Composite material, electrode, photoelectric device and display device

By using composite materials combined with modified polymer and conductive materials in flexible display technology, self-repair under deformation conditions is achieved, material crack problems are solved, the life of electrodes and optoelectronic devices is extended, and the flexible display device is improved. performance.

CN118946231APending Publication Date: 2024-11-12TCL TECHNOLOGY GROUP CORPORATION
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310542475.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In flexible display technology, cracks are prone to occur during repeated deformation of materials, resulting in loss of conductive properties and difficult to meet deformation needs.

Method used

Modified polymers containing amino, hydroxyl or disulfide bonds are used as repairing agents to combine with conductive materials, and the self-healing performance of the composite material is achieved through the formation of dynamic hydrogen bonds or disulfide bonds, ensuring that conductivity is maintained under deformation conditions.

Benefits of technology

Effectively prevent cracks from occurring during the deformation of the material, maintain conductive properties, extend the service life of electrodes and optoelectronic devices, and improve the flexibility and deformability of flexible display devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946231A_ABST
    Figure CN118946231A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material, an electrode, a photoelectric device and a display device. The composite material comprises a conductive material and a repairing agent, wherein the repairing agent is selected from a first polymer containing one or more of an amino group, a hydroxyl group or a disulfide bond, and a dynamic hydrogen bond or a dynamic disulfide bond is formed through the amino group or the hydroxyl group, so that self-repairing of the composite material is realized; or the repairing agent comprises a monomer of a conductive polymer and a catalyst, the monomer of the conductive polymer is catalyzed by the catalyst to polymerize to form the conductive polymer, and self-repairing of the composite material is achieved through polymerization and crosslinking.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of display technology, and in particular to a composite material, an electrode, a photoelectric device and a display apparatus. Background Art

[0002] At present, with the development of flexible display technology, foldable, bendable, wearable and other electronic devices are being used more and more widely. Flexible display technology needs to meet the requirements of deformation such as folding and bending, and the materials used in related electronic devices need to adapt to the requirements of deformation on the basis of meeting the basic performance requirements. However, during the repeated deformation process, the material is prone to cracks, resulting in the loss of its functionality. Taking electrodes as an example, the material of the electrode is generally a conductive material. During use, it is inevitable that cracks or breaks will occur due to scratches or bending, resulting in the loss of its conductive properties.

[0003] Therefore, how to improve the performance of materials and enhance their resistance to crack formation during deformation, thereby ensuring the functionality of materials, is one of the urgent issues to be solved in the development of flexible technology. Summary of the invention

[0004] In view of this, the present application provides a composite material, an electrode, an optoelectronic device and a display device, aiming to provide a material with self-healing properties.

[0005] An embodiment of the present application is implemented by providing a composite material, including a conductive material and a repair agent; the repair agent includes a first polymer containing one or more of an amino group, a hydroxyl group or a disulfide bond, and the first polymer includes one or more of a modified polyamide or a modified polyurethane; or the repair agent includes a monomer of a conductive polymer and a catalyst.

[0006] Optionally, in some embodiments of the present application, the modified polyamide includes one or more of hyperbranched polyamide, hydroxyl-modified polyamide, and disulfide-modified polyamide; and / or the modified polyurethane includes one or more of hyperbranched polyurethane, hydroxyl-modified polyurethane, amino-modified polyurethane, and disulfide-modified polyurethane.

[0007] Optionally, in some embodiments of the present application, the branching degree of the hyperbranched polyamide is 41% to 55%; and / or the grafting rate of the hydroxyl-modified polyamide is 2.8% to 3.5%; and / or the grafting rate of the disulfide-modified polyamide is 2.2% to 3.1%; and / or the branching degree of the hyperbranched polyurethane is 45% to 60%; and / or the grafting rate of the hydroxyl-modified polyurethane is 2.5% to 3.2%; and / or the grafting rate of the amino-modified polyurethane is 2.5% to 3.2%; and / or the grafting rate of the disulfide-modified polyurethane is 2.0% to 2.8%.

[0008] Optionally, in some embodiments of the present application, the repair agent includes a first repair agent and a second repair agent, the first repair agent includes a monomer of the conductive polymer, and the second repair agent includes the catalyst; wherein the first repair agent is a core-shell structure, including a first core and a first shell layer covering the first core, and the material of the first core includes a monomer of the conductive polymer; and / or the second repair agent is a core-shell structure, including a second core and a second shell layer covering the second core, and the material of the second core includes the catalyst.

[0009] Optionally, in some embodiments of the present application, when the monomer of the conductive polymer includes 3,4-ethylenedioxythiophene, the catalyst includes iron salt and persulfate; and / or when the monomer of the conductive polymer includes pyrrole, the catalyst includes AlCl3 and CuCl; and / or the monomer of the conductive polymer includes aniline, and the catalyst includes ammonium persulfate and hydrochloric acid; and / or the material of the first shell layer includes one or more of epoxy resin, polyurethane, and urea-formaldehyde resin; and / or the material of the second shell layer includes one or more of epoxy resin, polyurethane, and urea-formaldehyde resin.

[0010] Optionally, in some embodiments of the present application, the conductivity of the conductive polymer formed by catalyzing the polymerization of the monomer of the conductive polymer by the catalyst is greater than or equal to 50S / cm; and / or the conductive polymer includes one or more of polypyrrole and its derivatives, polyacetylene and its derivatives, polystyrene and its derivatives, polythiophene and its derivatives, polyparaphenylene and its derivatives.

[0011] Optionally, in some embodiments of the present application, the mass ratio of the repair agent to the conductive material is 1:(5-20); and / or the conductive material is an inorganic conductive material, an organic conductive material or an organic-inorganic hybrid material, wherein the organic-inorganic hybrid material is a mixed material of the inorganic conductive material and the organic conductive material, and the mass ratio of the organic conductive material to the inorganic conductive material is 1:

[0012] (1-10); and / or the molar ratio of the catalyst to the monomer of the conductive polymer is 1:3-10.

[0013] Optionally, in some embodiments of the present application, the inorganic conductive material includes one or more of a metal material and a carbon material, the metal material includes at least one of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg, the carbon material includes at least one of graphite, carbon nanotubes, graphene and carbon fiber; and / or the organic conductive material includes a second polymer, the conductivity of the second polymer being greater than or equal to 50S / cm.

[0014] Optionally, in some embodiments of the present application, the second polymer includes one or more of polypyrrole and its derivatives, polyacetylene and its derivatives, polystyrene and its derivatives, polythiophene and its derivatives, polyparaphenylene and its derivatives; and / or the repair agent includes the monomer of the conductive polymer and the catalyst, and the conductive material is selected from an organic conductive material or an organic-inorganic hybrid material, wherein the second polymer contained in the organic conductive material or the organic-inorganic hybrid material is the same as the conductive polymer formed by catalyzing the polymerization of the monomer of the conductive polymer by the catalyst.

[0015] Correspondingly, an embodiment of the present application also provides an electrode, comprising the above-mentioned composite material.

[0016] Correspondingly, an embodiment of the present application also provides a photoelectric device, comprising: a first electrode and a second electrode arranged opposite to each other; a functional layer arranged between the first electrode and the second electrode; wherein the material of the first electrode includes the above-mentioned composite material; and / or the material of the second electrode includes the above-mentioned composite material.

