Perovskite / crystalline silicon laminated cell and preparation method thereof

By using metal silicide as the intermediate series layer in perovskite/crystalline silicon stacked batteries, the problems of high series resistance and parasitic light absorption in the prior art are solved, the efficiency and short-circuit current of the battery are improved, the process is simplified and the process is reduced. The cost.

CN118946178APending Publication Date: 2024-11-12CHUZHOU JIETAI NEW ENERGY TECH CO LTD

Patent Information

Application Number
CN202411163118.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The middle series layer of the existing perovskite/crystalline silicon stacked battery has high series resistance and parasitic light absorption problems, resulting in carriers being easily passed through leakage points, short-circuit failure of the top battery, and low efficiency.

Method used

The metal silicide is used as the intermediate series layer between the second doped amorphous silicon film layer of the bottom battery and the first carrier transport layer of the top battery to replace the existing TCO composite layer or n+p+ tunneling composite layer, reducing the Series resistors and reduce parasitic light absorption.

Benefits of technology

It effectively reduces the series resistance, improves the battery filling factor (FF) and short-circuit current, simplifies the process and reduces manufacturing costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946178A_ABST
    Figure CN118946178A_ABST
Patent Text Reader

Abstract

The invention discloses a perovskite / crystalline silicon laminated cell and a preparation method thereof, and belongs to the field of perovskite / crystalline silicon lamination, the perovskite / crystalline silicon laminated cell comprises a bottom cell and a top cell, the bottom cell takes a crystalline silicon wafer as a substrate, and an intrinsic amorphous silicon film layer, a first doped amorphous silicon film layer, a transparent conductive oxide film layer and a metal conductive film layer are sequentially arranged on the back surface of the bottom cell; an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer are sequentially arranged on the front side; the top cell takes perovskite as a light absorption layer, a first carrier transport layer is arranged on the back surface, and a second carrier transport layer, a transparent conductive oxide film layer and a metal grid line electrode are sequentially arranged on the front surface; the second doped amorphous silicon film layer of the bottom cell and the first carrier transport layer of the top cell are connected by adopting metal silicide as an intermediate series layer, and the metal silicide replaces an existing TCO composite layer or an n + p + tunneling composite layer, so that the series resistance can be reduced, and the FF of the cell can be improved; parasitic light absorption can be reduced, and cell short-circuit current can be improved; the process is simple and easy to implement, and the manufacturing cost can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of perovskite / crystalline silicon stacking, and in particular to a perovskite / crystalline silicon stacking cell and a preparation method thereof. Background Art

[0002] The highest laboratory conversion efficiency of single-crystal silicon cells has reached 27.09%, close to the theoretical limit of 29.4%, and there is little room for efficiency improvement in the future. In order to break through the efficiency ceiling, perovskite / crystalline silicon tandem cells have become one of the new directions for photovoltaic technology transformation. The theoretical conversion efficiency of perovskite / crystalline silicon tandem cells formed by stacking crystalline silicon cells and perovskite cells is 43%, and the current highest laboratory conversion efficiency has reached 33.9%. Both the theoretical efficiency and laboratory efficiency of perovskite / crystalline silicon tandem cells are significantly higher than those of single-crystal silicon cells.

[0003] The stacked cell can be obtained by sequentially preparing an intermediate series layer and a top cell on a bottom cell, wherein the intermediate series layer can exchange carriers between the top and bottom cells. Therefore, its photoelectric performance will directly affect the photoelectric conversion efficiency of the stacked cell.

[0004] Existing perovskite / crystalline silicon tandem cells usually use a TCO composite junction as the intermediate series layer. Since the TCO film has strong parasitic light absorption, it reduces the short-circuit current of the bottom cell and causes current mismatch between the top and bottom cells. The excellent lateral conductivity of the TCO film makes it easy for carriers to pass through the leakage point, causing the top cell to short-circuit and fail. Another method uses an n+ / +p-type silicon-based tunneling composite junction as the intermediate series layer. Due to process conditions, the tunneling barrier of the n / p-type silicon-based tunneling junction is relatively high, which makes the probability of carrier tunneling low, resulting in high resistance loss at the tunneling junction in the solar cell. In addition, the n+ / +p-type silicon-based tunneling composite junction has a high doping concentration, which also leads to higher parasitic optical absorption, reducing the short-circuit current of the bottom cell and causing current loss in the tandem cell.

