Catalyst for non-oxidative conversion of hydrocarbons to hydrogen
By using a catalyst containing a specific matrix and metal dopants, hydrocarbons are converted into hydrogen, solving the problems of carbon-intensive and energy-intensive processes in existing technologies and achieving efficient and low-carbon hydrogen production.
Patent Information
- Application Number
- CN202380030609.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-01
- Filing Date
- 2023-03-01
- Publication Date
- 2024-11-12
AI Technical Summary
Existing technologies for hydrogen production suffer from carbon- and energy-intensive problems, necessitating a solution for efficient hydrogen production under non-oxidizing conditions.
A catalyst containing a specific matrix and metal dopants is used. The matrix includes molten silica, quartz, glass, zeolite, etc., and the metal dopants are Fe, Ni, Co, Cu, Zn, Mn, etc. Hydrocarbons are converted into hydrogen through a non-oxidative process, avoiding the product of high-temperature molten ferrous metasilicate and SiO2.
It enables efficient hydrogen production under non-oxidizing conditions, reducing carbon emissions and energy consumption while improving production efficiency.
Smart Images

Figure SMS_1
Abstract
Description
[0001] Inventors: Xiaoying OUYANG; Alexander KUPERMAN; Huping LUO; Lin LI Public content area
[0002] The present disclosure relates to systems, methods, and catalysts for the non-oxidative production of hydrogen from hydrocarbons, such as natural gas.
[0003] Background and Overview
[0004] Hydrogen is one of the more important options for future clean energy. Unfortunately, many commercially available technologies such as steam methane reforming to produce hydrogen are carbon intensive. Although the use of carbon capture and storage can reduce the carbon footprint, the available processes are often energy intensive. What is needed is a solution to produce hydrogen without being carbon intensive. It would also be advantageous if such a solution were relatively energy efficient and cost effective.
[0005] Advantageously, the present application relates to new systems, methods and catalysts that can non-oxidatively produce hydrogen from hydrocarbons such as natural gas. The solution is substantially non-carbon intensive, energy efficient and / or cost efficient.
[0006] The present application relates in one embodiment to a catalyst for the non-oxidative conversion of hydrocarbons into hydrogen. The catalyst comprises a matrix comprising fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y (where 4x+2y=4), SiO a N b (where 2a+3b=4), BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof. A metal dopant is embedded in the matrix, wherein the metal dopant comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof. The catalyst is not a product of melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
[0007] In another embodiment, the present application relates to a process for preparing a catalyst. The process comprises doping a metal in a matrix material, wherein the metal comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof. The matrix comprises fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y (where 4x+2y=4), SiO a N b(where 2a+3b=4), BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof. Doping does not include melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
[0008] In another embodiment, the present application relates to a process for the non-oxidative conversion of hydrocarbons into hydrogen. The process comprises contacting a hydrocarbon with a catalyst under conditions that convert the hydrocarbon into hydrogen. The catalyst comprises a matrix comprising fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y (where 4x+2y=4), SiO a N b (where 2a+3b=4), BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof. The metal dopant is embedded in the matrix, wherein the metal dopant comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof. The catalyst is not a product of melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
[0009] These and other objects, features and advantages of exemplary embodiments of the present disclosure will become apparent when the following detailed description of exemplary embodiments of the present disclosure is read in conjunction with the appended claims.
[0010] Detailed Description
[0011] The following description of the embodiments provides non-limiting representative examples, and its reference numbers particularly describe the features and teachings of different aspects of the present invention. The described embodiments should be considered to be able to be implemented alone or in combination with other embodiments from the description of the embodiments. Those of ordinary skill in the art who review the description of the embodiments should be able to learn and understand the different described aspects of the present invention. The description of the embodiments should promote understanding of the present invention, so that other implementations that are not specifically covered but within the knowledge of those skilled in the art reading the description of the embodiments will be understood to be consistent with the application of the present invention.
[0012] New catalyst and process for preparing catalyst
[0013] The present application relates in one embodiment to novel catalysts for the non-oxidative conversion of hydrocarbons to hydrogen.The catalyst typically comprises a matrix and a metal dopant.
[0014] The matrix used for the catalyst may vary depending on the desired application, metal dopants, and / or other factors. Typically, the matrix comprises fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC xO y (where 4x+2y=4), SiO a N b (where 2a+3b=4), BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite, or any mixture thereof. As used herein, perovskite refers to any material having a crystal structure similar to the mineral known as perovskite. In some embodiments, perovskite has the chemical formula ABX3, where A and B are two cations of very different sizes, and X is an anion such as oxygen bonded to both.