[0017] Optionally, in some embodiments of the present application, the functional layer includes a light-emitting layer, the material of the light-emitting layer is selected from an organic light-emitting material or a quantum dot light-emitting material, the organic light-emitting material is selected from at least one of a diaromatic anthracene derivative, a distyrene aromatic derivative, a pyrene derivative or a fluorene derivative, a blue-emitting TBPe fluorescent material, a green-emitting TTPA fluorescent material, an orange-emitting TBRb fluorescent material and a red-emitting DBP fluorescent material; the quantum dot light-emitting material is selected from at least one of a single-structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material, and the single-structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-II At least one of the I-VI group compounds, the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, At least one of HgZnSeS, HgZnSeTe and HgZnSTe, the IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe, the III-V group compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, Ga At least one of NSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, and the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2;The core of the quantum dots of the core-shell structure is selected from any one of the above-mentioned single-structure quantum dots, and the shell material of the quantum dots of the core-shell structure is selected from at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the general structural formula of the inorganic perovskite semiconductor is AMX3, wherein A is Cs; + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I -At least one of; and / or the functional layer includes a hole functional layer, the hole functional layer includes one or both of a hole injection layer and a hole transport layer, the material of the hole transport layer is selected from poly (9,9-dioctylfluorene-co-N-(4-butylphenyl) diphenylamine), polyvinyl carbazole, poly (N,N'-bis (4-butylphenyl) -N,N'-bis (phenyl) benzidine), poly (9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine), 4,4',4"-tri (carbazole-9-yl) triphenylamine, 4,4'-bis (9-carbazole) biphenyl, N,N'-diphenyl-N,N'-bis (3-methylphenyl) -1, 1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, poly(3,4-ethylenedioxythiophene)-poly(styrene sulfonic acid), Spiro-NPB, Spiro-TPD, TAPC, TPH; and / or the material of the hole injection layer is selected from poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanoquinone-dimethane, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, copper phthalocyanine, transition metal oxide The functional layer comprises one or more of a doped or undoped inorganic nanocrystal and an organic material, wherein the non-doped inorganic nanocrystal is selected from ZnO, TiO2, SnO2, Al2O3, GaO, SiO2, Ga2 O3, ZrO2, NiO, ZnS, ZnSe, CdS, InP, GaP, BaTiO3; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, and Mn; the organic material is selected from one or two of polymethyl methacrylate and polyvinyl butyral; and / or the material of the electron injection layer is selected from but not limited to at least one of LiF, LiF / Yb, MgP, MgF2, Al2O3, Ga2O3, ZnO, Cs2CO3, Rb2CO3, and RbBr.

[0018] Correspondingly, an embodiment of the present application further provides a display device, which includes the optoelectronic device as described above.

[0019] The composite material of the present application comprises a conductive material and a repair agent; wherein the repair agent is selected from a first polymer containing one or more of an amino group, a hydroxyl group or a disulfide bond, and forms dynamic hydrogen bonds or dynamic disulfide bonds through the amino group or the hydroxyl group to achieve self-repair of the composite material; or the repair agent comprises a monomer of a conductive polymer and a catalyst, and the catalyst catalyzes the polymerization of the monomer of the conductive polymer to form the conductive polymer, thereby enabling the composite material to have self-repairing properties through polymerization cross-linking. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0021] Figure 1 It is a structural schematic diagram of an embodiment of a photoelectric device provided in the present application. DETAILED DESCRIPTION

[0022] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0023] In the present application, unless otherwise specified, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited numbers (fractional or integer) within the indicated range.

[0024] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0025] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0026] The present application provides a composite material, comprising a conductive material and a repair agent.

[0027] Wherein, the conductive material may be an inorganic conductive material, an organic conductive material, or an organic-inorganic hybrid material.

[0028] The inorganic conductive material includes one or more of a metal material and a carbon material, the metal material includes at least one of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg; the carbon material includes at least one of graphite, carbon nanotubes, graphene and carbon fiber.

[0029] Among them, the metal material can be nanoparticles, such as silver nanoparticles, and the average particle size of the nanoparticles can be 5-50nm, specifically 5-10nm, 10-20nm, 20-30nm, 30-40nm, 40-50nm, etc.

[0030] The organic conductive material includes a conductive polymer, and the conductivity (or electrical conductivity) of the conductive polymer is greater than or equal to 50 S / cm, specifically 50-60 S / cm, 60-80 S / cm, 80-100 S / cm, etc. The conductive polymer with the conductivity can have good electrical conductivity, so that the composite material has good electrical conductivity.

[0031] Specifically, the conductive polymer may include one or more of polypyrrole and its derivatives, polyacetylene and its derivatives, polystyrene and its derivatives, polythiophene and its derivatives, polyparaphenylene and its derivatives, and the like.

[0032] Specifically, the polypyrrole and its derivatives may include one or more of pyrrole (PPy), poly(3-isoacylpyrrole), poly(methylpyrrole), etc.; the polyacetylene and its derivatives may include one or more of polyacetylene, fluorinated polyacetylene, polyvinylcarbazole (PVK), etc.; the polystyrene and its derivatives may include one or more of polystyrene, fluorinated polystyrene, chlorinated polystyrene, etc.; the polythiophene and its derivatives include one or more of polythiophene, poly(3-methylthiophene), poly(3,4-ethylenedioxythiophene) (PEDOT), etc.

[0033] In one embodiment, the organic-inorganic hybrid material may be a mixed material of the inorganic conductive material and the organic conductive material. Furthermore, the mass ratio of the organic conductive material to the inorganic conductive material is 1:(1-10), specifically 1:(1-3), 1:(3-5), 1:(5-8), 1:(8-10), etc. The mass ratio may improve the conductivity of the composite material.

[0034] In one embodiment, the repair agent is selected from a first polymer containing one or more of an amino group, a hydroxyl group, or a disulfide bond. In this embodiment, the repair agent can form dynamic hydrogen bonds through amino groups or hydroxyl groups, or through dynamic reversible formation and breaking of disulfide bonds, so as to further cross-link the first polymer and achieve self-repair of the composite material.

[0035] In one embodiment, the first polymer includes one or more of modified polyamide, modified polyurethane, etc. Specifically, the modified polyamide may include one or more of hyperbranched polyamide, hydroxyl-modified polyamide, and disulfide-modified polyamide. The modified polyurethane may include one or more of hyperbranched polyurethane, hydroxyl-modified polyurethane, amino-modified polyurethane, and disulfide-modified polyurethane.

[0036] In this embodiment, the modified polyamide and modified polyurethane can achieve self-repair of the composite material by forming dynamic hydrogen bonds or disulfide bonds in the composite material. In addition, the formation of dynamic hydrogen bonds or disulfide bonds can be carried out at room temperature without additional heating, etc., and will not cause thermal damage to the composite material, nor will it cause damage to the film layer or device containing or using the composite material.

[0037] In this embodiment, the hyperbranched polyamide contains a large number of amino groups, and the hydroxyl-modified polyamide contains a large number of hydroxyl groups, which can support the formation of a large number of dynamic hydrogen bonds in the composite material, increase the number of hydrogen bonds that can be formed, and can support the formation of multiple hydrogen bonds. Through the interaction of intramolecular and intermolecular hydrogen bonds, it is more conducive to the self-repair of the composite material. The disulfide bond-modified polyamide contains a large number of disulfide bonds, which are a kind of dynamic covalent bonds. The dynamic covalent bonds can be regenerated after breaking, thereby improving the self-repair performance of the composite material.

[0038] In this embodiment, the hydroxyl-modified polyurethane contains a large number of hydroxyl groups, and the amino-modified polyurethane contains a large number of amino groups, both of which can support the formation of a large number of dynamic hydrogen bonds in the composite material, and the intramolecular and intermolecular hydrogen bond interactions are beneficial to the self-repair of the composite material. The disulfide bond-modified polyurethane contains a large number of disulfide bonds, which are a type of dynamic covalent bond that can be regenerated after being broken, thereby improving the self-repair performance of the composite material.

[0039] In a specific embodiment, the hyperbranched polyamide can be obtained by the following steps: polyamine (such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, etc.) and acrylate compounds (such as ethyl acrylate, methyl acrylate, etc.) are dissolved in a solvent (such as methanol, ethanol, etc.) according to a molar ratio of (3-10): 1, reacting at 110-130°C in a nitrogen atmosphere for 2-3 hours, extracting and vacuum drying to obtain the hyperbranched polyamide. Further, the branching degree of the hyperbranched polyamide can be 41%-55%, specifically 41%-45%, 45%-48%, 48%-50%, 50%-55%, etc.

