in the first direction D1, and a first etch stop layer 360 may remain on the second gate structure 330, the first and second spacer structures, a portion of the insulating layer structure 210, the second active pattern 105, and the isolation structure 110. In addition, a capping layer 380 may remain on a portion of the first etch stop layer 360 located on upper surfaces of the second gate structure 330 and the first interlayer insulating layer 370.
[0060] refer to Fig. 22 and Fig.23 , a fifth spacer layer may be formed on the substrate 100 to cover the bit line structure 395 , the dummy bit line structure 397 , and the capping layer 380 , and a fourth insulating layer and a fifth insulating layer may be sequentially formed on the fifth spacer layer.
[0061] The fifth spacer layer may also cover sidewalls of the third insulation pattern 205 between the second insulation layer 190 and the bit line structure 395 , and the fifth insulation layer may fill the first opening 230 .
[0062] The fifth spacer layer may include nitride (eg, silicon nitride), the fourth insulating layer may include oxide (eg, silicon oxide), and the fifth insulating layer may include nitride (eg, silicon nitride).
[0063] The fourth insulating layer and the fifth insulating layer may be etched by an etching process. 3 PO 4 ), SC1, and an etching solution of hydrogen fluoride (HF) are used to perform the etching process, and the other portions of the fourth and fifth insulating layers except the portions in the first opening 230 can be removed. Therefore, most of the entire surface of the fifth spacer layer (i.e., the entire surface except the portion thereof in the first opening 230) can be exposed, and the portions of the fourth and fifth insulating layers remaining in the first opening 230 can form a fourth insulating pattern 410 and a fifth insulating pattern 420, respectively.
[0064] The sixth spacer layer may be formed on the exposed surface of the fifth spacer layer and the fourth and fifth insulating patterns 410 and 420 in the first opening 230, and may be anisotropically etched to form the sixth spacer 430 on the surface of the fifth spacer layer and the fourth and fifth insulating patterns 410 and 420 to cover the sidewalls of the bit line structure 395. The sixth spacer layer may also be formed on the sidewalls of the dummy bit line structure 397. The sixth spacer layer may include an oxide (e.g., silicon oxide).
[0065] A dry etching process may be performed to form the second opening 440 exposing the upper surface of the first active pattern 101. The upper surface of the isolation structure 110 and the upper surface of the first gate mask 160 may also be exposed through the second opening 440.
[0066] Through the dry etching process, the portion of the fifth spacer layer located on the upper surfaces of the first capping pattern 385 and the second capping pattern 387, the second insulating layer 190, and the capping layer 380 may be removed, thereby forming a fifth spacer 400 covering the sidewall of the bit line structure 395. The fifth spacer 400 may also cover the sidewall of the dummy bit line structure 397.
[0067] In addition, during the dry etching process, the first insulating layer 180 and the second insulating layer 190 may be partially removed so that the first insulating pattern 185 and the second insulating pattern 195 may remain under the bit line structure 395. The first to third insulating patterns 185, 195, and 205 sequentially stacked under the bit line structure 395 may collectively form an insulating pattern structure 215.
[0068] refer to Fig.24 and Fig.25 , a seventh spacer layer may be formed on upper surfaces of the first and second capping patterns 385 and 387, an upper surface of the capping layer 380, an outer sidewall of the sixth spacer 430, portions of upper surfaces of the fourth and fifth insulating patterns 410 and 420, and upper surfaces of the first active pattern 101, the isolation structure 110, and the first gate mask 160 exposed by the second opening 440, and may be anisotropically etched to form seventh spacers 450 covering the outer sidewalls of the sixth spacer 430 on sidewalls of the bit line structure 395 and the dummy bit line structure 397. The seventh spacer layer may include nitride (e.g., silicon nitride).
[0069] The fifth to seventh spacers 400 , 430 , and 450 sequentially stacked in a horizontal direction from the sidewall of the bit line structure 395 on the first region I of the substrate 100 may be referred to as a preliminary third spacer structure 460 .
[0070] A preliminary lower contact plug layer 470 may be formed on the first region I of the substrate 100 to fill the second opening 440 , and the first reflective layer 700 and the second reflective layer 710 may be stacked on the preliminary lower contact plug layer 470 .
[0071] In example embodiments, the preliminary lower contact plug layer 470 may include amorphous silicon doped with, for example, n-type impurities, and may have a first refractive index n. 1 .
[0072] Each of the first reflective layer 700 and the second reflective layer 710 may adjust the reflectivity of light incident on the first region I and the second region II of the substrate 100, and the first reflective layer 700 and the second reflective layer 710 may jointly form a reflective layer structure. However, the first reflective layer 700 and the second reflective layer 710 may also be referred to as a first anti-reflective layer 700 and a second anti-reflective layer 710, respectively, and they may jointly form an anti-reflective layer structure. In example embodiments, the first reflective layer 700 may include a first anti-reflective layer having a relatively low reflectivity (hereinafter, referred to as a second refractive index n 2 ) (eg, silicon oxide, tetraethyl orthosilicate (TEOS), etc.), and the second reflective layer 710 may include a material having a relatively high reflectivity (hereinafter, referred to as a third refractive index n 3 ) materials (e.g., silicon nitride, hafnium oxide, etc.).
[0073] The preliminary lower contact plug layer 470 may have a first thickness T1 in a vertical direction from an upper surface of the capping layer 380 on the second region II of the substrate 100 , and the first and second reflective layers 700 and 710 may have second and third thicknesses T2 and T3 in the vertical direction.
[0074] In example embodiments, the first thickness T1 of the preliminary lower contact plug layer 470 may satisfy Equation 1.
[0075] <Formula 1>
[0076] (N / 2+1 / 8+Δ)λ / n 1 +δ 1 ≤T1≤(N / 2+3 / 8+Δ)λ / n 1 +δ 2
[0077] N is one of 1, 2 and 3, λ is the wavelength of the incident light, Δ is the optical path correction factor, -1 / 4≤Δ≤1 / 4, δ 1 and δ 2 Each of is a thickness correction factor, and -8nm≤δ 1 ≤8nm, -8nm≤δ 2 ≤8nm.
[0078] Δ、δ1 and δ 2 Each of may have an optimal value according to process conditions.