[0005] In view of this, the inventor conducted in-depth research on this demand, and thus the present case was produced. Summary of the invention

[0006] In view of the series of problems existing in the middle series layer of perovskite / crystalline silicon tandem cells in the prior art, the present invention provides a perovskite / crystalline silicon tandem cell, which uses metal silicide as the middle series layer connection between the second doped amorphous silicon film layer of the bottom cell and the first carrier transport layer of the top cell, replacing the existing TCO composite layer or n+p+ tunneling composite layer, reducing the series resistance and improving the battery FF; at the same time, it reduces parasitic light absorption and improves the battery short-circuit current. The specific technical solution is as follows:

[0007] A perovskite / crystalline silicon stacked cell, comprising a bottom cell and a top cell,

[0008] The bottom cell is based on a crystalline silicon wafer, with an intrinsic amorphous silicon film layer, a first doped amorphous silicon film layer, a transparent conductive oxide film layer and a metal conductive film layer sequentially arranged on the back, and an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer sequentially arranged on the front;

[0009] The top cell uses a perovskite light-absorbing layer as the light-absorbing layer, a first carrier transport layer is arranged on the back, and a second carrier transport layer, a transparent conductive oxide film layer and a metal grid electrode are arranged in sequence on the front;

[0010] The second doped amorphous silicon film layer of the bottom cell and the first carrier transport layer of the top cell are connected via metal silicide as an intermediate series connection layer.

[0011] Preferably, the metal silicide includes at least one of Ni, V, Mo, W, Cu, Sn, Ti, Zn, Nb, and Zr silicides, and has a thickness of 0.2-2.0 nm.

[0012] Here, the crystalline silicon wafer may be a Czochralski single crystal silicon wafer, a cast single crystal silicon wafer or a polycrystalline silicon wafer, may be N-type doped or P-type doped, have a resistivity of 0.1-10.0 Ωcm, and a thickness of 50-500 um.

[0013] Preferably, the intrinsic amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, and a-SiCx:H, and has a thickness of 4-8 nm.

[0014] Preferably, the metal conductive film layer includes at least one of Ag, Al, Ni, Cu, and Fe, and has a thickness of 100-1000 nm.

[0015] Preferably, the first doped amorphous silicon film layer comprises at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, uc-SiCx:H, and has a thickness of 5-20 nm;

[0016] The second doped amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm.

[0017] Preferably, the first doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 The second doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3; The conductivity type of the second doped amorphous silicon film layer is opposite to that of the first doped amorphous silicon film layer.

[0018] Preferably, the first carrier transport layer comprises a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped amorphous silicon film layer have the same conductivity type;

[0019] The second carrier transport layer includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has a conductivity type opposite to that of the first carrier transport layer and the same conductivity type as the second doped amorphous silicon film layer.

[0020] Preferably, the first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types;

[0021] The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50nm; the inorganic electron transport layer includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0nm.

[0022] Preferably, the first organic carrier transport layer comprises an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer comprises an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types;

[0023] The organic hole transport layer includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, and has a thickness of 0.5-50.0 nm;

[0024] The organic electron transport layer includes at least one of fullerene C60, fullerene C70, and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

[0025] Preferably, the transparent conductive oxide film layer includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, and has a thickness of 60-150 nm.

[0026] Preferably, the general formula of the perovskite light-absorbing layer is ABX3, wherein A is a monovalent cation, and A includes but is not limited to at least one of lithium, sodium, potassium, cesium, amine and amidine, wherein B is a divalent cation, and B includes but is not limited to at least one of lead and tin; X is a monovalent anion, and X includes but is not limited to at least one of iodine, bromine and chlorine; the thickness of the perovskite light-absorbing layer is 500-1500nm.

[0027] Preferably, the metal gate line electrode is at least one of Ag, Al, Ni, Cu, and Fe, with a gate line thickness of 0.1-20 um and a spacing of 0.5-5.0 mm.