[0040] In a specific embodiment, the hydroxy-modified polyamide can be obtained by the following steps: a polyamine (such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, etc.) and an acrylate compound (such as ethyl acrylate, methyl acrylate, etc.) are dissolved in a solvent (such as methanol) at a molar ratio of (3-10):1, and reacted at 80°C in a nitrogen atmosphere for 1 hour to obtain a polymer precursor, and then 2-hydroxymethane-2-methyl-1,3-propanediol is added to the polyol at a molar ratio of (3-10):1 to the polymer precursor, and then the temperature is raised to 120°C and the reaction is continued with stirring for 2 hours. After extraction, the hydroxy-modified polyamide can be obtained.

[0041] Furthermore, the grafting rate of the hydroxyl-modified polyamide may be 2.8% to 3.5%, specifically 2.8% to 3.0%, 3.0% to 3.2%, 3.2% to 3.5%, etc.

[0042] In a specific embodiment, the disulfide bond-modified polyamide can be obtained by the following steps: a polyamine (such as diethylenetriamine, triethylenetetramine, tetraethylenepentamine, etc.) and an acrylate compound (such as ethyl acrylate, methyl acrylate, etc.) are dissolved in a solvent (such as methanol) at a molar ratio of (3-10):1, and reacted at 80°C in a nitrogen atmosphere for 1 hour to obtain a polymer precursor, and then the disulfide is added at a molar ratio of diallyl disulfide to the polymer precursor (3-10):1, and the temperature is raised to 120°C and stirred for 2.5 hours. After extraction, the disulfide-modified polyamide can be obtained.

[0043] Furthermore, the grafting rate of the disulfide bond-modified polyamide may be 2.2% to 3.1%, specifically 2.2% to 2.5%, 2.5% to 2.8%, 2.8% to 3.1%, etc.

[0044] In a specific embodiment, the hyperbranched polyurethane can be obtained by the following steps: The modified polyurethane can be obtained by the following steps: dissolving diphenylmethane 4,4′-diisocyanate and polyester diol in a molar ratio of 2:1 in N,N-dimethylformamide (DMF), heating to 80°C for reaction for 4 hours, and obtaining an isocyanate-terminated polyurethane prepolymer. 2,4,6-triaminopyridine is used as a chain extender and crosslinker, and is added to the polyurethane prepolymer, wherein the molar ratio of 2,4,6-triaminopyridine to the polyurethane prepolymer is diallyl disulfide: polyurethane prepolymer = (3-10): 1, and the hyperbranched polyurethane is obtained by reacting in a nitrogen atmosphere at 50-70°C for 1.5-2.5 hours.

[0045] Furthermore, the branching degree of the hyperbranched polyurethane may be 45% to 60%, specifically 45% to 48%, 48% to 50%, 50% to 55%, 55% to 60%, etc.

[0046] In a specific embodiment, the hydroxyl-modified polyurethane can be obtained by the following steps: dissolving diphenylmethane 4,4′-diisocyanate and polyester diol in a molar ratio of 2:1 in N,N-dimethylformamide (DMF), heating to 80°C for reaction for 4 hours, and obtaining an isocyanate-terminated polyurethane prepolymer. 2-amino-4-hydroxy-6-methylpyrimidine is used as a chain extender and crosslinker, and is added to the polyurethane prepolymer, wherein the molar ratio of 2-amino-4-hydroxy-6-methylpyrimidine to the polyurethane prepolymer is 2-amino-4-hydroxy-6-methylpyrimidine: polyurethane prepolymer = (3-10): 1, and then reacting in a nitrogen atmosphere at 70-90°C for 1.5-2.5 hours to obtain a hydroxyl-modified polyurethane.

[0047] Furthermore, the grafting rate of the hydroxyl-modified polyurethane is 2.5% to 3.2%, specifically 2.5% to 2.8%, 2.8% to 3.0%, 3.0% to 3.2%, etc.

[0048] In a specific embodiment, the amino-modified polyurethane can be obtained by the following steps: The modified polyurethane can be obtained by the following steps: dissolving diphenylmethane 4,4′-diisocyanate and polyester diol in a molar ratio of 2:1 in N,N-dimethylformamide (DMF), heating to 80°C for reaction for 4 hours, and obtaining an isocyanate-terminated polyurethane prepolymer. Using diazolidinyl urea as a chain extender and crosslinking agent, adding it to the polyurethane prepolymer, wherein the molar ratio of diazolidinyl urea to the polyurethane prepolymer is diallyl disulfide: polyurethane prepolymer = (3-10): 1, and reacting in a nitrogen atmosphere at 50-70°C for 1.5-2.5 hours to obtain the amino-modified polyurethane.

[0049] Furthermore, the grafting rate of the amino-modified polyurethane may be 2.5% to 3.2%, specifically 2.5% to 2.6%, 2.6% to 2.8%, 2.8% to 3.0%, 3.0% to 3.2%, etc.

[0050] In a specific embodiment, the disulfide bond-modified polyurethane can be obtained by the following steps: dissolving diphenylmethane 4,4′-diisocyanate and polyester diol in a molar ratio of 2:1 in N,N-dimethylformamide (DMF), heating to 80°C for reaction for 4 hours, and obtaining an isocyanate-terminated polyurethane prepolymer. Diallyl disulfide is used as a chain extender and crosslinker, and is added to the polyurethane prepolymer, wherein the molar ratio of diallyl disulfide to the polyurethane prepolymer is diallyl disulfide: polyurethane prepolymer = (3-10): 1, and reacting in a nitrogen atmosphere at 50-70°C for 1.5-2.5 hours to obtain the disulfide bond-modified polyurethane.

[0051] Furthermore, the grafting rate of the disulfide bond-modified polyurethane may be 2.0% to 2.8%, specifically 2.0% to 2.2%, 2.2% to 2.4%, 2.4% to 2.5%, 2.5% to 2.8%, 2.3% to 2.5%, etc.

[0052] In the above specific embodiments, the polyester diol may include one or more of polyethylene glycol, polytetrahydrofuran, polycaprolactone, etc. In a specific embodiment, the polyester diol is selected from polytetrahydrofuran.

[0053] It can be understood that in the above-mentioned hydroxyl-modified, amino-modified or disulfide-modified polyamides and polyurethanes, the polymer bodies are all hyperbranched and contain a large number of active functional groups. The polymers having hydroxyl groups, amino groups or disulfide bonds are grafted onto the functional groups of the polymer body by a grafting method for end-capping to obtain the corresponding modified polyamides and polyurethanes.

[0054] In another embodiment, the repair agent includes one or more of polyester, polyketone, polythiophene, epoxy resin, etc. The repair agent can achieve self-repair of the composite material based on a reversible Dieal-Alder reaction, and the reversible reaction condition is that the temperature is greater than or equal to 100°C, specifically 100-120°C, 120-140°C, 140-160°C, etc.

[0055] In one embodiment, the mass ratio of the repair agent to the conductive material is 1:(5-20), specifically 1:(5-18), 1:(8-18), 1:(8-15), 1:(10-15), 1:(10-13), 1:(5-8), 1:(18-20), etc. The mass ratio can provide the composite material with better conductivity and self-healing properties.

[0056] In one embodiment, when the conductor material is an organic conductive material or an organic-inorganic hybrid material, that is, when the conductor material includes a conductive polymer, the repair agent may include a first repair agent and a second repair agent, wherein the first repair agent includes a monomer of the conductive polymer, and the second repair agent includes a catalyst. The catalyst may catalyze the polymerization reaction of the monomer of the conductive polymer to form the conductive polymer.