[0015] The zeolite may be an MFI type zeolite and / or may have a pore diameter of 4 angstroms to 20 angstroms and / or have a Si / Al atomic ratio of 5-300.
[0016] The metal dopant is typically embedded in the matrix. The metal dopant comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof. In some embodiments, the embedded metal dopant comprises isolated metal atoms, which are substantially free of aggregates having a size greater than 1 nm and / or the embedded metal dopant comprises isolated metal atoms in an amount to substantially reduce coking in the non-oxidative conversion of hydrocarbons such as natural gas or methane to hydrogen. The amount of isolated metal atoms is generally as high as reasonably possible, and in some embodiments may be greater than about 40 or greater than about 50% of all embedded metal dopants. The catalyst is typically not the product of melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
[0017] Any suitable process may be used to produce the novel catalyst. Typically, a suitable process comprises doping a metal in a matrix material, wherein the metal comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof and the matrix comprises fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y (where 4x+2y=4), SiO a N b (where 2a+3b=4), BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof.
[0018] Doping can be accomplished in a number of different ways, which may be selected depending on available equipment, materials, desired catalysts, and other factors.
[0019] In one embodiment, doping includes ball milling the matrix material with one or more of SiO2, B2O3, Fe2O3 or mixtures thereof to form a ball milled product; melting the ball milled product to form a molten state and then cooling to form a cooled product; acid leaching the cooled product to remove at least a majority of the aggregated metals; and drying the acid leached product to form a catalyst.
[0020] In another embodiment, doping includes forming a gel. The process of forming the gel includes combining a liquid source for matrix formation with an inorganic metal salt or inorganic metal alkoxide; and hydrolyzing to form the gel. The gel can be dried, melted, and acid leached to remove at least a majority of the aggregated metal. Drying can also be used to form the catalyst.
[0021] In another embodiment, doping includes melting the metal-containing zeolite; acid leaching the molten metal-containing zeolite to remove at least a majority of the aggregated metal; and drying the acid-leached molten metal-containing zeolite to form the catalyst.
[0022] In another embodiment, doping includes inserting the desired metal into silanol nests within the silica matrix; melting the metal into the matrix; acid leaching the molten metal matrix; and drying the acid leached molten metal matrix to form the catalyst.
[0023] In another embodiment, doping includes sublimating an organometallic precursor onto high surface area dehydroxylated silica to form a single site iron product; melting the metal to the single site iron product; acid leaching the molten metal single site iron product; and drying the acid leached molten metal single site iron product to form a catalyst.
[0024] In another embodiment, doping includes washcoating a monolithic catalyst support, wherein the monolith comprises ceramic, silica, quartz, glass, metal, silicon carbide, silicon nitride, boron nitride, metal oxides, or any combination thereof; melting a metal to the washcoated monolithic catalyst support; acid leaching the melted washcoated monolithic catalyst support; and drying the acid leached melted washcoated monolithic catalyst support to form a catalyst. The metal oxide may be selected according to the desired catalyst and properties and may include titanium oxide, iron oxide, zirconium oxide, mixed metal oxides, or any combination thereof. In some embodiments, the catalyst may be melted to form an amorphous melted catalyst, and the amorphous melted catalyst may then be shaped to obtain a desired shape such as a honeycomb monolith or a column.
[0025] Process for the non-oxidative conversion of hydrocarbons into hydrogen using a novel catalyst
[0026] The catalyst described above can be used, for example, in a process for non-oxidative conversion of hydrocarbons such as natural gas to produce hydrogen and possible other products. The process typically includes contacting a hydrocarbon such as natural gas with a catalyst described above and / or a mixture of catalysts comprising one of the catalysts described above. The contact is typically performed under conditions where the hydrocarbon is converted into hydrogen. The process can also produce light hydrocarbon products such as ethylene, benzene, naphthalene or any mixture thereof.
