Solar cell perovskite surface molecular modification method and solar cell
The defects in perovskite layer crystallization process were solved by using the gentle passivation molecule 1-(3,4-dichlorophenyl)biguanide hydrochloride (DBGCl) in perovskite solar cells. The resulting performance reduction problems improve conductivity and air stability and improve photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202410901281.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-12
AI Technical Summary
The defects generated by perovskite solar cells during crystallization lead to a reduction in cell performance. The existing treatment methods excessively enhance the passivation intensity of passivation molecules on the side bases have negative effects on perovskites, and optimization and improvement methods are needed.
The perovskite layer is surface modified using a mild passivation molecule 1-(3,4-dichlorophenyl)biguanide hydrochloride (DBGCl), and perovskite is formed on the electron transport layer by spin coating precursors and post-treatment solution. The ore film regulates the side base and binds to defect sites to improve the battery's conductivity.
It effectively reduces the defect state density of perovskite solar cells, reduces non-radiative recombination, improves conductivity and air stability, and improves photoelectric conversion efficiency.
Smart Images

Figure CN118946220A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic power generation, and in particular to a method for modifying the surface molecules of perovskite of a solar cell and a solar cell. Background Art
[0002] Metal halide perovskite solar cells (PSCs) have attracted extensive attention from researchers due to their excellent optoelectronic properties and rapidly improving power conversion efficiency (PCE). At present, the certified efficiency of perovskite solar cells has reached 26.1%, which is comparable to that of single-crystal silicon cells. However, defects will inevitably occur during the crystallization of the perovskite layer, and studies have shown that most of the defects are concentrated on the surface of the perovskite. Existing treatment methods usually use passivators with Lewis acid or Lewis base groups to post-treat the perovskite layer to passivate surface defects. However, the side groups excessively enhance the passivation strength of the passivation molecules and also have a negative effect on the perovskite. Therefore, further optimization and improvement methods are needed for the defects generated during the crystallization process of perovskite solar cells. Summary of the invention
[0003] The present invention provides a method for modifying the surface molecule of a solar cell perovskite and a solar cell. By studying and designing a mild passivation molecule, the side group can be used to regulate the side group, and the side group can be effectively combined with the defect site without destroying the perovskite, thereby effectively improving the conductivity of the battery and solving the problem that the perovskite layer of the perovskite solar cell generates defects during the crystallization process, resulting in reduced battery performance.
[0004] In order to solve the above technical problems, the technical solution of the present invention is as follows:
[0005] The embodiment of the present invention provides a method for modifying the surface molecules of a solar cell perovskite, comprising:
[0006] providing a conductive glass substrate;
[0007] Processing the surface of the conductive glass substrate to obtain a base plate;
[0008] forming an electron transport layer on the substrate;
[0009] The substrate forming the electron transport layer is sequentially spin-coated with a precursor solution and a post-treatment solution to form a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer.
[0010] Optionally, the surface of the conductive glass substrate is processed to obtain a substrate, comprising:
[0011] The conductive glass substrate is rinsed with detergent, deionized water and ethanol in sequence;
[0012] The rinsed conductive glass substrate is immersed in anhydrous ethanol and ultrasonically cleaned;
[0013] The cleaned conductive glass substrate is dried using a dry air flow to obtain a base plate.
[0014] Optionally, forming an electron transport layer on the substrate includes:
[0015] Performing ultraviolet ozone cleaning on the substrate for a first preset time;
[0016] Heating the substrate after UV-ozone cleaning so that the temperature of the substrate reaches a first preset temperature;
[0017] Evenly spraying the c-TiO2 solution on the heated substrate and cooling it to room temperature to deposit the c-TiO2 on the substrate;
[0018] The m-TiO2 solution is spin-coated on the substrate on which the c-TiO2 is deposited. After the substrate is spin-coated, it is heated twice and then cooled to room temperature to form an electron transport layer.
