Non-grid control region doped oxide semiconductor field power device and preparation method thereof

By setting a doped layer on the oxide semiconductor channel layer, the contradiction between on-resistance and breakdown voltage in the oxide semiconductor power device is solved, and the combination of low on-resistance and high breakdown voltage is achieved, which is optimized. Device performance shows huge application potential.

CN119029048APending Publication Date: 2024-11-26PEKING UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411138961.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

There is a contradiction between the on-resistance and the breakdown voltage in oxide semiconductor power devices, and it is difficult to achieve both low on-resistance and high breakdown voltage.

Method used

Two doped layers are arranged on the oxide semiconductor channel layer. The doped layers are fully oxidized by the metal material, covering the non-gate control region, increasing the carrier concentration to reduce the series resistance, while maintaining the threshold voltage not Change.

Benefits of technology

It realizes the low on-resistance and high breakdown voltage of oxide semiconductor power devices, optimizes the performance of the device, and has huge application potential in the field of high-voltage power devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029048A_ABST
    Figure CN119029048A_ABST
Patent Text Reader

Abstract

The invention discloses a non-grid control region doped oxide semiconductor power device and a preparation method thereof. The power device is divided into a bottom gate structure device and a top gate structure device according to different positions of the gate electrode layer. According to the invention, the series resistance of the non-grid-control region is reduced by doping in the non-grid-control region, so that the on resistance of the oxide semiconductor power device is optimized, the good breakdown characteristic is maintained, and huge application potential is shown in the field of power devices compatible in a later channel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The patent of this invention relates to a non-gate-controlled region doped oxide semiconductor field power device and a preparation method, belonging to the field of information materials and device technology. Background Art

[0002] Oxide semiconductor materials are widely used in the display field due to their high transparency, high mobility and high uniformity. In recent years, due to their advantages such as low off-state leakage and low thermal budget, their applications in high-density, low-power logic and storage have also received a lot of attention and research. In addition, oxide semiconductors usually have a bandgap width greater than 2.5eV, which is a wide bandgap semiconductor, and their bandgap width can be flexibly adjusted by doping concentration, so they show great potential in the field of high-voltage power devices, but there is currently a relative lack of research in this area.

[0003] In order to increase the breakdown voltage of the device, traditional power devices usually need to design a certain distance between the gate and the drain to reduce the peak electric field near the drain edge. However, in order to increase the bandgap width of the oxide semiconductor material and realize enhanced power devices, it is necessary to reduce the carrier concentration of the oxide semiconductor channel, which will lead to an increase in the on-resistance of the non-gate-controlled area. Therefore, there is a contradiction between the on-resistance and breakdown voltage of oxide semiconductor power devices. Summary of the invention

[0004] In order to address the contradiction between on-resistance and breakdown voltage in oxide semiconductor power devices, the present invention proposes a non-gate-controlled region doping method, which can realize an oxide semiconductor power device with both low on-resistance and high breakdown voltage.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is:

[0006] An oxide semiconductor bottom-gate power device, the device structure includes, from bottom to top, a substrate, a gate electrode layer, a gate dielectric layer, an oxide semiconductor channel layer, a source / drain contact layer and a surface passivation layer, characterized in that two doping layers are arranged on the oxide semiconductor channel layer, the doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate control area, the doping layer is a metal oxide obtained by fully oxidizing a metal material, the thickness of the metal material is 1 to 10 nm, the metal material is fully oxidized during the preparation process, and the oxidation process captures oxygen atoms in the oxide semiconductor channel layer to increase the carrier concentration, thereby reducing the series resistance, and improving the carrier concentration of the region without affecting the threshold voltage of the device, while achieving low on-resistance and high breakdown voltage.