[0028] The present invention also provides a method for preparing the above-mentioned perovskite / crystalline silicon tandem battery, comprising the following steps:

[0029] S1, cleaning the surface of silicon wafer;

[0030] S2, depositing an intrinsic amorphous silicon film layer and a first doped amorphous silicon film layer on the back side of the silicon wafer, and depositing an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer on the front side of the silicon wafer;

[0031] S3, depositing a transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped amorphous silicon film layer on the back side; depositing an ultra-thin metal silicide film layer and a first inorganic carrier transport layer on the surface of the second doped amorphous silicon film layer on the front side;

[0032] S4, forming a first organic carrier transport layer and a perovskite light absorption layer on the surface of the first inorganic carrier transport layer;

[0033] S5, forming a second organic carrier transport layer on the surface of the perovskite light absorbing layer;

[0034] S6, forming a second inorganic carrier transport layer on the surface of the second organic carrier transport layer;

[0035] S7, forming a transparent conductive oxide film layer on the surface of the second inorganic carrier transport layer;

[0036] S8. Form a front gate line electrode on the surface of the transparent conductive oxide film layer.

[0037] The beneficial effects produced by the technical solution of the present invention are as follows: metal silicide is used as an intermediate series layer between the second doped amorphous silicon film layer of the bottom battery and the first carrier transport layer of the top battery to replace the existing TCO composite layer or n+p+ tunneling composite layer, which can reduce the series resistance and improve the battery FF; it can reduce parasitic light absorption and improve the battery short-circuit current; the process is simple and easy to implement, which can reduce the manufacturing cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 It is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in the present invention;

[0040] Figure 2 It is a process flow chart of the preparation of the perovskite / crystalline silicon tandem battery in the present invention;

[0041] Figure 3 is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Example 1 of the present invention;

[0042] Figure 4 is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Example 2 of the present invention;

[0043] Figure 5 It is a schematic diagram of the layer structure of the perovskite / crystalline silicon tandem battery in Comparative Example 1 of the present invention.

[0044] In the figure: 1. bottom cell; 11. crystalline silicon wafer; 12. intrinsic amorphous silicon film layer; 13. first doped amorphous silicon film layer; 14. transparent conductive oxide film layer; 15. metal conductive film layer; 16. second doped amorphous silicon film layer; 2. top cell; 21. perovskite light absorption layer; 22. first carrier transport layer; 23. second carrier transport layer; 24. metal gate electrode. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the claimed invention, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] like Figure 1 As shown, a perovskite / crystalline silicon stacked cell includes a bottom cell 1 and a top cell 2.

[0047] The bottom cell 1 is based on a crystalline silicon wafer 11, and an intrinsic amorphous silicon film layer 12, a first doped amorphous silicon film layer 13, a transparent conductive oxide film layer 14 and a metal conductive film layer 15 are sequentially arranged on the back side, and an intrinsic amorphous silicon film layer 12 and a second doped amorphous silicon film layer 16 are sequentially arranged on the front side;

[0048] The top cell 2 has a perovskite light absorption layer 21 as a light absorption layer, a first carrier transport layer 22 is arranged on the back, and a second carrier transport layer 23, a transparent conductive oxide film layer 14 and a metal grid electrode 24 are arranged in sequence on the front;

[0049] The second doped amorphous silicon film layer 16 of the bottom cell 1 and the first carrier transport layer 22 of the top cell 2 are connected via the metal silicide 3 as an intermediate series layer.

[0050] As a preferred embodiment, the metal silicide includes at least one of Ni, V, Mo, W, Cu, Sn, Ti, Zn, Nb, and Zr silicides, and has a thickness of 0.2-2.0 nm.

[0051] Here, the crystalline silicon wafer may be a Czochralski single crystal silicon wafer, a cast single crystal silicon wafer or a polycrystalline silicon wafer, may be N-type doped or P-type doped, have a resistivity of 0.1-10.0 Ωcm, and a thickness of 50-500 um.

[0052] As a preferred implementation, the intrinsic amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, and a-SiCx:H, and has a thickness of 4-8 nm.

[0053] As a preferred implementation, the metal conductive film layer includes at least one of Ag, Al, Ni, Cu, and Fe, and has a thickness of 100-1000 nm.

[0054] As a preferred embodiment, the first doped amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm;

[0055] The second doped amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm.

[0056] As a preferred embodiment, the first doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 The second doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 1017 -10 20 cm -3 ; The conductivity type of the second doped amorphous silicon film layer is opposite to that of the first doped amorphous silicon film layer.

[0057] As a preferred embodiment, the first carrier transport layer includes a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped amorphous silicon film layer have the same conductivity type;

[0058] The second carrier transport layer includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has a conductivity type opposite to that of the first carrier transport layer and the same as that of the second doped amorphous silicon film layer.