[0057] In this embodiment, the monomer of the conductive polymer is used as a repairing agent, and the monomer of the conductive polymer is subjected to a catalytic polymerization reaction to form the conductive polymer, and the polymerized cross-linking is performed to make the composite material have self-repairing properties. Moreover, the monomer of the conductive polymer is subjected to a polymerization reaction to achieve self-repairing of the composite material, and the conductive polymer is formed by polymerization, which can increase the conductivity of the composite material.

[0058] It can be understood that the catalyst can be selected according to the monomer of the conductive polymer.

[0059] In one embodiment, the monomers of the conductive polymer can be polymerized at room temperature (20-30° C.) under the catalytic action of the corresponding catalyst to achieve self-repair of the composite material. In other embodiments, the polymerization of the monomers of the conductive polymer requires other conditions, such as illumination, heating, etc., and the composite material can be illuminated to promote self-repair of the composite material.

[0060] In a specific embodiment, the catalyst may include a photoinitiator, so as to achieve self-repair of the composite material under light irradiation conditions.

[0061] Specifically, the amount of the catalyst used can also be set accordingly according to the needs of the polymerization reaction of the monomer of the conductive polymer. For example, in one embodiment, the molar ratio of the catalyst to the monomer of the conductive polymer can be 1:3-10, specifically 1:3-5, 1:5-8, 1:8-10, etc.

[0062] In a specific embodiment, the conductive polymer is PEDOT, the monomer of which is 3,4-ethylenedioxythiophene, and the catalyst is iron salt and persulfate. Specifically, the molar ratio of the catalyst to the conductive polymer can be 1:5.

[0063] In another specific embodiment, the conductive polymer is polypyrrole, the monomer of which is pyrrole, and the catalyst is AlCl3 and CuCl. Specifically, the molar ratio of the catalyst to the monomer may be 1:5.

[0064] In another specific embodiment, the conductive polymer is polyaniline, the monomer of which is aniline, and the catalyst is ammonium persulfate and hydrochloric acid. Specifically, the molar ratio of the catalyst to the monomer may be 1:5.

[0065] Furthermore, the first repair agent may be a core-shell structure, a first core-shell, wherein the first core-shell comprises a first core and a first shell layer covering the first core. The material of the first core comprises a monomer of a conductive polymer. The material of the first shell may comprise one or more of epoxy resin, polyurethane, urea-formaldehyde resin, etc.

[0066] The second repairing agent may be a core-shell structure, a second core-shell, wherein the second core-shell comprises a second core and a second shell layer covering the second core. The material of the second core comprises a catalyst. The material of the second shell may comprise one or more of epoxy resin, polyurethane, urea-formaldehyde resin, etc.

[0067] The first repair agent and the second repair agent having a core-shell structure can separate the monomer of the conductive polymer and the corresponding catalyst, and under certain conditions, make the two contact to carry out a polymerization cross-linking reaction.

[0068] In the above embodiment, the materials of the first shell layer and the second shell layer will not react with the monomers or catalysts of the conductive polymers encapsulated therein, and the first shell layer and the second shell layer can be destroyed under mechanical stress, thereby releasing the materials in the core, that is, releasing the monomers of the conductive polymer and the corresponding catalyst, thereby realizing self-repair of the composite material through polymerization and cross-linking of the monomers of the conductive polymer.

[0069] It can be understood that one of the first repair agent and the second repair agent can be a core-shell structure, or both can be a core-shell structure.

[0070] In a specific embodiment, the conductive polymer includes polypyrrole, the first repair agent is a first core-shell formed by a pyrrole monomer dissolved in acetonitrile coated with an epoxy resin layer, and the second repair agent is a second core-shell formed by a catalyst (AlCl3 and CuCl) coated with an epoxy resin layer.

[0071] In a specific embodiment, the preparation method of the first core-shell of the pyrrole monomer dissolved in acetonitrile coated with epoxy resin is as follows: epoxy resin and pyrrole acetonitrile solution are added to a dichloromethane solution in a molar ratio of 4:1, magnetic stirring is used to dissolve and mix evenly, and then a 3% surfactant sodium dodecyl sulfate aqueous solution is added, and mechanical stirring is performed at 500-1000 rpm at room temperature for 4-6 hours until the solvent is completely volatilized. After filtering, the pyrrole wrapped with epoxy resin, i.e., the first core-shell, can be obtained.

[0072] In a specific embodiment, the preparation method of the second core shell of the catalyst coated with the epoxy resin layer is as follows: diisocyanate and butanediol are reacted at a molar ratio of 1:2 at 90°C for 5 hours to obtain a polyurethane prepolymer; an aqueous solution of AlCl3 and CuCl is added at a mass ratio of diisocyanate: catalyst = 3:1, after stirring and dispersing, ethylenediamine is added as a chain extender at a molar ratio of diisocyanate: ethylenediamine = 1:2, and the reaction is carried out at room temperature for 5 to 8 hours. After the reaction, freeze-drying is performed to obtain polyurethane-coated AlCl3 and CuCl capsules.

[0073] In another specific embodiment, the conductive polymer includes polyaniline, the first repair agent is a first core-shell formed by an epoxy resin-coated aniline monomer dissolved in methyl pyrrolidone, and the second repair agent is a second core-shell formed by an epoxy resin-coated catalyst (ammonium persulfate and hydrochloric acid).

[0074] In one embodiment, the composite material is formed by mixing the conductive material and the repair agent. The conductive material and the repair agent can make the composite material have relatively uniform conductivity and good film-forming property.

[0075] The present application also provides a method for preparing a composite material, comprising: mixing a conductive material and a repair agent in a solvent to obtain a composite material. The conductive material and the repair agent can refer to the relevant description of the composite material described above, and will not be repeated here. The solvent can include one or more of water, acetone, acetone, toluene, dimethylformamide, tetrahydrofuran, etc.

[0076] The mixing may be performed by a combination of one or more of stirring and ultrasound to improve the mixing uniformity of the conductive material and the repairing agent in the composite material.

[0077] The present application also provides an electrode, including the composite material provided by the present application. The electrode has good electrical conductivity and self-repairing properties. When a crack is generated due to scratches, bending, curvature or other deformations, the electrode can maintain normal electrical conductivity through self-repairing properties in the early stage, without causing cracks or fractures to cause the electrode to lose its functionality, thereby improving the wide application of the electrode, such as in flexible display devices, and can also improve the life and yield of the electrode, and improve the service life of the device including the electrode.

[0078] In one embodiment, the thickness of the electrode is 80-5000 nm, specifically 80-300 nm, 80-100 nm, 100-200 nm, 20-300 nm, 300-5000 nm, 300-500 nm, 500-1000 nm, 1000-2000 nm, 2000-3000 nm, 3000-4000 nm, 4000-5000 nm, etc. The electrode with the above thickness can have good conductivity and self-healing properties.

[0079] The present application also provides a photoelectric device, see Figure 1 , Figure 1 1 is a schematic diagram of the structure of an embodiment of a photoelectric device provided in the present application. The photoelectric device 100 includes a first electrode 10, a second electrode 20, and a functional layer 30. The first electrode 10 and the second electrode 20 are arranged opposite to each other, and the functional layer 30 is arranged between the first electrode 10 and the second electrode 20, wherein the material of the first electrode 10 includes the composite material provided in the present application; and / or the material of the second electrode 20 includes the composite material provided in the present application.

[0080] In one embodiment, the first electrode 10 may be composed of the composite material. In other embodiments, the first electrode 10 may include other materials besides the composite material, such as a high refractive index material, a low refractive index material, etc.

[0081] In one embodiment, the second electrode 20 may be composed of the composite material. In other embodiments, the second electrode 20 may include other materials besides the composite material, such as high refractive index material, low refractive index material, etc.