[0007] An oxide semiconductor top-gate power device, the device structure includes, from bottom to top, a substrate, an oxide semiconductor channel layer, a source / drain contact layer, a gate dielectric layer and a gate electrode layer, characterized in that two doping layers are arranged on the oxide semiconductor channel layer, the doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate control area, the doping layer is a metal oxide obtained by fully oxidizing a metal material, the thickness of the doping layer is 1 to 10 nm, the metal material is fully oxidized during the preparation process, and the doping layer captures oxygen atoms in the oxide semiconductor channel layer during the oxidation process to increase the carrier concentration, thereby reducing the series resistance, and improving the carrier concentration of the region without affecting the threshold voltage of the device, while achieving low on-resistance and high breakdown voltage.

[0008] Furthermore, the substrate includes but is not limited to a silicon substrate, a sapphire substrate, a silicon carbide substrate, a diamond substrate, a diamond-like carbon film substrate, and the like.

[0009] Furthermore, the gate electrode material includes but is not limited to Ti, Al, Ni, Au, Mo, Pt, Pd, W, TiN and various alloys, and the recommended thickness is 5 to 100 nm.

[0010] Furthermore, the gate dielectric material includes but is not limited to SiO2, Al2O3, Y2O3, ZrO2, SiN x 、SiON x 、HfO2、HfSiO x 、HfLaO x 、HfAlO x 、HfZrO x And various element doping media, the recommended thickness is 5 to 50nm.

[0011] Furthermore, the source-drain contact materials include but are not limited to Ti, Al, Ni, Au, Mo, Pt, Pd, W, TiN, TaN, ITO, IZO, etc., and the recommended thickness is 5 to 100 nm.

[0012] Furthermore, the metal material of the doping layer includes but is not limited to easily oxidized metals such as Al and Y.

[0013] Furthermore, the oxide semiconductor channel layer includes but is not limited to In2O3, Ga2O3, ZnO, SnO2, ITO, IGO, IZO, IWO, IGZO, ITZO, IAZO, etc., and the recommended thickness is 0.5 to 20 nm.

[0014] Furthermore, the thickness of the passivation layer is 5 to 200 nm.

[0015] The present invention provides a method for preparing an oxide semiconductor bottom-gate power device, comprising the following steps:

[0016] Step 1.1, obtaining and cleaning the substrate;

[0017] Step 1.2, defining the bottom gate pattern by electron beam exposure, optical lithography, laser direct writing and other processes, and depositing the bottom gate electrode layer by electron beam evaporation, magnetron sputtering, thermal evaporation, atomic layer deposition and other processes;

[0018] Step 1.3, preparing the bottom gate dielectric layer by using processes such as atomic layer deposition, plasma enhanced chemical vapor deposition, pulsed laser deposition, magnetron sputtering, and electron beam evaporation;

[0019] Step 1.4, depositing an oxide semiconductor channel layer by atomic layer deposition or magnetron sputtering;

[0020] Step 1.5, using electron beam exposure, ultraviolet lithography, laser direct writing and other processes to define the channel active area range, and using wet, dry or dry-wet etching process to achieve device isolation;

[0021] Step 1.6, using electron beam exposure, ultraviolet lithography, laser direct and other processes to define the source / drain contact pattern, and using electron beam evaporation, magnetron sputtering, thermal evaporation, atomic layer deposition and other processes to prepare the source / drain contact layer;

[0022] Step 1.7, use electron beam exposure, ultraviolet lithography, laser direct writing and other processes to define the doping area pattern, use electron beam evaporation, magnetron sputtering, thermal evaporation and other processes to prepare the non-gate control area doping layer metal material, and fully oxidize it. When the nano-thick aluminum film evaporated by electron beam is used as the doping layer, the vacuum degree of the evaporation process chamber is controlled at 1×10 -6 If the temperature is above 1000 Torr and the thickness is below 3nm, the aluminum film will be completely oxidized to aluminum oxide in the air after evaporation;

[0023] Step 1.8, depositing a surface passivation layer using processes such as atomic layer deposition, plasma enhanced chemical vapor deposition, magnetron sputtering, pulsed laser deposition, and ion beam deposition.