[0059] As a preferred embodiment, the first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types;

[0060] The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50 nm; the inorganic electron transport layer includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0 nm.

[0061] As a preferred embodiment, the first organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types;

[0062] The organic hole transport layer includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, and has a thickness of 0.5-50.0 nm;

[0063] The organic electron transport layer comprises at least one of fullerene C60, fullerene C70 and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

[0064] As a preferred embodiment, the transparent conductive oxide film layer includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, and has a thickness of 60-150 nm.

[0065] As a preferred embodiment, the general formula of the perovskite light-absorbing layer is ABX3, wherein A is a monovalent cation, and A includes but is not limited to at least one of lithium, sodium, potassium, cesium, amine and amidine, wherein B is a divalent cation, and B includes but is not limited to at least one of lead and tin; X is a monovalent anion, and X includes but is not limited to at least one of iodine, bromine and chlorine; the thickness of the perovskite light-absorbing layer is 500-1500nm.

[0066] As a preferred implementation, the metal gate line electrode is at least one of Ag, Al, Ni, Cu, and Fe, the gate line thickness is 0.1-20 um, and the spacing is 0.5-5.0 mm.

[0067] like Figure 2 As shown, this embodiment also provides a method for preparing the above-mentioned perovskite / crystalline silicon stacked cell, comprising the following steps:

[0068] S1, using wet chemical method to clean the surface of silicon wafer;

[0069] S2, using a PECVD or Cat-CVD process to deposit an intrinsic amorphous silicon film layer and a first doped amorphous silicon film layer on the back side of the silicon wafer, and to deposit an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer on the front side of the silicon wafer;

[0070] S3, using magnetron sputtering, RPD, evaporation or ALD process, depositing a transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped amorphous silicon film layer on the back side; depositing an ultra-thin metal silicide film layer and a first inorganic carrier transport layer on the surface of the second doped amorphous silicon film layer on the front side;

[0071] S4, forming a first organic carrier transport layer and a perovskite light absorption layer on the surface of the first inorganic carrier transport layer by spin coating, slit coating, blade coating or evaporation;

[0072] S5, forming a second organic carrier transport layer on the surface of the perovskite light absorbing layer by spin coating, slit coating, blade coating or evaporation process;

[0073] S6, forming a second inorganic carrier transport layer on the surface of the second organic carrier transport layer by magnetron sputtering, RPD, evaporation or ALD process;

[0074] S7, forming a transparent conductive oxide film layer on the surface of the second inorganic carrier transport layer by magnetron sputtering, RPD or evaporation process;

[0075] S8. Form a front gate line electrode on the surface of the transparent conductive oxide film layer by using a screen printing or electroplating process.

[0076] The beneficial effects of the perovskite / crystalline silicon tandem cell and its preparation process in this embodiment are further reviewed through several groups of examples.

[0077] Embodiment 1:

[0078] like Figure 3 As shown, the perovskite / crystalline silicon stacked cell in this embodiment includes, from the back to the front, an Ag conductive film layer, an ITO layer, a pa-Si:H layer, an ia-Si:H layer, an n-CZ Si layer, an ia-Si:H layer, a na-Si:H layer, a NiSix layer, a NiOx layer, a 2PACz layer, a PVK layer, a LiF layer, a C60 layer, a SnO2 layer, an IZO layer and an Ag gate line.

[0079] The method for preparing the perovskite / crystalline silicon tandem cell in this embodiment comprises the following steps:

[0080] S1, using a wet process to perform texturing and cleaning on the surface of an N-type silicon wafer: using acid and alkali chemicals to remove organic contamination and metal impurities on the surface of the silicon wafer, forming a surface pyramid texture on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um;

[0081] S2, using PECVD method, depositing i / p type amorphous silicon layer on the back of silicon wafer, and depositing i / n type amorphous silicon layer on the front of silicon wafer: the thickness of i layer on the back is 4-8nm, the thickness of p layer is 5-10nm, and the boron doping concentration is 0.5%; the thickness of i layer on the front is 4-8nmn, the thickness of n layer is 5-10nm, and the phosphorus doping concentration is 1%; the deposition temperature is 200℃;

