Method for producing zeolite catalyst having silica coating, and zeolite catalyst

By forming a thin layer of silica coating on the zeolite catalyst, the problems of low activity and reduced harvesting rate in the production of xylene in the prior art are solved, and the preparation of xylene with high ratio and high harvesting rate is achieved, which improves the catalyst performance.

CN118946407APending Publication Date: 2024-11-12KAWASAKI JUKOGYO KK +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202380030860.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, when producing xylene, it is difficult to obtain paraxylene with high ratio and high harvest rate, and the catalyst activity is low, resulting in a decrease in the harvest rate of xylene.

Method used

Using a zeolite catalyst with a silica coating, a mixture of a structure guide agent containing tetraethylammonium and a silica source is prepared by mixing a zinc source with an MFI type zeolite, and hydrothermal synthesis is performed to form a thin layer of dioxide. Silicon coating improves the activity and harvesting rate of the catalyst.

Benefits of technology

The target compound is obtained with a high ratio and a high harvest rate when producing xylene, which improves the activity of the catalyst and the selectivity of xylene, and reduces the diffusion resistance of the generated gas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946407A_ABST
    Figure CN118946407A_ABST
Patent Text Reader

Abstract

One aspect of the present invention relates to a method for producing a zeolite catalyst having a silica coating film, comprising at least the steps of: mixing a zinc source with an MFI-type zeolite to obtain a zinced zeolite; preparing a mixed solution containing a structure-directing agent containing tetraethylammonium, a silicon dioxide source and water; and adding the mixed solution to the surface of the zinc-added zeolite, and carrying out hydrothermal synthesis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a zeolite catalyst having a silica coating and a zeolite catalyst. Background Art

[0002] In recent years, as an alternative production method for fossil resources, the materialization of carbon dioxide has been attracting attention. Specifically, the technology of making carbon dioxide react with hydrogen and the like to produce chemical raw materials is being studied. For example, the technology of converting carbon dioxide into benzene, methanol, ethylene, xylene, etc. is known.

[0003] As a method for producing aromatic compounds such as xylene, a method of producing xylene from alcohols, olefins or olefins using crystalline aluminosilicates or crystalline gallosilicates as catalysts is known. However, in the production method using the above catalyst, xylene is obtained as a mixture of isomers of para-, meta- and ortho-isomers, and therefore a special separation device is required to separate p-xylene from them. Therefore, a production method capable of selectively obtaining p-xylene from xylene is currently desired.

[0004] In the past, as a technology for obtaining an aromatic hydrocarbon mixture having a high paraxylene ratio in xylene isomers, a method for producing aromatic hydrocarbons has been reported, which is a method for producing aromatic hydrocarbons by synthesizing aromatic hydrocarbons from at least one compound selected from alcohols, olefins and olefins, and is characterized in that the reaction is carried out in the presence of a catalyst containing the following compound, wherein the compound is formed by modifying a silicate selected from crystalline aluminosilicates and crystalline gallosilicates with silicon dioxide (Patent Document 1).

[0005] The technology proposed in Patent Document 1 is reported to be able to obtain an aromatic hydrocarbon mixture having a high ratio of paraxylene among xylene isomers. However, the present inventors have found through studies that the yield of xylene itself decreases.

[0006] Prior art literature

[0007] Patent Literature

[0008] Patent Document 1: Japanese Patent Publication No. 2010-208948 Summary of the invention

[0009] Therefore, the main object of the present invention is to provide a zeolite catalyst capable of obtaining a target compound from isomers at a high ratio and high yield when producing an aromatic compound having multiple isomers such as the above-mentioned xylene, and to provide a method for producing the catalyst.

[0010] One aspect of the present invention relates to a method for producing a zeolite catalyst having a silica coating, which comprises at least the following steps: mixing a zinc source with an MFI-type zeolite to obtain a zinc-added zeolite; preparing a mixed solution comprising a structure directing agent containing tetraethylammonium, a silica source and water; and adding the mixed solution to the surface of the zinc-added zeolite for hydrothermal synthesis.

[0011] Another aspect of the present invention relates to a zeolite catalyst, which is a zeolite catalyst prepared by the production method. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 This is a schematic diagram showing one embodiment of a zeolite catalyst obtained by the production method of the present embodiment. DETAILED DESCRIPTION

[0013] Embodiments of the present invention will be described in detail below, but the present invention is not limited to these descriptions.