[0024] The present invention provides a method for preparing an oxide semiconductor top-gate power device, comprising the following steps:

[0025] Step 2.1, obtaining and cleaning the substrate;

[0026] Step 2.2, depositing an oxide semiconductor channel layer by atomic layer deposition or magnetron sputtering;

[0027] Step 2.3, using electron beam exposure, ultraviolet lithography, laser direct writing and other processes to define the channel active area range, and using wet, dry or dry-wet etching process to achieve device isolation;

[0028] Step 2.4, using electron beam exposure, ultraviolet lithography, laser direct and other processes to define the source / drain contact pattern, and using electron beam evaporation, magnetron sputtering, thermal evaporation, atomic layer deposition and other processes to prepare the source / drain contact layer;

[0029] Step 2.5, using electron beam exposure, ultraviolet lithography, laser direct writing and other processes to define the doping area pattern, using electron beam evaporation, magnetron sputtering, thermal evaporation and other processes to prepare the non-gate control area doping layer metal material, and fully oxidize it. When the nano-thick aluminum film evaporated by electron beam is used as the doping layer, the vacuum degree of the evaporation process chamber is controlled at 1×10 -6 If the temperature is above 1000 Torr and the thickness is below 3nm, the aluminum film will be completely oxidized to aluminum oxide in the air after evaporation;

[0030] Step 2.6, preparing a top gate dielectric layer by using processes such as atomic layer deposition, plasma enhanced chemical vapor deposition, pulsed laser deposition, magnetron sputtering, and electron beam evaporation;

[0031] In step 2.7, the top gate pattern is defined by electron beam exposure, optical lithography, laser direct writing and other processes, and the bottom gate electrode layer is deposited by electron beam evaporation, magnetron sputtering, thermal evaporation, atomic layer deposition and other processes.

[0032] The beneficial effects of the present invention are as follows:

[0033] The present invention reduces the series resistance of the non-gate-controlled region by doping in the region, thereby optimizing the on-resistance of the oxide semiconductor power device while maintaining good breakdown characteristics, showing great application potential in the field of back-end compatible power devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 A schematic diagram of the structure of a bottom-gate structured oxide semiconductor power device with doping in a non-gate control region in the present invention;

[0035] Figure 2 For specific implementation steps.

[0036] Figure 3 A schematic diagram of the structure of a non-gate-controlled region doped top-gate structure oxide semiconductor power device in the present invention;

[0037] Figure 4 For specific implementation steps.

[0038] Wherein: 1-substrate, 2-gate electrode layer, 3-gate dielectric layer, 4-oxide semiconductor channel layer, 5-source / drain contact layer, 6-non-gate control region doping layer, 7-surface passivation layer. DETAILED DESCRIPTION

[0039] The following will describe the implementation of the present invention in detail with reference to the examples in the accompanying drawings. The following embodiments are only part of the embodiments of the present invention, not all of them.

[0040] The present invention provides a non-gate-controlled region doped oxide semiconductor power device and a method for preparing the same. The transistor is divided into a bottom gate structure and a top gate structure according to the location of the gate electrode layer.

[0041] Bottom gate structure Figure 1 As shown, the structure from bottom to top is a substrate, a bottom gate electrode layer, a bottom gate dielectric layer, an oxide semiconductor channel layer, a source / drain contact layer, and a surface passivation layer. Two doping layers are arranged on the oxide semiconductor channel layer. The doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate-controlled area. The thickness of the doping layer is 1 to 10 nm.