[0082] S3, using PVD method, ITO / Ag is deposited on the surface of the back p amorphous silicon layer, ITO target material is 90wt% In2O3+10wt% SnO, sputtering atmosphere is 0.2% O2 / Ar, ITO thickness is 100nm, Ag target material purity is 99.99wt%, Ag thickness is 500nm; NiSix / NiOx is deposited on the front n amorphous silicon surface, NiSix sputtering deposition uses Ni2Si target material with purity of 99.99% and thickness of 1nm; NiOx uses RF sputtering process, NiO target material with purity of 99.99%, sputtering atmosphere is pure Ar, NiOx thickness is 20nm;

[0083] S4, using spin coating + drying method, deposit 2PACz and PVK layer on NiOx surface. First, use 1mg / mL 2PACz ethanol solution, spin coating at 4000 rpm for 30s, and then dry at 100℃ for 10min; the spin coating process deposits 1.7mol / LCs 0.05 FA 0.8 MA 0.15 Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500rpm, time 40s, and then drying at 100℃ / N2 for 30min, the resulting perovskite band gap width is 1.69eV;

[0084] S5, depositing LiF / C60 on the surface of the PVK layer by evaporation. 1 nm LiF is thermally evaporated on the PVK surface, and 18 nm C60 is thermally evaporated on the LiF surface;

[0085] S6, using ALD process to deposit SnO2 on the surface of C60. TDMASn and H2O are used as reaction gases, N2 is used as carrier gas, the deposition temperature is 80℃, and the thickness of SnO2 is 20nm;

[0086] S7, using PVD to deposit IZO on the surface of SnO2. The IZO target material composition is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, the IZO thickness is 100nm, the Ag target material purity is 99.99wt%, and the Ag thickness is 500nm;

[0087] S8, using printing + curing method, forming low-temperature Ag paste gate line electrodes on the IZO surface. The gate line width is 30um, the spacing is 2mm; the curing temperature is 120-130℃, and the time is 10min.

[0088] Embodiment 2:

[0089] like Figure 4 As shown, the perovskite / crystalline silicon stacked cell in this embodiment includes, from the back to the front, an Ag conductive film layer, an ITO layer, a na-Si:H layer, an ia-Si:H layer, an n-CZ Si layer, an ia-Si:H layer, a pa-Si:H layer, a NbSix layer, a NbOx layer, a PCBM layer, a PVK layer, a spiro-TTB layer, a MoOx layer, an IZO layer and an Ag gate line.

[0090] The method for preparing the perovskite / crystalline silicon tandem cell in this embodiment comprises the following steps:

[0091] S1, using a wet process to texturize and clean the surface of the N-type silicon wafer. Using acid and alkali chemicals, organic contamination and metal impurities on the surface of the silicon wafer are eliminated, and a surface pyramid texture is formed on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um;

[0092] S2, using PECVD method, depositing intrinsic amorphous silicon film layer and n-type amorphous silicon film layer on the back of silicon wafer, and depositing intrinsic amorphous silicon film layer and p-type amorphous silicon film layer on the front of silicon wafer. The intrinsic amorphous silicon film layer on the back uses SiH4 and H2 as reaction gases, the deposition temperature is 200℃, and the thickness is 5-10nm; the n-type amorphous silicon film layer is deposited at 200℃, the thickness is 5-10nm, SiH4, H2, PH3 are used as reaction gases, and the PH3 / SiH4 gas flow ratio is 1.5%; the intrinsic amorphous silicon film layer on the front uses SiH4 and H2 as reaction gases, the deposition temperature is 180℃, and the thickness is 4-8nm; the p-type amorphous silicon film layer is deposited at 180℃, the thickness is 5-10nm, SiH4, H2, B2H6 are used as reaction gases, and the B2H6 / SiH4 gas flow ratio is 1%.

