Alkali-soluble resin, alkali-soluble resin composition, and method for producing same
By controlling the content of ammonium salt compound and specific reaction steps, the coloring problem of alkali-soluble resin during heating and curing and the problem of low refractive index are solved, and alkali-soluble resin and resin composition with heat resistance and high refractive index are realized. Optical and electronic devices with high demands.
Patent Information
- Application Number
- CN202380029997.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-25
- Filing Date
- 2023-03-20
- Publication Date
- 2024-11-12
AI Technical Summary
The existing alkali-soluble resins are prone to coloring problems when heated and cured, and have a low refractive index, which cannot meet the optical application requirements of high refractive index.
The content of the ammonium salt compound is controlled below 0.06% in the alkali-soluble resin and utilizes specific structures and reaction processes, including the reaction of the difunctional epoxy compound with bisphenol, followed by further reaction with unsaturated monobasic acid and polyacid anhydride. , a cured substance with a high refractive index is formed.
An alkali-soluble resin and resin composition with excellent heat resistance and high refractive index is achieved, and is suitable for high-demand applications such as optical components and electronic equipment.
Smart Images

Figure CN118946613A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an alkali-soluble resin and an alkali-soluble resin composition. Specifically, the present invention relates to an alkali-soluble resin and an alkali-soluble resin composition capable of providing a cured product having excellent heat discoloration resistance and a high refractive index, and a method for producing the same. Background Art
[0002] Various studies have been conducted on the application of photosensitive resin compositions containing alkali-soluble resins in various applications such as color filters, inks, printing plates, printed wiring boards, semiconductor elements, photoresists, organic insulating films, organic protective films, and other optical components, motor / electronic equipment, etc. used in liquid crystal display devices, solid-state imaging elements, etc., and resins and resin compositions having excellent properties required for each application have been developed.
[0003] In recent years, the miniaturization, thinning, and energy saving of optical components, motors / electronic devices, etc. have been continuously developed, and with this, higher quality performance is required for various components used. In order to meet such requirements, alkali-soluble resins and photosensitive resin compositions that become materials of various components have been studied.
[0004] Hitherto, photosensitive resin compositions containing alkali-soluble resins have been developed to cope with various demands.
[0005] For example, Patent Document 1 describes a photosensitive resin composition for image formation, which contains an acid-modified vinyl ester synthesized from an epoxy compound, a phenol compound, an unsaturated monobasic acid, and a polyacid anhydride, and is obtained by using a crystalline epoxy resin having a melting point of 90° C. or above as at least a part of the epoxy compound and using a compound having a bisphenol S skeleton as at least a part of the phenol compound.
[0006] In addition, for example, Patent Document 2 discloses a photosensitive resin composition for image formation, which contains an acid-modified vinyl ester and epoxy acrylate, wherein the acid-modified vinyl ester is synthesized from a difunctional epoxy compound, a difunctional phenol compound, an unsaturated monobasic acid and / or an unsaturated monomer having a functional group capable of reacting with a phenolic hydroxyl group, and a polyacid anhydride, and at least a portion of the difunctional epoxy compound or the difunctional phenol compound uses a compound having a biphenyl skeleton.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2008-250306
[0010] Patent Document 2: Japanese Patent Application Publication No. 2008-250307 Summary of the invention
[0011] Problems to be solved by the invention
[0012] However, although these alkali-soluble resins can provide cured products that are excellent in alkali developability, photocurability, dimensional stability based on temperature changes, and do not show brittleness, they have the problem of coloring when heated and cured. In addition, the refractive index of existing alkali-soluble resins is low. When used for optical applications requiring a high refractive index, a resin with a high refractive index of about 1.60 is required, which cannot fully meet such requirements.
[0013] The present invention has been made in view of the above-mentioned current situation, and an object of the present invention is to provide an alkali-soluble resin and an alkali-soluble resin composition capable of providing a cured product having excellent heat discoloration resistance and a high refractive index, and a production method capable of efficiently obtaining the same.
[0014] Means for solving problems
[0015] The present inventors have made various studies on alkali-soluble resins and have found that a cured product having excellent heat coloration resistance and a high refractive index can be provided by having a specific structure and setting the content of an ammonium salt compound within a specific range, thereby completing the present invention.
[0016] That is, the present invention relates to an alkali-soluble resin having a structure represented by the following formula (1), wherein the content of the ammonium salt compound in the alkali-soluble resin is 0.06 mass % or less relative to 100 mass % of the alkali-soluble resin.
[0017] [Chemistry 1]
[0018]
[0019] (In formula (1), R 1 , R 2 and R 3 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 4 represents a direct bond or a divalent organic group. 5 , R 6 , R 7 and R 8 Same or different, represents hydrogen atom or Y, R 5 ~R 8 At least one of them is Y. The above Y is a group represented by the following formula (2). 9 and R 10 are the same or different and represent a substituent. W represents a divalent organic group. X represents a direct bond or a divalent organic group. l represents R 9 The number of is an integer from 0 to 4. m represents R 10 The number of is an integer from 0 to 4. 9 and R10 When there are two or more, each may be the same or different. n represents an integer greater than 1.)
[0020] [Chemistry 2]
[0021]
[0022] (In formula (2), R 11 represents a divalent organic group which may have a substituent. )
[0023] In addition, the present invention relates to an alkali-soluble resin composition, characterized in that it contains the above-mentioned alkali-soluble resin and an acid group-containing epoxy (meth)acrylate.
[0024] In addition, the present invention also relates to a method for producing an alkali-soluble resin, characterized in that the method for producing the alkali-soluble resin comprises: a step (a-1) of reacting a difunctional epoxy compound having a Gardner chromaticity of less than 12 and a melting point of 90°C or more obtained based on JIS K 0071-2 with a bisphenol compound; a step (a-2) of reacting the reaction product obtained in the step (a-1) with an unsaturated monobasic acid; and a step (a-3) of reacting the reaction product obtained in the step (a-2) with a polyacid anhydride, wherein the content of the ammonium salt compound in the alkali-soluble resin obtained by the above-mentioned production method is less than 0.06% by mass relative to 100% by mass of the alkali-soluble resin.
[0025] In addition, the present invention also relates to a method for producing an alkali-soluble resin composition, characterized in that the method for producing the alkali-soluble resin composition comprises: a step (b-1) of reacting a difunctional epoxy compound having a Gardner chromaticity of less than 12 and a melting point of 90°C or more obtained based on JIS K 0071-2 with a bisphenol compound; a step (b-2) of adding an epoxy resin to the reaction product obtained in the step (b-1); a step (b-3) of reacting the mixture obtained in the step (b-2) with an unsaturated monobasic acid; and a step (b-4) of reacting the reaction mixture obtained in the step (b-3) with a polyacid anhydride, wherein the content of the ammonium salt compound in the alkali-soluble resin composition obtained by the above-mentioned production method is less than 0.06% by mass relative to 100% by mass of the alkali-soluble resin.
[0026] The epoxy resin is preferably an aromatic epoxy resin.
[0027] The aromatic epoxy resin is preferably a bisphenol A type epoxy resin.
[0028] Effects of the Invention
[0029] The alkali-soluble resin and alkali-soluble resin composition of the present invention can provide a cured product having excellent heat discoloration resistance and a high refractive index. The alkali-soluble resin and alkali-soluble resin composition of the present invention can be widely used in various applications such as optical components, motor / electronic components, and display devices. DETAILED DESCRIPTION
[0030] Hereinafter, the present invention will be described in detail.
[0031] In addition, the embodiment in which two or more of the preferred embodiments of the present invention described below are combined is also a preferred embodiment of the present invention.
[0032] In addition, in this specification, "(meth)acrylate" means "acrylate and / or methacrylate", and "(meth)acrylic acid" means "acrylic acid and / or methacrylic acid".
[0033] 1. Alkali soluble resin
[0034] The alkali-soluble resin of the present invention has a structure represented by the following formula (1), wherein the content of the ammonium salt compound in the alkali-soluble resin is 0.06 mass % or less based on 100 mass % of the alkali-soluble resin.
[0035] [Chemistry 3]
[0036]
[0037] (In formula (1), R 1 , R 2 and R 3 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms. 4 represents a direct bond or a divalent organic group. 5 , R 6 , R 7 and R 8 Same or different, represents hydrogen atom or Y, R 5 ~R 8 At least one of them is Y. The above Y is a group represented by the following formula (2). 9 and R 10 are the same or different and represent a substituent. W represents a divalent organic group. X represents a direct bond or a divalent organic group. l represents R 9 The number of is an integer from 0 to 4. m represents R 10 The number of is an integer from 0 to 4. 9 and R 10 When there are two or more, each may be the same or different. n represents an integer greater than 1.)
[0038] [Chemistry 4]
[0039]
[0040] (In formula (2), R 11 represents a divalent organic group which may have a substituent. )
[0041] The reason why the alkali-soluble resin of the present invention can provide a cured product with excellent heat-resistant coloration is that the content of the ammonium salt compound is below the specified range, so the nitrogen content that causes coloration during heat curing becomes small, and coloration during heat curing can be suppressed. In addition, the reason why the refractive index of the alkali-soluble resin of the present invention is high is that a rigid skeleton such as a biphenyl skeleton or a skeleton formed by linking aromatic rings with a divalent organic group in the main chain can form a dense cured film through π-π stacking.
[0042] The alkali-soluble resin of the present invention has a structure represented by the above formula (1).
[0043] In the above formula (1), R 1 , R 2 and R 3 The same or different groups represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms.
[0044] Examples of the hydrocarbon group having 1 to 6 carbon atoms include chain or cyclic hydrocarbon groups having 1 to 6 carbon atoms, preferably chain hydrocarbon groups having 1 to 6 carbon atoms, and more preferably alkyl groups having 1 to 6 carbon atoms.
[0045] Among them, R is preferred because of good reactivity of the unsaturated double bond. 1 , R 2 and R 3 are the same or different, are hydrogen atoms or methyl groups, and more preferably R 1 , R 2 is a hydrogen atom, R 3 A hydrogen atom or a methyl group.
[0046] In the above formula (1), R 4 represents a direct bond or a divalent organic group.
[0047] As the above R 4 The divalent organic group represented by the present invention includes a divalent hydrocarbon group which may have a substituent, -O-, -CO-, -NH-, -S-, -SO-, -SO2-, or a group consisting of a combination thereof. Among them, from the perspective of better heat coloration resistance, a divalent hydrocarbon group which may have a substituent, -O-, -CO-, or a group consisting of a combination thereof is preferred, and a group consisting of a combination of a divalent hydrocarbon group, -O-, and -CO- is more preferred.
[0048] The divalent hydrocarbon group may be a saturated hydrocarbon group or an unsaturated hydrocarbon group, but a saturated hydrocarbon group is preferred from the viewpoint of better heat coloration resistance.
[0049] The divalent hydrocarbon group may be in the form of a chain (straight chain or branched chain) or a ring, but is preferably in the form of a chain from the viewpoint of excellent dimensional stability.
[0050] Examples of the divalent hydrocarbon group include a divalent aliphatic hydrocarbon group, a divalent alicyclic hydrocarbon group, and a divalent aromatic hydrocarbon group.
[0051] Examples of the divalent aliphatic hydrocarbon group include alkylene groups such as methylene, ethylene, propylene, isopropylene, butylene, isobutylene, tert-butylene, pentylene, neopentylene, hexamethylene, heptylene, octylene, 2-ethylhexylene, nonylene, decylene, undecylene, and dodecylene; and alkenylene groups such as vinylene, propenylene, isopropenylene, butenylene, butadienylene, pentenylene, hexenylene, and heptenylene.
[0052] Examples of the divalent alicyclic hydrocarbon group include cycloalkylene groups such as cyclopropylene, cyclobutylene, cyclopentylene, cyclohexylene, norbornylene and adamantylene; and cycloalkylidene groups such as cyclopentylidene and cyclohexylidene.
[0053] Examples of the divalent aromatic hydrocarbon group include arylene groups such as phenylene, tolylene, and naphthylene; cinnamylene, and biphenylene.
[0054] Among them, the divalent hydrocarbon group is preferably a divalent aliphatic hydrocarbon group or a divalent alicyclic hydrocarbon group, more preferably a divalent aliphatic hydrocarbon group, and still more preferably an alkylene group.
[0055] The divalent hydrocarbon group has preferably 1 to 7 carbon atoms, more preferably 1 to 5 carbon atoms, and even more preferably 1 to 3 carbon atoms, from the viewpoint of excellent dimensional stability.
[0056] Examples of the substituent which the divalent hydrocarbon group may have include a carboxyl group, a hydroxyl group, an alkoxy group, a halogen atom, and a hydrocarbon group having 1 to 7 carbon atoms.
[0057] As the above R 4 Preferred specific examples of the divalent organic group represented by include: -R a -COO-, -R a -OCO-R a -COO-, -R a -COO-R a -COO-(R a are identical or different and represent a divalent organic group which may or may not have a substituent), etc., and -R a -COO-(R arepresents a divalent hydrocarbon group).
[0058] The above R 4 Direct bonding is most preferred.
[0059] In the above formula (1), R 5 , R 6 , R 7 and R 8 Same or different, represents hydrogen atom or Y, R 5 , R 6 , R 7 and R 8 At least one of them is Y. The above Y is a group represented by the above formula (2).
[0060] In the above formula (2), R 11 is a divalent organic group which may have a substituent. 11 The divalent organic group represented by can include the same groups as the above-mentioned divalent organic groups. Among them, a divalent hydrocarbon group is preferred, a divalent aliphatic hydrocarbon group, a divalent alicyclic hydrocarbon group or a divalent aromatic hydrocarbon group is more preferred, and a divalent aliphatic hydrocarbon group or a divalent alicyclic hydrocarbon group is further preferred.
[0061] The above R 11 The number of carbon atoms of the divalent organic group represented is preferably 1 to 20, more preferably 1 to 10, further preferably 1 to 8, further more preferably 2 to 6, particularly preferably 2 or 6, and most preferably 6.
[0062] As the above R 11 Examples of the substituent that the divalent organic group represented may have include a carboxyl group and a hydrocarbon group having 1 to 20 carbon atoms. Among them, a carboxyl group is preferred because it can improve alkali solubility.
[0063] In the above formula (1), W represents a divalent organic group.
[0064] Examples of the divalent organic group represented by W include the above-mentioned divalent organic groups, and among them, a divalent hydrocarbon group which may have a substituent, -O-, or a combination thereof is preferred.
[0065] Examples of the divalent hydrocarbon group include the above-mentioned divalent hydrocarbon groups, among which a divalent aromatic hydrocarbon group is preferred, and a biphenylene group is more preferred.
[0066] Examples of the substituent that the divalent hydrocarbon group may have include a hydrocarbon group having 1 to 10 carbon atoms, a halogen atom, and a cyano group.
[0067] Preferred specific examples of the divalent organic group represented by W include groups represented by the following formula (3).