[0014] [Method for producing zeolite catalyst]

[0015] One embodiment of the present invention is a method for producing a zeolite catalyst having a silica coating, which comprises at least the following steps: mixing a zinc source with an MFI-type zeolite to obtain a zinc-added zeolite; preparing a mixed solution comprising a structure directing agent containing tetraethylammonium, a silica source and water; and adding the mixed solution to the surface of the zinc-added zeolite for hydrothermal synthesis.

[0016] This production method can produce a zeolite catalyst having a thinner silica coating than conventional zeolite catalysts. Figure 1 As shown, the zeolite catalyst obtained by this embodiment is a zeolite catalyst of a core-shell structure, and the surface of the zeolite crystal 1 that becomes the core is covered with a silica coating 2 that becomes an inert layer. The zeolite crystal 1 that becomes the core contains zinc ions 3. The zeolite catalyst can suppress the reaction on the outer surface by having a silica coating 2, so when the zeolite catalyst is used to manufacture an aromatic compound with multiple isomers such as xylene, the target compound can be obtained from the isomers at a high ratio. In addition, the above-mentioned silica coating 2 is a thinner film, so the diffusion resistance of the generated gas can be reduced and the catalytic activity can be improved. Therefore, there is an advantage of obtaining the target compound at a high yield.

[0017] In the production method of the present embodiment, a zinc source and MFI zeolite are first mixed to obtain zinc-added zeolite.

[0018] In the present embodiment, MFI zeolite is used as the core of the catalyst. MFI zeolite is a zeolite having an oxygen 10-ring structure, and aluminosilicate zeolites such as ZSM-5 zeolite are particularly preferably used. It is believed that by using the MFI zeolite, a desired compound can be selectively obtained from a compound having a variety of isomers according to the difference in molecular size. In addition, by using the MFI zeolite, it also has the following advantages: in xylene, p-xylene can be obtained with a high selectivity compared to o-xylene and m-xylene.

[0019] As the above-mentioned MFI type zeolite, commercially available zeolite may be used, or the zeolite may be synthesized by a known method.

[0020] The zinc source that can be used in the present embodiment is not particularly limited as long as it can add zinc ions to the above-mentioned zeolite, and examples thereof include zinc nitrate, zinc acetate, zinc chloride, zinc sulfate, etc. Among these, zinc nitrate, zinc chloride, etc. are preferably used from the viewpoint of solubility in aqueous solution. As the above-mentioned zinc source, hydrates thereof, etc. may also be used.

[0021] The mixing ratio of the zinc source and the MFI zeolite is not particularly limited, but is preferably mixed so that the MFI zeolite:zinc source ratio is about 100:1 to 1:10, and more preferably, the MFI zeolite:zinc source ratio is about 20:1 to 1:2, by weight.

[0022] When mixing, for example, the MFI zeolite is added to the aqueous solution containing the zinc source, and the mixed solution is stirred at a temperature of 20 to 100° C. for about 1 to 24 hours.

[0023] Then, the zeolite is filtered, washed, dried, and then calcined to obtain zinc-added zeolite. The methods of filtering, washing, and drying are not particularly limited, and known methods can be used appropriately. After drying, calcination is performed at about 400 to 600° C. for 1 to 24 hours.

[0024] Next, a mixed solution containing a structure directing agent including tetraethylammonium, a silica source and water is prepared.

[0025] The structure directing agent used in this embodiment contains at least tetraethylammonium. Tetrapropylammonium is used as a structure directing agent in the reported method for preparing zeolite catalysts. However, tetrapropylammonium has strong alkalinity and easily causes the core catalyst to dissolve and nucleate, so the silica coating that becomes the shell layer is formed using the coarse core. In this case, if the formation of the silica coating is not carried out multiple times, the core catalyst cannot be fully covered. As a result, the silica coating becomes thicker, the activity of the zeolite catalyst decreases, and the yield rate decreases when the catalyst is used for synthesis.

[0026] In contrast, by using a structure directing agent containing tetraethylammonium with low basicity as in the present embodiment, the crystal growth rate is suppressed when a silica film is formed on the catalyst surface, and the catalyst can be covered with a more uniform and thin silica film than in the conventional method. As a result, it is believed that the activity of the zeolite catalyst is improved, and the yield is improved when the catalyst is used for synthesis and production.