[0042] The specific implementation steps are as follows: Figure 2 As shown:

[0043] S001, obtaining and cleaning a substrate;

[0044] S002, defining the bottom gate pattern by electron beam exposure process, and depositing 20 nm of Pt as the bottom gate metal electrode layer by electron beam evaporation process;

[0045] S003, using atomic layer deposition process to deposit 10nm HfO2 as the bottom gate dielectric layer;

[0046] S004, depositing 10 nm IGZO oxide semiconductor as a channel layer using an atomic layer deposition process;

[0047] S005, defining the channel region by electron beam exposure process, and realizing device isolation by wet etching process;

[0048] S006, using electron beam exposure process to define the source and drain contact area, and using electron beam evaporation to deposit 20 / 40nm Ni / Au as the source and drain contact metal layer;

[0049] S007, electron beam exposure lithography process is used to define the doping area, and electron beam evaporation process is used to deposit 2nmAl, and after full oxidation, it is used as the doping layer of the non-gating area. During electron beam evaporation, the vacuum degree of the evaporation process chamber is controlled at 1×10 - 6 Torr or above, and the film thickness is below 3nm, the aluminum film will be completely oxidized to aluminum oxide in the air after evaporation;

[0050] S008, using plasma enhanced chemical vapor deposition process to deposit 100nm SiO2 as a surface passivation layer.

[0051] Top gate structure Figure 3 As shown, the device structure includes, from bottom to top, a substrate, an oxide semiconductor channel layer, a source / drain contact layer, a gate dielectric layer and a gate electrode layer. Two doping layers are arranged on the oxide semiconductor channel layer. The doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate-controlled area. The thickness of the doping layers is 1 to 10 nm.

[0052] The specific implementation steps are as follows: Figure 4 As shown:

[0053] S001, obtaining and cleaning a substrate;

[0054] S002, depositing 10nm IGZO oxide semiconductor as a channel layer using an atomic layer deposition process;

[0055] S003, defining the channel region by electron beam exposure process, and realizing device isolation by wet etching process;

[0056] S004, using electron beam exposure process to define the source and drain contact area, and using electron beam evaporation to deposit 20 / 40nm Ni / Au as the source and drain contact metal layer;

[0057] S005, electron beam exposure lithography process is used to define the doping area, and 2nmAl is deposited by electron beam evaporation process, and after full oxidation, it is used as the doping layer of the non-gating area. During electron beam evaporation, the vacuum degree of the evaporation process chamber is controlled at 1×10 - 6 Torr or above, and the film thickness is below 3nm, the aluminum film will be completely oxidized to aluminum oxide in the air after evaporation;

[0058] S006, using atomic layer deposition process to deposit 10nm HfO2 as the bottom gate dielectric layer

[0059] S007, using electron beam exposure process to define the bottom gate pattern, and using electron beam evaporation process to deposit 20 / 40nm Pt / Au as the bottom gate metal electrode layer.

[0060] There are many implementation methods of the present invention, and all technical solutions formed by equivalent transformation or equivalent transformation fall within the protection scope of the present invention.

[0061] It should be noted that the above-mentioned embodiments illustrate rather than limit the invention and that those skilled in the art will be able to design alternative embodiments without departing from the scope of the appended claims.

Claims

1. An oxide semiconductor bottom-gate power device, wherein the device structure is sequentially include: A substrate, a gate electrode layer, a gate dielectric layer, an oxide semiconductor channel layer, a source / drain contact layer and a surface passivation layer, characterized in that two doping layers are arranged on the oxide semiconductor channel layer, the doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate control area, the doping layer is a metal oxide obtained by fully oxidizing a metal material, and the thickness of the doping layer is 1 to 10 nm.

2. An oxide semiconductor top-gate power device, wherein the device structure is sequentially include: A substrate, an oxide semiconductor channel layer, a source / drain contact layer, a gate dielectric layer and a gate electrode layer, characterized in that two doping layers are arranged on the oxide semiconductor channel layer, the doping layers are respectively connected to the source / drain contact layers, and the doping layers partially or completely cover the non-gate control area, the doping layer is a metal oxide obtained by fully oxidizing a metal material, and the thickness of the doping layer is 1 to 10 nm.

3. The device according to claim 1 or 2, It is characterized in that The substrate is a silicon substrate, a sapphire substrate, a silicon carbide substrate, a diamond substrate or a diamond-like carbon film substrate.

4. The device according to claim 1 or 2, It is characterized in that The gate electrode layer is made of Ti, Al, Ni, Au, Mo, Pt, Pd, W, TiN and various alloy materials, and its thickness ranges from 5 to 100 nm.