[0019] Optionally, when the m-TiO2 solution is spin-coated on the substrate on which c-TiO2 is deposited, the spin-coating speed of the substrate is greater than 3000 rpm, and the spin-coating time is greater than 30 s.
[0020] Optionally, the substrate is subjected to two heating treatments after spin coating, including:
[0021] After spin coating, the substrate is first heated at a temperature greater than 80° C. for more than 10 minutes, and then heated at a temperature greater than 500° C. for more than 1 hour.
[0022] Optionally, the substrate forming the electron transport layer is sequentially spin-coated with a precursor solution and a post-treatment solution to form a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer, comprising:
[0023] The substrate on which the electron transport layer is formed is subjected to ultraviolet ozone cleaning;
[0024] Spin coating the substrate after UV-ozone cleaning with a precursor solution, and sequentially performing a first annealing treatment and a cooling treatment;
[0025] The cooled substrate is spin-coated with a post-treatment solution, and after a second annealing treatment, a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is formed on the electron transport layer.
[0026] Optionally, the precursor solution and the post-treatment solution are formed according to the following process:
[0027] The ingredients are prepared according to the molar ratio of the elements in the chemical formula MAPbI3; wherein the molar ratio of MAI to PbI2 is 1:1; dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 635:71 and stirred at room temperature for 4 hours to obtain a precursor solution;
[0028] 0.7 mg DBGCl was added to a mixed solution of isopropyl alcohol (IPA) and ethyl acetate (EA) in a volume ratio of 5:1, and heated and stirred at 70° C. for 2 to 6 h to obtain a post-treatment solution.
[0029] Optionally, the substrate after UV ozone cleaning is spin-coated with a precursor solution, and a first annealing treatment and a cooling treatment are sequentially performed, including:
[0030] The substrate cleaned by UV ozone was spin coated with the precursor solution at a spin coating speed of 3000-4000 rpm and a spin coating time of more than 25 s, and 120 μL EEA was added dropwise. After annealing at 65° C. for 1 min and 100° C. for 10 min, the substrate was cooled to room temperature.
[0031] Optionally, the cooled substrate is spin-coated with a post-treatment solution, and after a second annealing treatment, a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is formed on the electron transport layer, comprising:
[0032] The cooled substrate is spin-coated with the post-treatment solution at a spin-coating speed of 3000-4000 rpm and a spin-coating time of more than 30 seconds, and annealed at 100° C. for 5-10 minutes to obtain a perovskite film with a surface passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl).
[0033] An embodiment of the present invention further provides a solar cell, comprising:
[0034] substrate;
[0035] An electron transport layer, wherein the electron transport layer is located on the surface of the substrate;
[0036] A perovskite layer, wherein the perovskite layer is located on the surface of the electron transport layer, a surface-passivated perovskite film is formed on the surface of the perovskite layer, and the perovskite film is formed by a passivation treatment with 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl);
[0037] and a counter electrode layer, wherein the counter electrode layer is located on the surface of the perovskite film of the perovskite layer.
[0038] The technical solution of the present invention includes at least the following effects:
[0039] The method for modifying the surface molecule of solar cell perovskite comprises the following steps: providing a conductive glass substrate; treating the surface of the conductive glass substrate to obtain a base plate; forming an electron transport layer on the base plate; and sequentially spin coating the base plate with the electron transport layer with a precursor solution and a post-treatment solution to form a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer. A novel molecule is provided that can stably passivate the surface defects of perovskite without destroying the perovskite, thereby reducing the defect state density of the perovskite solar cell, reducing non-radiative recombination, and improving the conductivity and air stability of the perovskite solar cell. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1 is a flow chart of a method for modifying the surface of perovskite in a solar cell provided by an embodiment of the present invention;
[0041] Figure 2 is a comparison diagram of scanning electron microscope images of perovskite films prepared in the embodiment of the present invention and the comparative example;
[0042] Figure 3 It is a comparison diagram of the time-resolved photoluminescence spectra of the perovskite devices prepared in the embodiment of the present invention and the comparative example;
[0043] Figure 4 is a comparison chart of the photoelectric conversion efficiency of the perovskite devices prepared in the embodiment of the present invention and the comparative example;
[0044] Figure 5 is a comparison diagram of the integrated current of the perovskite devices prepared in the embodiment of the present invention and the comparative example;
[0045] Figure 6 is a comparison diagram of JV curves of the perovskite devices prepared in the embodiment of the present invention and the comparative example under reverse scanning;
[0046] Figure 7 It is a comparison diagram of PCE statistical box plots of the perovskite devices prepared in the embodiments of the present invention and the comparative examples. DETAILED DESCRIPTION
[0047] The exemplary embodiments of the present invention will be described in more detail below with reference to the accompanying drawings. Although the exemplary embodiments of the present invention are shown in the accompanying drawings, it should be understood that the present invention can be implemented in various forms and should not be limited by the embodiments set forth herein. On the contrary, these embodiments are provided in order to enable a more thorough understanding of the present invention and to enable the scope of the present invention to be fully communicated to those skilled in the art.