[0027] The structure directing agent of the present embodiment may further contain a structure directing agent other than the above-mentioned tetraethylammonium, for example, tetrapropylammonium, triethylamine, ethylenediamine, etc.

[0028] The silica source used in this embodiment is not particularly limited as long as it can cover the zinc-added zeolite, and can be appropriately selected according to the target silica coating composition. Specifically, examples thereof include tetraethyl orthosilicate, tetramethyl orthosilicate, sodium silicate, colloidal silica, and fumed silica.

[0029] The above-mentioned silica coating is preferably a coating of crystalline silica, and from the viewpoint of the diffusibility of reactants (molecules) and products (molecules), a porous silicate coating is particularly preferred. Therefore, as the above-mentioned silica source, tetraethyl orthosilicate, colloidal silica, fumed silica, etc. can be appropriately used.

[0030] The mixed solution containing the structure directing agent containing tetraethylammonium, the silica source and water can be used as a raw material solution for forming a silica coating on zinc-added zeolite. It should be noted that the solvent contained in the mixed solution can be only water, or in order to improve the solubility of the silica source, the mixed solution can contain a water-soluble organic solvent such as ethanol, propanol, glycerol, etc. in addition to water.

[0031] The amounts of the tetraethylammonium and the silica source in the mixed solution are not particularly limited and can be appropriately adjusted within a range in which a silica coating can be formed on the zinc-added zeolite.

[0032] The amount of tetraethylammonium in the mixed solution is adjusted, for example, so that the molar ratio of silica source to tetraethylammonium is about 100:1 to 1:1. More preferably, the molar ratio of silica source to tetraethylammonium is about 10:1 to 2:1.

[0033] The silica source is preferably adjusted in amount in the mixed solution so that the zinc zeolite:silica source weight ratio is about 20:1 to 1:5, and more preferably about 5:1 to 1:2.

[0034] Next, the mixed solution containing the structure directing agent including tetraethylammonium, the silica source and water is added to the surface of the zinc-added zeolite. The adding method is not particularly limited, and the zinc-added zeolite can be immersed in the mixed solution containing the silica source and the structure directing agent, or the mixed solution can be coated on the surface of the zinc-added zeolite.

[0035] Then, hydrothermal synthesis is performed. In the present embodiment, the method of hydrothermal synthesis is not particularly limited, and for example, it can be performed using a rotary autoclave, a stirring autoclave, a static (non-stirring) autoclave, etc. Specifically, the zinc-added zeolite can be immersed in the above-mentioned mixed solution and placed in an autoclave for hydrothermal synthesis, or the zinc-added zeolite with the above-mentioned mixed solution coated on the surface can be placed in hot water in an autoclave for hydrothermal synthesis.

[0036] The temperature of the hydrothermal synthesis is preferably about 100 to 200° C., and more preferably 150 to 190° C. The reaction time of the hydrothermal synthesis is preferably about 1 to 200 hours, and more preferably about 4 to 48 hours.

[0037] After the hydrothermal synthesis, the resulting product is washed and dried, and then calcined to obtain a zeolite catalyst having a silica coating. The washing and drying methods are not particularly limited, and known methods can be used appropriately. After drying, the silica coating is calcined at about 400 to 600° C. for 1 to 24 hours.

[0038] The zeolite catalyst of the present embodiment having a silica coating can be obtained through the above steps. The obtained zeolite catalyst can be used as it is, or the particle size can be adjusted by a known granulation method or the like as needed.

[0039] With respect to the zeolite catalyst obtained by the manufacturing method of the present embodiment, the weight increase rate of the zeolite catalyst after the silica coating is formed relative to the weight of the zinc-added zeolite before the silica coating is formed is preferably 40% or less. This weight increase rate is an indicator indicating that the zeolite catalyst obtained by the present embodiment forms a thin silica coating. A more preferred range of the above-mentioned weight increase rate is 20% or less. The lower limit is not particularly limited, and if the above-mentioned weight increase rate is less than 1%, a sufficient silica coating may not be formed, so it is preferably 1% or more.

[0040] The above-mentioned weight increase rate is a value obtained by the method described in the examples below.

[0041] [Zeolite Catalyst]

[0042] The zeolite catalyst having a silica coating (hereinafter sometimes simply referred to as a zeolite catalyst) obtained by the production method of the present embodiment is a novel zeolite catalyst that has not existed in the past. Therefore, the present embodiment also includes the zeolite catalyst obtained by the above production method.