[0079] For example, λ has a wavelength of about 532 nm, and n 1 has a value of about 4.8. If N is 1, then Δ = -1 / 8, δ 1 =2nm,δ 2 =2nm, and 57nm≤T1≤85nm. If N is 2, then Δ=-1 / 4, δ 1 =-8nm,δ 1 =8nm, and 89nm≤T1≤133nm. If N is 3, then Δ=-1 / 8, δ 1 =2nm,δ 1 =2nm, and 168nm≤T1≤196nm.
[0080] An upper portion of the portion of the second reflective layer 710 located on the second region II of the substrate 100 may be removed by an etching process, and thus the portion of the second reflective layer 710 located on the second region II of the substrate 100 may have a fourth thickness T4 that is smaller than the third thickness T3.
[0081] In example embodiments, the second thickness T2 and the fourth thickness T4 may satisfy Equation 2.
[0082] <Formula 2>
[0083] n 2 *T2=n 3 *T4=λ / 4
[0084] However, the second thickness T2 and the fourth thickness T4 may satisfy Equation 3 including an optical path correction factor according to process conditions.
[0085] <Formula 3>
[0086] T2=(1 / 4+Δ)λ / n 2
[0087] T4=(1 / 4+Δ)λ / n 3
[0088] (-1 / 8≤Δ≤1 / 8)
[0089] Similarly, the third thickness T3 may satisfy Formula 4.
[0090] <Formula 4>
[0091] T3=(1 / 4+Δ)λ / n 3
[0092] (-1 / 4≤Δ≤1 / 4)
[0093] If light is incident on the first reflective layer 700 and the second reflective layer 710 stacked on the preliminary lower contact plug layer 470, the light is reflected at the interface between the first reflective layer 700 and the second reflective layer 710, and constructive interference occurs between the first reflective layer 700 and the second reflective layer 710 due to the optical path difference between the incident light and the reflected light. In this case, the second to fourth thicknesses T2, T3, and T4 may satisfy Equations 3 and 4.
[0094] When the second to fourth thicknesses T2, T3, and T4 are calculated according to the density, arrangement, and process conditions of the structures under the first and second reflective layers 700 and 710, the optical path correction factors Δ in Equations 3 and 4 may have different values.
[0095] For example, λ may be about 532 nm, n 2 can be about 1.46, and n 2 It may be about 2.2. If Δ=0 in equation 3 and Δ=3 / 20 in equation 4, then T2=91 nm, T3=97 nm, and T4=60 nm.
[0096] In example embodiments, the third thickness T3 may satisfy Equation 5.
[0097] <Formula 5>
[0098] λ / (10*n 3 )≤T3≤9λ / (10*n 3 )
[0099] Therefore, if λ is about 532nm and n 3 is about 2.2, then 24nm≤T3≤218nm. However, Formula 5 shows the maximum range of the third thickness T3, and the actual value of the third thickness T3 can be determined by Formula 4 within its maximum range, for example, 87nm≤T3≤107nm.
[0100] In example embodiments, a portion of the second reflective layer 710 located on a portion of the second region II adjacent to the first region I may not be etched by the etching process. An end portion of the portion of the second reflective layer 710 maintaining the third thickness T3 in the first direction D1 may be spaced apart from a boundary of the first region I of the substrate 100 in the first direction D1 by a first distance S1, and an end portion of the portion of the second reflective layer 710 maintaining the third thickness T3 in the second direction D2 may be spaced apart from a boundary of the first region I of the substrate 100 in the second direction D2 by a second distance S2.
[0101] In example embodiments, the first distance S1 and the second distance S2 may be substantially the same as each other. Alternatively, the first distance S1 and the second distance S2 may be different from each other. In example embodiments, each of the first distance S1 and the second distance S2 may be less than about 500 nm, preferably, in the range of about 300 nm to about 400 nm.
[0102] refer to Fig.26 and Fig. 27 , a molten laser annealing (MLA) process may be performed in which laser is irradiated on the first region I and the second region II of the substrate 100 having the first reflective layer 700 and the second reflective layer 710 thereon, and thus, the preliminary contact plug layer 470 including amorphous silicon doped with impurities may be crystallized to be converted into a lower contact plug layer 472 including polycrystalline silicon doped with impurities.
[0103] In example embodiments, the laser may have a wavelength of visible light (e.g., a wavelength of about 400 nm to about 700 nm), and may include, for example, a pulsed laser, a continuous wave (CW) laser, etc. In example embodiments, the laser may have a wavelength of about 200 mJ / cm 2 About 1200mJ / cm 2 of power.
[0104] refer to Fig.28 After removing the first reflective layer 700 and the second reflective layer 710 , the lower contact plug layer 472 may be planarized until upper surfaces of the capping layer 380 and the first and second capping patterns 385 and 387 are exposed to form a lower contact plug 475 .
[0105] The lower contact plugs 475 may extend in the second direction D2 between the bit line structures 395 adjacent in the first direction D1 and between the bit line structures 395 and the dummy bit line structures 397 on the first region I of the substrate 100, and a plurality of the lower contact plugs 475 may be spaced apart from each other in the first direction D1. Each of the lower contact plugs 475 may contact an upper surface of an end portion of the first active pattern 101 extending in the third direction D3 in the third direction D3.
[0106] refer to Figure 29 to Figure 31 An etching mask having third openings (each third opening may extend in the first direction D1 and be spaced apart from each other in the second direction D2) may be formed on the capping layer 380, the bit line structure 395, the dummy bit line structure, and the lower contact plug layer, and an etching process may be performed on the lower contact plug 475 using the etching mask to form a fourth opening 445.
[0107] In example embodiments, the third opening may overlap the first gate structure 170 in a vertical direction, and the fourth opening 445 may expose an upper surface of the first gate mask 160 of the first gate structure 170. When the fourth opening 445 is formed, the lower contact plug 475 extending in the second direction D2 may be divided into a plurality of sections spaced apart from each other in the second direction D2.
[0108] After removing the etching mask, a fence pattern 480 may be formed to fill the fourth opening 445. A plurality of fence patterns 480 may be spaced apart from each other in the second direction D2 between the bit line structures 395 and between the bit line structures 395 and the dummy bit line structures 397. The fence pattern 480 may include nitride (eg, silicon nitride).