[0027] In the foregoing description, various embodiments have been described with reference to the accompanying drawings. However, it will be apparent that various modifications and changes may be made thereto and that additional embodiments may be implemented without departing from the broader scope of the invention as set forth in the following claims. The description and drawings are therefore to be regarded in an illustrative rather than a restrictive sense. Example
[0028] The following examples are provided by way of illustration and are not intended to be limiting. Example 1
[0029] 0.25% Fe / SiO2 catalyst
[0030] 0.18 g of Fe(NO3)3·9H2O and 10 g of industrial grade silica gel with a pore size of 60 Å and a particle size of 40–63 µm were mixed and ball milled at 400 rpm for 12 h under air. Next, the mixture was pressed into pellets in a die set using a hydraulic press and then calcined at 550°C in air. The final catalyst was obtained after sieving it to 20-40 mesh. Example 2
[0031] 0.5% Fe / SiO2 catalyst
[0032] 0.36 g Fe(NO3)3·9H2O and 10 g silica gel (high purity grade Davisil Grade 643, 150 Å, 200–425 mesh) were mixed and ball milled at 400 rpm for 12 h under air. Next, the mixture was pressed into pellets in a die set using a hydraulic press and then calcined at 700°C in air. The resulting sample was crushed and sieved to 100–200 mesh before being impregnated in an aqueous HNO3 solution (1 mol / L) at 60°C for 5 h. The impregnated sample was dried at 130°C overnight. The final loading of Fe was 0.37%. Example 3
[0033] 0.5% Fe / TiO2 catalyst (sample c)
[0034] This catalyst was prepared by an impregnation method. 10 g of TiO2 (HOMBIKAT 8602, Venator) was mixed with 0.36 g of Fe(NO3)3·9H2O dissolved in 10 g of deionized water and then aged for 24 h. The mixture was then dried at 130 °C for 5 h. Finally, the material was calcined at 550 °C for 4 h. The obtained sample was crushed and sieved to 100-200 mesh before being impregnated in an aqueous HNO3 solution (1 mol / L) at 60 °C for 5 h. The impregnated sample was dried at 130 °C overnight. The final loading of Fe was 0.13%. Example 4
[0035] Bc 0.9 Fe 0.07 Co 0.03 O3 Catalyst
[0036] 0.1 mol BaO2, 0.9 mol CeO2, 0.07 mol FeO and 0.01 mol Co3O4 were mixed and ball milled at 400 rpm for 24 hours in air. Next, the mixture was pressed into pellets in a die set using a hydraulic press and then calcined at 1000°C for 8 hours in air. The calcined sample was crushed and ball milled at 400 rpm for another 24 hours in air, followed by pressure granulation and calcination at 1000°C for another 8 hours in air. The final catalyst was obtained after sieving to 40-60 mesh. Example 5
[0037] 20% Zn / SiC catalyst
[0038] 40.5 g ZnO, 100 g SiC and 10 g deionized water were mixed and subjected to ball milling at 450 rpm for 4 hours under air. The mixture was filtered and dried at 130° C. for 4 hours to produce the final catalyst. Example 6
[0039] 1% Ni / Al2O3 catalyst
[0040] 2000 g Al2O3 (Sasol PURALOX TH 100), 100 g Ni(NO3)2.6H2O and 1600 g deionized water were mixed in a Littleford mixer for 9 hours at 60° C. The mixture was dried at 130° C. and then calcined at 600° C. for 2 hours. Example 7
[0041] 0.75% Fe / SiO2 catalyst
[0042] 0.11 g of Fe2O3 and 10 g of industrial grade silica gel with a pore size of 60 Å and a particle size of 40–63 µm were mixed and ball milled at 400 rpm for 12 h under air. Next, the mixture was pressed into pellets in a die set using a hydraulic press and then calcined at 1700°C in N2. The final catalyst was obtained after sieving to 20-40 mesh. Example 8
[0043] 0.8% Fe / SiO2 catalyst
[0044] This catalyst was prepared using a sol-gel method. 51.6 g of tetraethoxysilane (TEOS) was mixed with 662 mg of Fe(NO3)3·9H2O and 8 mL of ethanol in 48 g of aqueous nitric acid (15 wt%) and then stirred at 50°C for 4 hours. The resulting gel was first dried at 130°C in air for 3 hours and then heated at 1700°C in N2 for 2 hours. Example 9
[0045] Catalytic testing
[0046] The catalysts prepared in Examples 1-8 were tested for the non-oxidative conversion of methane to hydrogen. The operating conditions included a temperature of 1080° C., in a feed gas comprising 90% CH4 / 10% N2, at a total flow rate of 120 mL / min, at ambient pressure. The catalytic test results are reported in Table 1.
[0047] Table 1
Claims
1. A catalyst for the non-oxidative conversion of hydrocarbons into hydrogen, wherein the catalyst comprises: A matrix comprising fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y 、SiO a N b , BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof, wherein 4x+2y=4, and wherein 2a+3b=4; and a metal dopant embedded in the matrix, wherein the metal dopant comprises Fe, Ni, Co, Cu, Zn, Mn, or any mixture thereof; Provided that the catalyst is not the product of melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
2. The catalyst of claim 1, wherein the intercalated metal dopant comprises isolated metal atoms substantially free of aggregates.