[0043] One of the characteristics of the zeolite catalyst of the present embodiment is that the silica coating is thin. As described above, by using a method different from the conventional method to manufacture the zeolite catalyst, the silica coating can be made thinner than conventional methods. As a result, it is believed that the activity of the zeolite catalyst is improved, and when the catalyst is used to manufacture compounds, the yield is improved.

[0044] The film thickness of the silica coating of the zeolite catalyst of the present embodiment is preferably less than 500nm. The silica coating as thin as the present embodiment cannot be formed by the previous manufacturing method. By having a silica coating with a film thickness of less than 500nm, the zeolite catalyst can also improve the yield in addition to showing high selectivity of isomers. If the film thickness of the above-mentioned silica coating exceeds 500nm, sufficient yield cannot be obtained. The lower limit of the film thickness of the above-mentioned silica coating does not need to be particularly limited, and from the viewpoint of maintaining high selectivity of isomers, it is usually more than 1nm. The film thickness of the more preferred silica coating is more than 5nm and less than 50nm.

[0045] The film thickness of the silicon dioxide film is a value obtained by a method described in Examples below.

[0046] In addition, in the zeolite catalyst of the present embodiment, the amount of the silica coating is preferably 1 part by mass or more and 100 parts by mass or less relative to 100 parts by mass of the zinc-added zeolite as the core catalyst. If the amount of the above-mentioned silica coating exceeds 100 parts by mass, the yield may become insufficient when the above-mentioned zeolite catalyst is used to manufacture the compound. In a more preferred embodiment, the amount of the silica coating is preferably 3 parts by mass or more and 20 parts by mass or less relative to 100 parts by mass of the zinc-added zeolite as the core catalyst.

[0047] The amount of the silica film can be determined from the weight increase rate shown in the examples described later.

[0048] [Application of zeolite catalyst]

[0049] The zeolite catalyst of the present embodiment can be appropriately used for the manufacture of aromatic compounds. As aromatic compounds, aromatic hydrocarbons having substituents such as benzene, toluene, xylene, and ethylbenzene can be cited, and the zeolite catalyst of the present embodiment is particularly suitable for the manufacture of p-xylene. p-xylene is the starting raw material of terephthalic acid, which is the raw material of polybutylene terephthalate, and the catalyst of the present embodiment that can manufacture p-xylene with high selectivity and high yield is very useful in industrial utilization.

[0050] The method for producing p-xylene using the zeolite catalyst of the present embodiment is not particularly limited, and p-xylene can be produced by reacting aromatic hydrocarbons as raw materials with a methylating agent in the presence of the zeolite catalyst of the present embodiment.

[0051] Examples of the aromatic hydrocarbon as a raw material include benzene, alkylbenzene, etc. Examples of the methylating agent include methanol, dimethyl ether, dimethyl carbonate, methane, etc.

[0052] As described above, this specification discloses various aspects of technology, and the main technologies among them are summarized below.

[0053] The first aspect involves a method for producing a zeolite catalyst having a silica coating, which comprises at least the following steps: mixing a zinc source with an MFI-type zeolite to obtain a zinc-added zeolite; preparing a mixed solution comprising a structure directing agent containing tetraethylammonium, a silica source and water; and adding the mixed solution to the surface of the zinc-added zeolite for hydrothermal synthesis.

[0054] According to the above configuration, it is possible to provide a zeolite catalyst capable of obtaining a target compound from among isomers at a high ratio and high yield when producing an aromatic compound having a plurality of isomers such as xylene, and a method for producing the catalyst.

[0055] In addition, the method for producing a zeolite catalyst according to a second aspect is as follows: in the method for producing the first aspect, the silica coating is preferably a full-silica zeolite coating, which has the advantage of suppressing the reaction on the outer surface of the crystal.

[0056] The third aspect of the present invention relates to a method for producing a zeolite catalyst as follows: in the method of the first or second aspect, the weight increase rate of the zeolite catalyst having a silica coating relative to the weight of the zinc-added zeolite is 40% or less. It is believed that this results in a thinner silica coating being formed in the obtained zeolite catalyst.

[0057] Furthermore, a fourth aspect of the present invention provides a method for producing a zeolite catalyst according to any one of the first to third aspects, wherein the zeolite catalyst obtained by the method is a catalyst for producing paraxylene.