[0109] As shown above, lower contact plugs 475 and fence patterns 480 that may be alternately and repeatedly arranged in the second direction D2 may be formed in the following manner: a preliminary lower contact plug layer 470 extending in the second direction D2 is formed between the bit line structures 395, an MLA process is performed to form a lower contact plug layer 472, the lower contact plug layer 472 is planarized to form a lower contact plug 475, fourth openings 445 are formed passing through the lower contact plugs 475 and spaced apart from each other in the second direction D2, and the fourth openings 445 are filled by the fence pattern 480, however, the present invention may not be limited thereto.
[0110] Alternatively, the lower contact plugs 475 and the fence pattern 480 alternately and repeatedly arranged in the second direction D2 may be formed in the following manner: a fence layer extending in the second direction D2 is formed between the bit line structures 395, fifth openings are formed passing through the bit line structures 395 and spaced apart from each other in the second direction D2 to divide the fence layer into the fence patterns 480, a preliminary lower contact plug layer 470 is formed on the fence layer to fill the fifth openings, an MLA process is performed on the preliminary lower contact plug layer 470 to form a lower contact plug layer 472, and the lower contact plug layer 472 is planarized to form a lower contact plug 475.
[0111] Alternatively, the lower contact plugs 475 and the fence pattern 480 alternately and repeatedly arranged in the second direction D2 can be formed by forming a sacrificial layer including an oxide (e.g., silicon oxide) and extending along the second direction D2 between the bit line structures 395, forming the fence pattern 480 spaced apart from each other in the second direction D2 through the sacrificial layer, removing the sacrificial layer to form a sixth opening, forming a preliminary lower contact plug layer 470 to fill the sixth opening, performing an MLA process on the preliminary lower contact plug layer 470, and planarizing the lower contact plug layer 472 to form a lower contact plug 475.
[0112] refer to Fig.32, an upper portion of the lower contact plug 475 may be removed to expose an upper portion of the preliminary third spacer structure 460 located on the sidewalls of the bit line structure 395 and the dummy bit line structure 397, and a portion of the sixth spacer 430 and the seventh spacer 450 of the exposed preliminary third spacer structure 460 may be removed.
[0113] An etch-back process may be further performed to remove an upper portion of the lower contact plug 475 . Thus, an upper surface of the lower contact plug 475 may be lower than uppermost surfaces of the sixth and seventh spacers 430 and 450 .
[0114] An eighth spacer layer may be formed on the bit line structure 395, the dummy bit line structure 397, the preliminary third spacer structure 460, the fence pattern 480, the capping layer 380 and the lower contact plug 475, and may be anisotropically etched so that the eighth spacer 490 may be formed to cover the preliminary third spacer structure 460 on each of the opposite side walls of the bit line structure 395 in the first direction D1, and so that the upper surface of the lower contact plug 475 may be uncovered to be exposed.
[0115] The ohmic contact pattern 500 may be formed on the exposed upper surface of the lower contact plug 475. In example embodiments, the ohmic contact pattern 500 may be formed by forming a first metal layer on the first and second capping patterns 385 and 387, the capping layer 380, the fence pattern 480, the eighth spacer 490, and the lower contact plug 475, heat-treating the first metal layer, and removing an unreacted portion of the first metal layer. The ohmic contact pattern 500 may include a metal silicide, such as cobalt silicide, nickel silicide, titanium silicide, and the like.
[0116] refer to Fig.33 and Fig.34 The seventh opening 520 can be formed to pass through a portion of the capping layer 380 located on a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100, as well as the first insulating layer interlayer 370, the first etch stop layer 360, the insulating pattern structure 215, the isolation structure 110, the first gate mask 160 and the second conductive pattern 150 to expose the first conductive pattern 140, and the seventh opening 520 can also expose the first gate insulating pattern 120 on the sidewalls of the first conductive pattern 140.
[0117] refer to Fig.35 and Fig.36, a fifth barrier layer 530 may be formed on the first and second capping patterns 385 and 387, the fence pattern 480, the eighth spacer 490, the ohmic contact pattern 500, and the lower contact plug 475 on the first region I of the substrate 100, and may be formed on the capping layer 380, the sidewalls of the seventh opening 520, and the first conductive pattern 140, the first gate insulating pattern 120, and the isolation structure 110 exposed through the seventh opening 520 on the second region II of the substrate 100. A second metal layer 540 may be formed on the fifth barrier layer 530 to fill the spaces between the bit line structures 395, between the bit line structures 395 and the dummy bit line structures 397, and the seventh opening 520.
[0118] refer to Figure 37 to Figure 39 , the second metal layer 540 and the fifth barrier layer 530 may be patterned.
[0119] Thus, the upper contact plug 549 may be formed on the first region I of the substrate 100, and the second wiring 605 may be formed on the second region II of the substrate 100. In addition, the first wiring 600 may be formed on a portion of the second region II of the substrate 100 adjacent to the first region I of the substrate 100, and the third wiring 607 may be formed on a portion of the first region I of the substrate 100 adjacent to the second region II of the substrate 100. The eighth opening 547 may be formed between the upper contact plug 549 and the first to third wirings 600, 605, and 607.
[0120] The eighth opening 547 may be formed by removing not only the second metal layer 540 and the fifth barrier layer 530 but also the first and second capping patterns 385 and 387 , the fence pattern 480 , the capping layer 380 , the preliminary third spacer structure 460 , the eighth spacer 490 , the first etch stop layer 360 , the first etch stop pattern 365 , and the second mask 275 .
[0121] When the eighth opening 547 is formed, the second metal layer 540 and the fifth barrier layer 530 may be transformed into a first metal pattern 545 and a fifth barrier pattern 535 covering a lower surface of the first metal pattern 545, respectively, and the first metal pattern 545 and the fifth barrier pattern 535 may jointly form an upper contact plug 549 on the first region I of the substrate 100. In example embodiments, a plurality of upper contact plugs 549 may be formed to be spaced apart from each other in each of the first direction D1 and the second direction D2, and may be arranged in a honeycomb pattern or a lattice pattern in a plan view. Each of the upper contact plugs 549 may have a circular, elliptical, or polygonal shape in a plan view.
[0122] The lower contact plug 475 , the ohmic contact pattern 500 , and the upper contact plug 549 sequentially stacked on the first region I of the substrate 100 may collectively form a first contact plug structure.