[0068] [Chemistry 5]
[0069]
[0070] (Where R 12 and R 13 are the same or different and represent a divalent hydrocarbon group. 14 and R 15 The same or different, represents a substituent. a represents R 14 The number of is an integer from 0 to 4. b represents R 15 The number of is an integer from 0 to 4.)
[0071] As the above R 12 and R 13 The divalent hydrocarbon group represented by may preferably be the above-mentioned divalent hydrocarbon groups, among which a divalent aliphatic hydrocarbon group is preferred, a divalent saturated aliphatic hydrocarbon group having 1 to 3 carbon atoms is more preferred, and a methylene group is further preferred.
[0072] As the above R 14 and R 15 The substituent represented is not particularly limited and may be any monovalent substituent, among which a hydrocarbon group is preferred, a hydrocarbon group having 1 to 10 carbon atoms is more preferred, an aliphatic hydrocarbon group having 1 to 5 carbon atoms is further preferred, a saturated aliphatic hydrocarbon group having 1 to 5 carbon atoms is further preferred, and a methyl group is most preferred.
[0073] a is an integer of 0-4, preferably 0-2, and more preferably 2.
[0074] b is an integer of 0 to 4, preferably 0 to 2, and more preferably 2.
[0075] In the above formula (1), X represents a direct bond or a divalent organic group.
[0076] As the divalent organic group represented by X, the above-mentioned divalent organic groups can be cited, among which divalent hydrocarbon groups with or without substituents, -SO2- or combinations thereof are preferred, divalent hydrocarbon groups with or without substituents having 1 to 20 carbon atoms or -SO2- are more preferred, divalent aliphatic hydrocarbon groups with 1 to 10 carbon atoms or -SO2- are further preferred, divalent saturated aliphatic hydrocarbon groups with 1 to 5 carbon atoms or -SO2- are further preferred, and -SO2- is most preferred. The presence of S atoms can increase the refractive index.
[0077] Examples of the substituent include the substituents described above, and among them, preferred examples include halogen atoms such as a fluorine atom, a chlorine atom and an iodine atom.
[0078] When the divalent hydrocarbon group has a ring structure, preferred examples of the substituent include a halogen atom and an alkyl group.
[0079] Among them, X is preferably a direct bond, an alkylene group, or -SO2-, more preferably a direct bond, an alkylene group having 1 to 10 carbon atoms, or -SO2-, and further preferably a direct bond or -SO2-.
[0080] It should be noted that when n is 2 or more, two or more Xs may be the same or different.
[0081] In the above formula (1), R 9 and R 10 The same or different represent substituents.
[0082] As the above R 9 or R 10 The substituent represented by may be any monovalent substituent, for example, a carboxyl group, a hydroxyl group, an amino group, a hydrocarbon group having 1 to 20 carbon atoms, a halogen atom, or a group consisting of a combination thereof.
[0083] Even if the substituent is an arbitrary substituent, the alkali-soluble resin can form a dense cured product due to the stacking interaction of the aromatic rings, and a cured product having a high refractive index can be obtained.
[0084] l represents a substituent R 9 The number is an integer of 0 to 4, preferably 0 to 2, more preferably 0 or 2, and further preferably 0.
[0085] m represents a substituent R 10 The number is an integer of 0 to 4, preferably 0 to 2, more preferably 0 or 2, and further preferably 0.
[0086] R 9 and R 10 When there are two or more, they may be the same or different.
[0087] n represents an integer of 1 or greater.
[0088] In the above-mentioned alkali-soluble resin, the content of the ammonium salt compound is 0.06% by mass or less relative to 100% by mass of the alkali-soluble resin. When the content of the ammonium salt compound in the above-mentioned alkali-soluble resin is 0.06% by mass or less, a cured product having excellent heat-resistant coloration can be provided. In the past, when synthesizing the above-mentioned alkali-soluble resin, ammonium salt compounds such as benzyltriethylammonium chloride were used as catalysts. The present invention has found that such ammonium salt compounds become the cause of deterioration of the heat-resistant coloration of the alkali-soluble resin, and has found that by making the amount of the ammonium salt compound contained in the alkali-soluble resin be below the prescribed value, the heat-resistant coloration of the alkali-soluble resin can be significantly improved.
[0089] From the viewpoint of achieving better heat coloration resistance, the content of the ammonium salt compound is more preferably 0.03% by mass or less, further preferably 0.01% by mass or less, and most preferably 0% by mass based on 100% by mass of the alkali-soluble resin.
[0090] Examples of the ammonium salt compound include benzyltriethylammonium chloride, benzyltrimethylammonium chloride, tetra-n-butylammonium chloride, tetraethylammonium chloride, tetramethylammonium chloride, and quaternary ammonium salts such as bromides thereof.
[0091] The content of the ammonium salt compound can be determined by quantification based on ion chromatography of ammonium ions or by mass spectrometry. Alternatively, it can be calculated by dividing the mass of the ammonium salt compound used by the total mass of the monomer components constituting the alkali-soluble resin having the structure represented by the above formula (1).
[0092] The acid value of the alkali-soluble resin is preferably 30 to 150 mgKOH / g, more preferably 40 to 135 mgKOH / g, further preferably 50 to 120 mgKOH / g, and most preferably 70 to 100 mgKOH / g.
[0093] The acid value is a value measured by a neutralization titration method using a potassium hydroxide (KOH) solution, and is an acid value per 1 g of the resin solid content.
[0094] The weight average molecular weight of the alkali-soluble resin is preferably 400 to 30000. From the viewpoint of faster development speed, the weight average molecular weight of the alkali-soluble resin is more preferably 1000 to 10000, further preferably 2000 to 5000, and further more preferably 2500 to 3500.
[0095] The weight average molecular weight is a value measured by gel permeation chromatography (GPC method). Specifically, it can be measured by GPC method based on HLC-8220GPC (manufactured by Tosoh Corporation) and column: TSKgel SuperHZM-M (manufactured by Tosoh Corporation) using polystyrene as a standard substance and tetrahydrofuran as an eluent.
[0096] The double bond equivalent of the alkali-soluble resin is preferably 500 to 2000 g / equivalent, more preferably 530 to 1500 g / equivalent, further preferably 550 to 1100 g / equivalent, and further preferably 570 to 900 g / equivalent in order to improve curability.
[0097] The double bond here refers to a double bond having free radical polymerizability, that is, a double bond represented by a (meth)acryloyl group, and a double bond generated by, for example, adding tetrahydrophthalic anhydride to an OH group is not reactive and therefore is not included in the calculation as a double bond equivalent.
[0098] The double bond equivalent refers to the mass of the solid content of the polymer solution per 1 mol of double bonds of the resin. The mass of the solid content of the polymer solution refers to the mass of the monomer components constituting the resin. The double bond equivalent can be calculated by dividing the mass (g) of the resin solid content of the polymer solution by the amount of double bonds (mol) of the resin. In addition, it can also be measured using titration and various analyses such as elemental analysis, NMR, IR, and differential scanning calorimetry. For example, it can be calculated by measuring the number of olefinic double bonds contained in each 1 g of resin based on the test method for iodine value described in JIS K0070:1992.
[0099] 2. Method for producing alkali-soluble resin
[0100] As a method for manufacturing the above-mentioned alkali-soluble resin, there is no particular limitation as long as it is a method that can obtain an alkali-soluble resin having the above-mentioned structure, and it can be appropriately selected from known polymerization methods. Among them, from the aspect of being able to effectively obtain the above-mentioned alkali-soluble resin, the method for manufacturing the above-mentioned alkali-soluble resin preferably includes: a step (a-1) of reacting a difunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90°C or more obtained based on JIS K0071-2 with a bisphenol compound; a step (a-2) of reacting the reaction product obtained in the above-mentioned step (a-1) with an unsaturated monobasic acid; and a step (a-3) of reacting the reaction product obtained in the above-mentioned step (a-2) with a polyacid anhydride. Below, each step is explained.
[0101] Step (a-1)
[0102] In the above production method, first, a bifunctional epoxy compound having a Gardner color of less than 12 according to JIS K 0071-2 and a melting point of 90° C. or higher is reacted with a bisphenol compound.
[0103] In the reaction of the step (a-1), the epoxy group of the bifunctional epoxy compound reacts with the phenolic hydroxyl group of the bisphenol compound to form a compound in which the bifunctional epoxy compound and the bisphenol compound are linked.
[0104] The difunctional epoxy compound used in the reaction step preferably has a Gardner color of less than 12 based on JIS K 0071-2 and a melting point of 90° C. or more. When the Gardner color of the difunctional epoxy compound is less than 12, the obtained alkali-soluble resin can provide a cured product having excellent heat resistance, flexibility, and refractive index. This is believed to be because by using a raw material with a specified Gardner color, the oxidative degradation of the product caused by oxygen can be reduced.
[0105] The Gardner color of the difunctional epoxy compound is more preferably less than 11, further preferably less than 10, and most preferably less than 8, from the viewpoint of further improving the heat coloration resistance of the obtained alkali-soluble resin.
[0106] From the viewpoint of excellent heat resistance, the melting point of the bifunctional epoxy compound is more preferably 95° C. or higher, and further preferably 100° C. or higher.
[0107] The epoxy equivalent of the bifunctional epoxy compound is preferably 150 to 300 g / equivalent, more preferably 160 to 250 g / equivalent, and even more preferably 170 to 200 g / equivalent.
[0108] The epoxy equivalent can be determined by a method in accordance with JIS K7236:2001, and specifically, can be determined by a method described in Examples below.
[0109] The bifunctional epoxy compound is not particularly limited as long as it is a compound having two epoxy groups that satisfies the above-mentioned Gardner chromaticity and melting point, but preferably, a compound represented by the following formula (4) can be mentioned.
[0110] [Chemistry 6]
[0111]
[0112] (W represents a divalent organic group.)
[0113] In the above formula (4), W is preferably a divalent organic group similar to W in the above formula (1).
[0114] The compound represented by the above formula (4) may have a molecular weight distribution. The weight average molecular weight of the compound represented by the above formula (4) is preferably 80 to 5,000, more preferably 100 to 1,000, and even more preferably 150 to 500.
[0115] The weight average molecular weight is a value measured by gel permeation chromatography (GPC).
[0116] The compound represented by the above formula (4) can be synthesized by a known method, and for example, the method described in JP-A-2016-108562 can be mentioned. Usually, epichlorohydrin is added to a bisphenol compound for synthesis.
[0117] The bifunctional epoxy compound can also be obtained as a commercial product, for example, YL6121H, YX4000 (manufactured by Mitsubishi Chemical), YDC-1312, YSLV-120TE (manufactured by Nippon Steel Chemical Materials), etc. can be mentioned.
[0118] The above-mentioned bifunctional epoxy compounds may be used alone or in combination of two or more.
[0119] The bisphenol compound is not particularly limited as long as it is a compound having two phenolic hydroxyl groups, but preferably, a compound represented by the following formula (5) is mentioned.
[0120] [Chemistry 7]
[0121]
[0122] (wherein, X represents a direct bond or a divalent organic group. R 9 and R 10 The same or different, represents a substituent. l represents R 9 The number of is an integer from 0 to 4. m represents R 10 The number of is an integer from 0 to 4. 9 and R 10 When there are two or more, they may be the same or different.)
[0123] In the above formula (5), X, R 9 and R 10 Preferably, X, R 9 and R 10 In addition, l and m in the above formula (5) are preferably the same as l and m in the above formula (1), respectively.
[0124] Specific examples of the bisphenol compounds include bisphenol A, bisphenol AP, bisphenol AF, bisphenol B, bisphenol BP, bisphenol C, bisphenol E, bisphenol F, bisphenol G, bisphenol M, bisphenol S, bisphenol TMC, bisphenol P, bisphenol PH, bisphenol Z, and the like.
[0125] Among them, bisphenol A, bisphenol F, and bisphenol S are preferred, and bisphenol S is more preferred, from the viewpoint of relatively easy availability.
[0126] The above-mentioned bisphenol compounds may be used alone or in combination of two or more.
[0127] The reaction of the bifunctional epoxy compound and the bisphenol compound can be performed by mixing these components in a solvent.
[0128] Regarding the mixing ratio of the difunctional epoxy compound and the bisphenol compound, the bisphenol compound is preferably 10 to 60 parts by mass, more preferably 15 to 55 parts by mass, further preferably 20 to 50 parts by mass, and most preferably 30 to 40 parts by mass, relative to 100 parts by mass of the difunctional epoxy compound.
[0129] Examples of the solvent include ethers such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, and diethylene glycol dimethyl ether; ketones such as acetone and methyl ethyl ketone; esters such as ethyl acetate, butyl acetate, cellosolve acetate, carbitol acetate, (di)propylene glycol monomethyl ether acetate, and 3-methoxybutyl acetate; aromatic hydrocarbons such as toluene, xylene, and ethylbenzene; chloroform; dimethyl sulfoxide; and dimethyl carbonate. Among them, esters are preferred, and carbitol acetate and (di)propylene glycol monomethyl ether acetate are more preferred. These solvents may be used alone or in combination of two or more.
[0130] In the above reaction, a reaction catalyst is preferably used. As the reaction catalyst used, compounds other than the above ammonium salt compounds are preferred, for example, tertiary amines such as trimethylamine, triethylamine, tributylamine, tripropylamine, and trihexylamine; tertiary phosphines such as triphenylphosphine; quaternary phosphonium salts such as benzyltriphenylphosphonium bromide; chelate compounds, etc. Among them, as the above reaction catalyst, tertiary phosphines such as triphenylphosphine are preferred from the aspect of having excellent activity. In addition, when a tertiary phosphine is used, the voltage retention of the obtained cured product can also be improved.
[0131] The above reaction catalysts may be used alone or in combination of two or more.
[0132] Since metal compounds have electrical conductivity, there is a possibility that the electrical properties of the composition may be deteriorated, and therefore it is not preferable to use a catalyst containing a metal atom.
[0133] The amount of the reaction catalyst is not particularly limited, but is preferably 0.05 to 5 parts by mass, more preferably 0.07 to 1 part by mass, further preferably 0.08 to 0.8 part by mass, and most preferably 0.1 to 0.6 part by mass, based on 100 parts by mass of the bifunctional epoxy compound.
[0134] The reaction temperature of the above reaction is not particularly limited, but is preferably 80 to 150°C, more preferably 85 to 145°C, and further preferably 90 to 140°C.
[0135] The reaction time is not particularly limited, but is preferably 2 to 10 hours, more preferably 3 to 9 hours, and even more preferably 4 to 8 hours.
[0136] The above reaction may be carried out in an air atmosphere or in an inert gas atmosphere such as nitrogen or argon. Among them, an inert gas atmosphere is preferred from the viewpoint of suppressing the deactivation of the catalyst.
[0137] Step (a-2)
[0138] In step (a-2), the reaction product obtained in step (a-1) is reacted with an unsaturated monobasic acid. Through this reaction, the unsaturated monobasic acid reacts with the epoxy group of the bifunctional epoxy compound to introduce a radical polymerizable unsaturated bond at the terminal of the reaction product.