[0058] The zeolite catalyst for producing paraxylene according to the fifth aspect is a zeolite catalyst for producing paraxylene obtained by the production method according to any one of the first to fourth aspects. The zeolite catalyst is suitable for producing paraxylene and is useful in industrial applications.

[0059] Example

[0060] The present invention is further specifically described below by way of examples, but the present invention is not limited by the examples.

[0061] <Manufacturing of zeolite catalyst>

[0062] (Example 1)

[0063] Preparation of zinc-added zeolite

[0064] 1 g of zeolite "HSZ-840HOA" (particle size 3 μm) manufactured by Tosoh Corporation as a core catalyst, 2 g of zinc nitrate hexahydrate manufactured by Nacalai Tesque, Inc. as a zinc source, and 66.5 g of distilled water were mixed and stirred at 80°C for one night. Then, the mixed solution was filtered and washed with 1 L of distilled water. Thereafter, it was dried in a dryer at 90°C for about one night until the liquid disappeared. The obtained dried product was calcined at 550°C for 5 hours to obtain zinc-added zeolite. At this time, the temperature was increased at 5°C / minute, and the temperature was lowered by natural cooling. The Si / Al content ratio of the obtained zinc-added zeolite was 16.4.

[0065] ·Silicon dioxide film formation

[0066] 0.693 g of tetraethyl orthosilicate (TEOS) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. as a silica source, 0.28 g of a 35 wt% aqueous solution of tetraethylammonium hydroxide (TEAOH) manufactured by Sigma-Aldrich Co. LLC as a structure directing agent, and 5.28 g of distilled water were added to a Teflon (registered trademark) inner cylinder and stirred at room temperature for 1 hour to obtain a mixed solution containing the silica source, the structure directing agent and water.

[0067] To the obtained mixed solution was added 0.3 g of the zinc-added zeolite obtained above, and hydrothermal synthesis was carried out for 24 hours using a rotary autoclave (manufactured by HIRO Co., Ltd., "hydrothermal synthesis reaction apparatus (apparatus name)") at 180°C and 10 rpm.

[0068] Then, the supernatant was discarded, water was added, and centrifugation was performed for 10 minutes. This operation was repeated 3 times to perform washing. Thereafter, the mixture was dried in a 90° C. dryer for about one night until the liquid disappeared.

[0069] The obtained dried product was calcined at 550° C. for 5 hours to obtain a zeolite catalyst having a silica coating. At this time, the temperature was increased at 5° C. / min, and the temperature was decreased by natural cooling.

[0070] (Examples 2 to 4)

[0071] A zeolite catalyst having a silica coating was obtained by the same method as in Example 1 except that the amount of a 35 wt % aqueous solution of tetraethylammonium hydroxide (TEAOH) as a structure directing agent was changed to the amounts shown in Table 1 in the formation of the silica coating.

[0072] (Examples 5 to 7)

[0073] In the formation of the silica coating, a zeolite catalyst having a silica coating was obtained by the same method as in Example 1, except that the amount of a 35 wt % aqueous solution of tetraethylammonium hydroxide (TEAOH) as a structure directing agent was changed to the amount shown in Table 1, and a 10 wt % aqueous solution of tetrapropylammonium hydroxide (TPAOH) manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd. was added in the amount shown in Table 1.

[0074] (Example 8)

[0075] In forming the silica film, a zeolite catalyst having a silica film was obtained by the same method as in Example 3 except that the amount of TEOS as a silica source and the amount of distilled water were changed to the amounts shown in Table 1.

[0076] (Example 9)

[0077] In forming the silica film, a zeolite catalyst having a silica film was obtained by the same method as in Example 4 except that the amount of TEOS as a silica source and the amount of distilled water were changed to the amounts shown in Table 1.

[0078] (Comparative Example)

[0079] Preparation of zinc-added zeolite

[0080] The same method as in Example 1 was used.

[0081] ·Silicon dioxide film formation

[0082] 0.2 g of fumed silica manufactured by Sigma-Aldrich as a silica source, 0.81 g of a 10 wt% aqueous solution of tetrapropylammonium hydroxide (TPAOH) manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. as a structure-directing agent, 2.45 g of ethanol and 13.6 g of distilled water were added to a Teflon (registered trademark, homemade using PTFE resin round rods) inner cylinder, and stirred at room temperature for 1 hour to obtain a mixed solution containing the silica source, the structure-directing agent and water.