[0123] The first wiring 600 may include a third metal pattern 590 and a seventh barrier pattern 580 covering a lower surface of the third metal pattern 590, and a second contact plug 570 including a second metal pattern 560 and a sixth barrier pattern 550 may be formed in the seventh opening 520. The second wiring 605 may include a fourth metal pattern 595 and an eighth barrier pattern 585 covering a lower surface of the fourth metal pattern 595, and the third wiring 607 may include a fifth metal pattern 597 and a ninth barrier pattern 587 covering a lower surface of the fifth metal pattern 597.
[0124] In example embodiments, the first wiring 600 may overlap the seventh opening 520 in the vertical direction, and a plurality of first wirings 600 may be spaced apart from each other in the second direction D2. The first wiring 600 may be electrically connected to the first conductive pattern 140 through the second contact plug 570, and thus may apply an electrical signal to the first gate structure 170. The second wiring 605 may overlap the second gate structure 330 in the vertical direction. The third wiring 607 may overlap the dummy bit line structure 397 in the vertical direction.
[0125] refer to Figure 40 to Figure 43 , the sixth spacer 430 may be removed to form an air gap 435 connected to the eighth opening 547. The sixth spacer 430 may be removed by, for example, a wet etching process.
[0126] In example embodiments, not only a first portion of the sixth spacer 430 located on the sidewalls of the bit line structure 395 and the dummy bit line structure 397 and directly exposed by the eighth opening 547 may be removed, but also a second portion of the sixth spacer 430 parallel to the first portion in a horizontal direction may be removed. That is, not only a portion of the sixth spacer 430 exposed by the eighth opening 547 but not covered by the upper contact plug 549 may be removed, but also a portion of the sixth spacer 430 covered by the upper contact plug 549 may be removed.
[0127] A second interlayer insulating layer may be formed to fill the eighth opening 547 .
[0128] In example embodiments, the second interlayer insulating layer may include a sixth insulating layer 610 and a seventh insulating layer 620 stacked sequentially. The sixth insulating layer 610 may include a material having a poor gap filling property, and thus the air gap 435 may not be filled with the sixth insulating layer 610 but may remain, and the air gap 435 may be referred to as an air spacer 435. The fifth spacer 400 and the seventh spacer 450 and the air spacer 435 may collectively form a third spacer structure 465. The air spacer 435 may be a spacer including air. The seventh insulating layer 620 may include an oxide (e.g., silicon oxide) or a nitride (e.g., silicon nitride).
[0129] The capacitor 665 may be formed to contact an upper surface of the upper contact plug 549 .
[0130] Specifically, the second etch stop layer 630 and the mold layer may be sequentially formed on the upper contact plug 549, the second interlayer insulating layer, and the first to third wirings 600, 605, and 607, and may be partially etched to form a ninth opening partially exposing the upper surface of the upper contact plug 549. The second etch stop layer 630 may include a nitride (e.g., silicon nitride).
[0131] The lower electrode layer may be formed on the upper contact plug 549 and the exposed upper surface of the mold layer to fill the ninth opening, and may be planarized until the upper surface of the mold layer is exposed to form a lower electrode 640 having a columnar shape. Alternatively, the lower electrode 640 may be formed to have a cylindrical shape. The lower electrode may include, for example, metal, metal nitride, metal silicide, doped polysilicon, etc.
[0132] The mold layer may be removed by, for example, a wet etching process.
[0133] A dielectric layer 650 may be formed on a surface of the lower electrode 640 and an upper surface of the second etch stop layer 630 , and an upper electrode 660 may be formed on the dielectric layer 650 to form a capacitor 670 including the lower electrode 640 , the dielectric layer 650 , and the upper electrode 660 on the first region I of the substrate 100 .
[0134] The dielectric layer 650 may include, for example, a metal oxide, and the upper electrode 660 may include, for example, a metal, a metal nitride, a metal silicide, doped polysilicon, or the like.
[0135] Contact plugs and upper wirings may also be formed on the substrate 100 to be electrically connected to the capacitor 670 , the bit line structure 395 , and the first to third wirings 600 , 605 , and 607 , thereby completing the manufacture of the semiconductor device.
[0136] As shown above, before performing the MLA process on the preliminary lower contact plug layer 470 including amorphous silicon doped with impurities and having the first thickness T1 from the upper surface of the capping layer 380 on the second region II of the substrate 100, the first reflective layer 700 and the second reflective layer 710 can be formed on the preliminary lower contact plug layer 470, and the upper portion of the second reflective layer 710 located on the second region II of the substrate 100 can be removed, so that the first reflective layer 700 having the second thickness T2 and the second reflective layer 710 having the third thickness T3 can be stacked on the first region I of the substrate 100, and the first reflective layer 700 having the second thickness T2 and the second reflective layer 710 having the fourth thickness T4 can be stacked on the second region II of the substrate 100.
[0137] Fig.44 It shows Fig.24 and Fig.25 1 is a graph of a reflectance ratio (reflectivity) of light obtained through simulation, wherein light is incident on the first region I and the second region II of the substrate 100 having the preliminary lower contact plug layer 470 and the lower structure thereon.
[0138] The light has a wavelength of about 532 nm, and is incident on the upper surface of the substrate 100 in a vertical direction.
[0139] refer to Fig.44 , the first thickness T1 of the preliminary lower contact plug layer 470 increases from about 50 nm to about 150 nm, and a reflectance ratio of light incident on each of the first region I and the second region II of the substrate 100 is periodically changed.
[0140] For example, if the first thickness T1 is about 100 nm, the reflectance ratios of light incident on the first region I and the second region II of the substrate 100 are about 0.42 and 0.35, respectively, and thus the reflectance ratio of the second region II of the substrate 100 is less than the reflectance ratio of the first region I of the substrate 100. If the first thickness T1 is about 125 nm, the reflectance ratios of light incident on the first region I and the second region II of the substrate 100 are about 0.44 and 0.49, respectively, and thus the reflectance ratio of the second region II of the substrate 100 is greater than the reflectance ratio of the first region I of the substrate 100.
[0141] That is, the first thickness T1 of the preliminary lower contact plug layer 470 can be adjusted so that the reflectance ratio of light incident on the first region I and the second region II of the substrate 100 can be adjusted, and for example, if the first thickness T1 is about 70 nm or about 125 nm, the difference between the reflectance ratio of light incident on the second region II of the substrate 100 and the reflectance ratio of light incident on the first region I of the substrate 100 is maximized.