[0139] Examples of the unsaturated monobasic acid include monobasic acids having one carboxyl group and one or more free radical polymerizable unsaturated bonds. Specific examples include acrylic acid, methacrylic acid, crotonic acid, cinnamic acid, β-acryloxypropionic acid, reaction products of hydroxyalkyl (meth)acrylates having one hydroxyl group and one (meth)acryloyl group and dibasic acid anhydrides, reaction products of polyfunctional (meth)acrylates having one hydroxyl group and two or more (meth)acryloyl groups and dibasic acid anhydrides, caprolactone-modified products of these monobasic acids, and the like.
[0140] Among them, the unsaturated monobasic acid is preferably a compound having a (meth)acryloyl group such as acrylic acid and methacrylic acid, from the viewpoint of good reactivity of the unsaturated double bond, more preferably acrylic acid and methacrylic acid, and most preferably methacrylic acid.
[0141] The above-mentioned unsaturated monobasic acid may be used alone or in combination of two or more.
[0142] The amount of the unsaturated monobasic acid to be added is preferably such that 0.6 to 1.4 moles of the acid groups in the unsaturated monobasic acid are added to 1 mole of the epoxy groups in the reaction product obtained in the step (a-1), more preferably 0.7 to 1.3 moles, further preferably 0.8 to 1.2 moles, and further preferably 1.0 to 1.1 moles. When epoxy groups remain in the resin, the storage stability may be deteriorated.
[0143] The unsaturated monobasic acid may be added all at once, in portions or successively. However, in terms of suppressing side reactions, addition in portions or successively is preferred.
[0144] In the reaction of the step (a-2), it is preferred to use an addition catalyst.
[0145] As the addition catalyst, the same catalyst as the reaction catalyst used in the above step (a-1) can be mentioned, for example, tertiary amines such as trimethylamine, triethylamine, tributylamine, tripropylamine, and trihexylamine; tertiary phosphines such as triphenylphosphine; quaternary phosphonium salts such as benzyltriphenylphosphonium bromide; chelate compounds, etc. These can be used alone or in combination of two or more.
[0146] Among them, as the addition catalyst, a tertiary phosphine such as triphenylphosphine is preferred.
[0147] It should be noted that since metal compounds have electrical conductivity, there is a possibility that the electrical properties of the composition may be deteriorated, and therefore it is not preferable to use a catalyst containing a metal atom.
[0148] The amount of the addition catalyst is not particularly limited, but is preferably 0.05 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, further preferably 0.2 to 3 parts by mass, and most preferably 0.5 to 2.5 parts by mass relative to 100 parts by mass of the difunctional epoxy compound. It should be noted that the amount of the catalyst herein refers to the total amount of the catalyst and the reaction catalyst when a reaction catalyst is used in the step (a-1).
[0149] When the same catalyst is used as the reaction catalyst and the addition catalyst in the reaction of the above-mentioned step (a-1) and the above-mentioned step (a-2), the total amount of the catalyst used in the manufacturing process can be added at one time in the above-mentioned step (a-1), but it is preferably added in batches in the above-mentioned step (a-1) and the above-mentioned step (a-2). By adding in batches, the reduction in catalyst activity can be suppressed. In particular, when a tertiary phosphine is used as a catalyst, it will be oxidized in the presence of oxygen and the catalyst activity will be reduced, so it is preferably added in batches to make up for the deactivated part. If a large amount of phosphine is used in the early stage in anticipation of the deactivated part, the oxide of the phosphine will be yellow, and the coloring of the obtained resin may increase.
[0150] In the case of batch addition in the above-mentioned steps (a-1) and the above-mentioned step (a-2), the ratio of the amount of catalyst added in each step is preferably 5 / 95 to 95 / 5, more preferably 10 / 90 to 90 / 10, further preferably 15 / 85 to 85 / 15, and further more preferably 20 / 80 to 80 / 20, in terms of the amount of catalyst added in step (a-1) / the amount of catalyst added in step (a-2).
[0151] In each of the above steps (a-1) and (a-2), the catalyst may be added all at once, in batches, or in small amounts successively. From the perspective of suppressing the decrease in catalyst activity, batch addition or small amounts successively are preferred.
[0152] In the reaction of step (a-2), a polymerization inhibitor may be used. By using a polymerization inhibitor, gelation can be suppressed.
[0153] The polymerization inhibitor is not particularly limited, and a known polymerization inhibitor can be used, for example, benzoquinone, hydroquinones (for example, hydroquinone, methylhydroquinone, hydroquinone monomethyl ether, p-tert-butylhydroquinone, p-benzoquinone, etc.), phenols (for example, 2,6-di-tert-butyl-4-methylphenol, 6-tert-butyl-2,4-dimethylphenol, 2,2'-methylenebis(4-methyl-6-tert-butylphenol), etc.), catechols (for example, p-tert-butylcatechol, etc.), amines (for example, N,N-diethylhydroxylamine, etc.), 1,1-diphenyl-2-picrylhydrazyl, tri-p-nitrophenylmethyl, phenothiazine, piperidine 1-oxyl radicals (for example, 2,2,6,6-tetramethylpiperidine 1-oxyl radical, etc.), oxygen, etc. Among them, hydroquinones are preferred from the viewpoint of further improving the heat coloration resistance of the alkali-soluble resin, and hydroquinone is more preferred from the viewpoint of improving the flexibility of the cured product of the alkali-soluble resin.
[0154] The above-mentioned polymerization inhibitors may be used alone or in combination of two or more.
[0155] The reaction conditions of the step (a-2) are not particularly limited, but the reaction temperature is preferably 80 to 140° C., more preferably 85 to 135° C., and even more preferably 90 to 130° C. The reaction time is not particularly limited, but is preferably 5 to 30 hours, more preferably 6 to 25 hours, and even more preferably 7 to 20 hours.
[0156] Step (a-3)
[0157] In the step (a-3), the reaction product obtained in the step (a-2) is reacted with a polybasic acid anhydride. In the reaction in the step (a-3), the polybasic acid anhydride is added to the hydroxyl group of the reaction product obtained in the step (a-2) to introduce the acid group of the carboxyl group into the reaction product.
[0158] Examples of the polybasic acid anhydride include dibasic acid anhydrides such as phthalic anhydride, succinic anhydride, octenyl succinic anhydride, penta (dodecenyl) succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, hexahydrophthalic anhydride, methyltetrahydrophthalic anhydride, 3,6-endomethylenetetrahydrophthalic anhydride, methylendomethylenetetrahydrophthalic anhydride, tetrabromophthalic anhydride, and a reaction product of 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide and itaconic anhydride or maleic anhydride; trimellitic anhydride; and aliphatic or aromatic tetrabasic acid dianhydrides such as biphenyltetracarboxylic dianhydride, naphthalenetetracarboxylic dianhydride, diphenyl ether tetracarboxylic dianhydride, butanetetracarboxylic dianhydride, cyclopentanetetracarboxylic dianhydride, pyromellitic dianhydride, and benzophenonetetracarboxylic dianhydride. Among them, tetrahydrophthalic anhydride is preferred.
[0159] The above-mentioned polybasic acid anhydride may be used alone or in combination of two or more.
[0160] The polybasic acid anhydride is preferably added to react in an amount of 0.1 to 1.1 mol, more preferably 0.15 to 1 mol, further preferably 0.2 to 0.9 mol, and most preferably 0.4 to 0.7 mol, based on 1 mol of hydroxyl groups in the reaction product obtained in the step (a-2).
[0161] In the reaction of the step (a-3), a catalyst may be used as necessary. Examples of the catalyst to be used include the same catalysts as those mentioned above.
[0162] The reaction conditions of the step (a-3) are not particularly limited, but the reaction temperature is preferably 60 to 150° C., more preferably 70 to 135° C., and even more preferably 80 to 120° C. The reaction time is not particularly limited, but is preferably 1 to 10 hours, more preferably 2 to 9 hours, and even more preferably 3 to 8 hours.
[0163] The method for producing the alkali-soluble resin may include other steps in addition to the reaction step. Examples of the other steps include an aging step, a neutralization step, a dilution step, a drying step, a concentration step, and a purification step. These steps may be performed by known methods.
[0164] In the alkali-soluble resin obtained by the method for producing an alkali-soluble resin, the content of the ammonium salt compound is preferably 0.06 mass % or less, more preferably 0.03 mass % or less, further preferably 0.01 mass % or less, and most preferably 0 mass % based on 100 mass % of the alkali-soluble resin.
[0165] The above-mentioned production method can efficiently obtain an alkali-soluble resin that can provide a cured product having excellent heat discoloration resistance and a high refractive index.
[0166] The following method for producing an alkali-soluble resin is also one of the present invention, and the method for producing an alkali-soluble resin is characterized in that it includes: a step (a-1) of reacting a difunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90°C or more obtained based on JIS K 0071-2 with a bisphenol compound; a step (a-2) of reacting the reaction product obtained in the above step (a-1) with an unsaturated monobasic acid; and a step (a-3) of reacting the reaction product obtained in the above step (a-2) with a polyacid anhydride, wherein the content of the ammonium salt compound in the alkali-soluble resin obtained by the above production method is less than 0.06% by mass relative to 100% by mass of the alkali-soluble resin.
[0167] 3. Alkali-soluble resin composition
[0168] In addition, the present invention relates to an alkali-soluble resin composition, characterized in that it contains the above-mentioned alkali-soluble resin and an acid group-containing epoxy (meth)acrylate.
[0169] The alkali-soluble resin composition of the present invention comprises the above-mentioned alkali-soluble resin, and thus can provide a cured product having excellent heat-resistant coloration and a high refractive index. In addition, by further comprising an epoxy (meth) acrylate containing an acid group, it is possible to improve the developability and curability, and impart the characteristics derived from the epoxy (meth) acrylate skeleton containing an acid group.
[0170] The acid group-containing epoxy (meth)acrylate is an ester of an epoxy resin and (meth)acrylic acid, and is a compound containing an acid group.
[0171] From the viewpoint of increasing the crosslinking density of the cured product, the epoxy resin is preferably difunctional or higher, more preferably 2-20functional, further preferably 2-10functional, and most preferably difunctional.
[0172] The epoxy resin is not particularly limited as long as it is a compound having an epoxy group, and examples thereof include: known aliphatic epoxy resins, aromatic epoxy resins, etc. Among them, aromatic epoxy resins are preferred from the aspects of being able to form a dense cured film and being able to improve electrical insulation. The epoxy resin may include one or more kinds.
[0173] Examples of the aromatic epoxy resin include bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol S epoxy resin, biphenyl epoxy resin, tetramethylbiphenyl epoxy resin, phenol novolac epoxy resin, cresol novolac epoxy resin, bisphenol A novolac epoxy resin, triphenylmethane epoxy resin, tetraphenylethane epoxy resin, dicyclopentadiene-phenol addition reaction epoxy resin, phenol aralkyl epoxy resin, naphthol novolac epoxy resin, naphthol aralkyl epoxy resin, naphthol-phenol co-condensed novolac epoxy resin, naphthol-cresol co-condensed novolac epoxy resin, aromatic hydrocarbon formaldehyde resin-modified phenolic resin epoxy resin, and biphenyl novolac epoxy resin. Among them, as the above-mentioned aromatic epoxy resin, bisphenol A type epoxy resin and cresol novolac type epoxy resin are preferred from the viewpoint of good electrical properties, and bisphenol A type epoxy resin is more preferred from the viewpoint of being able to obtain a cured product with better heat discoloration resistance and a higher refractive index.
[0174] These epoxy resins may have a substituent such as a halogen atom, an alkyl group, an alkylene group, a cycloalkylene group, an arylene group, or a cyano group.
[0175] The epoxy resin may have a molecular weight distribution, and the weight average molecular weight of the epoxy resin is preferably 100 to 30,000, more preferably 150 to 2,000, and even more preferably 300 to 1,000.
[0176] The weight average molecular weight is a value measured by gel permeation chromatography (GPC).
[0177] The epoxy equivalent of the epoxy resin is preferably 150 to 5000 g / equivalent, more preferably 170 to 1000 g / equivalent, and even more preferably 200 to 300 g / equivalent, from the viewpoint of excellent physical properties of the obtained cured product.
[0178] The epoxy equivalent can be determined by a method in accordance with JIS K7236:2001, and specifically, can be determined by a method described in Examples below.
[0179] Examples of the acid group include a carboxyl group, a phenolic hydroxyl group, a carboxylic anhydride group, a phosphoric acid group, and a sulfonic acid group. Among these, a carboxyl group is preferred because of good developability.
[0180] The above-mentioned epoxy (meth)acrylate containing an acid group may be an epoxy (meth)acrylate containing an acid group obtained by reacting an epoxy (meth)acrylate obtained by reacting the above-mentioned epoxy resin with (meth)acrylic acid with a polybasic acid anhydride, or may be an epoxy (meth)acrylate containing an acid group obtained by reacting an epoxy resin having the above-mentioned acid group with (meth)acrylic acid. From the perspective of excellent production efficiency of the alkali-soluble resin composition, an epoxy (meth)acrylate containing an acid group obtained by reacting an epoxy (meth)acrylate obtained by reacting the above-mentioned epoxy resin with (meth)acrylic acid with a polybasic acid anhydride is preferred.
[0181] By reacting the epoxy resin with (meth)acrylic acid, the epoxy group is ring-opened to generate a hydroxyl group, and a structure is formed in which a polyacid anhydride is added to the hydroxyl group.
[0182] Examples of the polybasic acid anhydride include the same polybasic acid anhydrides as those described above.
[0183] The acid value of the acid group-containing epoxy (meth)acrylate is preferably 20 to 160 mgKOH / g, more preferably 30 to 150 mgKOH / g, further preferably 40 to 140 mgKOH / g, and most preferably 70 to 100 mgKOH / g.
[0184] In the above-mentioned alkali-soluble resin composition, the content of the above-mentioned alkali-soluble resin is preferably 1 to 99% by mass, more preferably 5 to 95% by mass, further preferably 10 to 90% by mass, and most preferably 20 to 40% by mass relative to 100% by mass of the total solid content of the alkali-soluble resin composition. It should be noted that in the present invention, the total solid content refers to the total amount of components forming a cured product (excluding components other than the solvent and the curing catalyst that volatilize when the cured product is formed).
[0185] In the above-mentioned alkali-soluble resin composition, the content of the above-mentioned acid group-containing epoxy (meth)acrylate is preferably 0.1 to 90 mass %, more preferably 1 to 85 mass %, further preferably 5 to 80 mass %, and most preferably 60 to 80 mass %, relative to 100 mass % of the total solid content of the alkali-soluble resin composition.
[0186] In the above-mentioned alkali-soluble resin composition, regarding the content ratio of the above-mentioned alkali-soluble resin and the above-mentioned epoxy (meth)acrylate containing an acid group, the above-mentioned epoxy (meth)acrylate containing an acid group is preferably 0.1 to 500 parts by mass, more preferably 10 to 400 parts by mass, and further preferably 100 to 300 parts by mass, relative to 100 parts by mass of the above-mentioned alkali-soluble resin.