[0048] The terms "first", "second", etc. in the specification and claims of the present invention are used to distinguish similar objects, and are not used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention can be implemented in an order other than those illustrated or described herein, and the objects distinguished by "first", "second", etc. are generally of the same type, and the number of objects is not limited. For example, the first object can be one or more. In addition, "and / or" in the specification and claims represents at least one of the connected objects, and the character " / " generally indicates that the objects associated with each other are in an "or" relationship.
[0049] like Figure 1 As shown, an embodiment of the present invention provides a method for modifying the surface molecule of a solar cell perovskite, comprising:
[0050] Step 11, providing a conductive glass substrate;
[0051] Step 12, treating the surface of the conductive glass substrate to obtain a substrate;
[0052] Step 13, forming an electron transport layer on the substrate;
[0053] Step 14, spin-coating the substrate on which the electron transport layer is formed with the precursor solution and the post-treatment solution in sequence, forming a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer.
[0054] In this embodiment, the conductive glass substrate is fluorine-doped SnO2 conductive glass (FTO glass); the conductive glass substrate is rinsed and dried in sequence to obtain a substrate; after the substrate is cleaned with ultraviolet ozone, an electron transport layer is formed on the substrate; the substrate forming the electron transport layer is spin-coated with a precursor solution and a post-treatment solution in sequence to form a perovskite film on the electron transport layer whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl); wherein 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is an amphiphilic molecule having an imine group and atomic chlorine that are Lewis basic and an amine group that are Lewis acidic, and having the same At the same time, the benzene ring carried by its side group not only reduces the Lewis basicity of the adjacent imine group, but also makes the electrostatic potential distribution of the entire molecule more uniform; its amine head group can also fill the methylamine vacancy, thereby forming a two-dimensional perovskite on the surface; experiments have shown that after DBGCl treats the perovskite surface, the surface defects are effectively passivated; the reconstructed surface has a uniform surface potential distribution, which promotes carrier transport; DBGCl induces the formation of parallel-arranged two-dimensional perovskites, which protect the underlying perovskite, reduce the defect state density of perovskite solar cells, reduce non-radiative recombination, and improve the conductivity and air stability of perovskite solar cells.
[0055] The present invention adopts new molecules to modify the surface of perovskite, with simple process and low cost; the new surface passivation molecules used react mildly with the surface of perovskite, and can generate a water-isolating two-dimensional layer to protect the underlying perovskite while effectively passivating surface defects. The treated devices have higher short-circuit current and fill factor, and better air environment stability.
[0056] In an optional embodiment of the present invention, step 12 may include:
[0057] Step 121, washing the conductive glass substrate with detergent, deionized water and ethanol in sequence;
[0058] Step 122, immersing the rinsed conductive glass substrate in anhydrous ethanol and performing ultrasonic cleaning;
[0059] Step 123, drying the cleaned conductive glass substrate using a dry air flow to obtain a substrate.