[0082] In the above embodiment, one or more of the first electrode 10 and the second electrode 20 in the photoelectric device 100 include the composite material provided in the present application. When scratched, bent, curved or otherwise deformed, the normal conductivity of the electrode can be maintained by the self-healing property of the material in the early stage of crack generation, without cracks or breaks causing the electrode to lose its functionality. This supports the bendability and deformability of the photoelectric device 100 including the first electrode 10 and the second electrode 20, and can be applied to the field of flexible displays, such as wearable devices. It can also improve the lifespan and conductivity uniformity of the first electrode 10 and the second electrode 20, thereby improving the lifespan of the photoelectric device 100.

[0083] In one embodiment, the functional layer 30 includes a light-emitting layer 33, and the light-emitting layer 33 is disposed between the first electrode 10 and the second electrode 20. The material of the light-emitting layer 33 is selected from organic light-emitting materials or quantum dot light-emitting materials.

[0084] The organic light-emitting material is selected from at least one of diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives or fluorene derivatives, TBPe fluorescent materials emitting blue light, TTPA fluorescent materials emitting green light, TBRb fluorescent materials emitting orange light, and DBP fluorescent materials emitting red light;

[0085] The quantum dots are selected from at least one of single structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials, the single structure quantum dots are selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds, the II-VI group compounds are selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe , CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe, and the IV-VI group compound is selected from SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, At least one of SnPbSSe, SnPbSeTe, and SnPbSTe, and the III-V compound is selected from GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, and GaI At least one of nNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; the core of the quantum dots of the core-shell structure is selected from any one of the above-mentioned single-structure quantum dots, and the shell material of the quantum dots of the core-shell structure is selected from at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS;

[0086] The perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n -2NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2 + At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

[0087] When n = 2, the inorganic metal halide octahedron MX6 4- The metal cation M is located at the center of the halogen octahedron, and the organic amine cation B fills the gap between the octahedrons to form an infinitely extended three-dimensional structure. When n>2, the inorganic metal halide octahedron MX6 connected by the top-sharing method 4-It extends in two dimensions to form a layered structure, with an organic amine cation bilayer (protonated monoamine) or an organic amine cation monolayer (protonated diamine) inserted between the layers, and the organic layer and the inorganic layer overlap to form a stable two-dimensional layered structure.

[0088] The thickness of the light emitting layer 33 may be 10-50 nm, specifically 10-40 nm, 20-40 nm, 20-30 nm, 10-20 nm, 40-50 nm, etc.

[0089] In one embodiment, the functional layer 30 further includes a hole functional layer 31, and the hole functional layer 31 is disposed between the first electrode 10 and the light-emitting layer 33. The hole functional layer 31 includes a hole injection layer 311 and / or a hole transport layer 312. When the hole functional layer 31 includes a two-layer structure of a hole injection layer 311 and a hole transport layer 312, the hole injection layer 311 is disposed close to the first electrode 10, and the hole transport layer 312 is disposed close to the light-emitting layer 33.

[0090] The material of the hole injection layer 311 is a material with hole injection capability, and can be selected from one or more of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid (PEDOT:PSS), 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanoquinone-dimethane (F4-TCNQ), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HATCN), copper phthalocyanine (CuPc), transition metal oxides, and transition metal sulfur compounds; wherein the transition metal oxides include one or more of NiO, MoO2, WO3, and CuO; and the metal sulfur compounds include one or more of MoS2, MoSe2, WS3, WSe3, and CuS.

[0091] The thickness of the hole injection layer 311 may be 30 nm to 50 nm, specifically 30 nm to 45 nm, 35 nm to 45 nm, 35 nm to 40 nm, 30 nm to 35 nm, 45 nm to 50 nm, etc.

[0092] The material of the hole transport layer 312 can be selected from materials having hole injection capability, such as poly(9,9-dioctylfluorene-co-N-(4-butylphenyl)diphenylamine) (TFB), polyvinylcarbazole (PVK), poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine) (poly-TPD), poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine) (PFB), 4,4',4"-tri(carbazole-9-yl)triphenylamine (TCATA), 4,4'-bis(9-carbazole)biphenyl (CBP), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine (TPD), N,N'-diphenyl-N,N'-(1-naphthyl)triphenylamine (TCATA), 4,4'-bis(9-carbazole)biphenyl (CBP), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine (TPD), N,N'-diphenyl-N,N'-(1-naphthyl)triphenylamine (TCATA), 4,4'-bis(9-carbazole)biphenyl (CBP), N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine (TPD), N,N'-diphenyl-N,N'-(1-naphthyl)triphenylamine (TCATA), 4,4'-diphenyl )-1,1'-biphenyl-4,4'-diamine (NPB), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonic acid) (PEDOT:PSS), 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanoquinone-dimethane (F4-TCNQ), 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene (HATCN), copper phthalocyanine (CuPc), Spiro-NPB, Spiro-TPD, doped graphene, undoped graphene, C60, P-type gallium nitride, doped or undoped NiO, V2O5, CrO3, CuO, CuS, MoO3, MoS2, MoSe2, WO3, WS2, WSe2 and CuSCN, etc., or one or more thereof.

[0093] The thickness of the hole transport layer 312 may be 30 nm to 50 nm, specifically 30 nm to 45 nm, 35 nm to 45 nm, 35 nm to 40 nm, 30 nm to 35 nm, 45 nm to 50 nm, etc.

[0094] In one embodiment, the functional layer 30 further includes an electronic functional layer 32, and the electronic functional layer 32 is disposed between the second electrode 20 and the light-emitting layer 33. The electronic functional layer 32 may include an electron injection layer 321 and / or an electron transport layer 322; when the electronic functional layer 32 includes the electron injection layer 321 and the electron transport layer 322, the electron injection layer 321 is disposed close to the second electrode 20, and the electron transport layer 322 is disposed close to the light-emitting layer 33.

[0095] In one embodiment, the material of the electron transport layer 322 may be a material known in the art for an electron transport layer. For example, it may be selected from one or more of doped or undoped inorganic nanocrystals and organic materials; wherein the undoped inorganic nanocrystals are selected from ZnO, TiO2, SnO2, Al2O3, GaO, Ga2O3, ZrO2, Fe2O3, CrO3, WO3, CdO, CuO, MoO2, ZnS, ZnSe, CdS, InP, GaP, SnO2, WO3, Ta2O3, HfO3, ZrSiO4, BaTiO3, BaZrO3, Si3N 4; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, In, Mn, Cd, Cs or Cu; the organic material is selected from one or more of polymethyl methacrylate, polyvinyl butyral, oxazole compounds, isoxazole compounds, triazole compounds, isothiazole compounds, oxadiazole compounds, thiadiazole compounds, perylene compounds or aluminum complexes.

[0096] The thickness of the electron transport layer 322 may be 30 nm to 60 nm, specifically 30 nm to 55 nm, 35 nm to 55 nm, 35 nm to 50 nm, 40 nm to 50 nm, 40 nm to 45 nm, etc.

[0097] In one embodiment, the material of the electron injection layer 321 is a material known in the art for electron injection layer, for example, it can be selected from but not limited to at least one of LiF, MgP, MgF2, Al2O3, Ga2O3, LiF / Yb, ZnO, Cs2CO3, RbBr, and Rb2CO3.

[0098] In one embodiment, when the materials of the second electrode 20 and the first electrode 10 do not use the composite material of the present application, their materials can be selected from electrode materials known in the art. For example, it can be selected from one or more of metal electrodes, carbon electrodes, doped or undoped metal oxide electrodes and composite electrodes; wherein the material of the metal electrode is selected from at least one of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg; the material of the carbon electrode is selected from at least one of graphite, carbon nanotubes, graphene and carbon fiber; the material of the doped or undoped metal oxide electrode is selected from at least one of ITO, FTO, ATO, AZO, GZO, IZO, MZO and AMO; the material of the composite electrode is selected from at least one of AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, TiO2 / Ag / TiO2 and TiO2 / Al / TiO2. Here, “ / ” represents a stacked structure. For example, the composite electrode AZO / Ag / AZO represents an electrode with a composite structure of three stacked layers consisting of an AZO layer, an Ag layer and an AZO layer.