[0142] If, during the MLA process, the reflectance ratio of light incident on the second region II of the substrate 100 is less than the reflectance ratio of light incident on the first region I of the substrate 100, even if the same amount of energy is transferred by light to the first region I and the second region II of the substrate 100, the amount of energy reaching the portion of the preliminary lower contact plug layer 470 located on the second region II of the substrate 100 may be greater than the amount of energy reaching the portion of the preliminary lower contact plug layer 470 located on the first region I of the substrate 100, and thus heat transfer occurs between the portion of the preliminary lower contact plug layer 470 located on the second region II of the substrate 100 and the portion of the preliminary lower contact plug layer 470 located on the first region I of the substrate 100.
[0143] Through heat transfer, in the bit line structure 395 on the first region I of the substrate 100, the polysilicon included in the fifth conductive pattern 245 can move to the third barrier pattern 255 including metal silicon nitride and contacting the fifth conductive pattern 245, so that a gap may be formed in the fifth conductive pattern 245, which may degrade the electrical characteristics of the bit line structure 395.
[0144] However, in example embodiments, the first thickness T1 of the preliminary lower contact plug layer 470 may be adjusted to satisfy Formula 1, which means that the first thickness T1 may be within a range in which a difference between a reflectance ratio of light incident on the second region II of the substrate 100 and a reflectance ratio of light incident on the first region I of the substrate 100 is maximized. Therefore, generation of voids in the fifth conductive pattern 245 included in the bit line structure 395 may be prevented by adjusting the first thickness T1 of the preliminary lower contact plug layer 470, and degradation of electrical characteristics of the bit line structure 395 may be prevented.
[0145] Fig.45 is through Fig.24 and Fig.25 1 is a graph of a reflectance ratio of light obtained through simulation, wherein light is incident on the first region I and the second region II of the substrate 100 having the preliminary lower contact plug layer 470, the first reflective layer 700 and the second reflective layer 710, and the lower structure thereon.
[0146] The light has a wavelength of about 532 nm and is incident in a vertical direction on the upper surface of the substrate 100. In addition, the second thickness T2 of the first reflective layer 700 is about 91 nm, and the third thickness T3 and the fourth thickness T4 of portions of the second reflective layer 710 respectively located on the first region I and the second region II of the substrate 100 are about 97 nm and 60 nm, respectively.
[0147] refer to Fig.45 ,and Fig.44Similarly, as the first thickness T1 of the preliminary lower contact plug layer 470 increases from about 50 nm to about 150 nm, a reflectance ratio of light incident on each of the first and second regions I and II of the substrate 100 periodically changes.
[0148] However, with Fig.44 Differently, regardless of the variation of the first thickness T1 within the above range, the reflectance ratio of light incident on the second region II of the substrate 100 is greater than the reflectance ratio of light incident on the first region I of the substrate 100 .
[0149] For example, if the first thickness T1 is about 100 nm, the reflectance ratios of light incident on the first region I and the second region II of the substrate 100 are about 0.5 and 0.62, respectively, and if the first thickness T1 is about 125 nm, the reflectance ratios of light incident on the first region I and the second region II of the substrate 100 are about 0.53 and 0.72, respectively. Therefore, the reflectance ratio of the second region II of the substrate 100 is greater than the reflectance ratio of the first region I of the substrate 100.
[0150] and Fig.44 Similarly, for example, if the first thickness T1 is about 70 nm or about 125 nm, a difference between a reflectance ratio of light incident on the second region II of the substrate 100 and a reflectance ratio of light incident on the first region I of the substrate 100 is maximized.
[0151] Figure 46 to Figure 48 is a graph showing the reflectance ratio of light obtained by simulation according to Comparative Example 1, Comparative Example 2 and Comparative Example 3, wherein the light is incident on the first region I and the second region II of the substrate 100 having the preliminary lower contact plug layer 470, the reflective layer structure and the lower layer structure thereon.
[0152] In Comparative Example 1, a reflective layer structure is not formed on the preliminary contact plug layer 470, in Comparative Example 2, a reflective layer structure is formed only on a portion of the preliminary lower contact plug layer 470 located on the second region II of the substrate 100, and in Comparative Example 3, a reflective layer structure is formed on both portions of the preliminary lower contact plug layer 470 located on the first region I and the second region II of the substrate 100.
[0153] A first thickness T1 of the preliminary lower contact plug layer 470 is about 100 nm, a second thickness T2 of the first reflective layer 700 included in the reflective layer structure is about 91 nm, a third thickness T3 of a portion of the second reflective layer 710 included in the reflective layer structure located on the first region I of the substrate 100 is about 97 nm, and a fourth thickness T4 of a portion of the second reflective layer 710 included in the reflective layer structure located on the second region II of the substrate 100 is about 60 nm.
[0154] refer to Figure 46 to Figure 48 In Comparative Example 1, the reflectance ratios of light respectively incident on the first region I and the second region II of the substrate 100 are approximately 0.42 and 0.35, respectively, in Comparative Example 2, the reflectance ratios of light respectively incident on the first region I and the second region II of the substrate 100 are approximately 0.42 and 0.62, respectively, and in Comparative Example 3, the reflectance ratios of light respectively incident on the first region I and the second region II of the substrate 100 are approximately 0.49 and 0.58, respectively.
[0155] That is, in Comparative Example 1, the reflectance ratio of the second region II of the substrate 100 is less than the reflectance ratio of the first region I of the substrate 100, while in Comparative Example 2 and Comparative Example 3, the reflectance ratio of the second region II of the substrate 100 is greater than the reflectance ratio of the first region I of the substrate 100. In Comparative Example 2, the difference (i.e., amplitude) between the maximum value and the minimum value of the reflectance ratio of the first region I of the substrate 100 is about 2.0%, while in Comparative Example 3, the amplitude of the reflectance ratio of the first region I of the substrate 100 is about 0.04%. That is, in both Comparative Example 2 and Comparative Example 3, the reflectance ratio of the second region II of the substrate 100 is greater than the reflectance ratio of the first region I of the substrate 100, and the distribution of the reflectance ratio in Comparative Example 3 is smaller than that in Comparative Example 2.