[0187] From the viewpoint of good developability, the acid value of the alkali-soluble resin composition is preferably 20 to 150 mgKOH / g, more preferably 30 to 135 mgKOH / g, further preferably 40 to 120 mgKOH / g, and most preferably 70 to 100 mgKOH / g.
[0188] The acid value of the alkali-soluble resin composition can be determined by the same method as that for the double bond equivalent of the alkali-soluble resin.
[0189] The double bond equivalent of the alkali-soluble resin composition is preferably 300 to 2000 g / equivalent, more preferably 330 to 1500 g / equivalent, further preferably 360 to 1100 g / equivalent, and further preferably 400 to 900 g / equivalent in order to improve curability.
[0190] The double bond equivalent of the alkali-soluble resin composition can be determined by the same method as the double bond equivalent of the alkali-soluble resin.
[0191] The above-mentioned alkali-soluble resin composition may contain other ingredients other than the above-mentioned ingredients as needed. As the above-mentioned other ingredients, for example, there can be mentioned: solvent; colorant (pigment, dye); dispersant; heat resistance improving agent; leveling agent; developing aid; inorganic particles such as silica particles; coupling agents such as silane, aluminum, and titanium; thermosetting resins such as fillers, phenolic resins, and polyvinylphenol; polymerizable compounds; curing aids such as multifunctional thiol compounds; plasticizers; polymerization initiators; inhibitors; ultraviolet absorbers; antioxidants; matting agents; defoamers; antistatic agents; slip agents; surface modifiers; thixotropic agents; thixotropic aids; quinonediazide compounds; polyphenol compounds; cationic polymerizable compounds; thermal acid generators; etc. These ingredients can be used alone or in combination of two or more. These other ingredients can be appropriately selected from known substances and their amounts can also be appropriately set.
[0192] Among them, the alkali-soluble resin composition preferably further comprises at least one selected from the group consisting of a polymerizable compound, a polymerization initiator, and inorganic fine particles.
[0193] (Polymerizable compound)
[0194] The above-mentioned polymerizable compound is a low molecular weight compound having a polymerizable unsaturated bond (also referred to as a polymerizable unsaturated group) that can be polymerized by irradiation with free radicals, electromagnetic waves (such as infrared rays, ultraviolet rays, X-rays, etc.), active energy rays such as electron beams, etc., and examples thereof include: a monofunctional compound having one polymerizable unsaturated group in the molecule and a polyfunctional compound having two or more polymerizable unsaturated groups in the molecule.
[0195] Examples of the monofunctional compound include: N-substituted maleimide monomers; (meth)acrylates; (meth)acrylamides; unsaturated monocarboxylic acids; unsaturated polycarboxylic acids; unsaturated monocarboxylic acids with extended chains between unsaturated groups and carboxyl groups; unsaturated acid anhydrides; aromatic vinyls; conjugated dienes; vinyl esters; vinyl ethers; N-vinyl compounds; unsaturated isocyanates; etc. In addition, monomers having active methylene groups or active methine groups may also be used.
[0196] Examples of the polyfunctional compound include the following compounds.
[0197] Bifunctional (meth)acrylate compounds such as ethylene glycol di(meth)acrylate, diethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, butanediol di(meth)acrylate, hexanediol di(meth)acrylate, cyclohexanedimethanol di(meth)acrylate, bisphenol A alkylene oxide di(meth)acrylate, and bisphenol F alkylene oxide di(meth)acrylate;
[0198] Trimethylolpropane tri(meth)acrylate, di(trimethylolpropane) tetra(meth)acrylate, glycerol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, ethylene oxide added trimethylolpropane tri(meth)acrylate, ethylene oxide added di(trimethylolpropane) tetra(meth)acrylate, ethylene oxide added pentaerythritol tetra(meth)acrylate, ethylene oxide added dipentaerythritol hexa(meth)acrylate, propylene oxide added trimethylolpropane tri(meth)acrylate, propylene oxide added di(trimethylolpropane) tetra(meth)acrylate, propylene oxide added pentaerythritol tetra(meth)acrylate, propylene oxide added dipentaerythritol hexa(meth)acrylate, ε-caprolactone added trimethylolpropane tri(meth)acrylate, ε-caprolactone added di(trimethylolpropane) tetra(meth)acrylate, ε-caprolactone added pentaerythritol tetra(meth)acrylate, ε-caprolactone added dipentaerythritol hexa(meth)acrylate, dipentaerythritol pentaacrylate succinic acid modified product, pentaerythritol triacrylate succinic acid modified product, dipentaerythritol pentaacrylate phthalic acid modified product, pentaerythritol triacrylate phthalic acid modified product, the following formula:
[0199]
[0200] A polyfunctional (meth)acrylate compound having three or more functionalities, such as a modified product of dipentaerythritol hexaacrylate represented above;
[0201] Ethylene glycol divinyl ether, diethylene glycol divinyl ether, polyethylene glycol divinyl ether, propylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, bisphenol A alkylene oxide divinyl ether, bisphenol F alkylene oxide divinyl ether, trimethylolpropane trivinyl ether, bis(trimethylolpropane) tetravinyl ether, glycerol trivinyl ether, pentaerythritol tetravinyl ether, dipentaerythritol pentavinyl ether, dipentaerythritol hexavinyl ether, ethylene oxide addition trimethylolpropane trivinyl ether, ethylene oxide addition bis(trimethylolpropane) tetravinyl ether, ethylene oxide addition pentaerythritol tetravinyl ether, ethylene oxide addition dipentaerythritol hexavinyl ether and other multifunctional vinyl ethers;
[0202] (meth)acrylates containing a vinyl ether group, such as 2-vinyloxyethyl (meth)acrylate, 3-vinyloxypropyl (meth)acrylate, 1-methyl-2-vinyloxyethyl (meth)acrylate, 2-vinyloxypropyl (meth)acrylate, 4-vinyloxybutyl (meth)acrylate, 4-vinyloxycyclohexyl (meth)acrylate, 5-vinyloxypentyl (meth)acrylate, 6-vinyloxyhexyl (meth)acrylate, 4-vinyloxymethylcyclohexylmethyl (meth)acrylate, p-vinyloxymethylphenylmethyl (meth)acrylate, 2-(vinyloxyethoxy)ethyl (meth)acrylate, and 2-(vinyloxyethoxyethoxyethoxy)ethyl (meth)acrylate;
[0203] Ethylene glycol diallyl ether, diethylene glycol diallyl ether, polyethylene glycol diallyl ether, propylene glycol diallyl ether, butanediol diallyl ether, hexanediol diallyl ether, bisphenol A alkylene oxide diallyl ether, bisphenol F alkylene oxide diallyl ether, trimethylolpropane triallyl ether, bis(trimethylolpropane) tetraallyl ether, glycerol triallyl ether, pentaerythritol tetraallyl ether, dipentaerythritol pentaallyl ether, dipentaerythritol hexaallyl ether, ethylene oxide addition trimethylolpropane triallyl ether, ethylene oxide addition bis(trimethylolpropane) tetraallyl ether, ethylene oxide addition pentaerythritol tetraallyl ether, ethylene oxide addition dipentaerythritol hexaallyl ether and other multifunctional allyl ethers;
[0204] Allyl (meth)acrylates such as allyl (meth)acrylate; polyfunctional (meth)acryloyl isocyanurates such as tris(acryloyloxyethyl)isocyanurate, tris(methacryloyloxyethyl)isocyanurate, alkylene oxide addition tris(acryloyloxyethyl)isocyanurate, and alkylene oxide addition tris(methacryloyloxyethyl)isocyanurate; polyfunctional allyl isocyanurates such as triallyl isocyanurate; polyfunctional polyurethane (meth)acrylates obtained by reacting polyfunctional isocyanates such as toluene diisocyanate, isophorone diisocyanate, and xylylene diisocyanate with hydroxyl-containing (meth)acrylates such as 2-hydroxyethyl (meth)acrylate and 2-hydroxypropyl (meth)acrylate; polyfunctional aromatic vinyls such as divinylbenzene; etc. These polymerizable compounds may be used alone or in combination of two or more.
[0205] Among the above-mentioned polymerizable compounds, it is preferred to use a multifunctional polymerizable compound from the aspect of further improving the curability of the curable resin composition. The functional number of the above-mentioned multifunctional polymerizable compound is preferably 3 or more, and more preferably 4 or more. In addition, the above-mentioned functional number is preferably 10 or less, and more preferably 8 or less.
[0206] The molecular weight of the polymerizable compound is not particularly limited, but is preferably 2000 or less, for example, from the viewpoint of handling.
[0207] As the above-mentioned multifunctional polymerizable compound, from the aspects of reactivity, economy, availability, etc., preferably, there can be mentioned: a compound having a (meth)acryloyl group such as a multifunctional (meth)acrylate compound, a multifunctional polyurethane (meth)acrylate compound, an isocyanurate compound containing a (meth)acryloyl group, and more preferably, a multifunctional (meth)acrylate compound. By including a compound having a (meth)acryloyl group, the photosensitivity and curability of the curable resin composition are more excellent, and a cured product with higher hardness and higher transparency can be obtained. As the above-mentioned multifunctional polymerizable compound, it is further preferred to use a multifunctional (meth)acrylate compound having more than three functions.
[0208] The content of the polymerizable compound is preferably 0 to 500 parts by mass, more preferably 5 to 300 parts by mass, and even more preferably 10 to 100 parts by mass, based on 100 parts by mass of the alkali-soluble resin (solid content).
[0209] (Polymerization initiator)
[0210] As the polymerization initiator, preferably, a photopolymerization initiator is used, and more preferably, a radical polymerizable photopolymerization initiator is used.
[0211] Specific examples of the photopolymerization initiator include aminoketone compounds such as 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone ("IRGACURE 907", manufactured by BASF), 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone ("IRGACURE 369", manufactured by BASF), and 2-dimethylamino-2-(4-methylbenzyl)-1-(4-morpholin-4-ylphenyl)-1-butanone ("IRGACURE 379", manufactured by BASF); 2,2-dimethoxy-1,2-diphenylethane-1-one ("IRGACURE 651", manufactured by BASF), methyl phenylglyoxylate ("DAROCURE 651", manufactured by BASF); MBF", manufactured by BASF), benzyl ketal compounds; 1-hydroxycyclohexyl phenyl ketone ("IRGACURE 184", manufactured by BASF), 2-hydroxy-2-methyl-1-phenylpropane-1-one ("DAROCUR 1173", manufactured by BASF), 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propane-1-one ("IRGACURE 2959", manufactured by BASF), 2 -hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropane-1-one ("IRGACURE 127", manufactured by BASF), [1-hydroxycyclohexyl phenyl ketone + benzophenone] ("IRGACURE 500", manufactured by BASF); and other alkylphenone compounds exemplified in paragraphs
[0084] to
[0086] of JP-A-2013-227485 Compounds; 1,2-octanedione, 1-[4-(phenylthio)phenyl]-, 2-(O-benzoyl oxime) ("OXE01", manufactured by BASF), ethyl ketone, 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime) ("OXE02", manufactured by BASF), 1,2-octanedione, 1-[4-(phenylthio)-, 2-, (O-benzoyl oxime)], ethyl ketone ("OXE03", manufactured by BASF) Oxime ester compounds such as oxime (manufactured by BASF), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-, 1-(O-acetyl oxime) ("OXE04", manufactured by BASF); benzophenone compounds; benzoin compounds; thioxanthone compounds; halomethylated triazine compounds; halomethylated oxadiazole compounds; biimidazole compounds; titanocene compounds; benzoate compounds; acridine compounds; phosphine oxide compounds; etc. Among them, aminoketone compounds and oxime ester compounds are preferred. The above-mentioned photopolymerization initiators can be used alone or in combination of two or more.
[0212] The content of the polymerization initiator is preferably 0 to 20% by mass, more preferably 0.3 to 15% by mass, further preferably 0.5 to 10% by mass, and further preferably 1 to 10% by mass, based on 100% by mass of the total solid content of the alkali-soluble resin composition.
[0213] (Inorganic particles)
[0214] As the above-mentioned inorganic fine particles, for example, inorganic particles described in Japanese Patent Laid-Open No. 2018-119086 can be cited. Among them, the above-mentioned inorganic fine particles are preferably metal particles or metal oxide particles, and more preferably metal oxide particles.
[0215] As the above-mentioned inorganic particles, for example, metal particles or metal oxide particles containing metal elements with high light transmittance and refractive index can be cited, and the metal elements include atoms such as Be, Mg, Ca, Sr, Ba, Sc, Y, La, Ce, Gd, Tb, Dy, Yb, Lu, Ti, Zr, Hf, Nb, Mo, W, Zn, B, Al, Si, Ge, Sn, Pb, Sb, Bi, and Te. Among them, from the aspect of being able to provide a cured product with a higher refractive index, the above-mentioned inorganic particles preferably include at least one metal element selected from the group consisting of Ti, Al, Zr, Zn, Sn, Ce, Nb and Si, and further, from the aspect of being able to provide a cured film with a high relative dielectric constant, it is more preferred to include Zr, and from the aspect of being able to provide a cured film with high hardness, it is more preferred to include Si.
[0216] The above-mentioned metal oxide may be an oxide of a single metal, a solid solution of two or more oxides, or a composite oxide. As a single metal oxide, for example, aluminum oxide (Al2O3), titanium oxide (TiO2), zirconium oxide (ZrO2), indium oxide (In2O3), zinc oxide (ZnO), tin oxide (SnO2), lanthanum oxide (La2O3), yttrium oxide (Y2O3), cerium oxide (CeO2), magnesium oxide (MgO), silicon oxide (SiO2), niobium oxide (Nb2O5), etc. As a solid solution of two or more oxides, for example, ITO, ATO, etc. may be mentioned. As a composite oxide, for example, barium titanate (BaTiO3), gray titanium oxide (CaTiO3), spinel (MgAl2O4), etc. may be mentioned.
[0217] Among them, from the perspective of being able to provide a cured product with a high refractive index, a high relative dielectric constant or a high hardness, the above-mentioned inorganic fine particles are particularly preferably zirconium dioxide particles (ZrO2 particles) and / or silicon dioxide particles (SiO2 particles).
[0218] The inorganic particles may or may not be surface-modified, but surface-modified inorganic particles are preferred from the perspective of improving dispersibility in the resin composition. The surface of the inorganic particles is lipophilized by surface modification, which can prevent aggregation of particles and make them micro-dispersed.
[0219] In the case where the inorganic particles are surface-modified, the mass of the inorganic particles also includes the mass of the surface modifier. The organic compound (surface modifier) that modifies the surface of the inorganic particles may be chemically bonded and / or coordinated, or attached to the inorganic particles through hydrogen bonding or salt formation, and the "surface modification" includes both the state in which the organic group is chemically bonded and / or coordinated to the inorganic particles, or the state in which the organic group is physically attached to the inorganic particles.