[0099] It can be understood that the first electrode 10 and the second electrode 20 are a pair of electrodes, the first electrode 10 can be an anode, and the second electrode 20 can be a cathode.

[0100] It can be understood that, in addition to the above-mentioned functional layers, the optoelectronic device 100 may also be provided with some functional layers conventionally used in optoelectronic devices that help improve the performance of the optoelectronic device, such as an electron blocking layer, a hole blocking layer, etc.

[0101] It can be understood that the material and thickness of each layer of the optoelectronic device 100 can be set and adjusted accordingly according to the light emitting requirements of the optoelectronic device 100 .

[0102] The optoelectronic device 100 further includes a substrate (not shown), which may also be referred to as a substrate. The substrate may be a rigid substrate or a flexible substrate. The rigid substrate may be a ceramic material or various glass materials. The flexible substrate may be a substrate formed of materials such as polyimide film (PI) and its derivatives, polyethylene naphthalate (PEN), phosphoenolpyruvic acid (PEP) or diphenylene ether resin. In one embodiment, the material of the substrate includes glass, silicon wafer, polycarbonate, polymethyl methacrylate, polyethylene terephthalate, polyethylene naphthalate, polyamide, polyether sulfone, or a combination thereof.

[0103] It can be understood that the photoelectric device 100 can be an upright or inverted photoelectric device. When the photoelectric device 100 is an upright photoelectric device, the substrate is combined with the side of the anode away from the light-emitting layer 33. When the photoelectric device 100 is an inverted photoelectric device, the substrate is combined with the side of the cathode away from the light-emitting layer 33.

[0104] It can be understood that the first electrode 10, the light-emitting layer 33, the second electrode 20, the hole injection layer 311, the hole transport layer 312, the electron injection layer 321, the electron transport layer 322 and other film layers in the optoelectronic device provided in the present application can be prepared by conventional techniques in the art, such as chemical methods or physical methods. Among them, the chemical method includes chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and coprecipitation. The physical method includes physical plating and solution method, wherein the physical plating method includes: thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; the solution method can be spin coating, printing, inkjet printing, scraping, printing, dip pulling, immersion, spraying, rolling, casting, slit coating, and strip coating.

[0105] After the above-mentioned film layers are prepared, the optoelectronic device also involves packaging. The packaging process can be a common machine packaging or a manual packaging. In a specific embodiment, the oxygen content and water content in the packaging process environment are both lower than 0.1ppm to ensure the stability of the optoelectronic device 100.

[0106] The present application also relates to a display device, which includes the optoelectronic device provided in the present application. The display device can be any electronic product with a display function, including but not limited to smart phones, tablet computers, laptop computers, digital cameras, digital video cameras, smart wearable devices, smart weighing electronic scales, car displays, televisions or e-book readers, wherein the smart wearable device can be, for example, a smart bracelet, a smart watch, a virtual reality (VR) helmet, etc.

[0107] The technical scheme and technical effects of the present application are described in detail below through specific embodiments, comparative examples and experimental examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0108] Example 1

[0109] This embodiment provides an electrode and a method for preparing the same, comprising the following steps:

[0110] Silver nanoparticles were added to a disulfide bond-modified polyurethane solution (the mass ratio of disulfide bond-modified polyurethane to silver nanoparticles was 1:10, and the grafting rate of disulfide bond-modified polyurethane was 2.3% to 2.5%), and after being uniformly mixed by ultrasonic, electrodes were prepared on a flexible substrate polyethylene naphthalate (PEN) by screen printing to obtain electrodes with a line width of 2 cm, a length of 15 cm, and a thickness of 500 nm. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changed from the initial 150Ω to 200Ω.

[0111] Example 2

[0112] This embodiment is basically the same as the embodiment 1, except that the mass ratio of the disulfide bond-modified polyurethane to the silver nanoparticles is 1: 5. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 350Ω to 450Ω.

[0113] Example 3

[0114] This embodiment is basically the same as the embodiment 1, except that the mass ratio of the disulfide bond-modified polyurethane to the silver nanoparticles is 1:20. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 100Ω to 280Ω.

[0115] Example 4

[0116] This embodiment is basically the same as the embodiment 1, except that the mass ratio of the disulfide bond-modified polyurethane to the silver nanoparticles is 1:3. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 500Ω to 580Ω.

[0117] Example 5

[0118] This embodiment is basically the same as the embodiment 1, except that the mass ratio of the disulfide bond-modified polyurethane to the silver nanoparticles is 1:30. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 50Ω to 600Ω.

[0119] Example 6

[0120] This embodiment is basically the same as the embodiment 1, except that hydroxyl-modified polyamide is used instead of disulfide-modified polyurethane, and the grafting rate of hydroxyl-modified polyamide is 2.8% to 3.0%. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 170Ω to 230Ω.

[0121] Example 7

[0122] This embodiment provides an electrode and a method for preparing the same, comprising the following steps:

[0123] Step 1, adding graphene nanomaterials into a PEDOT solution to obtain an organic-inorganic hybrid conductive material; wherein the mass ratio of PEDOT to graphene nanomaterials is 1:5;

[0124] Step 2: Add the monomer 3,4-ethylenedioxythiophene of PEDOT respectively coated with epoxy resin and the catalyst (iron salt and persulfate) to the mixture in step 1, and mix them evenly by ultrasonic wave; wherein the molar ratio of the catalyst to 3,4-ethylenedioxythiophene is 1:5, and the total mass ratio of the monomer 3,4-ethylenedioxythiophene of PEDOT respectively coated with epoxy resin and the catalyst (iron salt and persulfate) added in this step to the mass ratio of the organic-inorganic hybrid conductive material in step 1 is 1:10.

[0125] Step 3: Prepare an electrode on a flexible substrate polyethylene naphthalate (PEN) by inkjet printing the mixture of step 2 to obtain an electrode with a line width of 2 cm, a length of 15 cm, and a thickness of 1000 nm.

[0126] Test: After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changed from the initial 100Ω to 200Ω.

[0127] Example 8

[0128] This embodiment is basically the same as embodiment 7, except that in step 1, the mass ratio of PEDOT to graphene nanomaterial is 1: 1. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from an initial 200Ω to 270Ω.

[0129] Example 9

[0130] This embodiment is substantially the same as embodiment 7, except that in step 1, the mass ratio of PEDOT to graphene nanomaterial is 1:10. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from an initial 80Ω to 300Ω.

[0131] Example 10

[0132] This embodiment is basically the same as embodiment 7, except that in step 1, the mass ratio of PEDOT to graphene nanomaterial is 1:0.5. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from an initial 450Ω to 500Ω.

[0133] Embodiment 11

[0134] This embodiment is basically the same as embodiment 7, except that in step 1, the mass ratio of PEDOT to graphene nanomaterial is 1:20. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 20Ω to 550Ω.

[0135] Example 12

[0136] This embodiment is basically the same as embodiment 7, except that: polypyrrole is used in step 1 instead of PEDOT; in step 2, pyrrole and catalyst (ammonium persulfate and hydrochloric acid) respectively coated with epoxy resin are added to the mixture in step 1. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 140Ω to 220Ω.

[0137] Embodiment 13

[0138] This embodiment is basically the same as the embodiment 1, except that hydroxyl-modified polyurethane is used instead of disulfide-modified polyurethane, and the grafting rate of hydroxyl-modified polyurethane is 3.0% to 3.2%. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 180Ω to 220Ω.