[0156] Table 1 shows the reflectance ratio, incident energy, and conversion energy of light obtained by simulation according to Comparative Example 4, Comparative Example 5, and the example embodiment, wherein the light is incident on the first region I and the second region II of the substrate 100 having the preliminary lower contact plug layer 470, the reflective layer structure, and the lower layer structure thereon.
[0157] The first thickness T1 of the preliminary lower contact plug layer 470 on the upper surface of the capping layer 380 on the second region II of the substrate 100 is about 100 nm in Comparative Embodiment 4 and Comparative Embodiment 5, and is about 125 nm in the example embodiment. The thickness from the lower surface of the preliminary lower contact plug layer 470 located on the first region I of the substrate 100 is about 243 nm in Comparative Embodiment 4 and Comparative Embodiment 5, and is about 268 nm in the example embodiment.
[0158] In Comparative Example 4, a reflective layer structure including the first reflective layer 700 and the second reflective layer 710 is formed only on the second region II of the substrate 100, and in Comparative Example 5 and the example embodiments, a reflective layer structure including the first reflective layer 700 and the second reflective layer 710 is formed on both the first region I and the second region II of the substrate 100.
[0159] In Comparative Example 4, the first reflective layer 700 having the second thickness T2 of about 91 nm and the second reflective layer 710 having the fourth thickness T4 of about 60 nm are stacked on the upper surface of the portion of the preliminary lower contact plug layer 470 located on the second region II of the substrate 100. In Comparative Example 5 and the example embodiments, the first reflective layer 700 having the second thickness T2 of about 91 nm is formed on the upper surface of the preliminary lower contact plug layer 470 located on the first region I and the second region II of the substrate 100, and the second reflective layer 710 having the third thickness T3 of about 97 nm on the first region I of the substrate 100 and the fourth thickness T4 of about 60 nm on the second region II of the substrate 100 is formed.
[0160] [Table 1]
[0161]
[0162] Referring to Table 1, in Comparative Example 4, the transition energy required to recrystallize the preliminary lower contact plug layer 470 after melting the preliminary lower contact plug layer 470 by the MLA process on the first region I of the substrate 100 is in the range of about 320 mJ to about 354 mJ. If the transition energy is less than about 320 mJ, the preliminary lower contact plug layer 470 cannot be sufficiently melted and cannot be recrystallized, and if the transition energy is greater than about 354 mJ, a void may be generated in the fifth conductive pattern 245 due to overheating. The reflectivity of the first region I of the substrate 100 is about 0.42, and thus the transition ratio is about 0.58. Accordingly, the incident energy required to be incident on the first region I of the substrate 100 is in the range of about 551 mJ to about 611 mJ, and thus there is an energy margin of about 60 mJ.
[0163] In Comparative Example 5, the reflectance ratio of the first region I of the substrate 100 is about 0.53, and thus the conversion ratio is about 0.47. Therefore, considering that the conversion energy is in the range of about 320 mJ to about 354 mJ, the incident energy required to be incident on the first region I of the substrate 100 is in the range of about 680 mJ to about 754 mJ, and thus there is an energy margin of about 74 mJ.
[0164] In the example embodiment, the thickness of the preliminary lower contact plug layer 470 on the first region I of the substrate 100 is about 268 nm, which is 1.1 times the thickness (i.e., 243 nm) of the preliminary lower contact plug layer 470 on the first region I of the substrate 100 of Comparative Example 5. Accordingly, the transition energy is in the range of about 352 mJ to about 391 mJ, and the incident energy required to be incident on the first region I of the substrate 100 is in the range of about 750 mJ to about 831 mJ. Therefore, the energy margin is about 81 mJ.
[0165] Therefore, the energy margin for performing the MLA process of the example embodiment is greater than the energy margin for performing the MLA process of Comparative Examples 4 and 5. Specifically, the energy margin of the example embodiment is greater than that of Comparative Example 4 by about 21 mJ.
[0166] Table 2 shows distribution of a reflectance ratio of light incident on a portion of the first region I of the substrate 100 adjacent to the second region II of the substrate 100 when light is incident on the substrate 100 having the reflective layer structure of the example embodiment according to a change in a second distance S2 from an end of a portion of the second reflective layer 710 having the third thickness T3 in the second direction D2 to a boundary of the first region I of the substrate 100 in the second direction D2.
[0167] [Table 2]
[0168] S2(nm) Reflectance ratio distribution -200 0.056 -100 0.0537 0 0.0327 100 0.0166 200 0.025 300 0.019 400 0.017 500 0.0239
[0169] Referring to Table 2, when the end of the portion of the second reflective layer 710 having the third thickness T3 in the second direction D2 is spaced apart from the boundary of the first region I of the substrate 100 in the second direction D2 by about 500 nm, the reflectance distribution is equal to or less than about 5.6%.
[0170] Specifically, when the end of the portion of the second reflective layer 710 having the third thickness T3 in the second direction D2 is spaced apart from the boundary of the first region I of the substrate 100 in the second direction D2 by about 400 nm, the reflectance ratio distribution is equal to or less than about 2%.
[0171] Therefore, in example embodiments, the second distance S2 is equal to or less than about 500 nm, preferably, in the range of about 300 nm to about 400 nm. Since the reflectance ratio distribution of the portion of the first region I of the substrate 100 adjacent to the second region II of the substrate 100 is so low, the MLA process can be stably performed.
[0172] In a method of manufacturing a semiconductor device according to example embodiments, after forming a reflective layer structure on the preliminary lower contact plug layer 470 , an MLA process may be performed so that the preliminary lower contact plug layer 470 including amorphous silicon may be converted into a lower contact plug 472 including polysilicon.
[0173] The reflectivity of a portion of the reflective layer structure located on the second region II of the substrate 100 may not be greater than the reflectivity of a portion of the reflective layer structure located on the first region I of the substrate 100, and thus no voids are generated by the following phenomenon: silicon included in the fifth conductive pattern 245 of the bit line structure 395 on the first region I of the substrate 100 moves to the third barrier pattern 255 by heat transfer from the second region II of the substrate 100 to the first region I of the substrate 100.
[0174] The preliminary lower contact plug layer 470 under the reflective layer structure may have a first thickness T1 satisfying Formula 1, and the first reflective layer 700 and the second reflective layer 710 included in the reflective layer structure may have second to fourth thicknesses T2, T3 and T4 satisfying Formulas 2 to 4, so that the reflective layer structure may have a desired reflectance ratio.