[0093] S3, using PVD method, depositing ITO / Ag on the surface of the back n-type amorphous silicon film layer, ITO target material 90wt% In2O3+10wt% SnO, sputtering atmosphere 0.2% O2 / Ar, ITO thickness 100nm, Ag target material purity 99.99wt%, Ag thickness 500nm; depositing NbSix / NbOx on the front p-type amorphous silicon surface, NbSix sputtering deposition uses NbSi2 target material with a purity of 99.99% and a thickness of 1nm; NbOx uses RF sputtering process, Nb2O5 target material with a purity of 99.99%, sputtering atmosphere is pure Ar, and NbOx thickness is 15nm;

[0094] S4, using spin coating + drying method, PCBM and PVK layers are deposited on the NbOx surface. First, a 10mg / mL PCBM chlorobenzene solution is used, and the rotation speed is 3000 rpm for 60s, and then dried at 100℃ for 20min; the spin coating process is used to deposit a component of 1.7mol / LCs 0.05 FA 0.8 MA 0.15 Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500rpm, time 40s, and then drying at 100℃ / N2 for 30min, the resulting perovskite band gap width is 1.69eV;

[0095] S5, deposit spiro-TTB / MoOx on the surface of the PVK layer by evaporation. Co-evaporate F6-TCNNQ-doped spiro-TTB on the surface of the perovskite light-absorbing layer, the evaporation source temperature of spiro-TTB is controlled at 260-280°C, the evaporation source temperature of F6-TCNNQ is controlled at 160-170°C, the thickness of doped spiro-TTB is controlled at 25nm, and the doping ratio is 11wt%; then evaporate MoOx on the surface of the doped spiro-TTB, and the thickness is controlled at 3-5nm;

[0096] S6, using PVD method to deposit IZO on the surface of MoOx. The IZO target composition is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, the IZO thickness is 100nm, the Ag target purity is 99.99wt%, and the Ag thickness is 500nm;

[0097] S7, using printing + curing method, to form low-temperature Ag paste gate line electrodes on the IZO surface: gate line width 30um, spacing 2mm; curing temperature 120 ~ 130 ℃, time 10min.

[0098] Comparative Example 1:

[0099] like Figure 5 As shown, the perovskite / crystalline silicon stacked cell in this comparative example includes, from the back to the front, an Ag conductive film layer, an ITO layer, a pa-Si:H layer, an ia-Si:H layer, an n-CZ Si layer, an ia-Si:H layer, a na-Si:H layer, an ITO layer, a NiOx layer, a 2PACz layer, a PVK layer, a LiF layer, a C60 layer, a SnO2 layer, an IZO layer, and an Ag gate line;

[0100] The method for preparing the perovskite / crystalline silicon tandem cell in this embodiment comprises the following steps:

[0101] S1, using a wet process to texturize and clean the surface of the N-type silicon wafer. Using acid and alkali chemicals, organic contamination and metal impurities on the surface of the silicon wafer are eliminated, and a surface pyramid texture is formed on the surface of the single crystal silicon wafer to increase the absorption of sunlight and reduce reflection; the single crystal silicon wafer is a phosphorus-doped N-type single crystal silicon wafer with a resistivity of 1Ωcm and a thickness of 150um;

[0102] S2, using PECVD method, depositing i / p type amorphous silicon layer on the back of silicon wafer, and i / n type amorphous silicon layer on the front of silicon wafer. The thickness of i layer on the back is 4-8nm, the thickness of p layer is 5-10nm, and the boron doping concentration is 0.5%; the thickness of i layer on the front is 4-8nmn, the thickness of n layer is 5-10nm, and the phosphorus doping concentration is 1%; the deposition temperature is 200℃.

[0103] S3, using PVD method, depositing ITO / Ag on the surface of the back p amorphous silicon layer, ITO target material 90wt% In2O3+10wt% SnO, sputtering atmosphere 0.2% O2 / Ar, ITO thickness 100nm, Ag target material purity 99.99wt%, Ag thickness 500nm; depositing ITO / NiOx on the front n amorphous silicon surface, ITO target material composition 97wt% In2O3+3wt% SnO, sputtering atmosphere 0.5% O2 / Ar, front ITO thickness 20nm; NiOx adopts RF sputtering process, NiOx target material with purity of 99.99%, sputtering atmosphere is pure Ar, NiOx thickness is 20nm;

[0104] S4, using spin coating + drying method, deposit 2PACz and PVK layer on NiOx surface. First, use 1mg / mL 2PACz ethanol solution, spin coating at 4000 rpm for 30s, and then dry at 100℃ for 10min; the spin coating process deposits 1.7mol / LCs 0.05 FA 0.8 MA 0.15 Pb(I 0.755 Br 0.255 )3 DMF and DMSO mixed solution (volume ratio 4:1) perovskite precursor solution, rotation speed 3500 rpm, time 40 s, and then dried at 100 ° C / N2 conditions for 30 min, the resulting perovskite band gap width is 1.69 eV.