[0139] Embodiment 14

[0140] This embodiment is basically the same as the embodiment 1, except that amino-modified polyurethane is used instead of disulfide-modified polyurethane, and the grafting rate of amino-modified polyurethane is 2.6% to 2.8%. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 170Ω to 215Ω.

[0141] Embodiment 15

[0142] This embodiment is basically the same as embodiment 1, except that a hyperbranched polyamide is used instead of a disulfide bond-modified polyurethane, and the branching degree of the hyperbranched polyamide is 45% to 48%. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from an initial 150Ω to 240Ω.

[0143] Example 16

[0144] This embodiment is basically the same as the embodiment 1, except that disulfide bond-modified polyamide is used instead of disulfide bond-modified polyurethane, and the grafting rate of disulfide bond-modified polyamide is 2.5% to 2.8%. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changes from the initial 160Ω to 210Ω.

[0145] Comparative Example 1

[0146] Silver nanoparticles were screen-printed on a flexible substrate, polyethylene naphthalate (PEN), to prepare electrodes with a line width of 2 cm, a length of 15 cm, and a thickness of 500 nm. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changed from the initial 150 Ω to 8,000 Ω.

[0147] Comparative Example 2

[0148] The graphene nanomaterial was added to the PEDOT solution, and after being mixed evenly by ultrasonic wave, the electrode was prepared on the flexible substrate polyethylene naphthalate (PEN) by inkjet printing, and the electrode with a line width of 2cm, a length of 15cm and a thickness of 100nm was obtained. After 10,000 bending tests on a universal testing machine, the resistance of the flexible electrode changed from the initial 200Ω to 7000Ω.

[0149] From Examples 1-16 and Comparative Examples 1 and 2, it can be seen that:

[0150] Compared with Comparative Examples 1 and 2, the resistance of the electrodes of Examples 1-16 changes less before and after the bending test, and still has a relatively small resistance after the same bending test. The electrodes in Comparative Examples 1 and 2 may produce cracks during bending, resulting in an increase in the resistance of the electrodes, while the materials of the electrodes of Examples 1-16 are composite materials with self-healing properties, and self-heal at the early stage of cracks during the bending process, and still have a relatively small resistance after the same bending test, that is, still have good conductivity.

[0151] It can be seen from Examples 1-5 that the masses of the disulfide bond-modified polyurethane and silver nanoparticles are relatively small, and the square resistance of the formed flexible electrode changes greatly before and after the bending experiment, while the masses of the disulfide bond-modified polyurethane and silver nanoparticles are relatively large, and the initial square resistance of the formed flexible electrode will increase. That is, although the increase in the proportion of the disulfide bond-modified polyurethane increases the self-healing performance of the composite material, the increase to a certain extent will reduce the conductivity of the composite material.

[0152] Device Example 1

[0153] The device embodiment provides a quantum dot light emitting diode and a method for preparing the same, which specifically includes the following steps:

[0154] Step 1: The electrode prepared in Example 1 is used as the anode, the anode is cleaned, and then treated with ultraviolet-ozone for 15 minutes to improve the surface properties of the anode.

[0155] Step 2: In an air atmosphere, spin-coat PEDOT:PSS (the molar ratio of PEDOT to PSS is 1:1) on the anode and bake at 150°C for 15 min to obtain a hole injection layer with a thickness of 40 nm.

[0156] Step 3: In an argon atmosphere, spin-coat TFB on the hole injection layer and bake at 150° C. for 20 min to obtain a hole transport layer with a thickness of 40 nm.

[0157] Step 4: Spin-coat green quantum dots (CdSe / ZnSe) on the interface functional layer and bake at 100° C. for 10 min to obtain a light-emitting layer with a thickness of 25 nm.

[0158] Step 5: Spin-coat ZnO nanoparticles on the light-emitting layer and bake at 80° C. for 10 min to form an electron transport layer with a thickness of 50 nm.

[0159] Step 6: Prepare a cathode on the electron transport layer by the preparation method of Example 1 to obtain a cathode with a thickness of 35 nm.

[0160] Step 7: Perform UV curing adhesive encapsulation to obtain a quantum dot light emitting diode.

[0161] Device Example 2

[0162] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 2 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 2.

[0163] Device Example 3

[0164] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 3 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 3.

[0165] Device Example 4

[0166] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 4 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 4.

[0167] Device Example 5

[0168] This device embodiment is basically the same as device embodiment 1, and the only difference is that: in step 1, the electrode prepared in embodiment 5 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 5.

[0169] Device Example 6

[0170] This device embodiment is basically the same as device embodiment 1, and the only difference is that: in step 1, the electrode prepared in embodiment 6 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 6.

[0171] Device Example 7

[0172] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 7 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 7.

[0173] Device Example 8

[0174] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 8 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 8.

[0175] Device Example 9

[0176] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 9 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 9.

[0177] Device Example 10

[0178] This device embodiment is basically the same as device embodiment 1, and the only difference is that in step 1, the electrode prepared in embodiment 10 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 10.

[0179] Device Example 11

[0180] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 11 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 11.

[0181] Device Example 12

[0182] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 12 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 12.

[0183] Device Example 13

[0184] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 13 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 13.

[0185] Device Example 14

[0186] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 14 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 14.

[0187] Device Example 15

[0188] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 15 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 15.

[0189] Device Example 16

[0190] This device embodiment is basically the same as device embodiment 1, with the only difference being that in step 1, the electrode prepared in embodiment 16 is used as the anode; in step 6, a cathode is prepared on the electron transport layer by the preparation method of embodiment 16.

[0191] Device Comparison Example 1

[0192] The device embodiment of this invention is basically the same as the device embodiment 1, except that: in step 1, an ITO substrate is used as the anode substrate; in step 6, the vacuum degree is 4x10 -6 Pa, Ag is evaporated on the electronic functional layer at a rate of A cathode with a thickness of 100 nm was obtained.

[0193] Experimental example

[0194] The quantum dot light-emitting diodes of the unbent or bent device embodiments 1-16 and the device comparative example 1 were subjected to performance tests, including external quantum efficiency EQE and lifespan T95_1knit. Among them, the external quantum efficiency EQE was measured using an EQE optical test instrument, and the lifespan T95_1knit was measured when the quantum dot light-emitting diode was driven by a constant current (2mA current). The time required for the brightness to decay from 100% to 95% (measured T95) was first recorded, and then the time required for the brightness of each optoelectronic device to decay from 100% to 95% at a brightness of 1000nit (T95_1knit) was calculated. The test results are shown in Table 1 below.

[0195] Table 1

[0196]

[0197]

[0198] It can be seen from Table 1 that, compared with device comparison example 1, the lifespan of the quantum dot light-emitting diodes of device embodiments 1 to 16 after bending is significantly improved, and the lifespan of the quantum dot light-emitting diodes of device embodiments 1 to 16 is still maintained at a good level when not bent.

[0199] The composite materials and preparation methods thereof, optoelectronic devices and display devices provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technicians in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite material, characterized in that: Includes conductive materials and repair agents; Wherein, the repair agent comprises a first polymer containing one or more of an amino group, a hydroxyl group or a disulfide bond, and the first polymer comprises one or more of a modified polyamide or a modified polyurethane; or The repair agent includes a monomer of a conductive polymer and a catalyst.

2. The composite material according to claim 1, characterized in that The modified polyamide includes one or more of hyperbranched polyamide, hydroxyl-modified polyamide, and disulfide bond-modified polyamide; and / or The modified polyurethane includes one or more of hyperbranched polyurethane, hydroxyl-modified polyurethane, amino-modified polyurethane and disulfide bond-modified polyurethane.