[0175] In addition, since the preliminary lower contact plug layer 470 and the first and second reflective layers 700 and 710 have appropriate thicknesses, the incident energy that may be incident on the preliminary lower contact plug layer 470 may have an increased margin, by which the preliminary lower contact plug layer 470 including amorphous silicon may be melted into the lower contact plug layer 472 including polycrystalline silicon. Since the incident energy margin is reduced according to the high integration of the semiconductor device, the MLA process may not be easily performed. However, in example embodiments, the MLA process may have an increased process margin by forming a reflective layer structure, and thus may be easily performed.
[0176] Fig.49 and Fig.50 are cross-sectional views showing a method of manufacturing a semiconductor device according to example embodiments, which respectively correspond to Fig.26 and Fig. 27 .
[0177] The method may include reference to Figures 1 to 43 The processes shown are basically the same or similar processes, so their repeated description is omitted herein.
[0178] refer to Fig.49 and Fig.50 , can be executed with reference Fig.24 and Fig.25 The processes shown are substantially the same or similar processes to form the preliminary lower contact plug layer 470 and the first and second reflective layers 700 and 710 .
[0179] The first reflective layer 700 and the second reflective layer 710 may have a second thickness T2 and a fourth thickness T4. The upper portion of the portion of the second reflective layer 710 located on the first region I of the substrate 100 may be removed by an etching process, so the third thickness T3 of the portion of the second reflective layer 710 located on the first region I of the substrate 100 may be less than the fourth thickness T4.
[0180] Can be executed and referenced Fig.26 and Fig. 27 The process shown is substantially the same as or similar to the process shown, so that the preliminary lower contact plug layer 470 can be converted into the lower contact plug layer 472 by the MLA process, and the same as the reference numeral 470 can be performed. Figure 28 to Figure 43 The processes shown are basically the same or similar processes to complete the manufacture of the semiconductor device.
[0181] As shown above, if only the third thickness T3 of the portion of the second reflective layer 710 located on the first region I of the substrate 100 satisfies Formula 3 or Formula 4, the third thickness T3 may not be greater than the fourth thickness T4 and may be less than the fourth thickness T4. In this case, after forming the first reflective layer 700 and the second reflective layer 710, instead of removing the upper portion of the portion of the second reflective layer 710 located on the second region II of the substrate 100, the portion of the second reflective layer 710 located on the first region I of the substrate 100 may be removed to form a reflective layer structure.
[0182] One or more elements disclosed above may include or be implemented in a processing circuit, which may include, for example, hardware of a logic circuit; a hardware / software combination such as a processor that executes software; or a combination thereof. For example, the processing circuit may more specifically include, but is not limited to, a central processing unit (CPU), an arithmetic logic unit (ALU), a digital signal processor, a microcomputer, a field programmable gate array (FPGA), a system on a chip (SoC), a programmable logic unit, a microprocessor, an application specific integrated circuit (ASIC), etc.
[0183] While the inventive concept has been shown and described with reference to example embodiments thereof, it will be understood by those skilled in the art that various changes in form and details may be made without departing from the spirit and scope of the inventive concept as defined by the following claims.
Claims
1. A method for manufacturing a semiconductor device, the method include: forming a first gate structure on a first region of a substrate, the substrate comprising the first region and a second region; forming a bit line structure on the first gate structure; forming a preliminary contact plug layer including amorphous silicon on the substrate; forming a reflective layer structure on the preliminary contact plug layer, the reflective layer structure comprising a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, the second refractive index being greater than the first refractive index, and a thickness of a portion of the second reflective layer located on the first region of the substrate being different from a thickness of a portion of the second reflective layer located on the second region of the substrate; Forming a contact plug layer from the preliminary contact plug layer, wherein the forming of the contact plug layer includes performing a melt laser annealing (MLA) process of irradiating laser on the reflective layer structure so that the amorphous silicon of the preliminary contact plug layer is converted into polysilicon; and A capacitor is formed on the contact plug layer.
2. The method according to claim 1, in, A thickness of a portion of the second reflective layer located on the first region of the substrate is greater than a thickness of a portion of the second reflective layer located on the second region of the substrate.
3. The method according to claim 1, in, The thickness of the second reflective layer located on the second region of the substrate and adjacent to the first region of the substrate is equal to the thickness of the second reflective layer located on the first region of the substrate, and An end of the portion of the second reflective layer is above a portion of the substrate, and the portion of the substrate is spaced apart from a boundary between the first region of the substrate and the second region of the substrate by a distance equal to or less than 500 nm.
4. The method according to claim 3, in, The portion of the substrate is spaced apart from the boundary between the first region of the substrate and the second region of the substrate by a distance in a range of 300 nm to 400 nm.
5. The method according to claim 1, in, A thickness of a portion of the second reflective layer located on the first region of the substrate is smaller than a thickness of a portion of the second reflective layer located on the second region of the substrate.
6. The method according to claim 1, in, The first reflective layer has a first thickness denoted by T1, The thickness of a portion of the second reflective layer located on the first region of the substrate is a second thickness denoted by T2, The thickness of the portion of the second reflective layer located on the second region of the substrate is a third thickness denoted by T3, The first thickness, the second thickness and the third thickness satisfy the following equations 1, 2 and 3 respectively: T1 = (1 / 4 + Δ 1 )λ / n 1 Equation 1 T2=(1 / 4+Δ) 2 )λ / n 2 formula 2 T3 = (1 / 4 + Δ 3 )λ / n 2 Equation 3 Among them, in equations 1 to 3, Δ 1 , Δ 2 , Δ 3 are the first optical path correction factor, the second optical path correction factor and the third optical path correction factor, respectively. λ is the wavelength of the laser, n 1 is the first refractive index of the first reflecting layer, n 2 is the second refractive index of the second reflecting layer, -1 / 8≤Δ 1 ≤1 / 8, -1 / 4≤Δ 2 ≤1 / 4, and -1 / 8≤Δ 2 ≤1 / 8。 7. The method according to claim 6, in, The first thickness, the second thickness, and the third thickness have values of about 91 nm, about 97 nm, and about 60 nm, respectively.