[0105] S5, depositing LiF / C60 on the surface of the PVK layer by evaporation, thermally evaporating 1 nm LiF on the PVK surface, and thermally evaporating 18 nm C60 on the LiF surface.

[0106] S6, using ALD process, SnO2 is deposited on the surface of C60. TDMASn and H2O are used as reaction gases, N2 is used as carrier gas, the deposition temperature is 80°C, and SnO2 with a thickness of 20nm is deposited.

[0107] S7, using PVD to deposit IZO on the surface of SnO2. The IZO target material composition is 90wt% In2O3+10wt% ZnO, the sputtering atmosphere is 0.2% O2 / Ar, the IZO thickness is 100nm, the Ag target material purity is 99.99wt%, and the Ag thickness is 500nm.

[0108] S8, using printing + curing method, forming low-temperature Ag paste gate line electrodes on the IZO surface. The gate line width is 30um, the spacing is 2mm; the curing temperature is 120-130℃, and the time is 10min.

[0109] The performance of the batteries obtained in the above two groups of embodiments and one group of comparative example was tested. The parameters of the solar cell were measured using an IV tester. The results are shown in Table 1.

[0110] Table 1 Battery performance test results in each group of examples

[0111]

[0112] As shown in Table 1, the perovskite / crystalline silicon stacked cell in Comparative Example 1 uses a TCO composite junction as the intermediate series layer. Since the TCO film has strong parasitic light absorption, the short-circuit current of the bottom cell is reduced, and the high lateral conductivity of the TCO film makes it easy for carriers to pass through the leakage point, causing the top cell to short-circuit and fail, resulting in a low parallel resistance of the cell, and ultimately a low FF.

[0113] In Example 1, an ultra-thin NiSix layer is deposited between the bottom cell na-Si:H and the top cell hole transport layer NiOx as the intermediate series layer between the top and bottom cells, replacing the TCO composite layer in the comparative example; in Example 2, an ultra-thin NbSix layer is deposited between the bottom cell pa-Si:H and the top cell electron transport layer NbOx as the intermediate series layer between the top and bottom cells; the above-mentioned metal silicide replaces the TCO composite layer in Comparative Example 1; on the one hand, the series resistance of the intermediate series layer can be reduced and the battery FF can be improved; on the other hand, the parasitic light absorption of the intermediate series layer can be reduced and the battery short-circuit current can be improved; the process is simple, easy to implement, and can reduce the manufacturing cost.

[0114] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A perovskite / crystalline silicon tandem cell, It is characterized in that Including bottom battery and top battery, The bottom cell is based on a crystalline silicon wafer, with an intrinsic amorphous silicon film layer, a first doped amorphous silicon film layer, a transparent conductive oxide film layer and a metal conductive film layer sequentially arranged on the back, and an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer sequentially arranged on the front; The top cell uses a perovskite light-absorbing layer as the light-absorbing layer, a first carrier transport layer is arranged on the back, and a second carrier transport layer, a transparent conductive oxide film layer and a metal grid electrode are arranged in sequence on the front; The second doped amorphous silicon film layer of the bottom cell and the first carrier transport layer of the top cell are connected via metal silicide as an intermediate series connection layer.

2. A perovskite / crystalline silicon tandem cell according to claim 1, It is characterized in that The metal silicide includes at least one of Ni, V, Mo, W, Cu, Sn, Ti, Zn, Nb, and Zr silicides, and has a thickness of 0.2-2.0 nm.

3. A perovskite / crystalline silicon tandem cell according to claim 1, It is characterized in that The first doped amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm; The second doped amorphous silicon film layer includes at least one of a-Si:H, a-SiOx:H, a-SiCx:H, uc-Si:H, uc-SiOx:H, and uc-SiCx:H, and has a thickness of 5-20 nm.

4. A perovskite / crystalline silicon tandem cell according to claim 3, It is characterized in that The first doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 The second doped amorphous silicon film layer is n-type doped or p-type doped, with a doping concentration of 10 17 -10 20 cm -3 ; The conductivity type of the second doped amorphous silicon film layer is opposite to that of the first doped amorphous silicon film layer.