3. The composite material according to claim 2, characterized in that The branching degree of the hyperbranched polyamide is 41% to 55%; and / or The grafting rate of the hydroxyl-modified polyamide is 2.8% to 3.5%; and / or The grafting rate of the disulfide bond modified polyamide is 2.2% to 3.1%; and / or The branching degree of the hyperbranched polyurethane is 45% to 60%; and / or The grafting rate of the hydroxyl-modified polyurethane is 2.5% to 3.2%; and / or The grafting rate of the amino-modified polyurethane is 2.5% to 3.2%; and / or The grafting rate of the disulfide bond modified polyurethane is 2.0% to 2.8%.

4. The composite material according to claim 1, characterized in that The repair agent includes a first repair agent and a second repair agent, the first repair agent includes a monomer of the conductive polymer, and the second repair agent includes the catalyst; Wherein, the first repair agent is a core-shell structure, including a first core and a first shell layer covering the first core, and the material of the first core includes a monomer of a conductive polymer; and / or The second repair agent is a core-shell structure, including a second core and a second shell layer covering the second core, and the material of the second core includes the catalyst.

5. The composite material according to claim 4, characterized in that When the monomer of the conductive polymer includes 3,4-ethylenedioxythiophene, the catalyst includes iron salt and persulfate; and / or When the monomer of the conductive polymer includes pyrrole, the catalyst includes AlCl3 and CuCl; and / or When the monomer of the conductive polymer includes aniline, the catalyst includes ammonium persulfate and hydrochloric acid; and / or The material of the first shell layer includes one or more of epoxy resin, polyurethane, and urea-formaldehyde resin; and / or The material of the second shell layer includes one or more of epoxy resin, polyurethane, and urea-formaldehyde resin.

6. The composite material according to claim 1, characterized in that The conductivity of the conductive polymer formed by the polymerization of the conductive polymer monomer catalyzed by the catalyst is greater than or equal to 50 S / cm; and / or The conductive polymer includes one or more of polypyrrole and its derivatives, polyacetylene and its derivatives, polystyrene and its derivatives, polythiophene and its derivatives, polyparaphenylene and its derivatives.

7. The composite material according to any one of claims 1 to 6, characterized in that: The mass ratio of the repairing agent to the conductive material is 1:(5-20); and / or The conductive material is an inorganic conductive material, an organic conductive material or an organic-inorganic hybrid material, wherein the organic-inorganic hybrid material is a mixed material of the inorganic conductive material and the organic conductive material, and the mass ratio of the organic conductive material to the inorganic conductive material is 1:(1-10); and / or The molar ratio of the catalyst to the monomer of the conductive polymer is 1:3-10.

8. The composite material according to claim 7, characterized in that The inorganic conductive material includes one or more of a metal material and a carbon material, the metal material includes at least one of Al, Ag, Cu, Mo, Au, Ba, Ca and Mg, and the carbon material includes at least one of graphite, carbon nanotubes, graphene and carbon fiber; and / or The organic conductive material includes a second polymer, and the conductivity of the second polymer is greater than or equal to 50 S / cm.

9. The composite material according to claim 8, characterized in that The second polymer includes one or more of polypyrrole and its derivatives, polyacetylene and its derivatives, polystyrene and its derivatives, polythiophene and its derivatives, polyparaphenylene and its derivatives; and / or When the repair agent includes the monomer of the conductive polymer and the catalyst, the conductive material is selected from an organic conductive material or an organic-inorganic hybrid material, wherein the second polymer contained in the organic conductive material or the organic-inorganic hybrid material is the same as the conductive polymer formed by the polymerization of the monomer of the conductive polymer catalyzed by the catalyst.

10. An electrode, characterized in that: The composite material comprises the composite material according to any one of claims 1 to 9.

11. A photoelectric device, characterized in that: include: A first electrode and a second electrode arranged opposite to each other; A functional layer is disposed between the first electrode and the second electrode; Wherein, the material of the first electrode comprises the composite material according to any one of claims 1 to 9; and / or, the material of the second electrode comprises the composite material according to any one of claims 1 to 9.

12. The optoelectronic device according to claim 11, characterized in that: The functional layer comprises a light-emitting layer, the material of the light-emitting layer is selected from an organic light-emitting material or a quantum dot light-emitting material, the organic light-emitting material is selected from at least one of diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives or fluorene derivatives, TBPe fluorescent materials emitting blue light, TTPA fluorescent materials emitting green light, TBRb fluorescent materials emitting orange light and DBP fluorescent materials emitting red light; the quantum dot light-emitting material is selected from at least one of a single structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material, and the single structure quantum dot is selected from at least one of a II-VI group compound, a IV-VI group compound, a III-V group compound and a I-III-VI group compound. One, the II-VI compound is selected from the group consisting of CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe , CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, At least one of HgZnSeTe and HgZnSTe, the IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, SnPbSTe, the III-V group compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, At least one of GaPAs, GaPSb, AlNP, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb, and the I-III-VI group compound is at least one of CuInS2, CuInSe2 and AgInS2;The core of the quantum dots of the core-shell structure is selected from any one of the above-mentioned single-structure quantum dots, and the shell material of the quantum dots of the core-shell structure is selected from at least one of CdS, CdTe, CdSeTe, CdZnSe, CdZnS, CdSeS, ZnSe, ZnSeS and ZnS; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the general structural formula of the inorganic perovskite semiconductor is AMX3, wherein A is Cs; + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of; and / or The functional layer comprises a hole functional layer, and the hole functional layer comprises one or both of a hole injection layer and a hole transport layer, and the material of the hole transport layer is selected from poly(9,9-dioctylfluorene-co-N-(4-butylphenyl)diphenylamine), polyvinylcarbazole, poly(N,N'-bis(4-butylphenyl)-N,N'-bis(phenyl)benzidine), poly(9,9-dioctylfluorene-co-bis-N,N-phenyl-1,4-phenylenediamine), 4,4',4"-tri(carbazole-9-yl)triphenylamine, 4,4'-bis(9-carbazole)biphenyl, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-1,1'-biphenyl-4,4'-diamine, N,N'-diphenyl-N,N'-(1-naphthyl)-1,1'-biphenyl-4,4'-diamine, poly(3, 4-ethylenedioxythiophene)-poly(styrene sulfonic acid), Spiro-NPB, Spiro-TPD, TAPC, TPH; and / or the material of the hole injection layer is selected from one or more of poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid, 2,3,5,6-tetrafluoro-7,7',8,8'-tetracyanoquinone-dimethane, 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, copper phthalocyanine, transition metal oxides, transition metal sulfur compounds, the transition metal oxides include one or more of nickel oxide, molybdenum oxide, tungsten oxide, chromium oxide, copper oxide, the metal sulfur compounds include one or more of molybdenum sulfide, molybdenum selenide, tungsten sulfide, tungsten selenide, copper sulfide; and / or The functional layer includes an electronic functional layer, and the electronic functional layer includes one or both of an electron injection layer and an electron transport layer, and the material of the electron transport layer is selected from one or more of doped or undoped inorganic nanocrystals and organic materials; wherein the undoped inorganic nanocrystals are selected from one or more of ZnO, TiO2, SnO2, Al2O3, GaO, SiO2, Ga2O3, ZrO2, NiO, ZnS, ZnSe, CdS, InP, GaP, and BaTiO3; the doped inorganic nanocrystals include the undoped inorganic nanocrystals and doping elements, and the doping elements are selected from one or more of Mg, Ca, Li, Ga, Al, Co, and Mn; the organic material is selected from one or both of polymethyl methacrylate and polyvinyl butyral; and / or the material of the electron injection layer is selected from but not limited to at least one of LiF, LiF / Yb, MgP, MgF2, Al2O3, Ga2O3, ZnO, Cs2CO3, Rb2CO3, and RbBr.

13. A display device, characterized in that: The display device comprises the optoelectronic device according to any one of claims 11-12.

Citation Information

Cited By

  • Monoatom modified carbon composite wave-absorbing material and preparation method thereof

    CN119570444A