3. The catalyst of claim 1, wherein the embedded metal dopant comprises isolated metal atoms in an amount that substantially reduces coking in the non-oxidative conversion of hydrocarbons to hydrogen.
4. A method for preparing a catalyst, comprising: doping a matrix material with a metal, wherein the metal comprises Fe, Ni, Co, Cu, Zn, Mn or any mixture thereof; The matrix comprises fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y 、SiO a N b , BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof, wherein 4x+2y=4, and wherein 2a+3b=4; Provided that the doping does not include melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
5. The method of claim 4, wherein doping comprises: ball milling the matrix material and one or more of SiO2, B2O3, Fe2O3 or a mixture thereof to form a ball milling product; melting the ball-milled product to form a molten state and then cooling to form a cooled product; acid leaching the cooled product to remove at least a majority of the aggregated metals; and The acid leached product is dried to form a catalyst.
6. The method according to claim 4, wherein the doping comprises: Forming a gel, wherein the process of forming a gel comprises: combining a liquid source for matrix formation with an inorganic metal salt or an inorganic metal alkoxide; and Hydrolyze to form a gel; drying the gel; and melting the dried gel; acid leaching the molten dried gel to remove at least a majority of the aggregated metals; and The acid-impregnated melt-dried gel is dried to form a catalyst.
7. The method according to claim 4, wherein the doping comprises: melting a zeolite containing a metal; acid leaching the molten metal-containing zeolite to remove at least a majority of the aggregated metal; and The acid leached molten metal-containing zeolite is dried to form the catalyst.
8. The method according to claim 4, wherein the doping comprises: inserting the metal into silanol pockets within a silicon dioxide matrix; melting a metal into the matrix; Acid leaching the molten metal matrix; and The acid-leached molten metal matrix is dried to form the catalyst.
9. The method according to claim 4, wherein the doping comprises: subliming an organometallic precursor onto high surface area dehydroxylated silica to form a single site iron product; melting metal to the single site iron product; acid leaching the molten metallic single site iron product; and The acid leached molten metallic single site iron product is dried to form a catalyst.
10. The method according to claim 4, wherein the doping comprises: A support coated monolithic catalyst support, wherein the monolith comprises ceramic, silica, quartz, glass, metal, silicon carbide, silicon nitride, boron nitride, metal oxide, or any combination thereof; melting a metal to a support-coated monolithic catalyst support; acid leaching the melted support-coated monolithic catalyst support; and The acid-leached melt-supported coated monolith catalyst support is dried to form a catalyst.
11. The method of claim 10, wherein the metal oxide comprises titanium oxide, iron oxide, zirconium oxide, a mixed metal oxide, or any combination thereof.
12. The method of claim 10, further comprising melting the catalyst to form an amorphous molten catalyst, and shaping the amorphous molten catalyst to obtain a desired shape.
13. The method of claim 12, wherein the desired shape comprises a honeycomb monolith. The method of claim 12 , wherein the desired shape comprises a column.
15. A method for non-oxidative conversion of hydrocarbons into hydrogen, comprising: contacting the hydrocarbon with a catalyst under conditions to convert the hydrocarbon into hydrogen; The catalyst comprises: A matrix comprising fused silica, quartz, glass, zeolite, Si3N4, SiC, SiC x O y 、SiO a N b , BN, TiO2, ZrO2, Al2O3, CeO2, Nb2O5, La2O3, perovskite or any mixture thereof, wherein 4x+2y=4, and wherein 2a+3b=4; and a metal dopant embedded in the matrix, wherein the metal dopant comprises Fe, Ni, Co, Cu, Zn, Mn, or any mixture thereof; Provided that the catalyst is not the product of melting ferrous metasilicate and SiO2 at a temperature of 500°C to 2400°C.
16. The method of claim 15, wherein the method further comprises producing light hydrocarbon products.
17. The process of claim 16, wherein the light hydrocarbon product comprises ethylene, benzene, naphthalene, or any mixture thereof.
18. The method of claim 15, wherein the hydrocarbon comprises natural gas.
19. The method of claim 15, wherein the zeolite is an MFI-type zeolite.
20. The method of claim 15, wherein the zeolite comprises a pore diameter of 4 angstroms to 20 angstroms.
21. The method of claim 15, wherein the zeolite has a Si / Al atomic ratio of 5 to 300.