5. The device according to claim 1 or 2, It is characterized in that The gate dielectric material is SiO 2 、Al 2 O 3 , Y 2 O 3 、ZrO 2 、SiN x 、SiON x , HfO 2 、HfSiO x 、HfLaO x 、HfAlO x 、HfZrO x and various element-doped media, with a thickness ranging from 5 to 50 nm.

6. The device according to claim 1 or 2, It is characterized in that The source / drain contact layer is Ti, Al, Ni, Au, Mo, Pt, Pd, W, TiN, TaN, ITO or IZO, and its thickness ranges from 5 to 100 nm.

7. The device according to claim 1 or 2, It is characterized in that The metal material of the doping layer is Al or Y metal.

8. The device according to claim 1 or 2, It is characterized in that The oxide semiconductor channel layer is In 2 O 3 , Ga 2 O 3 、ZnO、SnO 2 , ITO, IGO, IZO, IWO, IGZO, ITZO or IAZO, with a thickness ranging from 0.5 to 20 nm.

9. The method for preparing an oxide semiconductor bottom-gate power device according to claim 1, comprising the following steps: Step 1.1, obtaining and cleaning the substrate; Step 1.2, using electron beam exposure, optical lithography, laser direct writing and other processes to define the bottom gate pattern, and using electron beam evaporation, magnetron sputtering, thermal evaporation, atomic layer deposition process to deposit the gate electrode layer; Step 1.3, preparing a gate dielectric layer by atomic layer deposition, plasma enhanced chemical vapor deposition, pulsed laser deposition, magnetron sputtering, or electron beam evaporation; Step 1.4, depositing an oxide semiconductor channel layer by atomic layer deposition or magnetron sputtering process; Step 1.5, using electron beam exposure, ultraviolet lithography, laser direct writing and other processes to define the channel active area range, and using wet, dry or dry-wet etching process to achieve device isolation; Step 1.6, using electron beam exposure, ultraviolet lithography, and laser direct process to define the source / drain contact pattern, and using electron beam evaporation, magnetron sputtering, thermal evaporation, and atomic layer deposition process to prepare the source / drain contact layer; Step 1.7, using electron beam exposure, ultraviolet lithography, laser direct writing process to determine the doping area pattern, using electron beam evaporation, magnetron sputtering process, thermal evaporation process to prepare the doping layer metal material, and fully oxidize it; Step 1.8, depositing a surface passivation layer using atomic layer deposition, plasma enhanced chemical vapor deposition, magnetron sputtering, pulsed laser deposition, or ion beam deposition.

10. The method for preparing an oxide semiconductor top-gate power device according to claim 2, comprising the following steps: Step 2.1, obtaining and cleaning the substrate; Step 2.2, depositing an oxide semiconductor channel layer by atomic layer deposition or magnetron sputtering process; Step 2.3, using electron beam exposure, ultraviolet lithography, and laser direct writing processes to define the channel active area range, and using wet, dry, or a combination of wet and dry etching processes to achieve device isolation; Step 2.4, using electron beam exposure, ultraviolet lithography, and laser direct process to define the source / drain contact pattern, and using electron beam evaporation, magnetron sputtering, thermal evaporation, and atomic layer deposition process to prepare the source / drain contact layer; Step 2.5, using electron beam exposure, ultraviolet lithography, laser direct writing process to determine the doping area pattern, using electron beam evaporation, magnetron sputtering process, thermal evaporation process to prepare the doping layer metal material, and fully oxidize it; Step 2.6, preparing a gate dielectric layer by atomic layer deposition, plasma enhanced chemical vapor deposition, pulsed laser deposition, magnetron sputtering, or electron beam evaporation; In step 2.7, the top gate pattern is defined by electron beam exposure, optical lithography, and laser direct writing processes, and the top gate electrode layer is deposited by electron beam evaporation, magnetron sputtering, thermal evaporation, and atomic layer deposition processes.