5. A perovskite / crystalline silicon tandem cell according to claim 1, It is characterized in that The first carrier transport layer comprises a stacked first inorganic carrier transport layer and a first organic carrier transport layer; the first carrier transport layer is a hole transport layer or an electron transport layer; the first carrier transport layer and the first doped amorphous silicon film layer have the same conductivity type; The second carrier transport layer includes a stacked second inorganic carrier transport layer and a second organic carrier transport layer; the second carrier transport layer is a hole transport layer or an electron transport layer; the second carrier transport layer has a conductivity type opposite to that of the first carrier transport layer and the same conductivity type as the second doped amorphous silicon film layer.

6. A perovskite / crystalline silicon tandem cell according to claim 5, It is characterized in that The first inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer; the second inorganic carrier transport layer includes an inorganic hole transport layer or an inorganic electron transport layer, and the first inorganic carrier transport layer and the second inorganic carrier transport layer have opposite conductivity types; The inorganic hole transport layer includes at least one of NiOx, V2O5, MoOx, WOx, and Cu2O, with a thickness of 0.5-50nm; the inorganic electron transport layer includes at least one of SnO2, TiO2, ZnO, Nb2O5, ZrO2, TiSnOx, SnZnOx, LiF, and MgFx, with a thickness of 0.5-50.0nm.

7. A perovskite / crystalline silicon tandem cell according to claim 5, It is characterized in that The first organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, the second organic carrier transport layer includes an organic hole transport layer or an organic electron transport layer, and the first organic carrier transport layer and the second organic carrier transport layer have opposite conductivity types; The organic hole transport layer includes at least one of 2PACz, Me-4PACz, MeO-2PACz, PTAA, P3HT, Poly-TPD, PEDOT:PSS, Spiro-OMeTAD, m-MTDATA, Spiro-TTB, F4-TCNQ, F6-TCNNQ, and TAPC, and has a thickness of 0.5-50.0 nm; The organic electron transport layer includes at least one of fullerene C60, fullerene C70, and fullerene derivative PCBM, and has a thickness of 0.5-50.0 nm.

8. A perovskite / crystalline silicon tandem cell according to claim 1, It is characterized in that The transparent conductive oxide film layer includes at least one of doped indium oxide, tin oxide, and zinc oxide-based films, and has a thickness of 60-150 nm.

9. The perovskite / crystalline silicon tandem cell according to claim 1, It is characterized in that The general formula of the perovskite light absorbing layer is ABX 3 , wherein A is a monovalent cation and includes at least one of lithium, sodium, potassium, cesium, amine and amidine, wherein B is a divalent cation and includes at least one of lead and tin; X is a monovalent anion and includes at least one of iodine, bromine and chlorine; the thickness of the perovskite light-absorbing layer is 500-1500nm.

10. A method for preparing a perovskite / crystalline silicon tandem cell according to any one of claims 1 to 9, It is characterized in that The steps include: S1, cleaning the surface of silicon wafer; S2, depositing an intrinsic amorphous silicon film layer and a first doped amorphous silicon film layer on the back side of the silicon wafer, and depositing an intrinsic amorphous silicon film layer and a second doped amorphous silicon film layer on the front side of the silicon wafer; S3, depositing a transparent conductive oxide film layer and a metal conductive film layer on the surface of the first doped amorphous silicon film layer on the back side; depositing an ultra-thin metal silicide film layer and a first inorganic carrier transport layer on the surface of the second doped amorphous silicon film layer on the front side; S4, forming a first organic carrier transport layer and a perovskite light absorption layer on the surface of the first inorganic carrier transport layer; S5, forming a second organic carrier transport layer on the surface of the perovskite light absorbing layer; S6, forming a second inorganic carrier transport layer on the surface of the second organic carrier transport layer; S7, forming a transparent conductive oxide film layer on the surface of the second inorganic carrier transport layer; S8. Form a front gate line electrode on the surface of the transparent conductive oxide film layer.

Citation Information

Patent Citations

  • Compositions and processes for forming photovoltaic devices

    CN102119445A

  • Heterojunction laminated solar cell and manufacturing method thereof

    CN116847672A

  • Solar cell and method for manufacturing the same

    KR1020090093191A

  • Multi-junction solar cell and method for manufacturing the same

    US20240213388A1

  • Semiconductor tandem solar cells with metal silicide barrier

    US4907052A

Cited By

  • Perovskite / crystalline silicon laminated solar cell and preparation method thereof

    CN122497261A

  • Perovskite / crystalline silicon tandem solar cell and preparation method thereof

    CN122497261B