[0060] In this embodiment, the etched FTO substrate is rinsed with detergent, deionized water and ethanol, immersed in a container filled with anhydrous ethanol and cleaned in an ultrasonic cleaner for 20 minutes, and then dried with a dry air flow to obtain a substrate.
[0061] In an optional embodiment of the present invention, step 13 may include:
[0062] Step 131, performing ultraviolet ozone cleaning on the substrate for a first preset time;
[0063] Step 132, heating the substrate after UV-ozone cleaning so that the temperature of the substrate reaches a first preset temperature;
[0064] Step 133, spraying the c-TiO2 solution uniformly on the heated substrate, and cooling to room temperature, so that the c-TiO2 is deposited on the substrate;
[0065] Step 134, spin-coating the m-TiO2 solution on the substrate on which the c-TiO2 is deposited, and the substrate is subjected to two heating treatments after spin coating and then cooled to room temperature to form an electron transport layer.
[0066] In this embodiment, the cleaned substrate (10 cm×10 cm) is transferred to an ultraviolet ozone cleaning machine for at least 15 minutes; after the cleaning is completed, the substrate is placed on a titanium hot plate, the temperature is gradually increased to 450°C, and the c-TiO2 solution is evenly sprayed on the substrate by a spray pyrolysis method and naturally cooled to room temperature; after the c-TiO2 is deposited, the substrate is cut into 1.67 cm×2.5 cm rectangular pieces, and the cut substrate is placed in an ultraviolet ozone cleaning machine for 15 minutes; after the cleaning is completed, the substrate is transferred to a spin coater, and the m- The TiO2 solution is statically spin-coated onto the substrate, wherein the spin-coating speed is above 3000rpm, which can ensure that the m-TiO2 solution can be completely diffused and retained on the c-TiO2 substrate, and the solution can completely cover the substrate after 30s of spin-coating; after the spin-coating is completed, the substrate is placed on an 80°C hot plate for heating for 10 minutes to evaporate the ethanol solvent of the spin-coated m-TiO2 layer, so that the m-TiO2 layer is initially fixed, and dust is prevented from being contaminated during the subsequent removal of the insulating tape and the transfer process; then the substrate is placed on a titanium plate hot plate and the temperature is gradually increased to 500°C for 1 hour; wherein the heating adopts gradient heating, and the highest temperature is greater than 500°C but less than 550°C. Above 500°C, mesoporous anatase TiO2 begins to form, and the mesoporous anatase TiO2 semiconductor has strong activity, and the energy level matches the light-absorbing layer, which can serve as a framework to support the growth of the perovskite layer; after annealing, it is naturally cooled to room temperature to form an electron transport layer on the substrate.
[0067] In an optional embodiment of the present invention, step 14 may include:
[0068] Step 141, performing ultraviolet ozone cleaning on the substrate on which the electron transport layer is formed;
[0069] Step 142, spin-coating the precursor solution on the substrate after UV-ozone cleaning, and sequentially performing a first annealing treatment and a cooling treatment;
[0070] Step 143, spin-coating the cooled substrate with a post-treatment solution, and forming a perovskite film on the electron transport layer after a second annealing treatment, the surface of which is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl).