[0220] Surface-modified inorganic fine particles (hereinafter also referred to as "coated inorganic fine particles") can be obtained by a known method such as a method of mixing the above-mentioned inorganic fine particles with a surface modifier in a solvent or a method of performing a hydrothermal reaction in the presence of water.
[0221] In the method of mixing the above-mentioned inorganic particles with a surface modifier in a solvent, the surface modifier used is not particularly limited as long as it is an organic compound that can make the surface of the above-mentioned inorganic particles lipophilic, prevent the aggregation of particles, and make them micro-dispersed, for example, it can be enumerated: organic acid, coupling agent, surfactant, etc. They can be used only one kind, and can also use two or more kinds.
[0222] As the organic acid, carboxylic acids having 5 or more carbon atoms (compounds having a carboxyl group) are preferably mentioned, and specific examples thereof include valeric acid, hexanoic acid, heptanoic acid, octanoic acid, nonanoic acid, 2-ethylhexanoic acid, 2-methylheptanoic acid, 4-methyloctanoic acid, salicylic acid, cycloalkane acid, decanoic acid, undecanoic acid, neodecanoic acid, lauric acid, tridecanoic acid, myristic acid, pentadecanoic acid, palmitic acid, heptadecanoic acid, pivalic acid, 2,2-dimethylbutanoic acid, 3,3-dimethylbutanoic acid, 2,2-dimethylvaleric acid, 2,2-diethylbutanoic acid, 3,3-diethylbutanoic acid, and stearic acid. , prismatic acid, 2-acryloyloxyethylhexahydrophthalic acid, 2-methacryloyloxyethylhexahydrophthalic acid, acrylic acid, methacrylic acid, 2-acryloyloxyethylsuccinic acid, 2-methacryloyloxyethylsuccinic acid, semi-lipids obtained from (meth)acryloyloxyC1-6 alkyl alcohols of C3-9 aliphatic dicarboxylic acids such as succinic acid; semi-lipids obtained from (meth)acryloyloxyC1-6 alkyl alcohols of C8-14 aromatic dicarboxylic acids such as 2-acryloyloxyethylphthalic acid and 2-methacryloyloxyethylphthalic acid. The above organic acids may be used alone or in combination of two or more.
[0223] As the coupling agent, there can be mentioned compounds having an organic group capable of forming a bond with the inorganic particles and a reactive functional group capable of being lipophilized. As the reactive functional group, for example, there can be mentioned: (meth)acryloyloxy, epoxy, amino, vinyl, sulfhydryl, anhydride, phenol, etc. By using the compound having the reactive functional group to carry out surface treatment, the inorganic particles can have reactive functional groups such as (meth)acryloyloxy, epoxy, amino, vinyl, sulfhydryl, anhydride, phenol, etc. from the coupling agent on the surface. The coupling agent can be used only one, or two or more.
[0224] Examples of the coupling agent include a silane coupling agent, a titanate coupling agent, and an aluminate coupling agent.
[0225] Examples of the silane coupling agent include (meth)acryloxy silane coupling agents such as 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane; diethoxy(glycidoxypropyl)methylsilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 3-(meth)acryloxypropyltriethoxysilane; and Epoxy silane coupling agents such as 2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane.
[0226] Examples of the titanate coupling agent include isopropyl triisostearoyl titanate, isopropyl dimethacryloyl isostearyl titanate, isopropyl tri(dodecyl)benzenesulfonyl titanate, neopentyl(diallyl)oxy-tri(dioctyl)phosphate titanate, and neopentyl(diallyl)oxy-trineodecanoyl titanate.
[0227] Examples of the aluminate coupling agent include acetoalkoxyaluminum diisopropoxide and the like.
[0228] Examples of the surfactant include ionic surfactants such as anionic surfactants, cationic surfactants, and zwitterionic surfactants, and nonionic surfactants. The surfactants may be used alone or in combination of two or more.
[0229] Examples of the anionic surfactant include fatty acid surfactants such as sodium oleate, sodium stearate, sodium laurate, fatty acid sodium sulfonates, and potassium fatty acids; phosphoric acid surfactants such as alkyl phosphoric acids, alkyl phosphate esters, and sodium alkyl phosphate esters; olefin surfactants such as sodium α-olefin sulfonate; alcohol surfactants such as sodium alkyl sulfate; alkylbenzene surfactants, and the like.
[0230] Examples of the cationic surfactant include alkyl methyl ammonium chloride, alkyl dimethyl ammonium chloride, alkyl trimethyl ammonium chloride, and alkyl dimethyl benzyl ammonium chloride.
[0231] Examples of the zwitterionic surfactant include carboxylic acid-based surfactants such as alkylaminocarboxylates and phosphate-based surfactants such as phosphobetaine.
[0232] Examples of the nonionic surfactant include fatty acid surfactants such as polyoxyethylene lanolin fatty acid esters and polyoxyethylene sorbitan fatty acid esters; polyoxyethylene alkylphenyl ethers; fatty acid alkanolamides; phosphoric acid surfactants such as organic phosphates, alkyl phosphates, phosphoric acid polyesters, and polyoxyalkylene alkyl ether phosphates.
[0233] The mixing of the inorganic particles and the surface modifier can be carried out in a solvent. When the inorganic particles and the surface modifier are mixed in a solvent, the inorganic particles in a mixed powder form can be added to the dispersion of the surface modifier, the mixed surface modifier can be added to the dispersion (slurry) of the inorganic particles, or they can be mixed after preparing the respective dispersions.
[0234] For example, in the case of preparing a dispersion of zirconium oxide (ZrO2) particles, the amount of the dispersion medium used is preferably an amount that can fully disperse the zirconium oxide particles. Relative to 100 parts by mass of zirconium oxide particles, the total amount of the dispersion medium is preferably 20 parts by mass or more, more preferably 40 parts by mass or more, and further preferably 60 parts by mass or more, and is preferably 600 parts by mass or less, more preferably 550 parts by mass or less, and further preferably 500 parts by mass or less.
[0235] The solvent used in the above dispersion is also included. The solvent (dispersion medium) used in the above mixing is not particularly limited, and examples thereof include: water; alcohols such as methanol, ethanol, propanol, 2-propanol (IPA), butanol, diacetone alcohol, furfuryl alcohol, and tetrahydrofurfuryl alcohol; methyl acetate, ethyl acetate, isopropyl acetate, propyl acetate, isobutyl acetate, butyl acetate, isopentyl acetate, amyl acetate, 3-methoxybutyl acetate, and 2-ethylbutyl acetate. Esters such as ethylene glycol, cyclohexyl acetate, and ethylene glycol monoacetate; glycols such as ethylene glycol and hexylene glycol; ethers such as diethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, ethylene glycol isopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, propylene glycol monomethyl ether, and propylene glycol monoethyl ether; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, methyl butyl ketone, cyclohexanone, methylcyclohexanone, diacetone, methyl amyl ketone, and diisobutyl ketone; toluene, etc. These may be used alone or in combination of two or more.
[0236] The mixing ratio of the inorganic particles and the surface modifier is not particularly limited and can be appropriately set according to a known method. For example, when a (silane) coupling agent is used as the surface modifier, the amount of the (silane) coupling agent is preferably 0.01 to 100 parts by mass, more preferably 1 to 70 parts by mass, and further preferably 1 to 40 parts by mass relative to 100 parts by mass of the inorganic particles.
[0237] The temperature at which the inorganic fine particles and the surface modifier are mixed in a solvent can be appropriately selected according to a known method. After mixing, the inorganic fine particles and the surface modifier can be reacted by heating or the like as needed.
[0238] The coated inorganic fine particles can also be obtained by a method of hydrothermal reaction in the presence of water. Examples of the method of hydrothermal reaction in the presence of water include a method of heating a compound that generates the coated inorganic fine particles by hydrothermal reaction in the presence of water.
[0239] Examples of the compound that generates coated inorganic fine particles by hydrothermal reaction include various coated inorganic fine particle precursors, such as various metal hydroxides, chlorides, oxychlorides, sulfates, acetates, organic acid salts, alkoxides, etc., and salts of various metals and carboxylic acids.
[0240] As specific examples of the compounds that generate coated inorganic fine particles by hydrothermal reaction, for example, in the example of compounds containing zirconium, zirconium hydroxide, zirconium chloride, zirconium oxychloride, zirconium oxyacetate, zirconium oxynitrate, zirconium sulfate, zirconium octanoate, zirconium 2-ethylhexanoate, zirconium oxide oleate, zirconium acetate, zirconium oxide stearate, zirconium oxide laurate, zirconium tetrabutoxy, and other zirconium alkoxides can be cited. In addition, in the example of compounds containing titanium, titanium hydroxide, titanium chloride, titanium oxychloride, titanium oxyacetate, titanium oxynitrate, titanium sulfate, titanium octanoate, titanium oxide oleate, titanium acetate, titanium oxide stearate, titanium oxide laurate, titanium oxide tetrabutoxy (e.g., tetra-n-butoxytitanium) and other titanium alkoxides can be cited. For example, in the case of subjecting zirconium 2-ethylhexanoate to hydrothermal reaction, zirconium oxide coated with 2-ethylhexanoic acid and / or carboxylic acid derived from 2-ethylhexanoic acid can be obtained.
[0241] The reaction conditions in the hydrothermal reaction, such as the amount of water used, the reaction temperature, and the reaction time, are not particularly limited and can be appropriately selected according to a known method.
[0242] The coated inorganic fine particles obtained by the hydrothermal reaction may be further treated with the surface modifier (organic acid, coupling agent, surfactant) as described above. The method of treating with the surface modifier may be the same as the method of modifying the surface of the inorganic fine particles with the surface modifier.
[0243] The coated inorganic particles have affinity with organic solvents because the surface is modified by reactive functional groups. Therefore, even in the above-mentioned various organic solvents, the state of stable dispersion in the form of nanoparticles is reached. Specifically, the solution state with high transparency can be processed. The coated inorganic particles can be used usually in the state of the dispersion liquid of inorganic particles dispersed in the surface modification liquid for surface modification, or can be used by vacuum distillation to remove the powder after the solvent by distillation.
[0244] In the coated inorganic fine particles, the modification amount of the surface modifier is preferably 0 to 50 parts by mass, more preferably 1 to 40 parts by mass, and further preferably 2 to 30 parts by mass relative to 100 parts by mass of the inorganic fine particles. When the modification amount of the surface modifier is within the above range, the refractive index of the alkali-soluble resin composition of the present invention can be made higher, and the hardness, relative dielectric constant, etc. can also be improved.
[0245] As the shape of the above-mentioned inorganic particles (including coated inorganic particles; the same below), spherical, ellipsoidal, cubic, rectangular, pyramidal, needle-shaped, columnar, rod-shaped, cylindrical, flaky, plate-shaped, thin sheet, etc. When considering the dispersibility in the solvent, spherical, columnar, etc. are preferred as the above-mentioned shapes.
[0246] The crystallite diameter of the inorganic particles is preferably 20 nm or less. When the crystallite diameter of the inorganic particles is within the above range, the transparency of the curable resin composition containing the inorganic particles can be improved. The crystallite diameter is more preferably 15 nm or less, and further preferably 10 nm or less. The lower limit of the crystallite diameter is usually about 1 nm. That is, the crystallite diameter is preferably 1 to 20 nm, more preferably 1 to 15 nm, and further preferably 1 to 10 nm. The crystallite diameter can be calculated by X-ray diffraction analysis.
[0247] The number average primary particle size of the above-mentioned inorganic fine particles is preferably less than 30nm, and more preferably less than 25nm. When the number average primary particle size of the above-mentioned inorganic fine particles is within the above-mentioned range, the transparency of the resin composition containing the above-mentioned inorganic fine particles can be improved. The above-mentioned number average primary particle size is more preferably less than 20nm, and further preferably less than 15nm. The lower limit of the above-mentioned number average primary particle size is preferably greater than 1nm, more preferably greater than 3nm, and further preferably greater than 5nm. That is, the above-mentioned number average primary particle size is preferably greater than 1nm and less than 30nm, more preferably 3 to 25nm, and further preferably 5 to 20nm. It is further preferably 5 to 15nm.
[0248] The above-mentioned number average primary particle size can be determined as follows: the inorganic fine particles are magnified and observed using a transmission electron microscope (TEM), a field emission transmission electron microscope (FE-TEM), a field emission scanning electron microscope (FE-SEM), etc., 100 particles are randomly selected, the length of their major axis direction is measured, and the arithmetic average is calculated.
[0249] The refractive index of the inorganic fine particles is not particularly limited, but is preferably 1.70 to 2.70, more preferably 1.90 to 2.70, from the viewpoint of obtaining a high refractive index. The refractive index is a refractive index with respect to NaD line (589 nm), and can be determined by the method described in the Examples below.
[0250] The specific surface area of the inorganic fine particles is preferably 10 to 400 m 2 / g, more preferably 20 to 200 m 2 / g, and most preferably 30 to 150 m 2 / g.
[0251] The content of the inorganic fine particles is preferably 0 to 95% by mass, more preferably 5 to 90% by mass, further preferably 10 to 80% by mass, and further preferably 20 to 70% by mass, based on 100% by mass of the total solid content of the alkali-soluble resin composition.
[0252] The alkali-soluble resin composition can also be produced by mixing the alkali-soluble resin and the acid group-containing epoxy (meth) acrylate using a known method, but the composition containing the alkali-soluble resin and the acid group-containing epoxy (meth) acrylate can be effectively produced by the following production method. A preferred production method of the alkali-soluble resin composition is described below.
[0253] 4. Method for producing alkali-soluble resin composition
[0254] A preferred method for producing the alkali-soluble resin composition comprises: a step (b-1) of reacting a difunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90° C. or more obtained based on JIS K 0071-2 with a bisphenol compound; a step (b-2) of adding an epoxy resin to the reaction product obtained in the step (b-1); a step (b-3) of reacting the mixture obtained in the step (b-2) with an unsaturated monobasic acid; and a step (b-4) of reacting the reaction mixture obtained in the step (b-3) with a polyacid anhydride.
[0255] Process (b-1)
[0256] Examples of the step (b-1) include the same steps as those in the step (a-1) in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0257] Process (b-2)
[0258] Step (b-2) is a step of adding an epoxy resin to the reaction product obtained in step (b-1). By adding the epoxy resin, the properties derived from the epoxy resin skeleton can be imparted to the obtained cured product of the alkali-soluble resin composition.
[0259] As the epoxy resin, preferably, there can be mentioned the epoxy resins listed as the starting materials of the acid group-containing epoxy (meth)acrylate.
[0260] The above epoxy resins may be used alone or in combination of two or more.
[0261] The amount of the epoxy resin added is preferably 1 to 1000 parts by mass, more preferably 100 to 500 parts by mass, and even more preferably 200 to 300 parts by mass, based on 100 parts by mass of the bifunctional epoxy compound used in the step (b-1).