[0083] To the obtained mixed solution was added 0.3 g of the zinc-added zeolite obtained above, and hydrothermal synthesis was carried out for 24 hours at 180° C. and 10 rpm using a rotary autoclave (manufactured by HIRO Corporation, “Hydrothermal Synthesis Reactor (Apparatus Name)”).

[0084] Then, the supernatant was discarded, water was added, and centrifugation was performed for 10 minutes. This operation was repeated 3 times to perform washing. Thereafter, the mixture was dried in a 90° C. dryer for about one night until the liquid disappeared.

[0085] The obtained dried product was calcined at 550° C. for 5 hours to obtain a zeolite catalyst partially having a silica coating. At this time, the temperature was increased at 5° C. / min, and the temperature was decreased by natural cooling.

[0086] In the zeolite catalyst obtained above, there are still parts not covered by the silica film, so the above-mentioned silica film forming step is repeated again from the beginning. That is, a mixed solution containing a silica source, a structure directing agent and water is prepared again, and the zeolite catalyst obtained by the first calcination is added to the mixed solution, and the autoclave, washing, drying and calcination are carried out under the same conditions as the first time, thereby obtaining a zeolite catalyst with a silica film.

[0087] Table 1

[0088]

[0089] <Evaluation Method>

[0090] (Si / Al content ratio)

[0091] The content ratio of Si to Al (Si / Al ratio) in the zeolite catalyst having a silica coating obtained in each of the Examples and Comparative Examples was analyzed by EDX (energy dispersive X-ray analysis).

[0092] (Weight Increase Rate Due to Formation of Silicon Dioxide Film and Film Thickness of Silicon Dioxide Film)

[0093] The zinc-added zeolite as the core catalyst is composed of the elements Si, Al, Zn and O, while the shell layer, i.e., the silica coating, is composed only of Si and O. Assumption: The content of Zn and Al does not change when synthesizing the coating. In addition, assumption: The weight of the catalyst is proportional to the volume (= the cube of the particle size). As the core catalyst particle size, a zeolite particle size of 3 μm manufactured by Tosoh Corporation was used.

[0094] It should be noted that in the following formula, core (or core catalyst) = zinc-added zeolite, core shell (or core shell catalyst) = zeolite catalyst having a silica coating.

[0095] First, since the increase in the Si / Al ratio obtained above is derived from Si contained in the silica film, the weight increase rate (%) is calculated by the following formula (1).

[0096] Formula (1):

[0097] [Weight increase rate (%)] = ([core-shell Si / Al ratio] - [core Si / Al ratio]) / ([core Si / Al ratio] + 1) × 100

[0098] In addition, from [weight increase rate (%)]={[core-shell catalyst weight] / [core catalyst weight]-1}×100, the following formula (2) can be derived.

[0099] Formula (2):

[0100] [Core-shell catalyst weight] / [Core catalyst weight]=[Weight increase rate (%)] / 100+1

[0101] Based on the above-described assumption, the weight of the catalyst is proportional to the volume (= cube of the catalyst particle size), and therefore the following formula (3) can be derived.

[0102] Formula (3):

[0103] {[Core-shell catalyst particle size] / [Core catalyst particle size]} 3 =[core-shell catalyst weight] / [core catalyst weight]

[0104] The film thickness of the silica film can be calculated by the following formula (4) based on the difference in catalyst particle diameter between the core-shell catalyst and the core catalyst.

[0105] Formula (4):

[0106] [Thickness of silica coating] = {[Core-shell catalyst particle size] - [Core catalyst particle size]} / 2 = [Core catalyst particle size] × {([Core-shell catalyst particle size] / [Core catalyst particle size]) - 1} / 2

[0107] In addition, based on the assumption, formula (5): core catalyst particle size = 3 μm.

[0108] It should be noted that, with respect to the core-shell catalyst particle size in the above formula (3) and formula (4), the following formula (6) can be obtained by substituting formula (3) into formula (4):

[0109] [Thickness of silica coating] = [Core catalyst particle size] × {{[Core-shell catalyst weight] / [Core catalyst weight]} 1 / 3 - 1} / 2

[0110] The "core-shell catalyst particle size" is canceled out, so the film thickness can be calculated from the ratio of catalyst weight and core particle size.