[0071] In this embodiment, the substrate with c-TiO2 deposited thereon is first subjected to UV ozone cleaning treatment, and then the ingredients are prepared according to the molar ratio of the elements in the chemical formula MAPbI3. 159 mg of MAI and 461 mg of PbI2 are weighed and dissolved in a mixed solvent of 635 μL of N, N-dimethylformamide (DMF) and 71 μL of dimethyl sulfoxide (DMSO) and stirred at room temperature for 4 hours to fully dissolve the raw materials to obtain a precursor solution; 0.7 mg of DBGCl is added to isopropyl alcohol (IPA) and ethyl acetate (EA) by volume. In a mixed solution with a ratio of 5:1 (DBGCl is not easy to agglomerate in an environment with IPA as the main solvent, 1 / 5 volume of EA is added to reduce the dissolution of the post-treatment solution on the perovskite surface), heating and stirring at 70°C for 2 to 6 hours can accelerate the dissolution rate of DBGCl and DBGCl is not easy to agglomerate, so that the DBGCl powder is completely dissolved to obtain a post-treatment solution; the precursor solution is spin-coated on a substrate formed with an electron transport layer, and annealed, wherein the spin coating speed is 3000 rpm and the spin coating acceleration is 1000 rpm / s 2 , the spin coating time is 30s, and 120μL of EA is dropped at the 19th second of spin coating; the annealing conditions are 65℃ / 1min and 100℃ / 10min, and a perovskite film is formed on the surface of the electron transport layer; after the perovskite film is cooled to room temperature, post-treatment is carried out, and under the conditions of a spin coating speed of 3000-4000rpm and a spin coating time of 30s, the post-treatment solution can fully cover the perovskite surface; the spin coating adopts dynamic spin coating, and after the substrate reaches the maximum speed, 45μL of the post-treatment solution is slowly added to the center of the perovskite with a pipette, and the surface of the electron transport layer is spun with the post-treatment solution. After annealing at 100℃ for 5-10min, the solvent is evaporated, and DBGCl can form a parallel-arranged two-dimensional perovskite with lead iodide on the perovskite surface, thereby obtaining a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanide hydrochloride (DBGCl).
[0072] An embodiment of the present invention further provides a solar cell, comprising:
[0073] substrate;
[0074] an electron transport layer formed on the substrate;
[0075] A precursor solution and a post-treatment solution are spin-coated on the electron transport layer to form a surface-passivated perovskite film, and the perovskite film is passivated by an IPA / EA dispersion of 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl).
[0076] Example
[0077] This embodiment provides a method for modifying the surface molecules of a solar cell perovskite, comprising:
[0078] (1) Preparation of conductive FTO transparent substrate
[0079] The etched FTO substrate was rinsed with detergent, deionized water and ethanol, immersed in a container filled with anhydrous ethanol and cleaned in an ultrasonic cleaner for 20 minutes, and then dried with a dry air flow to obtain a substrate.
[0080] (2) Preparation of electron transport layer
[0081] The cleaned substrate (10cm×10cm) was transferred to a UV-ozone cleaning machine and treated for at least 15 minutes. After cleaning, the substrate was placed on a titanium hot plate, the temperature was gradually increased to 450°C, and the c-TiO2 solution was evenly sprayed on the substrate by spray pyrolysis and naturally cooled to room temperature. After the deposition of c-TiO2 was completed, the substrate was cut into rectangular pieces of 1.67cm×2.5cm, and the cut substrate was placed in a UV-ozone cleaning machine for 15 minutes. After cleaning, the substrate was transferred to a spin coater, and the m-TiO2 solution was statically spin-coated onto the substrate at a spin coating speed of 3000rpm and a spin coating time of 30s. After the spin coating was completed, the substrate was placed on a 80°C hot plate and heated for 10 minutes, and then placed on a titanium hot plate and the temperature was gradually increased to 500°C for 1 hour. After annealing, it was naturally cooled to room temperature to form an electron transport layer on the substrate.
[0082] (3) Preparation of perovskite layer and surface passivation layer
[0083] The substrate with c-TiO2 deposited was cleaned with ultraviolet ozone, and then the ingredients were prepared according to the molar ratio of elements in the chemical formula MAPbI3. 159 mg of MAI and 461 mg of PbI2 were weighed and dissolved in a mixed solvent of 635 μL of N, N-dimethylformamide (DMF) and 71 μL of dimethyl sulfoxide (DMSO), and stirred at room temperature for 4 hours to obtain a precursor solution; 0.7 mg of DBGCl was added to a mixed solution of isopropanol (IPA) and ethyl acetate (EA) in a volume ratio of 5:1, heated and stirred at 70°C for 4 hours to obtain a post-treatment solution; the precursor solution was spin-coated on a substrate formed with an electron transport layer, and annealed, wherein the spin coating speed was 4000 rpm and the spin coating acceleration was 2000 rpm / s 2, the spin coating time is 25s, and 120μL of EA is dropped at the 19th second of spin coating; the annealing conditions are 65℃ / 1min and 100℃ / 10min to form a perovskite film on the surface of the electron transport layer; after the perovskite film is cooled to room temperature, post-treatment is carried out, and under the conditions of a spin coating speed of 3000rpm and a spin coating time of 30s, the surface of the electron transport layer is spin-treated with a post-treatment solution, and after annealing at 100℃ for 5min, a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is obtained.