[0262] Process (b-3)
[0263] Step (b-3) is a step of reacting the mixture obtained in the above step (b-2) with an unsaturated monobasic acid. In this reaction, the unsaturated monobasic acid reacts with the epoxy group of the reaction product obtained in the above step (b-1) and the epoxy group of the above epoxy resin in the above mixture, and introduces a free radical polymerizable unsaturated bond into the above reaction product and the epoxy resin. Therefore, by the reaction of step (b-3), a mixture of a compound having a free radical polymerizable unsaturated bond introduced into the reaction product obtained in the above step (b-1) and a compound having a free radical polymerizable unsaturated bond introduced into the above epoxy resin can be obtained.
[0264] Examples of the unsaturated monobasic acid include the unsaturated monobasic acids described in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0265] The unsaturated monobasic acid in the step (b-3) is preferably reacted in an amount of 0.6 to 1.4 moles of acid groups in the unsaturated monobasic acid relative to 1 mole of epoxy groups in the mixture obtained in the step (b-2), more preferably 0.7 to 1.3 moles, further preferably 0.8 to 1.2 moles, and most preferably 1.0 to 1.1 moles. If epoxy groups remain, storage stability may be deteriorated.
[0266] Regarding the above-mentioned unsaturated monobasic acid, in order to reduce the acid concentration in the reaction system, it is preferred to add the unsaturated monobasic acid in multiple batches or in small amounts in succession rather than adding the total amount at once. When the acid concentration in the reaction system becomes high, there is a possibility that the acid and the hydroxyl group by-produced by the reaction of the epoxy group may undergo a dehydration condensation reaction, or the acid may undergo thermal polymerization.
[0267] In the reaction of the above step (b-3), it is preferred to use a catalyst.
[0268] Examples of the catalyst include the catalysts described in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0269] In the reaction of the above step (b-3), the catalyst may be added in the total amount of the catalyst at one time or in batches, preferably in batches. By adding in batches, the deactivated portion of the catalyst can be compensated and the decrease in catalyst activity can be suppressed. If a large amount of phosphine or the like is used in the early stage in anticipation of the deactivated portion, the oxide of the phosphine will be yellow, and the coloring of the obtained resin may increase.
[0270] Examples of the method for the batch addition include the same method as described in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0271] In the reaction of the step (b-3), a polymerization inhibitor may be used.
[0272] Examples of the polymerization inhibitor include the polymerization inhibitors described in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0273] The reaction conditions of the step (b-3) are not particularly limited, but preferably, the same conditions as those for the reaction with the unsaturated monobasic acid in the step (a-2) of the above-mentioned "2. Method for producing an alkali-soluble resin" can be used.
[0274] Process (b-4)
[0275] Step (b-4) is a step of reacting the reaction mixture obtained in step (b-3) with a polybasic acid anhydride. In step (b-4), a polybasic acid anhydride is added to the hydroxyl groups of the reaction mixture obtained in step (b-3) to introduce carboxyl groups.
[0276] Examples of the polybasic acid anhydride include the polybasic acid anhydrides described in the above-mentioned "2. Method for producing an alkali-soluble resin".
[0277] The polyacid anhydride in the above step (b-4) is preferably fed to react in an amount of 0.1 to 1.1 mol, more preferably 0.15 to 1 mol, further preferably 0.2 to 0.9 mol, and most preferably 0.4 to 0.6 mol, relative to 1 mol of hydroxyl groups in the reaction mixture obtained in the above step (b-3).
[0278] The reaction conditions of the step (b-4) are not particularly limited, but preferably, the same conditions as those for the reaction with the polybasic acid anhydride in the step (a-3) of the above-mentioned "2. Method for producing an alkali-soluble resin" can be used.
[0279] The method for producing the alkali-soluble resin composition may include other steps in addition to the reaction step. Examples of the other steps include an aging step, a neutralization step, a dilution step, a drying step, a concentration step, and a purification step. These steps may be performed by known methods.
[0280] The alkali-soluble resin composition obtained by the above production method has an ammonium salt compound content of 0.06 mass % or less relative to 100 mass % of the alkali-soluble resin represented by the above formula (1). The ammonium salt compound content is within the above range, so a cured product having excellent heat coloration resistance can be provided.
[0281] In the alkali-soluble resin composition, the content of the ammonium salt compound is more preferably 0.03% by mass or less, further preferably 0.01% by mass or less, and most preferably 0% by mass, relative to 100% by mass of the alkali-soluble resin.
[0282] In addition, the following method for producing an alkali-soluble resin composition is also one of the present invention, and the method for producing an alkali-soluble resin composition comprises: a step (b-1) of reacting a difunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90° C. or more obtained based on JIS K 0071-2 with a bisphenol compound; a step (b-2) of adding an epoxy resin to the reaction product obtained in the above step (b-1); a step (b-3) of reacting the mixture obtained in the above step (b-2) with an unsaturated monobasic acid; and a step (b-4) of reacting the reaction mixture obtained in the above step (b-3) with a polyacid anhydride. In the alkali-soluble resin composition obtained by the above production method, the content of the ammonium salt compound is less than 0.06% by mass relative to 100% by mass of the alkali-soluble resin.
[0283] (Curing method)
[0284] There is no particular limitation on the method for curing the alkali-soluble resin or alkali-soluble resin composition of the present invention to obtain a cured product, and a known method may be used. For example, the following method can be cited: the alkali-soluble resin composition is applied or molded onto a substrate, and cured by heating or irradiation with active energy rays such as ultraviolet rays, or a combination thereof to obtain a cured product.
[0285] As a method for curing the above-mentioned alkali-soluble resin composition, for example, the following method can be preferably cited, which method includes: a step (1) of applying the above-mentioned alkali-soluble resin composition on a substrate to form a coating film; a step (2) of irradiating the formed coating film with light; a step (3) of developing and removing the unirradiated portion; and a step (4) of heating the coating film after light irradiation.
[0286] The substrate is not particularly limited and may be appropriately selected depending on the purpose and application. Examples thereof include substrates made of various materials such as a glass plate and a plastic plate.
[0287] In the step (1), the method for forming a coating film by applying the alkali-soluble resin composition is not particularly limited, and the coating can be carried out by a known method such as spin coating, slit coating, roll coating, and cast coating.
[0288] In the above-mentioned curing method, it is preferred that after the above-mentioned alkali-soluble resin composition is applied to the substrate, the coating is dried to form a coating film. The above-mentioned drying can be carried out by a known method, for example, a hot plate, an IR oven, a convection oven, etc. can be used. The drying conditions are appropriately selected according to the boiling point of the solvent component included, the type of curing component, the film thickness, the performance of the dryer, etc., and are usually preferably carried out at a temperature of 50 to 160° C. for 10 seconds to 300 seconds.
[0289] In the above step (2), there is no particular limitation on the method for irradiating the formed coating film with light, and the method can be carried out by a known method. As the light source of the active light used for the light irradiation, for example, there can be mentioned: a xenon lamp, a halogen lamp, a tungsten lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a metal halide lamp, a medium-pressure mercury lamp, a low-pressure mercury lamp, a carbon arc lamp, a fluorescent lamp and other lamp light sources, an argon ion laser, a YAG laser, an excimer laser, a nitrogen laser, a helium-cadmium laser, a semiconductor laser and the like laser sources, and the like.
[0290] When the coating film is irradiated with light, the light irradiation may be performed through a photomask. As the photomask, a mask having a light shielding portion formed according to a target pattern may be used.
[0291] In the above step (3), after the above light irradiation step, a developing treatment is performed with a developer to remove the unirradiated portion. The irradiated portion is cured by light irradiation, and the cured product is insoluble or difficult to dissolve in the developer. On the other hand, the unirradiated portion is dissolved in the developer and is therefore removed by the developing treatment, thereby obtaining a patterned cured film. The developing treatment can usually be performed at a developing temperature of 10 to 50° C. by immersion developing, spray developing, brush developing, ultrasonic developing, or the like.
[0292] The developer used in the above step (3) is not particularly limited as long as it is a developer that dissolves the above alkali-soluble resin composition. An organic solvent or an alkaline aqueous solution is generally used, and a mixture thereof may also be used. It should be noted that when an alkaline aqueous solution is used as a developer, it is preferably washed with water after development. As an organic solvent or an alkaline aqueous solution, for example, the same substances as those described in Japanese Patent Publication No. 2015-157909 can be cited.
[0293] In the above step (4), the coating film after the development treatment is heated at 260° C. or less. In the heating step (post-curing step) after the light irradiation in the above step (4), the heating temperature is preferably 260° C. or less, and more preferably 200° C. or less. The lower limit of the heating temperature is preferably 70° C. or more, and more preferably 90° C. or more, from the perspective of maintaining curability.
[0294] The heating time in the heating step is not particularly limited, and is preferably 5 to 60 minutes, for example. The heating method is also not particularly limited, and for example, a known heating device such as a hot plate, a convection oven, or a high-frequency heater may be used.
[0295] When the cured product obtained by the above curing method is a cured film, the film thickness is preferably 0.1 to 50 μm, more preferably 0.5 to 40 μm, and even more preferably 1 to 30 μm in order to fully exhibit the characteristics as a protective film.
[0296] The above cured film showed a good thermal coloration resistance. * The value is preferably 6.0 or less, and more preferably 5.5 or less. The heat coloration resistance test is an evaluation test of heat coloration resistance performed by the method described in the examples described later.
[0297] 5. Purpose
[0298] The alkali-soluble resin and alkali-soluble resin composition of the present invention can provide a cured product with excellent heat-resistant coloration and a high refractive index, and therefore can be appropriately used for applications requiring heat-resistant coloration and a high refractive index. In addition, the alkali-soluble resin and alkali-soluble resin composition of the present invention can also be appropriately used for applications requiring a fast developing speed and developing properties. In addition, the voltage holding ratio of the alkali-soluble resin and alkali-soluble resin composition of the present invention is also good, and therefore can also be appropriately used for applications requiring a voltage holding ratio.
[0299] The alkali-soluble resin and alkali-soluble resin composition of the present invention can be widely used, for example, in magnetic recording materials, catalyst materials, ultraviolet absorbing materials, dental materials, contact lenses, intraocular lenses, high-refractive lenses for glasses, optical computer devices, optical storage media, anti-reflection films, conformal coatings, microlens arrays, automotive top coatings, coatings, coating agents, hair cosmetics, gradient refractive index optical components and dynamic gradient refractive index components, nanoimprint materials, photocurable plastics, polymerizable compounds for holographic recording, surface coating materials for glass, transparent coating materials for solar cells, plastic lenses, printing plates, semiconductor light-emitting elements (light-emitting diodes, organic light-emitting diodes), etc. tube, laser diode), light guide (geometric shape of both plane and "fiber"), semiconductor element, light diffusion component, prism sheet, hard coating material, optical wiring component, diffraction grating, LED and other packaging materials, pressure-sensitive adhesive, protective film for the surface of glass, film and sheet used in sensor elements such as CCD / CMOS, display elements such as display screens, photocurable resin (OCR) for laminating image display components such as liquid crystals and plastic cover plates, reflection protective film for transparent electrodes, refractive index matching layer for preventing the see-through of ITO electrodes of touch panels, anti-adhesion layer, anti-reflection film of display screens, interlayer insulation film for semiconductors, etc. Among them, the alkali-soluble resin and alkali-soluble resin composition of the present invention are suitable for microlens arrays and nanoimprint materials because the resin has flexibility.
[0300] Furthermore, the alkali-soluble resin and alkali-soluble resin composition of the present invention are particularly suitable as a curable resin or resin composition for an optical material, and can provide, for example, a cured film having excellent transparency, substrate adhesion, and electrical properties.
[0301] It should be noted that in the present invention, "optical material" refers to materials used in the components of devices in the optical field, motor / electronic field, etc., for example, it refers to color filters, light extraction layers, black matrices, photo spacers, black column spacers, photoresists, outer coatings, TFT flattening layers, TFT insulating films, and surface coatings of optical lenses used in liquid crystals, organic EL, quantum dots, small / micro LED display devices / solid-state imaging elements / touch panel display devices, etc. Materials used as materials. From the aspect of having alkali solubility, the resin of the present invention can also be appropriately used for the purpose of applying photolithography, and can form a cured film with high refraction, high hardness, high transparency, and high relative dielectric constant, so the resin composition of the present invention is most preferably a curable resin composition for color filters, light extraction layers, and color conversion layers for organic EL display devices. As the light source of the light extraction layer, various LEDs, small / micro LEDs, and quantum dots can be cited, and from the aspect of being flexible, organic EL is preferred. Specific examples of the light extraction layer for organic EL include the structure described in Japanese Patent Application Laid-Open No. 2021-34545. As a high-refractive member that can be photolithographically processed and has high transparency, the alkali-soluble resin and alkali-soluble resin composition of the present invention can be suitably used.
[0302] Example
[0303] The present invention will be described in more detail below with reference to Examples, but the present invention is not limited to these Examples. It should be noted that, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass".
[0304] Various evaluation methods used in this example are as follows.
[0305] <Acid value>
[0306] 0.5 g of the resin solution was accurately weighed and dissolved in a mixed solvent of 90 g of acetone and 10 g of water, and titrated using a 0.1 N aqueous KOH solution as a titrant. The titration was performed using an automatic titrator (trade name: COM-555, manufactured by Hiranuma Sangyo Co., Ltd.), and the acid value (mgKOH / g) per 1 g of the solid content was determined based on the acid value of the resin solution and the solid content of the resin solution.
[0307] It should be noted that the solid content of the resin solution is determined by the following method. That is, about 1 g of the resin solution is weighed in an aluminum cup, about 1 g of acetone is added to dissolve it, and then it is naturally dried at room temperature. Then, a hot air dryer (trade name: PHH-101, manufactured by Espec) is used to dry it at 160°C for 1.5 hours, and then it is naturally cooled in the dryer and the mass is measured. The solid content (mass %) of the resin solution is calculated based on the mass loss.
[0308] <Double bond equivalent (g / equivalent)>
[0309] The double bond amount is determined by dividing the mass (g) of the solid content of the resin solution by the double bond amount (mol) of the resin. The double bond amount is determined by dividing the mass of the compound having a polymerizable double bond used to introduce the polymerizable double bond by the molecular weight.
[0310] <Heat coloration resistance>
[0311] The obtained resin solution was evenly coated on a 5 cm square glass substrate (soda lime glass AS-2K, manufactured by Toshin Riko Co., Ltd.) using a spin coater (manufactured by MIKASA, 1H-D7). The coated plate was dried at 90°C for 3 minutes to obtain a laminate having a coating film formed on the glass substrate. After removing the resin attached to the end of the glass substrate, the obtained laminate was heated at 230°C for 30 minutes using a perfect oven thermostat (manufactured by Espec), cooled to room temperature, and a laminate with a film thickness of 15 μm was obtained. The coating surface of the obtained laminate was measured using a colorimeter ZE6000 (manufactured by Nippon Denshoku Industries Co., Ltd.) to obtain b after the heating test. * value.