8. The method according to claim 6, in, The second thickness has a value in the range of 24 nm to 218 nm.
9. The method according to claim 8, in, The second thickness has a value in the range of 87 nm to 107 nm.
10. The method according to claim 1, further comprising: include: forming a second gate structure on the second region of the substrate; as well as forming a capping layer on the second gate structure, wherein the capping layer comprises silicon nitride, wherein the preliminary contact plug layer has a first thickness indicated by T1 from the upper surface of the capping layer, and The first thickness T1 satisfies the following formula 1: (N / 2+1 / 8+Δ)λ / n 1 +d 1 ≤T1≤(N / 2+3 / 8+Δ)λ / n 1 +d 2 formula 1 Among them, in formula 1, N is 1, 2, or 3, Δ is the optical path correction factor, λ is the wavelength of the laser, n 1 is the refractive index of the preliminary contact plug layer, -8nm≤δ 1 ≤8nm, -8nm≤δ 2 ≤8nm, and -1 / 4≤Δ≤1 / 4.
11. The method according to claim 10, in, The first thickness is in the range of 89 nm to 133 nm.
12. A method for manufacturing a semiconductor device, the method include: forming a first gate structure on a cell region of a substrate, wherein the substrate includes the cell region and a peripheral circuit region; forming a bit line structure on the first gate structure; forming a preliminary contact plug layer including amorphous silicon on the substrate; forming a reflective layer structure on the preliminary contact plug layer, wherein the reflective layer structure includes a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, wherein the second refractive index is greater than the first refractive index; Forming a contact plug layer from the preliminary contact plug layer, wherein the forming of the contact plug layer includes performing a melt laser annealing (MLA) process of irradiating laser on the reflective layer structure so that the amorphous silicon of the preliminary contact plug layer is converted into polysilicon; and forming a capacitor on the contact plug layer, The reflectance ratio of light in the peripheral circuit area of the substrate is greater than the reflectance ratio of light in the unit area of the substrate.
13. The method according to claim 12, in, A thickness of a portion of the second reflective layer located on the cell region of the substrate is different from a thickness of a portion of the second reflective layer located on the peripheral circuit region of the substrate.
14. The method according to claim 12, in, The thickness of the second reflective layer located on the peripheral circuit region of the substrate and adjacent to the cell region of the substrate is equal to the thickness of the second reflective layer located on the cell region of the substrate, and An end of the portion of the second reflective layer is above a portion of the substrate, and the portion of the substrate is spaced apart from a boundary between the cell region and the peripheral circuit region of the substrate by a distance equal to or less than 500 nm.
15. The method according to claim 12, further comprising: include: forming a second gate structure on the peripheral circuit region of the substrate; as well as forming a capping layer on the second gate structure, wherein the capping layer comprises silicon nitride, wherein the preliminary contact plug layer has a first thickness indicated by T1 from the upper surface of the capping layer, and The first thickness T1 satisfies the following formula 1: (N / 2+1 / 8+Δ)λ / n 1 +d 1 ≤T1≤(N / 2+3 / 8+Δ)λ / n 1 +d 2 formula 1 Among them, in formula 1, Δ is the optical path correction factor, λ is the wavelength of the laser, n 1 is the refractive index of the preliminary contact plug layer, -8nm≤δ 1 ≤8nm, -8nm≤δ 2 ≤8nm, and -1 / 4≤Δ≤1 / 4.
16. The method according to claim 15, in, The first reflective layer has a second thickness denoted by T2, The portion of the second reflective layer located on the cell region of the substrate has a third thickness denoted by T3, A portion of the second reflective layer located on the peripheral circuit region has a fourth thickness denoted by T4, and The second thickness to the fourth thickness satisfy the following formula 2, formula 3 and formula 4: T2=(1 / 4+Δ) 2 )λ / n 2 formula 2 T3 = (1 / 4 + Δ 3 )λ / n 3 Equation 3 T4 = (1 / 4 + Δ 4 )λ / n 3 Equation 4 Among them, in Formula 2 to Formula 4, λ is the wavelength of the laser, n 2 is the first refractive index of the first reflecting layer, n 3 is the second refractive index of the second reflecting layer, -1 / 8≤Δ 2 ≤1 / 8, -1 / 4≤Δ 3 ≤1 / 4, and -1 / 8≤Δ 4 ≤1 / 8。 17. A method for manufacturing a semiconductor device, the method include: forming a first gate structure on a cell region of a substrate, wherein the substrate includes the cell region and a peripheral circuit region; forming a bit line structure and a second gate structure on the cell region and the peripheral circuit region of the substrate respectively; forming a preliminary contact plug layer including amorphous silicon on the substrate to cover the bit line structure and the second gate structure; forming a reflective layer structure on the preliminary contact plug layer, the reflective layer structure comprising a first reflective layer having a first refractive index and a second reflective layer having a second refractive index, the second refractive index being greater than the first refractive index, and a thickness of a portion of the second reflective layer located on the cell region of the substrate being different from a thickness of a portion of the second reflective layer located on the peripheral circuit region of the substrate; performing a molten laser annealing (MLA) process, the MLA process comprising irradiating a laser on the reflective layer structure so that the preliminary contact plug layer is converted into a contact plug layer including polysilicon; planarizing the contact plug layer to form a lower contact plug; forming an upper contact plug on the lower contact plug; as well as A capacitor is formed on the upper contact plug.
18. The method according to claim 17, further comprising: include: removing an upper portion of the substrate to form an active pattern, wherein the first gate structure extends through an upper portion of the active pattern, The bit line structure is on a central portion of the active pattern, and The lower contact plug is on an end portion of the active pattern.
19. The method according to claim 17, in, A thickness of a portion of the second reflective layer located on the cell region of the substrate is greater than a thickness of a portion of the second reflective layer located on the peripheral circuit region of the substrate.
20. The method according to claim 17, in, The first gate structure extends in a first direction, The bit line structure extends in a second direction, The first direction and the second direction are parallel to the upper surface of the substrate, The second direction is perpendicular to the first direction, The thickness of the second reflective layer located on the peripheral circuit region of the substrate and adjacent to the unit region of the substrate in the second direction is equal to the thickness of the second reflective layer located on the unit region of the substrate, and An end of the portion of the second reflective layer is above a portion of the substrate, and the portion of the substrate is spaced apart from a boundary between the cell region of the substrate and the peripheral circuit region of the substrate by a distance equal to or less than 500 nm.