[0084] (4) Preparation of counter electrode layer
[0085] The C electrode was prepared by flat plate coating method.
[0086] Comparative Example
[0087] The difference between the comparative example and the embodiment is that the precursor solution is spin-coated on the substrate having the electron transport layer formed thereon and annealed, and after the perovskite film is formed on the surface of the electron transport layer, no post-processing operation is performed.
[0088] The scanning electron microscope (SEM) images of the perovskite films prepared in the embodiments of the present invention and the comparative examples are as follows: Figure 2 As shown by Figure 2 It can be seen that after DBGCl post-treatment, the lead iodide residual on the surface of the embodiment disappears compared to the comparative example, and is replaced by a lamellar two-dimensional perovskite grown parallel to the substrate, indicating that DBGCl can protect the underlying bulk perovskite by forming a two-dimensional perovskite while passivating surface defects.
[0089] The time-resolved photoluminescence spectra (TRPL) of the perovskite devices prepared in the embodiments of the present invention and the comparative examples are as follows: Figure 3 As shown by Figure 3 It can be seen that after double exponential fitting, the average lifetime of photogenerated carriers in the comparative example is 47.43ns, while the average lifetime of carriers in the embodiment is 79.58ns. It can be seen that the embodiment has a longer carrier lifetime than the comparative example, indicating that the non-radiative coincidence caused by the interface defects in the embodiment is suppressed.
[0090] Comparison of conversion efficiency of the perovskite devices prepared in the embodiment of the present invention and the comparative example Figures 4 to 5 As shown by Figures 4 to 5 It can be seen that the short-circuit current excited by the embodiment in the 380nm-760nm band is higher than that of the comparative example, and it has higher photoelectric conversion efficiency and integrated current, which indirectly illustrates that the embodiment has higher energy conversion efficiency than that of the comparative example.
[0091] The JV curves of the perovskite devices prepared in the embodiments of the present invention and the comparative examples under reverse scanning are as follows: Figure 6 As shown by Figure 6 It can be seen that the short-circuit current of the device in the embodiment is significantly improved after DBGCl post-treatment.
[0092] The PCE statistical box plots of the perovskite devices prepared in the embodiments of the present invention and the comparative examples are shown in FIG. Figure 7 As shown in the figure, the energy conversion efficiency of 20 devices was statistically analyzed. Figure 7 It can be seen that the efficiency of the embodiment is significantly improved compared with the comparison example.
[0093] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific implementation", or "some implementations" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic expressions of the above terms do not necessarily refer to the same embodiment or example.
[0094] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for modifying the surface molecules of solar cell perovskite, characterized in that: include: providing a conductive glass substrate; Processing the surface of the conductive glass substrate to obtain a base plate; forming an electron transport layer on the substrate; The substrate forming the electron transport layer is sequentially spin-coated with a precursor solution and a post-treatment solution to form a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer.
2. The method for modifying the surface of solar cell perovskite according to claim 1, characterized in that: The surface of the conductive glass substrate is processed to obtain a substrate, comprising: The conductive glass substrate is rinsed with detergent, deionized water and ethanol in sequence; The rinsed conductive glass substrate is immersed in anhydrous ethanol and ultrasonically cleaned; The cleaned conductive glass substrate is dried using a dry air flow to obtain a base plate.