[0312] <Refractive Index>
[0313] The obtained resin solution was evenly coated on a glass substrate (Matsunami glass slide S9111, manufactured by Matsunami Glass Industries) using a spin coater (manufactured by MIKASA, 1H-D7). The coated plate was dried at 90°C for 3 minutes to obtain a laminate having a coating formed on the glass substrate. After removing the resin attached to the end of the glass substrate, the obtained laminate was heated at 230°C for 30 minutes using a perfect oven thermostat (manufactured by Espec), cooled to room temperature, and a laminate having a film thickness of 0.5 μm was obtained. The refractive index of the obtained laminate was obtained by measuring the reflection spectrum. Specifically, the reflectivity was measured by the following method: a film coated on a substrate such as a slide was used as a sample to be measured, and the following device was used to simulate the reflectivity of the thin film according to the Fresnel formula based on the measured reflectivity based on thin film interference, thereby calculating the refractive index value at 589 nm.
[0314] Device: Film thickness measurement system F-20 manufactured by Filmetrics
[0315] Standard fiber stage SS-1 (spot diameter 1.5mm)
[0316] <Quantitative Quantification of Epoxy Groups>
[0317] The measurement was performed according to the method of JIS K7236: 2001. That is, 0.5 g of the resin solution was accurately weighed in a beaker, 25 ml of chloroform, 75 ml of acetic acid, and 2 g of tetraethylammonium bromide were added and stirred to dissolve, and titrated using a 0.1 N perchloric acid-acetic acid standard solution using an automatic titrator (trade name: COM-555, manufactured by Hiranuma Sangyo Co., Ltd.), and the mass of the resin solution containing 1 equivalent of epoxy group was calculated.
[0318] <Developability Test>
[0319] The resin solution was applied on a 10 cm square glass substrate by spin coating, and after heat treatment (90°C, 3 minutes), the solution was irradiated at 60 mJ / cm at a distance of 50 μm from the coating film through a photomask having an opening with a line width and spacing of 30 μm, and a UV aligner (manufactured by Dainippon Scientific Co., Ltd., trade name "MA-1100") equipped with a 2.0 kW ultrahigh pressure mercury lamp was used. 2 The film was exposed at an exposure amount of 100 nm (365 nm illumination conversion), and a 0.05% potassium hydroxide aqueous solution was spread using a rotary developer to dissolve and remove the unexposed portion. The remaining exposed portion was developed by washing with pure water for 10 seconds, thereby evaluating the developability.
[0320] Specifically, the coating film developed through the photomask as described above was observed using a surface roughness meter (manufactured by Ryoka Systems, trade name "VertScan 2.0"), and the time required to spray the 0.05% potassium hydroxide aqueous solution to wash away the unexposed portion was defined as the development time. The presence of residue during the development time was also observed.
[0321] <Bending resistance evaluation>
[0322] The resin solution was applied to a copper plate with a thickness of 0.5 mm at a thickness of 20 to 30 μm, dried in a hot air circulation drying oven at 80° C. for 30 minutes, and then cooled to room temperature to obtain a coating film. 2 The cured product was irradiated with light to obtain a cured product. The cured product was heated at 150°C for 1 hour to serve as a test substrate. The test substrate was used to evaluate the bending resistance of the cured coating film when the mandrel diameter was Φ10 mm by the cylindrical mandrel method.
[0323] <Measurement of Mass Reduction Rate>
[0324] The coated zirconium oxide particles were heated from room temperature to 800°C at 10°C / min in an air atmosphere using a TG-DTA (thermogravimetric-differential thermal analysis) apparatus, and the mass reduction rate of the particles was measured. The mass reduction rate can be used to determine the ratio of the carboxylate compound and the ratio of the metal oxide in the coated metal oxide particles.
[0325] (Synthesis Example 1) Synthesis of Resin Solution (A-1)
[0326] 188 parts of 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6, epoxy equivalent 188 g / equivalent, Gardner color 6), 62.6 parts of bisphenol S, 244.3 parts of propylene glycol monomethyl ether acetate, and 0.3 parts of triphenylphosphine as a reaction catalyst were added to a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction tube, and reacted at 140°C for 6 hours. The reaction of the phenolic hydroxyl group and the epoxy group was confirmed to be completed by quantitative analysis of the epoxy group. Then, 43.5 parts of methacrylic acid, 0.9 parts of triphenylphosphine as an esterification catalyst, and 0.4 parts of hydroquinone as a polymerization inhibitor were added, and reacted at 120°C for 20 hours. The acid value of the reaction product was confirmed to be 1.9 mgKOH / g. Then, 88.1 parts of tetrahydrophthalic anhydride were added, and reacted at 110°C for 5 hours while stirring. As a result, a resin solution (A-1) containing 61% of an alkali-soluble resin in a propylene glycol monomethyl ether acetate solution was obtained. Table 1 shows the acid value and double bond equivalent of the obtained resin solution (A-1) in terms of solid content.
[0327] (Synthesis Example 2) Synthesis of Resin Solution (A-2)
[0328] 187 parts of 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6, epoxy equivalent 187 g / equivalent, Gardner color 10), 62.6 parts of bisphenol S, 243.5 parts of propylene glycol monomethyl ether acetate, and 0.3 parts of triphenylphosphine as a reaction catalyst were added to a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction tube, and reacted at 140°C for 6 hours. The reaction of the phenolic hydroxyl group and the epoxy group was confirmed to be completed by quantitative analysis of the epoxy group. Then, 43.5 parts of methacrylic acid, 0.9 parts of triphenylphosphine as an esterification catalyst, and 0.4 parts of hydroquinone as a polymerization inhibitor were added, and reacted at 120°C for 20 hours. The acid value of the reaction product was confirmed to be 1.8 mgKOH / g. Then, 87.8 parts of tetrahydrophthalic anhydride were added, and reacted at 110°C for 5 hours while stirring. As a result, a resin solution (A-2) containing 61% of an alkali-soluble resin in a propylene glycol monomethyl ether acetate solution was obtained. Table 1 shows the acid value and double bond equivalent of the obtained resin solution (A-2) in terms of solid content.
[0329] (Synthesis Example 3) Synthesis of Resin Solution (A-3)
[0330] Into a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 94 parts of the same 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6) as used in Synthesis Example 1, 31.3 parts of bisphenol S, 202.3 parts of propylene glycol monomethyl ether acetate, and 0.5 parts of triphenylphosphine as a reaction catalyst were added, and reacted at 140°C for 6 hours. The completion of the reaction of the phenolic hydroxyl group and the epoxy group was confirmed by quantitative analysis of the epoxy group. Then, 251.8 parts of bisphenol A type epoxy resin (trade name "jER834"; manufactured by Mitsubishi Chemical; epoxy equivalent 248 g / equivalent) and 202.3 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, the internal temperature was maintained at 110°C, 0.75 parts of triphenylphosphine as an esterification catalyst and 0.6 parts of methylhydroquinone as a polymerization inhibitor were added, and 110 parts of methacrylic acid were continuously added dropwise for 2 hours using a dropping pump. After the addition was completed, 0.75 parts of triphenylphosphine was added as an additional catalyst, and then the temperature was raised to 120°C and reacted for 15 hours. It was confirmed that the acid value of the reaction product was 2.1 mgKOH / g. Next, 145.9 parts of tetrahydrophthalic anhydride was added, and the reaction was carried out at 110°C for 5 hours to obtain a resin solution (A-3) containing 61% of a mixture of an alkali-soluble resin and a carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (A-3) calculated as the solid content are shown in Table 1.
[0331] (Synthesis Example 4) Synthesis of Resin Solution (A-4)
[0332] Into a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 93 parts of 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6, epoxy equivalent 186 g / equivalent, Gardner color 7), 31.3 parts of bisphenol S, 174.3 parts of propylene glycol monomethyl ether acetate, and 0.5 parts of triphenylphosphine as a reaction catalyst were added, and reacted at 140°C for 6 hours. The reaction of the phenolic hydroxyl group and the epoxy group was confirmed to be completed by quantitative analysis of the epoxy group. Then, 251.8 parts of the same bisphenol A type epoxy resin "jER834" as used in Synthesis Example 3 and 174.3 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, 110 parts of methacrylic acid, 1.5 parts of triphenylphosphine as an esterification catalyst, and 0.5 parts of hydroquinone as a polymerization inhibitor were added, and the mixture was reacted at 120°C for 20 hours. It was confirmed that the acid value of the reaction product was 2.2 mgKOH / g. Next, 59.1 parts of tetrahydrophthalic anhydride were added, and the mixture was reacted at 110°C for 5 hours to obtain a resin solution (A-4) containing 61% of a mixture of an alkali-soluble resin and a carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (A-4) in terms of solid content are shown in Table 1.
[0333] (Synthesis Example 5) Synthesis of Resin Solution (A-5)
[0334] Into a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas inlet pipe, 75.2 parts of the same 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6) as used in Synthesis Example 1, 25 parts of bisphenol S, 135.5 parts of propylene glycol monomethyl ether acetate, and 0.3 parts of triphenylphosphine as a reaction catalyst were added, and the mixture was reacted at 140°C for 6 hours. The reaction between the phenolic hydroxyl group and the epoxy group was confirmed to be complete by quantitative analysis of the epoxy group. Then, 131.4 parts of a cresol novolac type epoxy resin (trade name "EOCN-104S"; manufactured by Nippon Kayaku; epoxy equivalent 219 g / equivalent) and 135.5 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, 69.6 parts of methacrylic acid, 0.9 parts of triphenylphosphine as an esterification catalyst, and 0.4 parts of methylhydroquinone as a polymerization inhibitor were added, and the mixture was reacted at 120°C for 20 hours. It was confirmed that the acid value of the reaction product was 1.9 mgKOH / g. Next, 122.7 parts of tetrahydrophthalic anhydride were added, and the mixture was reacted at 110°C for 5 hours to obtain a resin solution (A-5) containing 61% of a mixture of an alkali-soluble resin and a carboxyl-containing novolac-type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (A-5) in terms of solid content are shown in Table 1.
[0335] (Synthesis Example 6) Synthesis of Resin Solution (A-6)
[0336] Into a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 94 parts of the same 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6) as used in Synthesis Example 1, 31.3 parts of bisphenol S, 202.3 parts of propylene glycol monomethyl ether acetate, and 0.5 parts of triphenylphosphine as a reaction catalyst were added, and reacted at 140°C for 6 hours. The completion of the reaction of the phenolic hydroxyl group and the epoxy group was confirmed by quantitative analysis of the epoxy group. Then, 251.8 parts of bisphenol A type epoxy resin (trade name "jER834"; manufactured by Mitsubishi Chemical; epoxy equivalent 248 g / equivalent) and 202.3 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, the internal temperature was maintained at 110°C, 0.75 parts of triphenylphosphine as an esterification catalyst and 0.6 parts of hydroquinone as a polymerization inhibitor were added, and 110 parts of methacrylic acid were continuously added dropwise for 2 hours using a dropping pump. After the addition was completed, 0.75 parts of triphenylphosphine was added as an additional catalyst, and then the temperature was raised to 120°C and reacted for 15 hours. It was confirmed that the acid value of the reaction product was 2.1 mgKOH / g. Next, 145.9 parts of tetrahydrophthalic anhydride was added, and the reaction was carried out at 110°C for 5 hours to obtain a resin solution (A-6) containing 61% of a mixture of an alkali-soluble resin and a carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (A-6) calculated as the solid content are shown in Table 1.
[0337] (Synthesis Example 7) Synthesis of Resin Solution (A-7)
[0338] In a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 248 parts of the same bisphenol A type epoxy resin "jER834" as used in Synthesis Example 3, 87 parts of methacrylic acid, 278.3 parts of propylene glycol monomethyl ether acetate, 1 part of triphenylphosphine as an esterification catalyst, and 0.4 parts of hydroquinone as a polymerization inhibitor were added, and the mixture was reacted at 120°C for 20 hours. It was confirmed that the acid value of the reaction product was 1.8 mgKOH / g. Then, 100.3 parts of tetrahydrophthalic anhydride was added, and the mixture was reacted at 110°C for 5 hours to obtain a resin solution (A-7) containing 61% of carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (A-7) in terms of solid content are shown in Table 1.
[0339] (Synthesis Example 8) Synthesis of Resin Solution (B-1)
[0340] Into a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction tube, 94 parts of the same 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6) used in Synthesis Example 1, 31.3 parts of bisphenol S, 202.3 parts of propylene glycol monomethyl ether acetate, and 0.5 parts of benzyltriethylammonium chloride as a reaction catalyst were added, and reacted at 140°C for 6 hours. The completion of the reaction of the phenolic hydroxyl group and the epoxy group was confirmed by quantitative analysis of the epoxy group, and then 251.8 parts of the same bisphenol A type epoxy resin "jER834" used in Synthesis Example 3 and 202.3 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, 110 parts of methacrylic acid, 1.5 parts of triphenylphosphine as an esterification catalyst, and 0.6 parts of methylhydroquinone as a polymerization inhibitor were added, and the mixture was reacted at 120°C for 20 hours. It was confirmed that the acid value of the reaction product was 2.5 mgKOH / g. Next, 145.9 parts of tetrahydrophthalic anhydride were added, and the mixture was reacted at 110°C for 5 hours to obtain a resin solution (B-1) containing 61% of a mixture of a comparative alkali-soluble resin and a carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (B-1) calculated as the solid content are shown in Table 1.
[0341] (Synthesis Example 9) Synthesis of Resin Solution (B-2)
[0342] In a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 113 parts of the same bisphenol A type epoxy resin "jER834" as used in Synthesis Example 3, 63.2 parts of a different bisphenol A type epoxy resin (trade name "YD-901"; manufactured by Nippon Steel Chemicals; epoxy equivalent 464 g / equivalent), 51.5 parts of methacrylic acid, 189.1 parts of propylene glycol monomethyl ether acetate, 0.7 parts of triphenylphosphine as an esterification catalyst, and 0.3 parts of hydroquinone as a polymerization inhibitor were charged, and reacted at 120° C. for 20 hours. It was confirmed that the acid value of the reaction product was 2.0 mgKOH / g. Then, 68.2 parts of tetrahydrophthalic anhydride was added, and reacted at 110° C. for 5 hours to obtain a resin solution (B-2) containing 61% of carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. Table 1 shows the acid value and double bond equivalent of the obtained resin solution (B-2) in terms of solid content.