[0111] The film thickness of the silicon dioxide film was calculated by substituting the above-mentioned formulas (1), (2), and (5) into the formula (6).

[0112]

[0113] (Catalyst Performance)

[0114] Using the zeolite catalysts of Examples 1 to 5, 8 and Comparative Example, p-xylene was produced by the following method, and the p-xylene yield and p-xylene selectivity of each catalyst were evaluated.

[0115] ·Manufacturing of paraxylene

[0116] A fixed bed reactor was filled with 0.05 g of a zeolite catalyst, and a methanol gas was supplied to react at atmospheric pressure and 400° C. The generated gas was analyzed 20 minutes after the start of the reaction to evaluate the catalyst activity.

[0117] ·Analysis method of generated gas

[0118] The analysis was performed using the following analytical equipment and conditions:

[0119] Analytical device: GC-2014 manufactured by Shimadzu Corporation

[0120] Column: Capillary column Xylene Master

[0121] Initial column temperature: 70°C

[0122] Heating rate: 2℃ / min

[0123] Detector temperature: 200°C

[0124] · Calculation method of yield and para-xylene selectivity

[0125] It was found by the following formula:

[0126] [p-xylene yield (C mol%)] = [p-xylene production (mol)] / [methanol supply (mol)] / 8 × 100

[0127] [p-xylene selectivity (%)] = [p-xylene production (mol)] / [xylene (ortho, meta, para) production (mol)] × 100

[0128] The results are shown in Table 3.

[0129] Table 3

[0130]

[0131] (Inspection)

[0132] According to the results of Table 2, it is confirmed that the zeolite catalyst obtained by the manufacturing method of the embodiment has a thinner film thickness of the silica film than the zeolite catalyst obtained by the manufacturing method of the comparative example as the conventional method. This point can also be supported by the weight increase rate after the silica film is formed. In addition, according to the results of Table 3, it is confirmed that the zeolite catalyst obtained by the manufacturing method of the embodiment has a silica film with a film thickness of 500nm or less, and the yield in the production of para-xylene is high and the para-xylene selectivity is also high.

[0133] On the other hand, it was confirmed that the silica coating of the zeolite catalyst obtained by the production method of the comparative example had a thickness of more than 500 nm and had a high paraxylene selectivity in the production of paraxylene, but the yield was lower than that of the zeolite catalyst of the example.

[0134] This application is based on Japanese patent application No. 2022-58510 filed on March 31, 2022, and the contents are included in this application.

[0135] In order to describe the present invention, the present invention has been appropriately and fully described above by referring to specific embodiments and drawings, but it should be recognized that those skilled in the art can easily change and / or improve the above-mentioned embodiments. Therefore, as long as the modified embodiments or improved embodiments implemented by those skilled in the art do not deviate from the protection scope of the claims recorded in the claims, the modified embodiments or improved embodiments can be interpreted as being included in the protection scope of the claims.

Claims

1. A method for producing a zeolite catalyst having a silicon dioxide coating, characterized in that At least the following steps are included: Mixing a zinc source with an MFI zeolite to obtain a zinc-added zeolite; preparing a mixed solution comprising a structure directing agent including tetraethylammonium, a silica source and water; and, The mixed solution is added to the surface of the zinc-added zeolite to perform hydrothermal synthesis.

2. The method for producing a zeolite catalyst according to claim 1, characterized in that: The silicon dioxide coating is a full-silicon zeolite coating.

3. The method for producing a zeolite catalyst according to claim 1, characterized in that: The increase rate of the weight of the zeolite catalyst having a silica coating relative to the weight of the zinc-added zeolite is 40% or less.

4. The method for producing a zeolite catalyst according to claim 1, characterized in that: Zeolite catalysts are catalysts used to produce paraxylene.

5. A zeolite catalyst for producing paraxylene, characterized in that: It is obtained by the method according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Core-shell type aromatic conversion catalyst, preparation method and application thereof

    CN101722033A

  • Catalyst for selectively preparing paraxylene and method for synthesizing catalyst

    CN102671694A

  • HZSM-5@silicalite-1 core-shell structure molecular sieve, and preparation method and application thereof

    CN103708496A

  • Method for synthesizing ZSM-5 / Silicalite core-shell molecular sieve by using vapor phase process

    CN104556130A

  • Catalyst for directly preparing p-xylene from synthetic gas as well as preparation and application thereof

    CN109590019A