3. The method for modifying the surface of solar cell perovskite according to claim 2, characterized in that: Forming an electron transport layer on the substrate, comprising: Performing ultraviolet ozone cleaning on the substrate for a first preset time; Heating the substrate after UV-ozone cleaning so that the temperature of the substrate reaches a first preset temperature; Evenly spraying the c-TiO2 solution on the heated substrate and cooling it to room temperature to deposit the c-TiO2 on the substrate; The m-TiO2 solution is spin-coated on the substrate on which the c-TiO2 is deposited. After the substrate is spin-coated, it is heated twice and then cooled to room temperature to form an electron transport layer.
4. The method for modifying the surface of solar cell perovskite according to claim 3, characterized in that: When the m-TiO2 solution is spin-coated on the substrate on which c-TiO2 is deposited, the spin-coating speed of the substrate is greater than 3000 rpm, and the spin-coating time is greater than 30 seconds.
5. The method for modifying the surface of solar cell perovskite according to claim 3, characterized in that: The substrate is subjected to two heating treatments after spin coating, including: After spin coating, the substrate is first heated at a temperature greater than 80° C. for more than 10 minutes, and then heated at a temperature greater than 500° C. for more than 1 hour.
6. The method for surface molecular modification of solar cell perovskite according to claim 1, characterized in that: The substrate forming the electron transport layer is sequentially spin-coated with a precursor solution and a post-treatment solution to form a perovskite layer and a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) on the electron transport layer, comprising: The substrate on which the electron transport layer is formed is subjected to ultraviolet ozone cleaning; Spin coating the substrate after UV-ozone cleaning with a precursor solution, and sequentially performing a first annealing treatment and a cooling treatment; The cooled substrate is spin-coated with a post-treatment solution, and after a second annealing treatment, a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is formed on the electron transport layer.
7. The method for modifying the surface of solar cell perovskite molecules according to claim 6, characterized in that: The precursor solution and the post-treatment solution are formed according to the following process: The ingredients are prepared according to the molar ratio of the elements in the chemical formula MAPbI3; wherein the molar ratio of MAI to PbI2 is 1:1; dissolved in a mixed solvent of N,N-dimethylformamide (DMF) and dimethyl sulfoxide (DMSO) in a volume ratio of 635:71 and stirred at room temperature for 4 hours to obtain a precursor solution; 0.7 mg DBGCl was added to a mixed solution of isopropyl alcohol (IPA) and ethyl acetate (EA) in a volume ratio of 5:1, and heated and stirred at 70° C. for 2 to 6 h to obtain a post-treatment solution.
8. The method for modifying the surface of solar cell perovskite molecules according to claim 6, characterized in that: The substrate after UV ozone cleaning is spin-coated with a precursor solution, and a first annealing treatment and a cooling treatment are sequentially performed, including: The substrate cleaned by UV ozone was spin coated with the precursor solution at a spin coating speed of 3000-4000 rpm and a spin coating time of more than 25 s, and 120 μL EEA was added dropwise. After annealing at 65° C. for 1 min and 100° C. for 10 min, the substrate was cooled to room temperature.
9. The method for modifying the surface of solar cell perovskite molecules according to claim 6, characterized in that: The cooled substrate is spin-coated with a post-treatment solution, and after a second annealing treatment, a perovskite film whose surface is passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl) is formed on the electron transport layer, comprising: The cooled substrate is spin-coated with the post-treatment solution at a spin-coating speed of 3000-4000 rpm and a spin-coating time of more than 30 seconds, and annealed at 100° C. for 5-10 minutes to obtain a perovskite film with a surface passivated by 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl).
10. A solar cell, characterized in that: include: substrate; An electron transport layer, wherein the electron transport layer is located on the surface of the substrate; A perovskite layer, wherein the perovskite layer is located on the surface of the electron transport layer, a surface-passivated perovskite film is formed on the surface of the perovskite layer, and the perovskite film is formed by a passivation treatment with 1-(3,4-dichlorophenyl)biguanidine hydrochloride (DBGCl); and a counter electrode layer, wherein the counter electrode layer is located on the surface of the perovskite film of the perovskite layer.