[0343] (Synthesis Example 10) Synthesis of Resin Solution (B-3)
[0344] In a container equipped with a stirring device, a thermometer, a reflux cooler, and a gas introduction pipe, 94 parts of 3,3',5,5'-tetramethyl-4,4'-bis(glycidoxy)-1,1'-biphenyl (cas.85954-11-6, epoxy equivalent 188 g / equivalent, Gardner color 13), 31.3 parts of bisphenol S, 202.3 parts of propylene glycol monomethyl ether acetate, and 0.5 parts of triphenylphosphine as a reaction catalyst were added, and reacted at 140°C for 6 hours. The completion of the reaction of the phenolic hydroxyl group and the epoxy group was confirmed by quantitative analysis of the epoxy group, and then 251.8 parts of bisphenol A type epoxy resin (trade name "jER834"; manufactured by Mitsubishi Chemical; epoxy equivalent 248 g / equivalent) and 202.3 parts of propylene glycol monomethyl ether acetate were added and dissolved to prepare a uniform solution. Next, 110 parts of methacrylic acid, 1.5 parts of triphenylphosphine as an esterification catalyst, and 0.6 parts of methylhydroquinone as a polymerization inhibitor were added, and the mixture was reacted at 120°C for 20 hours. It was confirmed that the acid value of the reaction product was 2.1 mgKOH / g. Next, 145.9 parts of tetrahydrophthalic anhydride were added, and the mixture was reacted at 110°C for 5 hours to obtain a resin solution (B-3) containing 61% of a mixture of an alkali-soluble resin and a carboxyl-containing bisphenol A type epoxy acrylate in a propylene glycol monomethyl ether acetate solution. The acid value and double bond equivalent of the obtained resin solution (B-3) in terms of solid content are shown in Table 1. Compared with the resin solution (A-3), the resin solution (B-3) has a brown color.
[0345] (Synthesis Example 11) Synthesis of Resin Solution (B-4)
[0346] Into a reaction vessel equipped with a thermometer, a stirrer, a gas introduction pipe, a cooling pipe, and a dripping tank inlet, 119.2 parts of propylene glycol monomethyl ether acetate and 50.7 parts of propylene glycol monomethyl ether were charged, the atmosphere was replaced with nitrogen, and the temperature was raised to 90°C.
[0347] On the other hand, a stirred mixture of 55.0 parts of benzyl methacrylate, 45.0 parts of methacrylic acid, and 1.0 part of tert-butyl peroxy(2-ethylhexanoate) was prepared in a dropping tank (A), and a stirred mixture of 2.8 parts of n-dodecyl mercaptan and 15.9 parts of propylene glycol monomethyl ether acetate was prepared in a dropping tank (B).
[0348] After the temperature of the reaction tank reaches 90°C, while maintaining the temperature, dripping is started from the dripping tank for 3 hours to carry out polymerization. After the dripping is completed, after maintaining at 90°C for 30 minutes, the temperature is raised to 115°C and matured for 90 minutes. 41.3 parts of glycidyl methacrylate, 0.4 parts of triethylamine, and 0.2 parts of ANTAGE W400 are added to the obtained base polymer solution, and the oxygen / nitrogen mixed gas with an oxygen concentration adjusted to 7% is bubbled at 20 ml / min, while the temperature is raised to 115°C and the reaction is carried out for 8 hours. Then, it is cooled to room temperature to obtain a resin solution (B-4) containing an alkali-soluble resin. The acid value and double bond equivalent of the obtained resin solution (B-4) converted to solid content are shown in Table 2.
[0349] <Preparation of Inorganic Fine Particles>
[0350] Production Example 1
[0351] (Manufacture of coated zirconium oxide nanoparticles (coated ZrO2 particles 1) coated with 2-ethylhexanoic acid and / or carboxylate derived from 2-ethylhexanoic acid)
[0352] Pure water (268 g) was mixed in a 2-ethylhexanoic acid zirconium mineral oil solution (782 g, 2-ethylhexanoic acid zirconium content 44% by mass, manufactured by Daiichi Rare Element Chemical Industry Co., Ltd.). The resulting mixed solution was put into an autoclave with a stirrer, and the atmosphere in the autoclave was replaced with nitrogen. Then, the mixed solution was heated to 180°C and kept at this temperature for 16 hours (the pressure in the autoclave was 0.94 MPa) to react and generate zirconium oxide particles. Next, the mixed solution after the reaction was taken out, the precipitate accumulated at the bottom was filtered out, washed with acetone, and then dried. The dried precipitate (100 g) was dispersed in toluene (800 mL), resulting in a turbid solution. Then, as a refining process, quantitative filter paper (manufactured by ADVANTEC Toyo Co., Ltd., No. 5C) was used to filter again to remove coarse particles in the precipitate. Furthermore, the filtrate was concentrated under reduced pressure to remove toluene, thereby recovering white zirconium oxide nanoparticles 1 (coated ZrO2 particles 1).
[0353] The crystal structure of the obtained coated ZrO2 particle 1 was confirmed by XRD diffraction pattern, and the diffraction lines belonging to tetragonal and monoclinic crystals were detected. According to the intensity of the diffraction lines, the ratio of tetragonal to monoclinic crystals was 54 / 46, and the particle size (crystal size) was 5nm.
[0354] The average particle size (number average primary particle size) of the coated ZrO2 particles 1 measured by an electron microscope (manufactured by JEOL Ltd., FE-TEM JEM-2100F, 600,000 times magnification) was 12 nm. In addition, the coated ZrO2 particles 1 obtained by infrared absorption spectroscopy analysis can confirm absorption from CH and absorption from COOH. It is believed that the absorption is caused by 2-ethylhexanoic acid and / or carboxylic acid esters from 2-ethylhexanoic acid coating the surface of the coated ZrO2 particles 1.
[0355] In addition, the mass reduction rate of the coated ZrO2 particle 1 measured according to the above <Determination of Mass Reduction Rate> is 12 mass %. Therefore, it can be seen that the 2-ethylhexanoic acid and / or the carboxylate derived from 2-ethylhexanoic acid coating the surface of the coated ZrO2 particle 1 is 12 mass % of the entire coated ZrO2 particle 1.
[0356] Production Example 2
[0357] (Manufacture of Zirconium Oxide Nanoparticles Coated with 2-Ethylhexanoic Acid and / or Carboxylate Ester Derived from 2-Ethylhexanoic Acid and 2-Acryloyloxyethyl Succinate (Coated ZrO2 Particles 2))
[0358] The coated ZrO2 particles 1 (10 g) obtained in the above-mentioned manufacturing example 1 and 2-acryloyloxyethyl succinate (1.5 g) are stirred and mixed in propylene glycol monomethyl ether acetate (12 g, hereinafter referred to as "PGMEA") until they are uniformly dispersed. Next, n-hexane (36 g) is added to agglomerate the dispersed particles, making the solution turbid, and the agglomerated particles are separated from the turbid solution using filter paper. Then, the separated agglomerated particles are added to n-hexane (36 g), stirred for 10 minutes, and then the agglomerated particles are separated using filter paper, and the obtained particles are vacuum dried at room temperature, thereby preparing zirconium oxide nanoparticles (coated ZrO2 particles 2) surface-treated with 2-ethylhexanoic acid and / or carboxylic acid esters from 2-ethylhexanoic acid and 2-acryloyloxyethyl succinate.
[0359] The obtained coated ZrO2 particles 2 were dispersed in deuterated chloroform to prepare a measurement sample. 1 H-NMR analysis revealed that the molar ratio of 2-ethylhexanoic acid and / or a carboxylate derived from 2-ethylhexanoic acid to 2-acryloyloxyethyl succinate was 24:76.
[0360] The mass reduction rate of the coated ZrO2 particles 2 measured according to the above <Measurement of Mass Reduction Rate> is 18 mass %. Therefore, it can be seen that the 2-ethylhexanoic acid and / or carboxylate derived from 2-ethylhexanoic acid and 2-acryloyloxyethyl succinate coated on the coated zirconia particles account for 18 mass % of the entire coated zirconia particles.
[0361] The coated ZrO2 particles 2 (7 g), methyl ethyl ketone (3 g), and DISPER BYK-111 (manufactured by BYK Chemie Japan, 0.14 g) were mixed and stirred uniformly to obtain a zirconium oxide particle dispersion. The number average primary particle size of the coated ZrO2 particles 2 measured by electron microscopy was 12 nm.
[0362] (Examples 1 to 8, Comparative Examples 1 to 4)
[0363] The resin solutions obtained in Synthesis Examples 1 to 11 or the alkali-soluble resin compositions prepared by mixing the resin solutions were evaluated for heat discoloration resistance and refractive index by the above method according to the formulations shown in Table 3. The results are shown in Table 3. The values shown in Table 3 are resin solid content.
[0364] (Examples 9-10, Comparative Example 5)
[0365] Propylene glycol monomethyl ether acetate (PGMEA) was mixed with the resin solution, mill base (MB), dipentaerythritol hexaacrylate (DPHA) and photopolymerization initiator (Irgacure 907, manufactured by BASF) in the proportions (solid content) shown in Table 4 so that the solid content of the composition was 20%, thereby preparing an alkali-soluble resin composition. The developability of the obtained alkali-soluble resin composition was evaluated by the above method. The results are shown in Table 4.
[0366] The millbase (MB) used was prepared by the following method.
[0367] (Preparation of paint paste)
[0368] 12.9 parts of propylene glycol monomethyl ether acetate, 0.4 parts of Disparlon DA-7301 as a dispersant, 2.25 parts of CI Pigment Green 58 as a colorant, and 1.5 parts of CI Pigment Yellow 138 were mixed and dispersed for 3 hours using a paint shaker to obtain a mill base (MB).
[0369] (Examples 11 to 13, Comparative Example 6)
[0370] Propylene glycol monomethyl ether acetate (PGMEA) was mixed with a resin solution, dipentaerythritol hexaacrylate (DPHA), and a photopolymerization initiator (Irgacure 907, manufactured by BASF) in a ratio (solid content) shown in Table 5 so that the solid content of the composition was 30%, thereby preparing a resin composition. The bending resistance of the obtained resin composition was evaluated by the above method. The results are shown in Table 5.
[0371] [Table 1]
[0372]
[0373] [Table 2]
[0374]
[0375]
[0376] [Table 4]
[0377]
[0378] [Table 5]
[0379]
[0380] According to Table 3, the resin solutions of Examples 1 to 8 have both excellent heat coloration resistance and high refractive index. In Examples 7 and 8 to which inorganic fine particles were further added, improved heat coloration resistance and higher refractive index were shown.
[0381] As shown in the comparative examples, the resin containing resin solution (B-1) has extremely poor heat coloration resistance due to the presence of ammonium salt (Comparative Example 1). The resin containing no skeleton of the above formula (1) such as resin solution (B-2) has a low refractive index (Comparative Example 2). The resin having a high Gardner chromaticity of the raw material such as resin solution (B-3) has extremely poor heat coloration resistance (Comparative Example 3). In addition, the resin of this example shows a high refractive index at a level that cannot be achieved in an acrylic resin such as resin solution (B-4).
[0382] As can be seen from Table 4, the resin composition using the resin solution of the example has the characteristics of being faster in development speed and less in residue, compared with the resin composition using the acrylic resin.
[0383] According to Table 5, the resin composition using the resin solution of the example has better bending resistance than the resin composition using the resin solution of the comparative example. This is considered to be because the resin using a raw material with a large Gardner chromaticity is easily oxidatively degraded and becomes brittle.
[0384] In addition, in the comparison between the embodiments, compared with the resin combination of the resin solution A-3 using methylhydroquinone as a polymerization inhibitor, the resin combination of the resin solutions A-1 and A-7 using hydroquinone as a polymerization inhibitor has good bending resistance. The hydroquinone present in the resin combination is different from methylhydroquinone in that it does not have a substituent other than the phenolic hydroxyl group, and is not subject to steric hindrance, so it is believed that 2 phenolic hydroxyl groups are easily interacted with the resin backbone separately. Therefore, it is believed that it is more likely to play a role as a buffer material between the resin backbones, and has an advantage in improving flexibility.
[0385] In addition, although not shown in the table, the voltage holding ratio of the display device including the color filter made using the resin solutions (A-1) to (A-7) as materials was good. In contrast, when the resin solution (B-1) was used, it was found that the ionic compound seeped into the liquid crystal layer and the voltage holding ratio was extremely deteriorated.
Claims
1. An alkali-soluble resin having a structure represented by the following formula (1), characterized in that: The alkali-soluble resin has an ammonium salt compound content of 0.06% by mass or less relative to 100% by mass of the alkali-soluble resin. [Chemistry 1] In formula (1), R 1 , R 2 and R 3 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 6 carbon atoms; R 4 Represents a direct bond or a divalent organic group; R 5 , R 6 , R 7 and R 8 Same or different, represents hydrogen atom or Y, R 5 ~R 8 At least one of them is Y; the Y is a group represented by the following formula (2); R 9 and R 10 are the same or different and represent a substituent; W represents a divalent organic group; X represents a direct bond or a divalent organic group; l represents R 9 The number of is an integer from 0 to 4; m represents R 10 The number of is an integer from 0 to 4; R 9 and R 10 When there are 2 or more, they are the same or different; n represents an integer greater than 1, [Chemistry 2] In formula (2), R 11 It represents a divalent organic group which may have a substituent.
2. An alkali-soluble resin composition, characterized in that The invention comprises the alkali-soluble resin according to claim 1 and epoxy (meth)acrylate containing an acid group.
3. A method for producing an alkali-soluble resin, characterized in that: The method for preparing the alkali-soluble resin comprises: A step (a-1) of reacting a bifunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90° C. or higher obtained in accordance with JIS K 0071-2 with a bisphenol compound; a step (a-2) of reacting the reaction product obtained in the step (a-1) with an unsaturated monobasic acid; and a step (a-3) of reacting the reaction product obtained in the step (a-2) with a polybasic acid anhydride, In the alkali-soluble resin obtained by this production method, the content of the ammonium salt compound is 0.06% by mass or less relative to 100% by mass of the alkali-soluble resin.
4. A method for producing an alkali-soluble resin composition, characterized in that: The method for preparing the alkali-soluble resin composition comprises: A step (b-1) of reacting a bifunctional epoxy compound having a Gardner color of less than 12 and a melting point of 90° C. or higher obtained in accordance with JIS K 0071-2 with a bisphenol compound; A step (b-2) of adding an epoxy resin to the reaction product obtained in the step (b-1); a step (b-3) of reacting the mixture obtained in the step (b-2) with an unsaturated monobasic acid; and a step (b-4) of reacting the reaction mixture obtained in the step (b-3) with a polybasic acid anhydride, In the alkali-soluble resin composition obtained by this production method, the content of the ammonium salt compound is 0.06% by mass or less relative to 100% by mass of the alkali-soluble resin.
5. The method for producing an alkali-soluble resin composition according to claim 4, wherein: The epoxy resin is an aromatic epoxy resin.
6. The method for producing an alkali-soluble resin composition according to claim 5, wherein: The aromatic epoxy resin is a bisphenol A type epoxy resin.
Citation Information
Patent Citations
Photosensitive resin composition for image formation and method for preparing the same
JP2008250306A
Photosensitive resin composition for image formation
JP2008250307A
Curable resin composition and its use
JP2013227485A
Curable resin composition and use of the same
JP2015157909A
Tetramethylbiphenol type epoxy resin, epoxy resin composition, cured product and semiconductor sealing material
JP2016108562A